A high-strength catalyst support and its preparation method
By using specific components and processes to prepare high-strength catalyst supports, the defects of alumina-based catalyst supports in terms of molding and pore stability have been solved, achieving high mechanical strength and large specific surface area, which is suitable for petrochemical, coal chemical and fine chemical fields.
Patent Information
- Application Number
- CN202611136268.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-29
- Publication Date
- 2026-11-17
AI Technical Summary
Existing alumina-based catalyst supports suffer from problems such as insufficient plasticity and toughness of the formed preform, easy cracking, and pore blockage during the preparation process, resulting in low mechanical strength and small specific surface area, which makes it difficult to meet the application requirements of high-end chemical catalysis.
Using aluminum source, lanthanum nitrate, silica sol, modified guar gum powder, hydroxypropyl methylcellulose ether, PEG and glyceryl monostearate as raw materials, a flexible polymer network is formed through spray drying, gradient drying and calcination processes, which improves the plasticity and molding toughness of the mixture system and avoids organic carbon residue clogging the pores.
The mechanical strength and specific surface area of the catalyst support were improved, the problems of molding cracking and pore blockage were solved, and the overall performance and production efficiency of the catalyst were enhanced.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalyst support technology, and specifically to a high-strength catalyst support and its preparation method. Background Technology
[0002] Alumina-based supports are the most widely used catalyst support materials in the petrochemical, coal chemical, and fine chemical industries. Their mechanical strength, molding integrity, and pore structure stability directly determine the catalyst's lifespan, mass transfer efficiency, and catalytic activity. Extrusion molding is the mainstream process for the industrial preparation of alumina catalyst supports, offering advantages such as high molding efficiency, regular product structure, and suitability for large-scale production. However, existing preparation systems and molding processes still have many inherent technical defects.
[0003] Currently, in the preparation of conventional catalyst supports, the organic additive systems used are characterized by single components, poor compatibility, poor uniformity of powder mixing, insufficient plasticity and toughness of the formed green body, and stress concentration during the extrusion molding stage. Defects such as strip delamination, strip breakage, surface microcracks, and overall cracking are common, which seriously reduce the structural stability of the green body and the sintering strength of the finished product. At the same time, the thermal decomposition range of conventional organic additives is concentrated and the decomposition rate is uncontrollable. During the calcination process, problems such as local combustion carbonization and incomplete decomposition are prone to occur. The residual carbon components can easily block the micropores of the support, significantly reducing the effective specific surface area and pore volume of the support, which restricts the mass transfer performance of the catalyst and its ability to load active components.
[0004] Furthermore, traditional preparation processes often employ single powder modification methods and constant-temperature drying and calcination modes, which cannot match the volatilization and decomposition patterns of organic additives with the sintering characteristics of powders. This can easily exacerbate problems such as uneven shrinkage of the green body and concentration of thermal stress, further amplifying molding defects and pore blockage. Consequently, the finished catalyst carriers suffer from defects such as low sintering strength, poor molding qualification rate, and imperfect pore structure, making it difficult to meet the industrial application requirements of high-strength, high specific surface area, and structurally stable carriers in the field of high-end chemical catalysis.
[0005] Therefore, in order to overcome the shortcomings of the existing technologies, it is necessary to develop a catalyst support that balances mechanical strength and pore structure integrity. This has significant research value and engineering implications for improving the overall performance of catalysts and reducing production costs. Summary of the Invention
[0006] To address the aforementioned technical problems, this invention provides a high-strength catalyst support and its preparation method.
[0007] The objective of this invention can be achieved through the following technical solutions: A high-strength catalyst support comprises the following raw materials: aluminum source, lanthanum nitrate, silica sol, modified guar gum powder, hydroxypropyl methylcellulose ether, PEG, glyceryl monostearate, and deionized water; Furthermore, based on the total mass of the aluminum source; lanthanum nitrate accounts for 0.25-0.35% of the total mass of the aluminum source, and silica sol accounts for 0.6-0.8% of the total mass of the aluminum source; the total mass of modified guar gum powder, hydroxypropyl methylcellulose ether, PEG, and glyceryl monostearate accounts for 2.0-2.8% of the total mass of the aluminum source, and the mass ratio of modified guar gum powder, hydroxypropyl methylcellulose ether, PEG, and glyceryl monostearate is 0.8-1.2:0.4-0.6:0.15-0.25:0.1-0.2; and deionized water accounts for 32.5-33.5% of the total mass of the aluminum source.
