Lateritic nickel ore-based heavy metal adsorbent materials, their preparation methods and applications

By using liquid-phase co-modification of lateritic nickel ore and lignocellulosic biomass and pressure reduction roasting, the high temperature and high consumption problem in the preparation of heavy metal adsorbent materials from lateritic nickel ore was solved, and the low-temperature and high-efficiency preparation of highly active nanoparticle materials was achieved, which improved the heavy metal adsorption effect and resource utilization rate.

CN123102303APending Publication Date: 2026-11-17CENT SOUTH UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611632580.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing methods for preparing heavy metal adsorbents from laterite nickel ore suffer from problems such as high reduction temperature, low efficiency, and unsatisfactory heavy metal adsorption activity. Furthermore, traditional fossil reducing agents increase carbon emissions and are difficult to achieve selective reduction and efficient recovery of nickel, cobalt, and iron at low temperatures.

Method used

A magnetite-supported Ni-Co-Fe nanoparticle composite material was prepared by liquid-phase co-modification of laterite nickel ore and lignocellulosic biomass under specific pH conditions followed by pressure reduction calcination. Through the combined control of liquid-phase co-modification and pressure reduction, a high-activity adsorbent material was prepared at low temperature and with high efficiency.

Benefits of technology

Highly dispersed nanoparticle materials were prepared at low temperature and in a short time, which improved the adsorption effect of heavy metals, reduced energy consumption and carbon emissions, and realized the synergistic conversion of nickel, cobalt and iron and efficient resource utilization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102303A_ABST
    Figure CN123102303A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of mineral resource processing, specifically relating to laterite nickel ore-based heavy metal adsorbent materials, their preparation methods, and applications. The preparation method involves: liquid-phase co-modification of laterite nickel ore and lignocellulosic biomass at a weight ratio of 100:2-5 to obtain a co-modified material; wherein the solvent for liquid-phase co-modification includes water and has a pH above 10; the co-modified material is then subjected to pressure reduction; thus, the laterite nickel ore-based heavy metal adsorbent material is obtained; wherein the pressure reduction process is carried out at a temperature of 700-850℃, a pressure of 0.4-0.8 MPa, and a time of 5-30 min. The material prepared by the method of this invention, possessing the aforementioned characteristics, unexpectedly meets the requirements for heavy metal treatment and can achieve excellent heavy metal adsorption effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of mineral resource processing, specifically to the field of lateritic nickel ore-based heavy metal adsorption materials, their preparation methods, and applications. Background Technology

[0002] Laterite nickel ore is one of the world's major sources of nickel resources, accounting for more than 70% of global nickel reserves. However, the grade of laterite nickel ore is currently low, and the mineral composition is complex. It mainly exists in the form of goethite and nickel silicate, with nickel and cobalt dispersed in iron oxides and silicate minerals, and the associated iron content is high.

[0003] Traditional laterite nickel ore processing technologies are mainly divided into two categories: pyrometallurgical and hydrometallurgical processes. Pyrometallurgical processes, primarily using rotary kiln-electric furnace (RKEF) and blast furnace / small blast furnace smelting, suffer from high energy consumption, large carbon emissions, severe equipment corrosion, and significant environmental pollution. Furthermore, the products are mostly nickel-iron alloys, making it difficult to achieve efficient and synergistic recovery and high-value utilization of nickel, cobalt, and iron. Hydrometallurgical processes, such as high-pressure acid leaching (HPAL), can recover nickel and cobalt relatively well, but they also suffer from high equipment investment, high acid consumption, severe scaling, significant safety risks associated with high-pressure operation, poor adaptability to different ores (especially high-magnesium ores), and the generation of large amounts of acid leaching slag. The overall process is complex, costly, and difficult to meet green and low-carbon requirements.

