A UV regeneration process for TiO2-modified CHA molecular sieve membranes used for dehydration in highly polar solvents

By constructing a TiO2 coating on the surface of a molecular sieve membrane and combining it with ultraviolet light regeneration technology, the problem of easy fouling of molecular sieve membranes during dehydration in highly polar solvents was solved, achieving efficient separation and green regeneration, and extending the service life of the membrane.

CN123102170APending Publication Date: 2026-11-17NANJING TECH UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610521045.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-04-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing molecular sieve membranes are prone to fouling during dehydration in highly polar solvents. Traditional regeneration methods are ineffective and damage the membrane structure, leading to flux decline and reduced separation performance.

Method used

A TiO2 coating is constructed on the surface of a molecular sieve membrane. Combined with ultraviolet light irradiation, the TiO2 coating generates active species under ultraviolet light to oxidize and degrade organic pollutants, inhibit the adsorption of strongly polar solvents, and achieve membrane regeneration under mild conditions.

Benefits of technology

It improves the pervaporation stability and regeneration performance of molecular sieve membranes during dehydration in highly polar solvents, extends the membrane's service life, and requires no chemical reagents, making it green and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102170A_ABST
    Figure CN123102170A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of membrane separation technology and discloses a UV-regenerated metal oxide-modified molecular sieve composite membrane and its preparation method and regeneration process. The composite membrane uses a CHA-type molecular sieve membrane as a substrate, with an outer surface loaded with a layer of IVB group metal oxides such as TiO2 for modification. Chemical anchoring is achieved through hydroxyl sites regulated by the silicon-to-aluminum ratio. The preparation method includes preparing a metal oxide sol using a sol-gel method, coating, and drying / calcining. This composite membrane is used for pervaporation dehydration of highly polar solvents. When contamination leads to flux decline, in-situ regeneration can be achieved using UV irradiation to restore hydrophilicity and separation performance. This invention solves the problem of irreversible performance degradation caused by contamination in traditional molecular sieve membranes through the synergistic effect of molecular sieve pore sieving, hydroxyl anchoring, and photocatalysis. It has the advantages of simple operation, environmental friendliness, and long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of membrane separation technology, specifically to a method for preparing TiO2-modified molecular sieve membranes for dehydration of strongly polar solvents and a UV regeneration process. Background Technology

[0002] Strongly polar organic solvents (such as NMP and DMF) are widely used in chemical, pharmaceutical, and electronics industries. During their production and recycling, dehydration treatment is often required to meet process requirements. Pervaporation technology, as a highly efficient membrane separation technology, has advantages such as low energy consumption, high separation efficiency, and simple operation, and has become an important means of dehydrating strongly polar solvents.

[0003] CHA molecular sieve membranes, due to their regular microporous structure and excellent thermal and chemical stability, have shown great application potential in solvent dehydration. However, during long-term contact with highly polar solvents, the surface and pores of the molecular sieve membrane easily adsorb solvent molecules or organic impurities, leading to decreased membrane hydrophilicity and pore blockage. This manifests as a significant decrease in flux, reduced separation performance, and membrane fouling.

[0004] TiO2, as a typical photocatalytic material, can generate electron-hole pairs with strong oxidizing properties under ultraviolet light irradiation, which are then converted into hydroxyl radicals (·OH) and superoxide anions (·O2). - These active species can both oxidize and degrade organic pollutants and form hydroxyl groups (-OH) on the TiO2 surface, enhancing the membrane's hydrophilicity. Studies have shown (J.Membr. Sci., 2000, 179, 185-205) that dimethylformamide (DMF) and water compete for adsorption on the molecular sieve membrane surface, and that DMF interacts with Na+ in the molecular sieve cages. + Strong electrostatic interactions exist between them, easily clogging water channels and leading to a decrease in flux. CN108014654B discloses a method for preparing a TiO2-modified NaA molecular sieve membrane and its application. This patent obtains a TiO2-modified NaA molecular sieve membrane by impregnating a NaA-type molecular sieve membrane with TiO2 sol and then calcining it. This membrane is used for pervaporation dehydration of low-concentration ethanol aqueous solutions, which can improve the membrane's separation factor and flux. Existing regeneration technologies for molecular sieve membranes used for dehydration of strongly polar solvents mainly rely on high-temperature regeneration or chemical cleaning methods. These methods generally suffer from high energy consumption, easy damage to the membrane structure, and long regeneration cycles. Currently, research on TiO2-modified molecular sieve membranes focuses on hydrophilicity control and separation performance improvement, while there is still a gap in the design of dedicated membranes, systematic preparation processes, and regeneration processes for dehydration scenarios using strongly polar solvents, which urgently require further research and improvement. Summary of the Invention

