A bamboo-based cellulose and lignin biochar aerogel composite adsorbent, its preparation method and application

By preparing a composite adsorbent of bamboo-based cellulose and lignin biochar aerogel, the problems of underdeveloped pore structure and weak loading of poly(VI) in bamboo-based biochar materials were solved, achieving efficient adsorption and regeneration of U(VI) and meeting the needs of radioactive wastewater treatment.

CN123102301APending Publication Date: 2026-11-17NANHUA UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611454592.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing bamboo-based biochar materials do not adequately utilize the synergistic effects of cellulose and lignin during preparation, resulting in underdeveloped pore structures, poor pore connectivity, and limited intrinsic adsorption capacity for U(VI), making it difficult to meet the requirements for radioactive wastewater treatment. In addition, the polyamine oxime is not firmly loaded, affecting adsorption performance and regeneration.

Method used

Cellulose in bamboo is extracted by peroxyformic acid treatment, mixed with lignin and carbonized to form a porous biochar framework, and then loaded with polyamine oxime to form a bamboo-based cellulose and lignin biochar aerogel composite adsorbent. The porous structure is constructed by the synergistic effect of cellulose and lignin, and polyamine oxime is stably loaded on the biochar framework.

Benefits of technology

This improves the adsorption selectivity and capacity of the material for U(VI), forms porous mass transfer channels, enhances adsorption efficiency, and the composite adsorbent can be reused, showing promise for regeneration applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102301A_ABST
    Figure CN123102301A_ABST
Patent Text Reader

Abstract

This invention relates to a bamboo-based cellulose and lignin biochar aerogel composite adsorbent, its preparation method, and its applications. The invention pertains to the fields of biomass resource utilization and radioactive wastewater treatment. The preparation method includes: using bamboo as raw material, treating it with formic acid and washing it with alkali to obtain self-extracted cellulose; mixing the self-extracted cellulose with lignin and carbonizing it under an inert atmosphere to obtain biochar material; dissolving poly(xylene)amine oxime in an alkaline solution and aging it, mixing it with the biochar material, adding glutaraldehyde for crosslinking, washing, and freeze-drying to obtain the aerogel composite adsorbent. This invention utilizes the cellulose framework support and the carbon-rich char-forming properties of lignin to construct a porous carbon material, and introduces xylene oxime groups to enhance the complexation and adsorption capacity for U(VI). This composite adsorbent can be used for uranium-containing wastewater treatment, has abundant raw material sources, tunable pore structure, multiple adsorption sites, and has potential for regenerative applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the fields of biomass resource utilization and radioactive wastewater treatment, and in particular to a bamboo-based cellulose and lignin biochar aerogel composite adsorbent, its preparation method, and its application. Background Technology

[0002] With the development of nuclear energy technology, nuclear fuel cycle technology, and the nuclear industry, radioactive wastewater treatment has become an important research area in environmental protection. Uranium is a common radioactive pollutant in nuclear wastewater, mainly existing in the form of hexavalent uranium (U(VI)) in the aquatic environment. It poses radioactive hazards and chemical toxicity, and direct discharge without effective treatment will have adverse effects on the ecological environment and human health. Currently, methods for removing U(VI) from wastewater mainly include chemical precipitation, ion exchange, membrane separation, electrochemical methods, and adsorption. Among these, adsorption has received widespread attention due to its simple process, convenient operation, wide applicability, and relatively low secondary pollution. Existing materials for adsorbing U(VI) include activated carbon, mineral materials, polymer materials, metal oxide materials, and biomass-based carbon materials. However, these materials generally suffer from high preparation costs, underdeveloped pore structures, few effective adsorption sites, insufficient adsorption selectivity, or poor recycling performance, which limits their application in practical uranium-containing wastewater treatment.