[0004] In addition, existing technologies have also reported some schemes for the direct resource utilization of laterite nickel ore to prepare heavy metal adsorbents. For example, Chinese patent document CN110745936A discloses a method for removing heavy metal pollution from water based on laterite nickel ore, including the following steps: Step S1, preparing nano-zero-valent iron-nickel composite material; Step S2, adding the nano-zero-valent iron-nickel composite material to industrial wastewater containing heavy metal pollution, reacting at room temperature, and then separating the solid and liquid after settling and precipitation. The nano-zero-valent iron-nickel composite material is obtained by liquid-phase reduction reaction of natural laterite nickel-iron ore with borohydride salt. Chinese patent document CN118561288A discloses a method for preparing porous magnesium silicate-based adsorbents using laterite nickel ore smelting tailings and magnesite tailings. Using laterite nickel ore smelting tailings and magnesite tailings as raw materials and low-cost coal powder as fuel, the porous magnesium silicate-based adsorbent is prepared by a heat preservation crystallization-fine grinding activation-calcination crystallization method.

[0005] In summary, although existing technologies disclose some methods for preparing heavy metal adsorbent materials from laterite nickel ore, the reduction process of laterite nickel ore in these technologies largely relies on traditional fossil reducing agents such as coal and coke. This not only increases carbon emissions but also makes it difficult to achieve selective reduction at lower temperatures and shorter time periods, leading to excessive iron reduction or low nickel-cobalt recovery rates. Furthermore, preparing composite functional materials with specific nanostructures is challenging, resulting in low added value and failing to meet the requirements for heavy metal adsorption. Summary of the Invention

[0006] To address the problems of high reduction temperature, low efficiency, and unsatisfactory heavy metal adsorption activity in existing lateritic nickel ore-based heavy metal adsorption materials, the primary objective of this invention is to provide a method for preparing lateritic nickel ore-based heavy metal adsorption materials, aiming to efficiently prepare materials with high heavy metal adsorption activity at low temperatures.

[0007] The second objective of this invention is to provide a lateritic nickel ore-based heavy metal adsorbent material prepared by the aforementioned method.

[0008] The third objective of this invention is to provide the application of the laterite nickel ore-based heavy metal adsorbent material in heavy metal adsorption.

[0009] Current utilization of laterite nickel ore resources mainly focuses on nickel-cobalt extraction. However, the development of environmental remediation materials still faces challenges such as complex mineral phase structures, difficulty in the directional construction of active FeNi components, easy sintering and deactivation of nanoparticles, and unsatisfactory heavy metal adsorption activity in the prepared materials. To address these problems in the preparation of heavy metal adsorption materials from laterite nickel ore, this invention provides the following solution:

[0010] The preparation method of lateritic nickel ore-based heavy metal adsorbent material involves liquid-phase co-modification of lateritic nickel ore and lignocellulosic biomass in a weight ratio of 100:2~5 to obtain co-modified material; wherein the solvent for liquid-phase co-modification contains water and has a pH of 10 or higher.

[0011] The co-modified material is then subjected to pressure reduction to obtain the laterite nickel ore-based heavy metal adsorbent material.

[0012] The pressure reduction process involves a temperature of 700-850℃, a pressure of 0.4-0.8MPa, and a time of 5-30min.

[0013] This invention innovatively involves co-modifying lateritic nickel ore and lignocellulosic biomass at the specified weight ratio under the specified pH, followed by pressure reduction at the specified temperature and pressure. Based on the combined control of the co-modification-pressure reduction and parameter conditions, a synergistic effect is achieved, enabling the preparation of adsorbent materials with unique physicochemical properties at low temperatures and within a short time. This invention also demonstrates that the material prepared by this method unexpectedly meets the requirements for heavy metal treatment, achieving high heavy metal adsorption efficiency.

[0014] The particle size of laterite nickel ore is less than 200 mesh, with MgO content not exceeding 5% and SiO2 content not exceeding 10%.

[0015] Furthermore, laterite nickel ore is a low-grade mineral, containing 0.5-1.5% Ni, 0.04-0.15% Co, 30-60% Fe, 1-5% MgO, 5-10% SiO2, 1-5% Al2O3, and 1-5% Cr2O3. All component contents refer to weight percentages. Even using low-grade laterite nickel ore as raw material, this invention, based on the preparation method described herein, can still reliably prepare materials with excellent heavy metal adsorption activity.