[0005] The purpose of this invention is to provide a method and regeneration process for preparing a UV-regenerated TiO2-modified molecular sieve membrane for dehydration in strongly polar solvents. This addresses the problems of existing molecular sieve membranes being prone to fouling during dehydration in strongly polar solvents, and the poor effectiveness and structural damage caused by traditional regeneration methods. The invention achieves efficient separation and green regeneration of the membrane, and extends its service life. The processing method of this invention is simple to operate, operates under mild conditions, and can improve the stability of the molecular sieve membrane during the pervaporation process of strongly polar solvents. To achieve the technical objective of this invention, the following technical solution is adopted: TiO2 sol is used to coat and modify the surface of the molecular sieve membrane, constructing a dense barrier layer on the membrane surface that possesses both high hydrophilicity and high photocatalytic activity. This barrier layer can selectively adsorb water molecules, inhibit the interaction between strongly polar solvent molecules and the membrane substrate, and, under UV irradiation, oxidize and degrade organic pollutants adsorbed on the membrane surface and within the pores. This significantly improves the pervaporation stability and regeneration performance of the molecular sieve membrane during the dehydration process of strongly polar solvents.

[0006] The first aspect of the present invention provides: A UV-regenerated metal oxide-modified molecular sieve membrane for dehydration of highly polar solvents, wherein the surface of the molecular sieve membrane has a metal oxide modification layer.

[0007] In one embodiment, the metal oxide is a metal oxide that combines strong hydrophilicity with ultraviolet light responsiveness.

[0008] In one embodiment, the strong hydrophilicity refers to the contact angle of water droplets on the surface of the metal oxide modified layer being less than 90°, more preferably less than 70°, and even more preferably less than 40°; the ultraviolet light responsiveness refers to the ability of the metal oxide to generate hydroxyl radicals (·OH) and superoxide anions (·O2) under ultraviolet light irradiation at a wavelength of 365 nm. - Active species such as )

[0009] In one embodiment, the metal is selected from group IVB metals; more preferably, it is titanium (Ti) or zirconium (Zr); even more preferably, it is titanium, and the corresponding metal oxide is TiO2.

[0010] In one embodiment, the molecular sieve membrane is made of inorganic molecular sieve material.

[0011] In one embodiment, the thickness of the metal oxide modification layer is between 0.01 and 10 µm; the metal oxide is uniformly dispersed in the modification layer without obvious agglomeration.

[0012] In one embodiment, the strongly polar solvent includes one or a mixture of several amide solvents and sulfone solvents.

[0013] A second aspect of the present invention provides: A method for preparing an ultraviolet-regenerated metal oxide-modified molecular sieve membrane as described in the first aspect above includes the following steps: i) Preparation of metal oxide sols; ii) Apply metal oxide sol to the surface of the molecular sieve membrane; iii) The coated molecular sieve membrane is subjected to drying and calcination treatments in sequence.

[0014] In one embodiment, the metal oxide sol in step i) is prepared by the sol-gel method; when the metal oxide is TiO2, the sol preparation process is as follows: mix tetrabutyl titanate: anhydrous ethanol: deionized water in a volume ratio of 0.5:10:0.2, add 0.5 ml of acetic acid to the mixture, stir magnetically for 30 min, and let stand for 4 h to obtain a uniform and transparent TiO2 sol.