[0008] Furthermore, the aluminum source includes boehmite and gibbsite, with boehmite accounting for 75-85% of the total mass of the aluminum source and gibbsite accounting for 15-25% of the total mass of the aluminum source.
[0009] Furthermore, PEG is obtained by mixing PEG1000 and PEG4000 in a mass ratio of 2:1-1.2.
[0010] A method for preparing a high-strength catalyst support includes the following steps: Step (1): Mix aluminum source and lanthanum nitrate, stir, and then add silica sol by spraying. After spraying is complete, continue stirring and dry to obtain mixed powder 1. Step (2): Mix powder 1, modified guar gum powder, hydroxypropyl methylcellulose ether, and glyceryl monostearate. After stirring, spray in deionized water. Mix PEG with deionized water and stir to obtain a PEG mixture. Then spray in the PEG mixture. After the spraying is complete, stir and then seal and let stand, extrude and mold, gradient dry, gradient temperature calcination, and cool to obtain a high-strength catalyst support.
[0011] Furthermore, a method for preparing a high-strength catalyst support includes the following specific steps: Step (1): Mix aluminum source and lanthanum nitrate, stir at room temperature and 500-600 rpm for 15-17 min, add silica sol by spraying, continue stirring at room temperature for 30-35 min after spraying, and dry at 80-85℃ for 1.5-2.0 h to obtain mixed powder 1; Furthermore, the spray control nozzle pressure is 0.18-0.22 MPa and the feed rate is 8-14 mL / min.
[0012] Step (II): Mix powder 1, modified guar gum powder, hydroxypropyl methylcellulose ether, and glyceryl monostearate. Stir at room temperature and 280-320 rpm for 10-15 min. Spray 50 wt% deionized water in three separate applications, with an interval of 1.5-2.5 min between each application. The amount of water sprayed in each application is equal. Mix PEG with deionized water and stir to obtain a PEG mixture. Spray the PEG mixture into the mixture. After spraying, stir at room temperature and 180-220 rpm for 20-22 min. Then stir at room temperature and 80-120 rpm for 40-45 min. Seal and let stand for 12-13 h. Extrude the mixture and control the extrusion rate at 30-40 rpm. Perform gradient drying, then gradient heating calcination, and finally cool naturally to room temperature to obtain a high-strength catalyst support.
[0013] Furthermore, the specific preparation method of the PEG mixture is as follows: heat PEG to 40-45℃, add it to deionized water preheated to 40-45℃, stir for 10-15 minutes to obtain the PEG mixture.
[0014] Further, the gradient drying process includes: drying at 40-42℃ and 80-85% humidity for 6-6.5 hours; then heating to 80-82℃ at a rate of 1-2℃ / min and drying at 50-55% humidity for 8-8.5 hours; and then heating to 115-120℃ at a rate of 1-2℃ / min and drying for 4-4.5 hours.
[0015] Furthermore, the gradient heating calcination includes: heating to 480-485℃ at a rate of 1-2℃ / min and holding for 2 hours; then heating to 650-655℃ at a rate of 2-3℃ / min and holding for 3 hours; and then heating to 890-900℃ at a rate of 1.5-2.5℃ / min and holding for 4 hours.
[0016] Furthermore, the modified guar gum powder is prepared by the following steps: Guaranteed guar powder and anhydrous ethanol were mixed and stirred. Sodium hydroxide solution was added and stirred continuously. A protective gas was then introduced and heated. Butylene oxide was added and stirred continuously. The mixture was then cooled and acetic acid solution was added. After stirring, the mixture was dried, pulverized, and sieved to obtain modified guaranteed guar powder.
[0017] Furthermore, the preparation method of modified guar gum powder includes the following specific steps: Mix guar gum powder and anhydrous ethanol, stir at room temperature and 500-600 rpm for 15-20 min, add sodium hydroxide solution, continue stirring at room temperature and 500-600 rpm for 40-45 min, introduce protective gas, heat to 40-42℃, add 30wt% epoxide butane, stir for 30-35 min, raise the temperature to 50-52℃, add 70wt% epoxide butane, stir for 1.2-1.4 h, cool to 35-37℃, add acetic acid solution, stir for 10-15 min, dry at 55℃ for 6 h, pulverize and pass through an 180 mesh sieve to obtain modified guar gum powder; Furthermore, the mass ratio of guar gum powder, anhydrous ethanol, sodium hydroxide solution, epoxide butane, and acetic acid solution is 10-11:30-31:3.6-3.8:5.2-5.4:5.3-5.5.