[0016] The woody biomass is one or more of pine powder and bamboo powder, preferably bamboo powder. The research of this invention shows that by using this woody biomass in conjunction with the co-modification, pressure reduction and process control described in this invention, synergy can be achieved, which can further enhance the heavy metal adsorption performance of the prepared material.

[0017] The weight ratio of lateritic nickel ore to lignocellulosic biomass is 100:2.5~3. This preferred weight ratio helps to further improve the synergistic modification of the physicochemical structure of lateritic nickel ore and lignocellulosic biomass, and helps to further enhance the heavy metal adsorption performance of the prepared material.

[0018] In this invention, the solid-liquid ratio of lateritic nickel ore in the liquid-phase co-modification is 0.5~1.0 g / mL;

[0019] pH regulators used in liquid-phase co-modification processes include at least one of alkali metal hydroxides and ammonia water;

[0020] The temperature for liquid-phase co-modification is 55~95℃; the pH is 12~14.

[0021] The liquid phase co-modification time can be adjusted reasonably as needed, for example, it can be more than 1 hour, further can be 1~10 hours, and further can be 2~6 hours.

[0022] After liquid-phase co-modification is completed, solid-liquid separation and drying are performed to obtain the co-modified material;

[0023] The co-modified material is sealed in a pressure-resistant reactor for pressurized reduction.

[0024] The temperature of the pressurized reduction process is 750~800℃, preferably 750~780℃, the pressure is 0.5~0.7MPa, and the time is 10~20min, which can be further 15~20min.

[0025] In this invention, the initial gas atmosphere and the pressurized atmosphere in the pressure-resistant reactor are protective atmospheres, which include at least one of nitrogen and a rare gas. The rare gas is, for example, Ar.

[0026] Preferably, the initial gas atmosphere and pressurized atmosphere in the pressure-resistant reactor are hydrogen-containing atmospheres (a mixture of hydrogen and protective gas), wherein the hydrogen content is below 15 vol%, preferably 1 to 10 vol%. Studies have shown that the preferred initial atmosphere helps to further endow the adsorbent material with a physicochemical structure suitable for heavy metal adsorption, and helps to further enhance the adsorption effect of heavy metals.

[0027] The present invention also provides a lateritic nickel ore-based heavy metal adsorbent material prepared by the aforementioned preparation method.

[0028] The present invention also provides an application of the laterite nickel ore-based heavy metal adsorbent material prepared by the above preparation method, using it as an adsorbent for heavy metals.

[0029] The aforementioned application uses it as an adsorbent to adsorb heavy metals in water.

[0030] The application in question includes at least one of Cr, Pb, and Cd.

[0031] In this invention, the adsorption method and the amount of adsorbent can be reasonably adjusted as needed.

[0032] For example, there are no specific requirements for the concentration of heavy metals in the water to be treated; it can be below 50 mg / L, or even 1–20 mg / L. The water can be acidic, for example, with a pH of 1–5. The amount of adsorbent used can be, for example, 1–10 g / L. The adsorption temperature can be room temperature, and the adsorption time can be within 20 minutes, or even 5–20 minutes.

[0033] Beneficial effects

[0034] This invention utilizes lignocellulosic biomass as a green reducing agent and carbon source. Through liquid-phase co-modification combined with closed-loop pressure reduction roasting, selective reduction is achieved at relatively low temperatures (700~850℃) and within a short time (5~30min), avoiding the high temperature, high energy consumption, and large carbon emissions of traditional pyrometallurgical processes. Furthermore, it eliminates the need for complex wet processes such as high-pressure acid leaching, significantly reducing energy consumption and environmental impact. Simultaneously, it achieves the synergistic conversion of nickel, cobalt, and iron elements in laterite nickel ore, directly preparing magnetite-supported Ni-Co-Fe nanoparticle composite materials. The nanoparticles are highly dispersed (particle size <120nm), avoiding the problems of excessive iron reduction or low nickel-cobalt recovery rates in traditional processes, thus improving the comprehensive utilization rate of resources.