[0015] In one embodiment, step ii) involves applying the sol to the surface of the molecular sieve membrane by a coating method such as soaking, spraying, or suction.

[0016] In one embodiment, the drying process in step iii) is carried out at 70–150 °C for 1–24 h.

[0017] A third aspect of the invention provides: A regeneration process for UV-regenerated molecular sieve membranes used for dehydration in highly polar solvents includes the following steps: a) Pretreatment of fouled membrane: The metal oxide modified molecular sieve membrane that was contaminated during the dehydration process of the strongly polar solvent was rinsed with deionized water to remove the residual solvent-water solution on the surface, thus obtaining the pretreated fouled membrane. b) Regeneration by ultraviolet light irradiation: Fix the pretreated contaminated membrane on the ultraviolet light irradiation frame, adjust the wavelength of the ultraviolet lamp to 365 nm, the distance between the ultraviolet lamp and the membrane to 3-15 cm, and the irradiation time to 0.5-2 h.

[0018] c) Post-treatment of regenerated membrane: After UV irradiation, rinse the membrane surface with deionized water to remove degradation products; after rinsing, place it in a drying oven and dry at 60-80 ℃ for 1-4 h to obtain the regenerated metal oxide modified molecular sieve membrane.

[0019] In one embodiment, the ultraviolet lamp power described in step b) is 10 to 50 W.

[0020] In one embodiment, the irradiation time in step b) is adjusted according to the degree of membrane fouling: for mild fouling (flux attenuation rate 10-20%), the irradiation time is 0.5-1 h; for moderate fouling (flux attenuation rate 20-30%), the irradiation time is 1-1.5 h; and for severe fouling (flux attenuation rate >30%), the irradiation time is 1.5-2 h.

[0021] A fourth aspect of the present invention provides: A method for dehydrating a highly polar solvent includes the following steps: using a molecular sieve membrane modified with an ultraviolet light-regenerating metal oxide as described in the first aspect above for pervaporation dehydration; when the membrane flux decay rate reaches 10% or more, using the regeneration process described in the third aspect above to regenerate the membrane, and then using the regenerated membrane in the dehydration process.

[0022] A fifth aspect of the present invention provides: The application of the ultraviolet light regenerable metal oxide modified molecular sieve membrane described in the first aspect above in the dehydration process of highly polar solvents. The beneficial effects of this invention are as follows: After surface modification of the molecular sieve membrane using the method of this invention, a TiO2 nano-coating with a thickness of 0.01–10 µm is formed on the membrane surface. This coating, while maintaining hydrophilicity, can selectively adsorb water molecules during pervaporation, blocking direct contact between strongly polar solvents and the molecular sieve surface, inhibiting the adsorption of solvent molecules on the membrane surface and within the pores, and weakening the electrostatic interaction between cations and solvent molecules in the molecular sieve cages, thereby reducing membrane fouling at its source. Simultaneously, this invention innovatively combines the photocatalytic properties of TiO2 to design an ultraviolet light regeneration process, eliminating the need for chemical reagents such as acids, alkalis, or organic solvents, resulting in no secondary pollution and environmental friendliness. The modified coating exhibits high bonding strength with the membrane substrate, and the regeneration process does not damage the membrane structure. Currently, there is a lack of efficient regeneration methods to address the problem of short lifespan of molecular sieve membranes in strongly polar solvent pervaporation dehydration applications. This invention proposes for the first time a regeneration method that can be completed rapidly under mild conditions. The breakthrough of this method lies in its ability to efficiently remove contaminants from within the membrane, fundamentally extending the membrane's lifespan. Attached Figure Description

[0023] Figure 1 The images show SEM images of the surface and cross-section of the modified CHA molecular sieve membrane from Example 2.

[0024] Figure 2 The images show SEM images of the CHA molecular sieve membrane obtained in Example 2 before and after modification, after a 365-hour pervaporation experiment, and after regeneration treatment with ultraviolet light irradiation.