[0003] Bamboo is an abundant, renewable biomass resource with a short growth cycle. Its main components include cellulose, hemicellulose, and lignin. Cellulose has a good fiber network structure, which can play a skeletal supporting role in the material construction process; lignin has a high carbon content and good char-forming properties, and can form a carbon skeleton during pyrolysis and carbonization. Theoretically, the synergistic use of cellulose and lignin can help improve the problems of agglomeration and unclear pores that easily occur during the carbonization of lignin alone. However, existing bamboo-based biochar materials often fail to make sufficient synergistic use of cellulose and lignin in the preparation process, or simply carbonize bamboo powder directly, or simply mix cellulose and lignin for pyrolysis. This results in materials with underdeveloped pore structure, poor pore connectivity, and limited intrinsic adsorption capacity for U(VI), making it difficult to meet the requirements of adsorption capacity and selectivity for radioactive wastewater treatment.

[0004] Poly(xyleneamine) oximes contain xyleneamine oxime groups, whose nitrogen and oxygen coordinating atoms can complex or coordinate with uranyl ions, thus they are considered promising functional components for improving the adsorption selectivity of U(VI). However, when poly(xyleneamine) oximes are used directly as adsorbents, they often suffer from low mechanical strength, easy swelling, and difficulty in recovery after adsorption. If they are simply loaded onto the surface of ordinary biochar materials, defects such as unstable loading, burying of active sites, pore blockage, or impaired mass transfer may occur, thus affecting adsorption performance and regeneration. Therefore, how to use bamboo as raw material, fully utilize the synergistic effect of cellulose and lignin to construct a biochar framework with a well-porous structure, and stably load poly(xyleneamine) oximes into this framework to form a biochar aerogel composite adsorbent with both porous mass transfer channels and abundant xyleneamine oxime adsorption sites for the removal of radioactive U(VI) from wastewater remains a technical problem to be solved in this field. Summary of the Invention

[0005] The purpose of this invention is to address the problems in the prior art by providing a bamboo-based cellulose and lignin biochar aerogel composite adsorbent, its preparation method, and its application.

[0006] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: a method for preparing a bamboo-based cellulose and lignin biochar aerogel composite adsorbent, comprising the following steps:

[0007] (1) After pretreatment of bamboo, it is added to a formic acid solution for treatment. After being taken out, it is soaked in an alkaline solution, washed with water until neutral, and dried to obtain self-extracted cellulose.

[0008] (2) Mix the self-extracted cellulose with lignin evenly to obtain a cellulose / lignin mixed precursor;

[0009] (3) The cellulose / lignin mixed precursor is carbonized under an inert atmosphere to obtain cellulose / lignin-based biochar material;

[0010] (4) Polyamine oxime (PAO) is dissolved in an alkaline solution and aged, then mixed with the cellulose / lignin-based biochar material, and glutaraldehyde is added for cross-linking. After washing and freeze-drying, bamboo-based cellulose and lignin biochar aerogel composite adsorbent is obtained.

[0011] Preferably, in step (1), the bamboo material is moso bamboo; the pretreatment is to cut the bamboo material and boil it for 1 hour.

[0012] More preferably, in step (1), the peroxyformic acid solution is prepared by mixing hydrogen peroxide and formic acid in a molar ratio of 1:1, and 1wt% sulfuric acid is added as a catalyst; the volume ratio of bamboo to peroxyformic acid solution is 1:10; the temperature of the peroxyformic acid solution treatment is 50°C, and the treatment time is 12h.

[0013] More preferably, in step (1), the alkaline solution is a sodium hydroxide solution with a mass concentration of 0.5 wt%, the soaking time is 5 to 10 minutes, and after washing with water until neutral, it is naturally air-dried at room temperature.

[0014] More preferably, in step (2), the lignin is dealkalized lignin; the mass ratio of the self-extracted cellulose to lignin is 2:1, 2:3, 2:5, or 2:7.