[0035] The material prepared by the method described in this invention has a physicochemical structure suitable for heavy metal adsorption. When used for heavy metal adsorption, it can achieve excellent heavy metal adsorption effect. Attached Figure Description

[0036] Figure 1This is a process flow diagram of the present invention.

[0037] Figure 2 The image shows the XRD pattern of the heavy metal adsorbent material prepared in Example 1.

[0038] Figure 3 The magnetic analysis of the heavy metal adsorbent material prepared in Example 1 is shown in (a) as the overall hysteresis loop diagram and (b) as a magnified view of a local area in the low magnetic field region.

[0039] Figure 4 This is a SEM image of the heavy metal adsorbent material prepared in Example 1. Detailed Implementation

[0040] The present invention will be further described in detail below with reference to specific embodiments.

[0041] In the implementation of this invention, low-grade laterite nickel ore is selected as raw material, wherein the contents of each component are as follows: Ni 0.92%, Co 0.084%, Fe 47.53%, MgO 3.99%, SiO2 7.34%, Al2O3 2.94%, Cr2O3 3.39%.

[0042] Specific implementation according to Figure 1 Perform the steps shown:

[0043] The present invention discloses a method for preparing an optional lateritic nickel ore-based heavy metal adsorbent material, comprising the following steps:

[0044] (1) The laterite nickel ore is pre-classified to obtain -200 mesh fine-grained laterite nickel ore;

[0045] (2) Mix the -200 mesh fine-grained laterite nickel ore with woody biomass evenly, and then perform liquid-phase co-modification on the mixture;

[0046] The woody biomass is selected from one or more of pine powder and bamboo powder, and the amount of woody biomass added is 2 to 5 wt.% of the mass of laterite nickel ore, preferably 2.5 to 3 wt.%.

[0047] In liquid-phase co-modification, the solid-liquid ratio of laterite nickel ore is 0.5~1.0 g / mL;

[0048] pH regulators used in liquid-phase co-modification processes include at least one of alkali metal hydroxides and ammonia.

[0049] In liquid-phase co-modification, the reaction temperature is 55~95℃, the reaction time is 1~10h, and the system pH value is 10~14, preferably the reaction temperature is 75~95℃, the reaction time is 2~6h, and the system pH value is 12~14.

[0050] (3) After the liquid phase co-modification is completed, the obtained material is placed in a closed reduction system for pressure reduction calcination. The reduction temperature is 700~850℃ and the calcination time is 5~30min.

[0051] The pressurized reduction roasting is carried out in a sealed stainless steel reaction vessel.

[0052] (4) After calcination, the material is cooled to room temperature to obtain a composite material with magnetite (Fe3O4) as the carrier and nickel-cobalt-iron (Ni-Co-Fe) nanoparticles loaded on the surface and / or inside.

[0053] Example 1

[0054] Step 1: Take lateritic nickel ore raw material and grade it to obtain -200 mesh fine-grained lateritic nickel ore. Mix the fine-grained lateritic nickel ore with bamboo powder (moso bamboo powder) evenly, wherein the amount of bamboo powder added is 2.5 wt.% of the fine-grained lateritic nickel ore. Add NaOH solution to adjust the pH of the system to 13, place it in a liquid phase co-modification kettle (the solid-liquid ratio of lateritic nickel ore is 0.5 g / mL), and carry out liquid phase co-modification at 95℃ for 4 h.

[0055] Step 2: After liquid-phase co-modification, solid-liquid separation and drying are performed to obtain the co-modified material. This material is then transferred to a sealed stainless steel reduction vessel (the initial and pressurized atmosphere of the reaction vessel is 1v%H2 + 99v%N2) for reduction calcination. The reduction temperature is 750℃, the reduction calcination pressure is 0.5MPa, and the reduction time is 15min. After calcination, the material is naturally cooled to room temperature to obtain the heavy metal adsorbent material.