[0025] Figure 3The permeation flux decay curve of the CHA molecular sieve membrane modified with TiO2 but without UV irradiation after continuous operation for 700 h in a 10 wt.% water / NMP system at 90 ℃ is used to compare with the long-term stability of the TiO2-modified + UV-regenerated membrane.

[0026] Figure 4 , 5 Figures 1 and 6 show the flux attenuation and recovery performance of the molecular sieve membranes in Examples 1, 2 and 3 during long-term operation.

[0027] Figure 7 This shows the change in the contact angle of the molecular sieve membrane before and after ultraviolet irradiation treatment in Example 2. Detailed Implementation

[0028] This invention involves coating a molecular sieve membrane with a layer of micro / nano-scale, highly hydrophilic TiO2 metal oxide. The high hydrophilicity refers to a contact angle of water droplets on the metal oxide surface of less than 90°, more preferably less than 70°, and even more preferably less than 40°. Furthermore, this TiO2 coating exhibits UV-responsive properties, allowing for flux regeneration of the fouled membrane through UV irradiation. On one hand, N-methylpyrrolidone (NMP) can be adsorbed onto the TiO2 metal oxide coating surface, preventing its accumulation at the molecular sieve membrane pores and subsequent clogging. On the other hand, the high hydrophilicity of the TiO2 metal oxide coating ensures rapid water permeation. Combined with the UV regeneration function, this effectively mitigates flux decline caused by membrane fouling, resulting in a composite membrane with high separation performance and excellent long-term operational stability. Specifically, the molecular sieve membrane containing hydroxyl groups is treated using a sol-gel method and an dip-coating method to coat the membrane surface with a micro / nano-scale metal oxide coating, thereby improving its pervaporation stability in highly polar solvents.

[0029] There are no particular limitations on the molecular sieve membranes mentioned above. They are mainly inorganic material molecular sieves, such as NaA, T-type, CHA, ZSM-5, MOR, and NaY molecular sieve membranes, with CHA molecular sieve membranes being more preferred.

[0030] The TiO2 metal oxide layer on the surface of the molecular sieve membrane can be prepared by sol-coating method. A titanium-containing sol is coated on the surface of the molecular sieve membrane, and after drying, a stable TiO2 metal oxide layer is formed on the membrane surface.

[0031] The sol here can be prepared using conventional sol-gel methods. Taking titanium as an example, it involves the hydrolysis, polymerization, and dehydration of a titanium precursor in solution to obtain the corresponding metal oxide sol. There are no particular restrictions on how the sol is applied to the surface of the molecular sieve membrane; it can be applied by immersion, spraying, or suction. To improve the coating effect, the process can be repeated multiple times. The drying step can be performed at 70–150 °C for 1–24 h.

[0032] The ultraviolet light irradiation regeneration process here can be achieved using a conventional ultraviolet light irradiation device: the wavelength of the ultraviolet light can be set to 365 nm, the power of the ultraviolet lamp is 10–50 W, the irradiation distance can be controlled at 3–15 cm, and the irradiation time is 0.5–2 h; after the ultraviolet light irradiation is completed, the membrane surface is rinsed with deionized water to remove the pollutant products generated by photocatalytic degradation; after rinsing, the membrane is placed in a drying oven and dried at 60–80 ℃ for 1–4 h to obtain the regenerated metal oxide modified molecular sieve membrane.

[0033] The aforementioned molecular sieve membrane is suitable for dehydration processes using highly polar solvents, overcoming the problems of flux reduction and poor operational stability caused by the adsorption of highly polar solvents on the membrane surface. Applicable organic solvents include one or a mixture of several of amide, alcohol, nitrile, amine, ether, or sulfone solvents. In the dehydration process using highly polar solvents, the aforementioned molecular sieve membrane exhibits advantages such as increased filtration flux and good operational stability.