[0015] More preferably, in step (3), the inert atmosphere is nitrogen; the heating rate of carbonization is 5℃ / min, the carbonization temperature is 200~700℃, the holding time is 2h, and the preferred carbonization temperature is 600℃.

[0016] More preferably, in step (4), the poly(dimethylformamide) oxime is prepared by reacting polyacrylonitrile, hydroxylamine hydrochloride, sodium hydroxide and sodium carbonate in N,N-dimethylformamide, specifically including: dissolving hydroxylamine hydrochloride in N,N-dimethylformamide at 45°C, adding sodium hydroxide and sodium carbonate, stirring at 45°C for 1 h; adding polyacrylonitrile and dissolving for 15 min, then heating to 65°C and reacting for 24 h; adding N,N-dimethylformamide, hydroxylamine hydrochloride, sodium hydroxide and sodium carbonate, and continuing to react at 65°C for 24 h; centrifuging, dropping the supernatant into anhydrous ethanol to precipitate, collecting the precipitate and drying under vacuum to obtain poly(dimethylformamide) oxime.

[0017] More preferably, in step (4), the alkaline solution is a 0.3M sodium hydroxide solution; the mass ratio of the poly(glyoxime) to the cellulose / lignin-based biochar material is 10:1; the glutaraldehyde is a 50% glutaraldehyde solution, and the mixture is crosslinked until it is completely gelled.

[0018] In addition, the present invention also provides a bamboo-based cellulose and lignin biochar aerogel composite adsorbent, which is prepared by the above-mentioned preparation method; the composite adsorbent includes a cellulose / lignin-based porous biochar framework and polyamine oxime loaded on the surface and / or pores of the porous biochar framework.

[0019] This bamboo-based cellulose and lignin biochar aerogel composite adsorbent can be used to remove radioactive U(VI) from wastewater.

[0020] In this invention, whenever the expression "cellulose / lignin" appears, the " / " indicates "and," meaning that cellulose and lignin coexist and participate together, rather than one or the other being chosen. Specifically, "cellulose / lignin mixed precursor" refers to a precursor obtained by mixing self-extracted cellulose and lignin; "cellulose / lignin-based biochar material" refers to biochar material obtained by co-carbonizing cellulose and lignin; "cellulose / lignin-based porous biochar framework" refers to a porous biochar framework formed by the synergistic carbonization of cellulose and lignin; and "mass ratio of poly(xime) to cellulose / lignin-based biochar material" refers to the mass ratio between poly(xime) and the biochar material obtained by co-carbonizing cellulose and lignin.

[0021] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0022] (1) This invention uses bamboo as raw material and extracts self-extractable cellulose from bamboo through steps such as peroxyformic acid treatment and alkali washing. It also synergistically constructs biochar material with lignin, which is conducive to realizing the high-value utilization of bamboo resources. Moreover, the raw materials are widely available, renewable, and relatively low in cost.

[0023] (2) In this invention, self-extracted cellulose can form a fiber network skeleton during the material construction process, and lignin can participate in carbonization as a carbon-rich precursor. The synergistic effect of cellulose and lignin helps to form a richer pore structure, improves the problem of easy agglomeration and unclear pores when lignin is carbonized alone, and thus obtains a cellulose / lignin-based porous biochar skeleton with better pore structure.

[0024] (3) In this invention, polyamine oxime is loaded onto the surface and / or pores of a cellulose / lignin-based porous biochar framework, thereby giving the material surface and pores a polyamine oxime functional group. The nitrogen-containing and oxygen-containing coordination sites in the polyamine oxime group can complex or coordinate with uranyl ions, thereby improving the material's adsorption capacity and selectivity for U(VI).

[0025] (4) In this invention, poly(ammonia oxime) is mixed with biochar material and then crosslinked with glutaraldehyde. After washing and freeze-drying, an aerogel is prepared. The resulting composite adsorbent has both a porous carbon skeleton and functional adsorption sites, which is beneficial for mass transfer and contact of U(VI) inside the material and improves adsorption efficiency. At the same time, the aerogel morphology is beneficial for maintaining the porous structure of the material, which is convenient for use and recycling in water treatment.