[0056] The total metal phase content in the heavy metal adsorbent material was 3.57 wt.%; the median particle size (D50) of the Ni-Co-Fe nanoparticles was 79 nm, and they were highly dispersed on the Fe3O4 support; the saturation magnetization reached 43.61 emu / g. The XRD pattern analysis of the obtained composite material is as follows: Figure 2 As shown, the magnetic analysis is as follows. Figure 3 SEM images such as Figure 4 As shown.

[0057] The composite material prepared above was used to treat industrial wastewater containing Cr(VI). Under the conditions of material dosage of 5 g / L, wastewater temperature of 30℃, pH of 3.5, and initial Cr(VI) concentration of 15 mg / L in the wastewater, the Cr(VI) removal rate reached 99.96% after 10 min of reaction.

[0058] Example 2

[0059] Compared with Example 1, only the amount of bamboo powder added in step 1 of Example 1 was changed. All other operations, parameters, and tests were the same as in Example 1. The experimental groups and results are as follows:

[0060] Group A: Bamboo powder addition was 2.0 wt.%; the total metal phase content in the resulting composite material was 3.21 wt.%; the median particle size (D50) of Ni-Co-Fe nanoparticles was 73 nm, highly dispersed on the Fe3O4 support; the saturation magnetization reached 42.85 emu / g. The Cr(VI) removal rate reached 93.21%.

[0061] Group B: Bamboo powder addition was 3.0 wt.%; the total metal phase content in the resulting composite material was 3.86 wt.%; the median particle size (D50) of Ni-Co-Fe nanoparticles was 86 nm, highly dispersed on the Fe3O4 support; the saturation magnetization reached 43.04 emu / g. The Cr(VI) removal rate reached 99.84%.

[0062] Group C: Bamboo powder addition was 3.5 wt.%; the total metal phase content in the resulting composite material was 4.35 wt.%; the median particle size (D50) of Ni-Co-Fe nanoparticles was 97 nm, dispersed on Fe3O4 support; the saturation magnetization reached 41.55 emu / g. The Cr(VI) removal rate reached 94.18%.

[0063] Compared with Group A: the bamboo powder addition was 1.5 wt.%; the total metal phase content in the resulting composite material was 2.75 wt.%; the median particle size (D50) of Ni-Co-Fe nanoparticles was 61 nm, dispersed on Fe3O4 support; the saturation magnetization reached 39.24 emu / g. The Cr(VI) removal rate reached 81.04%.

[0064] As can be seen from Examples 1 and 2, controlling the weight ratio of lateritic nickel ore and lignocellulosic biomass to 100:2~5, preferably 100:2.5~3, helps to further enhance the synergistic pressure reduction performance of the two, helps to optimize the physicochemical structure, and improves the short-term heavy metal adsorption effect of the prepared material.

[0065] Example 3

[0066] Compared with Example 1, only the liquid phase co-modification treatment conditions in step 1 of Example 1 were changed. All other operations, parameters, and tests were the same as in Example 1. The experimental groups and results are as follows:

[0067] Group A: The liquid-phase co-modification treatment temperature was 55℃, pH was 13, and the treatment time was 4h; the total metal phase content in the resulting composite material was 3.21wt.%; the median particle size (D50) of the Ni-Co-Fe nanoparticles was 108nm, and they were highly dispersed on the Fe3O4 support; the saturation magnetization reached 40.72 emu / g. The Cr(VI) removal rate reached 95.84%.

[0068] Group B: The liquid-phase co-modification treatment was carried out at 75℃, pH 13, and time 4h; the total metal phase content in the resulting composite material was 3.38wt.%; the median particle size (D50) of Ni-Co-Fe nanoparticles was 97nm, and they were highly dispersed on the Fe3O4 support; the saturation magnetization reached 41.97 emu / g. The Cr(VI) removal rate reached 98.49%.