[0034] Methods for testing the pervaporation performance of molecular sieve membranes: The pervaporation performance of a membrane is typically measured by the permeate flux passing through a unit membrane area per unit time. J (kg / m 2 ·h) and separation factor α Two parameters are used to measure it. α and J The definition is as follows:

[0035] In the formula y i and y j These represent the mass fractions of organic matter and water on the osmotic side, respectively. x i and x j These represent the mass fractions of organic matter and water in the raw materials, respectively.

[0036]

[0037] In the formula Indicates the quality of the permeate. SIndicates the membrane area. t Indicates the infiltration time.

[0038] Example 1 The CHA molecular sieve membrane was tested in a pervaporation apparatus. The test conditions were: feed liquid 10 wt.% water / ethanol, temperature 75 ℃, downstream pressure 95 Pa. The measured permeation flux was 0.20 kg m⁻² h⁻¹, and the separation factor was 1054.

[0039] 2.5 ml of tetrabutyl titanate was uniformly dissolved in 50 ml of ethanol. 0.5 ml of acetic acid was added to the mixture, and 1 ml of deionized water was slowly added dropwise while stirring vigorously to obtain a TiO2 sol. The CHA molecular sieve membrane was vertically placed in the TiO2 sol and treated at 20 °C for 5 min, then the process was repeated once. The modified CHA molecular sieve membrane was washed with deionized water and then dried in an oven at 100 °C for 24 h.

[0040] The dried molecular sieve membrane was subjected to stability testing in a pervaporation unit. Test conditions: feed solution 10 wt.% water / NMP, temperature 90 ℃, downstream pressure 98 Pa, and the initial flux was measured to be 0.42 kg / m³. 2 The flux was 0.27 kg / m³ after 335 h. 2 h, separation factor 8634, flux decay rate 36%.

[0041] The contaminated CHA membrane was rinsed with deionized water and then fixed on a UV irradiation frame. The irradiation distance was adjusted and the membrane was irradiated for 0.5 h. The irradiated CHA membrane was then subjected to a stability test under the following conditions: feed solution 10 wt.% water / NMP, temperature 90℃, downstream pressure 95 Pa. The measured permeation flux was 0.31 kg / m³. 2 •h, separation factor 8377, flux recovery rate 74%. Continue to carry out multiple cycles of ultraviolet irradiation, each round of irradiation operation can achieve a certain degree of regeneration and recovery of membrane flux. Example

[0042] The performance of the CHA molecular sieve membrane was tested in a pervaporation unit. The test conditions were: feed solution of 10 wt.% water / ethanol, temperature of 75 ℃, downstream pressure of 114 Pa, and the measured permeation flux was 1.0 kg / m³. 2 ·h, separation factor 1135.

[0043] 2.5 ml of tetrabutyl titanate was uniformly dissolved in 50 ml of ethanol. 0.5 ml of acetic acid was added to the mixture, and 1 ml of deionized water was slowly added dropwise while stirring vigorously to obtain a TiO2 sol. The CHA molecular sieve membrane was vertically placed in the TiO2 sol and treated at 20 °C for 5 min. This process was repeated twice. The modified CHA molecular sieve membrane was then washed with deionized water and dried in an oven at 100 °C for 24 h.

[0044] The dried molecular sieve membrane was subjected to stability testing in a pervaporation unit. Test conditions: feed solution 10 wt.% water / NMP, temperature 90 ℃, downstream pressure 98 Pa, and the initial flux was measured to be 1.73 kg / m³. 2 The flux is 1.57 kg / m³ after 365 hours. 2 h, separation factor 6987, flux decay rate 9%.

[0045] The contaminated CHA membrane was rinsed with deionized water and then fixed on a UV irradiation frame. The irradiation distance was adjusted, and the membrane was irradiated for 0.5 h. The irradiated CHA membrane was then subjected to a stability test in a pervaporation apparatus. The test conditions were: feed solution 10 wt.% water / NMP, temperature 90 ℃, downstream pressure 147 Pa. The measured permeation flux was 1.63 kg / m³. 2 •h, separation factor 6748, flux recovery rate 94%. Continue to carry out multiple cycles of ultraviolet irradiation, each round of irradiation operation can achieve a certain degree of regeneration and recovery of membrane flux. Example

[0046] The performance of the CHA molecular sieve membrane was tested in a pervaporation unit. The test conditions were: feed liquid 10 wt.% water / ethanol, temperature 75 ℃, downstream pressure 130 Pa, and the measured permeation flux was 0.27 kg / m³. 2 ·h, separation factor 1079.