[0026] (5) The composite adsorbent described in this invention can be reused after desorption treatment, and has certain prospects for regeneration applications. Experimental results show that the removal rate of U(VI) by biochar materials without poly(xime) loading is relatively limited, while the removal rate of U(VI) by the composite adsorbent loaded with poly(xime) loading is significantly improved, indicating that poly(xime) functionalization can effectively enhance the adsorption performance of materials for U(VI). Attached Figure Description

[0027] Figure 1 A photograph showing the appearance of the BC-600-CL3-PAO composite adsorbent prepared in Example 9 of this invention.

[0028] Figure 2 A comparison of U(VI) removal rates at different carbonization temperatures for biochar without added lignin and without polyamine oxime modification.

[0029] Figure 3 This is a comparison of the removal rates of U(VI) by unmodified biochar with different self-extracted cellulose to lignin mass ratios obtained at a carbonization temperature of 600℃.

[0030] Figure 4 The graph shows a comparison of the removal rates of U(VI) by composite adsorbents and pure poly(xime) aerogels obtained from biochar with different self-extracted cellulose to lignin mass ratios after modification with poly(xime) oxime at a carbonization temperature of 600℃. Detailed Implementation

[0031] The following examples are for illustrative purposes only and do not constitute a limitation on the scope of protection of this invention. Unless otherwise stated, all reagents used in the following examples are of analytical grade, and the water used is deionized water.

[0032] This invention first prepares cellulose / lignin-based biochar at different carbonization temperatures and investigates its adsorption performance for U(VI). After determining a suitable carbonization temperature, the mass ratio of self-extracted cellulose to lignin is further adjusted to screen biochar matrices with superior U(VI) adsorption performance. The materials obtained in the temperature and proportion screening stages were not loaded with poly(amine)oximes to eliminate the influence of PAO functional groups, and the effects of carbonization temperature and biomass composition on the pore structure and intrinsic adsorption performance of the biochar were investigated.

[0033] Example 1

[0034] Bamboo stems were selected and boiled for 1 hour. Performic acid solution (30% hydrogen peroxide to formic acid in a 1:10 molar ratio) was added, along with 1 wt% sulfuric acid as a catalyst. The reaction was carried out at 50°C for 12 hours. The bamboo fibers were then removed and soaked in 0.5 wt% NaOH solution for 5-10 minutes, followed by repeated rinsing with deionized water until neutral. Finally, the solution was air-dried at room temperature for 48 hours to obtain self-extracted cellulose. 0.2 g of the self-extracted cellulose was heated to 600°C at a rate of 5°C / min, held at that temperature for 2 hours, and then cooled to obtain biochar, named BC-600.

[0035] Example 2

[0036] The only difference between this embodiment and Embodiment 1 is the carbonization target temperature. Specifically, the carbonization target temperature in this embodiment is 200°C, and the final product is named BC-200.

[0037] Example 3

[0038] The only difference between this embodiment and Example 1 is the carbonization target temperature. Specifically, the carbonization target temperature in this embodiment is 300°C, and the final product is named BC-300.

[0039] Example 4

[0040] The only difference between this embodiment and Embodiment 1 is the carbonization target temperature. Specifically, the carbonization target temperature in this embodiment is 400°C, and the final product is named BC-400.

[0041] Example 5

[0042] The only difference between this embodiment and Example 1 is the carbonization target temperature. Specifically, the carbonization target temperature in this embodiment is 500°C, and the final product is named BC-500.

[0043] Example 6

[0044] The only difference between this embodiment and Embodiment 1 is the carbonization target temperature. Specifically, the carbonization target temperature in this embodiment is 700℃, and the final product is named BC-700.