[0069] Group C: The liquid-phase co-modification treatment was carried out at a temperature of 95℃, a pH of 12, and a time of 4 hours; the total metal phase content in the resulting composite material was 3.42 wt.%; the median particle size (D50) of the Ni-Co-Fe nanoparticles was 96 nm, and they were highly dispersed on the Fe3O4 support; the saturation magnetization reached 41.86 emu / g. The Cr(VI) removal rate reached 99.21%.

[0070] Group D: The liquid-phase co-modification treatment temperature was 95℃, pH was 14, and the time was 4h; the total metal phase content in the resulting composite material was 3.46wt.%; the median particle size (D50) of Ni-Co-Fe nanoparticles was 91nm, and they were highly dispersed on the Fe3O4 support; the saturation magnetization reached 42.38 emu / g. The Cr(VI) removal rate reached 99.43%.

[0071] Group E: The liquid-phase co-modification treatment temperature was 95℃, pH was 13, and the time was 2h; the total metal phase content in the resulting composite material was 3.39wt.%; the median particle size (D50) of Ni-Co-Fe nanoparticles was 99nm, and they were highly dispersed on the Fe3O4 support; the saturation magnetization reached 41.25 emu / g. The Cr(VI) removal rate reached 98.52%.

[0072] Group F: The liquid-phase co-modification treatment was carried out at a temperature of 95℃, a pH of 13, and a time of 6 hours; the total metal phase content in the resulting composite material was 3.55 wt.%; the median particle size (D50) of the Ni-Co-Fe nanoparticles was 83 nm, and they were highly dispersed on the Fe3O4 support; the saturation magnetization reached 43.19 emu / g. The Cr(VI) removal rate reached 99.83%.

[0073] Example 4

[0074] Compared with Example 1, only the reduction temperature in step 2 of Example 1 was changed. All other operations, parameters, and tests were the same as in Example 1. The experimental groups and results are as follows:

[0075] Group A: The reduction temperature was 800℃; the total metal phase content in the resulting composite material was 4.02 wt.%; the median particle size (D50) of the Ni-Co-Fe nanoparticles was 106 nm, and they were highly dispersed on the Fe3O4 support; the saturation magnetization reached 38.27 emu / g. The Cr(VI) removal rate reached 97.54%.

[0076] Compared with Group A: the reduction temperature was 650℃; the total metal phase content in the resulting composite material was 2.84 wt.%; the median particle size (D50) of Ni-Co-Fe nanoparticles was 68 nm, highly dispersed on the Fe3O4 support; the saturation magnetization reached 41.39 emu / g. The Cr(VI) removal rate reached 84.91%.

[0077] This invention discovers that by combining the pressure reduction of laterite nickel ore and lignocellulosic biomass with temperature control, a synergistic effect can be achieved, enhancing the short-term removal of heavy metals from the resulting material.

[0078] Example 5

[0079] Compared with Example 1, only the reduction time in step 2 of Example 1 was changed. All other operations, parameters, and tests were the same as in Example 1. The experimental group and results are as follows:

[0080] Group A: Reduction time was 10 min; the total metal phase content in the resulting composite material was 3.29 wt.%; the median particle size (D50) of Ni-Co-Fe nanoparticles was 71 nm, highly dispersed on the Fe3O4 support; the saturation magnetization reached 42.96 emu / g. The Cr(VI) removal rate reached 93.39%.

[0081] Group B: Reduction time was 20 min; the total metal phase content in the resulting composite material was 3.61 wt.%; the median particle size (D50) of Ni-Co-Fe nanoparticles was 80 nm, highly dispersed on the Fe3O4 support; the saturation magnetization reached 43.37 emu / g. The Cr(VI) removal rate reached 99.91%.

[0082] Example 6

[0083] Compared with Example 1, pine powder was selected instead of bamboo powder, and all other operations and parameters were the same as in Example 1; the total metal phase content in the resulting composite material was 3.79 wt.%; the median particle size (D50) of Ni-Co-Fe nanoparticles was 106 nm, dispersed on Fe3O4 support; the saturation magnetization reached 39.93 emu / g. The Cr(VI) removal rate reached 96.84%.