[0047] 2.5 ml of tetrabutyl titanate was uniformly dissolved in 50 ml of ethanol. 0.5 ml of acetic acid was added to the mixture, and 1 ml of deionized water was slowly added dropwise while stirring vigorously to obtain a TiO2 sol. The CHA molecular sieve membrane was vertically placed in the TiO2 sol and treated at 20 °C for 5 min. This process was repeated three times. The modified CHA molecular sieve membrane was then washed with deionized water and dried in an oven at 100 °C for 24 h.

[0048] The dried molecular sieve membrane was subjected to stability testing in a pervaporation unit. The test conditions were: feed liquid of 10 wt.% water / NMP, temperature of 90 ℃, downstream pressure of 110 Pa, and the initial flux was measured to be 0.55 kg / m³. 2The permeability flux was measured to be 0.30 kg / m³ after 335 h. 2 h, separation factor 4081, flux decay rate 45%.

[0049] The contaminated CHA membrane was rinsed with deionized water and then fixed on a UV irradiation frame. The irradiation distance was adjusted, and the membrane was irradiated for 0.5 h. The irradiated CHA membrane was then subjected to a stability test in a pervaporation apparatus. The test conditions were: feed solution of 10 wt.% water / NMP system, temperature of 90 ℃, downstream pressure of 130 Pa, and the measured permeation flux was 0.47 kg / m³. 2 •h, separation factor 3791, flux recovery rate 85%. Continue to carry out multiple cycles of ultraviolet irradiation, each round of irradiation operation can achieve a certain degree of regeneration and recovery of membrane flux. Comparative Example 1 To visually compare the modification and regeneration effects, compared with Example 1, the permeation flux change of the original CHA molecular sieve membrane modified with TiO2 and without UV irradiation was tested under the same conditions (10 wt.% water / NMP, 90 ℃) for 700 h of continuous operation. The results are as follows: Figure 3 As shown. The initial flux was 1.24 kg / m³. 2 Due to the lack of ultraviolet light regeneration treatment, adsorbed organic pollutants continued to accumulate during operation, and the flux decreased continuously with the extension of operating time. After 700 hours, the permeation flux was measured to be only 0.60 kg / m³. 2 •h, flux decay rate reaches 52%, separation factor 3179. Comparative Example 2 Chemical cleaning and regeneration method was adopted: The CHA molecular sieve membrane to be regenerated after being contaminated by NMP was completely immersed in a 50% ethanol / water mixed solution and statically soaked for 4 h at room temperature and normal pressure. After soaking, the membrane surface and membrane pores were repeatedly rinsed with deionized water, and then the membrane was placed in a 60 ℃ vacuum drying oven for 24 h to complete the chemical cleaning and regeneration.

[0050] The regenerated CHA molecular sieve membrane was used to test the pervaporation stability of a 10 wt.% water / NMP mixture at an operating temperature of 90 °C. The results showed that the membrane's permeate flux recovered to only 5% of the initial flux of a new membrane. In comparison, the regeneration method of this invention has advantages in terms of membrane flux recovery and membrane structure protection.

Claims

1. A UV-regenerated metal oxide-modified molecular sieve composite membrane, characterized in that, The composite membrane includes a molecular sieve membrane substrate and a metal oxide modification layer loaded on the outer surface of the molecular sieve membrane. The metal oxide modification layer has ultraviolet light responsive activity, and the composite membrane can reversibly restore its hydrophilicity and pervaporation separation performance after being irradiated with ultraviolet light.