[0045] Example 7

[0046] Bamboo stems were selected and boiled for 1 hour. Performic acid solution (30% hydrogen peroxide to formic acid in a 1:10 molar ratio) was added, along with 1 wt% sulfuric acid as a catalyst. The reaction was carried out at 50°C for 12 hours. The bamboo fibers were then removed and soaked in 0.5 wt% NaOH solution for 5-10 minutes, followed by repeated rinsing with deionized water until neutral. Finally, the mixture was air-dried at room temperature for 48 hours to obtain self-extracted cellulose. 0.2 g of self-extracted cellulose and 0.1 g of lignin were weighed and mixed thoroughly. The mixture was placed in a tube furnace and heated to 600°C at a rate of 5°C / min under a nitrogen atmosphere. After holding at this temperature for 2 hours, the mixture was naturally cooled to room temperature to obtain biochar material, designated BC-600-CL1.

[0047] Example 8

[0048] The preliminary steps of Example 6 were the same as those of Example 7. 0.2g of extracted cellulose and 0.3g of lignin were weighed and mixed thoroughly. The remaining steps were the same as in Example 7, yielding biochar material, denoted as BC-600-CL2.

[0049] Example 9

[0050] The preliminary steps were the same as in Example 7. 0.2g of extracted cellulose and 0.5g of lignin were weighed and mixed thoroughly. The remaining steps were the same as in Example 7, yielding biochar material, denoted as BC-600-CL3.

[0051] Example 10

[0052] The preliminary steps were the same as in Example 7. 0.2g of extracted cellulose and 0.7g of lignin were weighed and mixed thoroughly. The remaining steps were the same as in Example 7, yielding biochar material, denoted as BC-600-CL4.

[0053] Example 11

[0054] The initial steps of this embodiment are the same as in Example 9, yielding biochar material BC-600-CL3. 5.6 g of NH₂OH·HCl was dissolved in DMF (60 mL, 45°C), followed by 1.6 g of NaOH and 4.12 g of Na₂CO₃. The mixture was then stirred at 45°C for 1 hour. 4 g of PAN was then slowly added to the solution and allowed to dissolve completely over 15 minutes, after which the temperature was raised to 65°C. After 24 hours, 30 mL of DMF was added to the reaction flask, followed by 2.8 g of NH₂OH·HCl to dissolve completely. After 15 minutes, 0.8 g of NaOH and 2.06 g of Na₂CO₃ were successively added to the reaction flask, and the reaction was continued at 65°C for 24 hours. Finally, the reaction mixture was transferred to centrifuge tubes and centrifuged (11000 rpm, 25 minutes). Next, the supernatant was added dropwise to 1000 mL of anhydrous ethanol, and white particles precipitated under stirring. After 12 hours, the precipitate was collected by suction filtration and then dried in a vacuum oven (40°C, 12 hours) to obtain the prepared PAO. 0.2 g of PAO powder was added to 2 mL of 0.3 M NaOH solution, and the mixture was stirred until the PAO was completely dissolved to obtain a light yellow transparent solution. Next, the solution was allowed to stand at room temperature for 12 hours to obtain an aged PAO solution. 0.02 g of BC-600-CL3 was mixed with the above PAO solution by stirring. Then, 0.2 mL of 50% glutaraldehyde solution was immediately added to the suspension, and the mixture was stirred until it completely gelled. After washing and freeze-drying, an aerogel was prepared, designated BC-600-CL3-PAO. Its appearance is as follows. Figure 1 As shown, it appears as a black aerogel.

[0055] Comparative Example 1

[0056] The preliminary steps are the same as in Example 7. Weigh 0.2g of the self-extracted cellulose prepared in Example 1, without adding lignin, place it in a tube furnace, and heat it to 600℃ at a heating rate of 5℃ / min under a nitrogen protective atmosphere. After holding at this temperature for 2 hours, it is naturally cooled to room temperature to obtain pure cellulose biochar, denoted as BC-600-C.