[0084] As can be seen from Examples 1 and 6, using bamboo powder as a raw material has better compatibility with laterite nickel ore, which helps to combine with the pressure reduction process and helps to form a physicochemical structure that is conducive to reduction, thereby unexpectedly improving the short-term heavy metal adsorption activity of the prepared material.

[0085] Example 7

[0086] Compared with Example 1, the atmosphere and pressure in the initial reaction vessel were changed, while other operations, parameters, and tests were the same as in Example 1. The experimental group and results are as follows:

[0087] Group A: The initial reaction vessel atmosphere and the pressurized atmosphere were both 2.5 wt% H2 + 97.5 wt% N2. The total metallic phase content in the resulting composite material was 3.78 wt.%; the median particle size (D50) of the Ni-Co-Fe nanoparticles was 66 nm, highly dispersed on the Fe3O4 support; the saturation magnetization reached 42.43 emu / g. The Cr(VI) removal rate reached 99.98%.

[0088] Group B: The initial reaction vessel atmosphere and the pressurized atmosphere were both 5v% H2 + 95v% N2. The total metal phase content in the resulting composite material was 4.13 wt.%; the median particle size (D50) of the Ni-Co-Fe nanoparticles was 81 nm, and they were highly dispersed on the Fe3O4 support; the saturation magnetization reached 40.90 emu / g. The Cr(VI) removal rate reached 99.98%.

[0089] Group C: The initial reaction vessel atmosphere and the pressurized atmosphere were both 10v% H2 + 90v% N2. The total metal phase content in the resulting composite material was 5.09 wt.%; the median particle size (D50) of the Ni-Co-Fe nanoparticles was 87 nm, dispersed on the Fe3O4 support; the saturation magnetization reached 37.53 emu / g. The Cr(VI) removal rate reached 96.18%.

[0090] Group D: The system pressure during the reduction roasting process was controlled at 0.7 MPa; the Cr(VI) removal rate reached 99.32%.

[0091] Group E: The initial reaction vessel atmosphere and the pressurized atmosphere were both N2. The Cr(VI) removal rate reached 94.31%.

[0092] As can be seen from Examples 1 and 7, pressurizing with a hydrogen-containing atmosphere helps to further optimize the pressurized reduction characteristics of lateritic nickel ore-lignocellulosic biomass and helps to further enhance the heavy metal adsorption activity of the prepared material.

[0093] Comparative Example 1

[0094] Compared to Example 1, the only difference is that the liquid-phase co-modification in step 1 was not performed. Instead, the physical mixture of laterite nickel ore, bamboo powder, and alkali was directly processed in step 2. The resulting composite material had a total metal phase content of 3.08 wt.%; the median particle size (D50) of Ni-Co-Fe nanoparticles was 138 nm, dispersed on a Fe3O4 support; the saturation magnetization reached 39.53 emu / g; and the Cr(VI) removal rate reached 80.37%.

[0095] Comparative Example 2

[0096] Compared with Example 1, the only differences are that the reduction temperature is 900℃; the total metal phase content in the resulting composite material is 4.86 wt.%; the median particle size (D50) of the Ni-Co-Fe nanoparticles is 162 nm, dispersed on the Fe3O4 support; the saturation magnetization reaches 28.51 emu / g; and the Cr(VI) removal rate reaches 73.17%.

[0097] Comparative Example 3

[0098] Compared to Example 1, the only difference is that an atmospheric pressure calcination mode was used, i.e., sealed pressurized reduction was not employed; the reduction was carried out in a tube furnace at atmospheric pressure. The total metallic phase content in the resulting composite material was 2.09 wt.%; the median particle size (D50) of the Ni-Co-Fe nanoparticles was 51 nm, highly dispersed on the Fe3O4 support; the saturation magnetization reached 29.94 emu / g. The Cr(VI) removal rate reached 58.49%.