[0018] Furthermore, the sodium hydroxide solution has a mass fraction of 28-30%; the acetic acid solution has a mass fraction of 9-10%.
[0019] The beneficial effects of this invention are: This invention discloses a method for preparing a high-strength catalyst support, which comprises the following raw materials: aluminum source, lanthanum nitrate, silica sol, modified guar gum powder, hydroxypropyl methylcellulose ether, PEG, glyceryl monostearate, and deionized water. The high-strength catalyst support is prepared by mixing and drying the aluminum source, lanthanum nitrate, and silica sol, then mixing them with the modified guar gum powder, hydroxypropyl methylcellulose ether, and glyceryl monostearate, followed by sequential spraying of deionized water and PEG mixture. The mixture is then sealed and allowed to stand, extruded, gradient dried, gradient heated and calcined, and cooled to obtain the final product. Through the synergistic effect of inorganic doping modification of the powder and organic toughening system, combined with gradient drying and segmented calcination processes, this method helps to solve problems such as molding cracking, low sintering strength of the support, and pore blockage caused by residual organic carbon.
[0020] This invention utilizes modified guar gum powder, hydroxypropyl methylcellulose ether, PEG, and glyceryl monostearate in specific mass ratios. The modified guar gum powder is prepared by modifying guar gum powder with epoxide to obtain guar gum powder containing hydroxybutyl groups on its surface. In this preparation method, anhydrous ethanol is first used to pre-disperse and stir the guar gum powder. The lower dielectric constant of ethanol allows it to penetrate into the hydrophobic regions inside the guar gum powder, disrupting the hydrophobic association structure within the particles. This makes it easier for sodium hydroxide solution to enter the particles, increasing the number of exposed hydroxyl groups. Compared to directly soaking in sodium hydroxide solution, this allows for better grafting with epoxide, enabling the polysaccharide molecules to graft flexible hydroxyethyl branches, thus improving the flexibility and extensibility of the polymer network.
[0021] The modified guar gum powder of this invention forms a flexible polymer network that enhances the overall plasticity and molding toughness of the mixture system, alleviating stress concentration during extrusion molding. Highly substituted hydroxypropyl methylcellulose ether coats aluminum source particles to form a flexible polymer film, constraining the particle packing structure and improving the overall structural stability of the green body. Low-molecular-weight PEG1000 in the PEG penetrates the interparticle gaps to reduce internal friction and improve mixing uniformity, while high-molecular-weight PEG4000 forms a lubricating layer at the molding interface, reducing extrusion shear stress and avoiding delamination and breakage defects. The amphiphilic structure of glycerol monostearate interpenetrates the polymer network, relaxing rigid molecular chains, alleviating molding stress concentration, and significantly improving the deformation resistance and molding compatibility of the mixture system. The synergistic effect of the multi-component organic additives ensures excellent molding performance and green body strength, while also allowing for stable and complete decomposition during gradient calcination without residual carbon, preventing clogging of carrier pores and reduction of the effective catalytic surface area. Detailed Implementation
[0022] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0023] Example 1 The preparation method of modified guar gum powder includes the following steps: Guaranteed sesame powder and anhydrous ethanol were mixed and stirred at 500 rpm for 15 min at room temperature. A 28% sodium hydroxide solution was added, and stirring continued at 500 rpm for 40 min at room temperature. Nitrogen gas was introduced, and the mixture was heated to 40°C. 30 wt% epoxide was added, and the mixture was stirred for 30 min. The temperature was raised to 50°C, and 70 wt% epoxide was added. The mixture was stirred for 1.2 h, cooled to 35°C, and a 9% acetic acid solution was added. The mixture was stirred for 10 min, dried at 55°C for 6 h, and pulverized through an 180-mesh sieve to obtain modified guaranteed sesame powder. The mass ratio of guaranteed sesame powder, anhydrous ethanol, 28% sodium hydroxide solution, epoxide, and 9% acetic acid solution was 10:30:3.6:5.2:5.3.