[0057] Comparative Example 2

[0058] Weigh 0.2g of lignin without adding self-extracted cellulose, place it in a tube furnace, and heat it to 600℃ at a heating rate of 5℃ / min under a nitrogen protective atmosphere. After holding at this temperature for 2 hours, allow it to cool naturally to room temperature to obtain pure lignin biochar, denoted as BC-600-L.

[0059] Comparative Example 3

[0060] 0.2 g of PAO powder was added to 2 mL of 0.3 M NaOH solution, and the mixture was stirred until the PAO was completely dissolved to obtain a light yellow, transparent solution. Next, the solution was allowed to stand at room temperature for 12 hours to obtain an aged PAO solution. Then, 0.2 mL of 50% glutaraldehyde solution was immediately added to the solution, and the mixture was stirred until it completely gelled. After washing and freeze-drying, PAO aerogel was prepared.

[0061] Performance Testing and Effect Analysis

[0062] The materials obtained in the above examples and comparative examples were used in U(VI) adsorption experiments, and the results are as follows: Figures 2 to 4 As shown.

[0063] Depend on Figure 2 It is evident that for biochar without lignin addition and without polyamine oxime modification, carbonization temperature significantly affects the removal rate of U(VI). As the carbonization temperature increases from 200℃ to 600℃, the removal rate of U(VI) by biochar generally exhibits a fluctuating pattern of first increasing, then decreasing, and then increasing again. BC-300 and BC-600 show relatively high removal rates, with BC-600 exhibiting the highest removal rate. However, when the carbonization temperature is further increased to 700℃, the removal rate of BC-700 decreases significantly, falling below that of BC-200, BC-300, BC-400, BC-500, and BC-600. These results indicate that both excessively low and excessively high carbonization temperatures are detrimental to the adsorption of U(VI) by biochar, and 600℃ is the preferred carbonization temperature for this invention.

[0064] Depend on Figure 3 It is evident that, at a carbonization temperature of 600℃, among BC-600-C obtained without lignin, BC-600-CL1, BC-600-CL2, BC-600-CL3, BC-600-CL4 obtained with different mass ratios of self-extracted cellulose to lignin, and BC-600-L obtained with pure lignin, BC-600-CL3 exhibited the highest removal rate of U(VI). This indicates that when the mass ratio of self-extracted cellulose to lignin is 2:5, the biochar matrix synergistically constructed by the two exhibits superior intrinsic adsorption performance.

[0065] Depend on Figure 4It is evident that, after modification with polyamine oxime, the removal rates of U(VI) by BC-600-C-PAO, BC-600-CL1-PAO, BC-600-CL2-PAO, BC-600-CL3-PAO, BC-600-CL4-PAO, BC-600-L-PAO, and pure PAO aerogel were significantly higher than those of unmodified biochar. Among them, BC-600-CL3-PAO had the highest removal rate. This indicates that the optimal scheme of the present invention, which uses a self-extracted cellulose to lignin mass ratio of 2:5, a carbonization temperature of 600℃, and polyamine oxime loading, results in a composite adsorbent with the best adsorption performance for U(VI).

[0066] To facilitate understanding by those skilled in the art of the improvements of this invention over the prior art, some of the accompanying drawings and descriptions have been simplified. The above embodiments are preferred implementations of this invention. In addition, this invention can be implemented in other ways. Any obvious substitutions without departing from the concept of this technical solution are within the protection scope of this invention.

Claims

1. A method for preparing a bamboo-based cellulose and lignin biochar aerogel composite adsorbent, characterized in that, Includes the following steps: (1) After pretreatment of bamboo, it is added to a formic acid solution for treatment. After being taken out, it is soaked in an alkaline solution, washed with water until neutral, and dried to obtain self-extracted cellulose. (2) Mix the self-extracted cellulose with lignin evenly to obtain a cellulose / lignin mixed precursor; (3) The cellulose / lignin mixed precursor is carbonized under an inert atmosphere to obtain cellulose / lignin-based biochar material; (4) Polyamine oxime is dissolved in an alkaline solution and aged, then mixed with the cellulose / lignin-based biochar material, and glutaraldehyde is added for cross-linking. After washing and freeze-drying, bamboo-based cellulose and lignin biochar aerogel composite adsorbent is obtained.