[0099] Comparative Example 4

[0100] Compared with Example 1, the only difference is that no alkali was added in step 1, while all other operations and parameters are the same as in Example 1.

[0101] The total metallic phase content in the obtained composite material was 3.76 wt.%; the median particle size (D50) of the Ni-Co-Fe nanoparticles was 104 nm, dispersed on the Fe3O4 support; the saturation magnetization reached 37.85 emu / g. The Cr(VI) removal rate reached 83.71%.

[0102] Comparative Example 5

[0103] Compared with Example 1, the only difference is that in step 1, anthracite was used instead of lignocellulosic biomass; all other operations and parameters are the same as in Example 1. The total metal phase content in the resulting composite material is 4.09 wt.%; the median particle size (D50) of Ni-Co-Fe nanoparticles is 306 nm; the saturation magnetization is 33.48 emu / g; and the Cr(VI) removal rate reaches 69.71%.

Claims

1. A method for preparing laterite nickel ore-based heavy metal adsorbent materials, characterized in that, Lateritic nickel ore and lignocellulosic biomass in a weight ratio of 100:2~5 were subjected to liquid-phase co-modification to obtain co-modified material; wherein the solvent for liquid-phase co-modification contained water and had a pH of 10 or higher. The co-modified material is then subjected to pressure reduction to obtain the laterite nickel ore-based heavy metal adsorbent material. The pressure reduction process involves a temperature of 700-850℃, a pressure of 0.4-0.8MPa, and a time of 5-30min.

2. The preparation method of the laterite nickel ore-based heavy metal adsorbent material as described in claim 1, characterized in that, The particle size of laterite nickel ore is less than 200 mesh, and it contains 0.5~1.5% Ni, 0.04~0.15% Co, 30~60% Fe, 1~5% MgO, 5~10% SiO2, 1~5% Al2O3, and 1~5% Cr2O3.

3. The preparation method of the laterite nickel ore-based heavy metal adsorbent material as described in claim 1, characterized in that, Wood-based biomass includes one or more of pine powder and bamboo powder; The weight ratio of lateritic nickel ore to lignocellulosic biomass is 100:2.5~3.

4. The preparation method of the laterite nickel ore-based heavy metal adsorbent material as described in claim 1, characterized in that, In liquid-phase co-modification, the solid-liquid ratio of laterite nickel ore is 0.5~1.0 g / mL; The pH regulators used in the liquid-phase co-modification process include at least one of alkali metal hydroxides and ammonia.

5. The preparation method of the laterite nickel ore-based heavy metal adsorbent material as described in claim 1, characterized in that, The temperature for liquid-phase co-modification is 55~95℃; the pH is 12~14; and the time is 2~6h.

6. The preparation method of the laterite nickel ore-based heavy metal adsorbent material as described in claim 1, characterized in that, The co-modified material was sealed in a pressure-resistant reactor and subjected to pressurized reduction. The pressure reduction process involves a temperature of 750-800℃, a pressure of 0.5-0.7MPa, and a time of 10-20min. The initial gas atmosphere and pressurized atmosphere in the pressure reactor are hydrogen-containing atmospheres, wherein the hydrogen content is below 15v%.

7. A lateritic nickel ore-based heavy metal adsorbent material prepared by the preparation method according to any one of claims 1 to 6.

8. The application of the laterite nickel ore-based heavy metal adsorbent material according to claim 7, characterized in that, It can be used as an adsorbent for heavy metals.

9. The application as described in claim 8, characterized in that, It can be used as an adsorbent to adsorb heavy metals in water.

10. The application as described in claim 8 or 9, characterized in that, The heavy metals mentioned include at least one of Cr, Pb, and Cd.

Citation Information

Patent Citations

  • Method for removing heavy metal pollution in water based on laterite-nickel ore

    CN110745936A

  • Method for preparing porous magnesium silicate-based adsorbent from laterite-nickel ore smelting tailings and magnesite tailings

    CN118561288A