2. The composite membrane according to claim 1, characterized in that, The metal oxide is selected from oxides of group IVB metals; preferably, the metal oxide is TiO2 or ZrO2; more preferably, it is TiO2; The molecular sieve membrane substrate is selected from CHA type, T type, NaA type, ZSM-5 type, MOR type or NaY type molecular sieve membranes; preferably, it is a CHA type molecular sieve membrane. The CHA-type molecular sieve membrane has a silicon-to-aluminum ratio of 1-10, preferably 2-6; and / or, the CHA-type molecular sieve membrane has an octagonal ring cross-channel structure with a pore size of 0.3-0.4 nm.

3. The composite membrane according to claim 1, characterized in that, The thickness of the metal oxide modification layer is 0.005-20 μm, preferably 0.01-10 μm; After the composite film is irradiated with ultraviolet light, the contact angle of water droplets on the surface of the modified layer is less than 90°, preferably less than 70°, and more preferably less than 40°. The metal oxide modified layer is chemically anchored to the substrate surface through hydroxyl sites in the molecular sieve membrane framework, and the hydroxyl sites are modulated by the silicon-to-aluminum ratio of the molecular sieve membrane.

4. A method for preparing the ultraviolet-regenerated metal oxide-modified molecular sieve composite membrane according to any one of claims 1-3, characterized in that, Includes the following steps: Preparation of metal oxide sols; The metal oxide sol is applied to the surface of the molecular sieve membrane; The coated molecular sieve membrane is then dried and calcined.

5. The method according to claim 4, characterized in that, The metal oxide sol in step (i) is prepared by the sol-gel method; when the metal oxide is TiO2, the preparation of the sol includes: mixing tetrabutyl titanate, anhydrous ethanol and deionized water at a volume ratio of 0.5: (15-20): (0.1-0.3), adding acetic acid, stirring magnetically and then allowing it to stand for aging to obtain TiO2 sol.

6. The method according to claim 4, characterized in that, The application method in step (ii) is selected from immersion, spraying, or suction; preferably, the coating is performed at 10-40°C for a preset time and repeated 1-5 times; The drying and calcining temperature in step (iii) is 50-200℃, preferably 70-150℃; the drying and calcining time is 0.5-48h, preferably 1-24h.

7. A regeneration method for improving the pervaporation stability of the ultraviolet-regenerated metal oxide-modified molecular sieve composite membrane according to any one of claims 6, characterized in that, During or after the process of using the composite membrane for dehydration with a highly polar solvent, the composite membrane is subjected to ultraviolet light irradiation treatment to restore and maintain its separation performance. The wavelength of the ultraviolet light irradiation is 200-400nm, preferably 300-400nm, and more preferably 365nm; the power of the ultraviolet light source is 5-100W, preferably 10-50W; the distance between the ultraviolet light source and the film surface is 1-30cm, preferably 3-15cm; and the irradiation time is 0.1-5h, preferably 0.5-2h.

8. The regeneration method according to claim 7, characterized in that, The irradiation time is determined according to the degree of membrane fouling: when the flux decay rate is 10-20%, the irradiation time is 0.5-1h; when the flux decay rate is 20-30%, the irradiation time is 1-1.5h; when the flux decay rate is greater than 30%, the irradiation time is 1.5-2h. The regeneration method is carried out in a periodic cycle mode, which is an alternating cycle of operation and ultraviolet light regeneration.

9. The regeneration method according to claim 7, characterized in that, The process before ultraviolet light irradiation includes a pretreatment step of rinsing the membrane surface with deionized water to remove residual solvent-water solution; the process after ultraviolet light irradiation includes a posttreatment step of rinsing the membrane surface with deionized water and drying it at 40-100℃ for 0.5-8 hours.

10. The application of the ultraviolet light regenerating metal oxide modified molecular sieve composite membrane as described in any one of claims 1-3 in organic solvent pervaporation dehydration.

Citation Information

Patent Citations

  • A method for modifying molecular sieve membranes for dehydration separation of highly polar solvents

    CN108014654B