2. The preparation method of the bamboo-based cellulose and lignin biochar aerogel composite adsorbent according to claim 1, characterized in that: In step (1), the bamboo material is moso bamboo; the pretreatment is to cut the bamboo material and boil it for 1 hour.

3. The preparation method of the bamboo-based cellulose and lignin biochar aerogel composite adsorbent according to claim 1, characterized in that: In step (1), the peroxyformic acid solution is prepared by mixing hydrogen peroxide and formic acid in a molar ratio of 1:1, and 1wt% sulfuric acid is added as a catalyst; the volume ratio of bamboo to peroxyformic acid solution is 1:10; the temperature of the peroxyformic acid solution treatment is 50℃, and the treatment time is 12h.

4. The preparation method of the bamboo-based cellulose and lignin biochar aerogel composite adsorbent according to claim 1, characterized in that: In step (1), the alkaline solution is a sodium hydroxide solution with a mass concentration of 0.5 wt%, the soaking time is 5 to 10 minutes, and after washing with water until neutral, it is naturally air-dried at room temperature.

5. The preparation method of the bamboo-based cellulose and lignin biochar aerogel composite adsorbent according to claim 1, characterized in that: In step (2), the lignin is dealkalized lignin; the mass ratio of the self-extracted cellulose to lignin is 2:1, 2:3, 2:5, or 2:

7.

6. The preparation method of the bamboo-based cellulose and lignin biochar aerogel composite adsorbent according to claim 1, characterized in that: In step (3), the inert atmosphere is nitrogen; the heating rate of carbonization is 5℃ / min, the carbonization temperature is 200~700℃, the holding time is 2h, and the preferred carbonization temperature is 600℃.

7. The preparation method of the bamboo-based cellulose and lignin biochar aerogel composite adsorbent according to claim 1, characterized in that: In step (4), the poly(dimethylformamide) oxime is prepared by reacting polyacrylonitrile, hydroxylamine hydrochloride, sodium hydroxide and sodium carbonate in N,N-dimethylformamide. Specifically, the reaction includes: dissolving hydroxylamine hydrochloride in N,N-dimethylformamide at 45°C, adding sodium hydroxide and sodium carbonate, and stirring at 45°C for 1 hour; adding polyacrylonitrile and dissolving it for 15 minutes, then heating to 65°C and reacting for 24 hours; adding N,N-dimethylformamide, hydroxylamine hydrochloride, sodium hydroxide and sodium carbonate, and continuing to react at 65°C for 24 hours; centrifuging, dropping the supernatant into anhydrous ethanol to precipitate, collecting the precipitate and drying it under vacuum to obtain poly(dimethylformamide) oxime.

8. The preparation method of the bamboo-based cellulose and lignin biochar aerogel composite adsorbent according to claim 1, characterized in that: In step (4), the alkaline solution is a 0.3M sodium hydroxide solution; the mass ratio of the poly(amine oxime) to the cellulose / lignin-based biochar material is 10:1; the glutaraldehyde is a 50% glutaraldehyde solution, and the mixture is crosslinked until it is completely gelled.

9. A bamboo-based cellulose and lignin biochar aerogel composite adsorbent, characterized in that: The composite adsorbent is prepared by any one of the preparation methods described in claims 1 to 8; the composite adsorbent comprises a cellulose / lignin-based porous biochar framework and polyamine oxime loaded on the surface and / or in the pores of the porous biochar framework.

10. The application of the bamboo-based cellulose and lignin biochar aerogel composite adsorbent according to claim 9 in the removal of radioactive U(VI) from wastewater.