[0024] Example 2 The preparation method of modified guar gum powder includes the following steps: Guaranteed sesame powder and anhydrous ethanol were mixed and stirred at 550 rpm for 18 min at room temperature. A 29% sodium hydroxide solution was added, and stirring continued at 550 rpm for 43 min at room temperature. Nitrogen gas was introduced, and the mixture was heated to 41°C. 30 wt% epoxide was added, and the mixture was stirred for 33 min. The temperature was raised to 51°C, and 70 wt% epoxide was added. The mixture was stirred for 1.3 h, cooled to 36°C, and a 9.5% acetic acid solution was added. The mixture was stirred for 13 min, dried at 55°C for 6 h, and pulverized through an 180-mesh sieve to obtain modified guaranteed sesame powder. The mass ratio of guaranteed sesame powder, anhydrous ethanol, 29% sodium hydroxide solution, epoxide, and 9.5% acetic acid solution was 10.5:30.5:3.7:5.3:5.4.
[0025] Example 3 The preparation method of modified guar gum powder includes the following steps: Guaranteed sesame powder and anhydrous ethanol were mixed and stirred at 600 rpm for 20 min at room temperature. A 30% sodium hydroxide solution was added, and stirring continued at 600 rpm for 45 min at room temperature. Nitrogen gas was introduced, and the mixture was heated to 42°C. 30 wt% epoxide was added, and the mixture was stirred for 35 min. The temperature was raised to 52°C, and 70 wt% epoxide was added. The mixture was stirred for 1.4 h, cooled to 37°C, and a 10% acetic acid solution was added. The mixture was stirred for 15 min, dried at 55°C for 6 h, and pulverized through an 180-mesh sieve to obtain modified guaranteed sesame powder. The mass ratio of guaranteed sesame powder, anhydrous ethanol, 30% sodium hydroxide solution, epoxide, and 10% acetic acid solution was 11:31:3.8:5.4:5.5.
[0026] Example 4 A high-strength catalyst support comprises the following raw materials: aluminum source, lanthanum nitrate, silica sol, modified guar gum powder, hydroxypropyl methylcellulose ether, PEG, glyceryl monostearate, and deionized water; based on the total mass of the aluminum source; the aluminum source includes boehmite and gibbsite, with boehmite accounting for 75% and gibbsite accounting for 25% of the total mass of the aluminum source; lanthanum nitrate accounting for 0.25% of the total mass of the aluminum source; silica sol accounting for 0.6% of the total mass of the aluminum source; and the modified guar gum powder, hydroxypropyl methylcellulose ether, and PEG obtained in Example 1. The total mass of G and glyceryl monostearate accounted for 2.0% of the total mass of the aluminum source. The mass ratio of modified guar gum powder, hydroxypropyl methylcellulose ether, PEG and glyceryl monostearate obtained in Example 1 was 0.8:0.4:0.15:0.1. PEG was obtained by mixing PEG1000 (supplier: Jiangsu Haian Petrochemical Plant, packaging specification: 50kg) and PEG4000 (supplier: Jiangsu Haian Petrochemical Plant, packaging specification: 25kg) in a mass ratio of 2:1. The mass of deionized water accounted for 32.5% of the total mass of the aluminum source.
[0027] A method for preparing a high-strength catalyst support includes the following steps: Step (1): Mix aluminum source and lanthanum nitrate, stir at room temperature and 500 rpm for 15 min, add silica sol (supplier: Tengyi Material Supply Station, Xigong District, Luoyang City, model: XH5170EHC5TD) by spraying, control the nozzle pressure at 0.18 MPa and the feed rate at 8 mL / min. After spraying, continue stirring at room temperature for 30 min, and dry at 80℃ for 1.5 h to obtain mixed powder 1; Step (II): Mix powder 1, modified guar gum powder obtained in Example 1, hydroxypropyl methylcellulose ether (supplier: Hebei Chuangzhiyuan Biotechnology Co., Ltd., packaging specification: 25kg), and glyceryl monostearate. Stir at room temperature and 280 rpm for 10 min. Spray 50 wt% deionized water in three batches, with an interval of 1.5 min between each spray. The amount of water sprayed in each batch is equal. After spraying, mix PEG with deionized water and stir to obtain a PEG mixture. Spray the PEG mixture in. After spraying, stir at room temperature and 180 rpm for 20 min, then stir at room temperature and 80 rpm for 40 min. Seal and let stand for 12 h. Extrude and shape the mixture, controlling the extrusion rate at 30 rpm. Perform gradient drying, then gradient heating calcination, and finally cool naturally to room temperature to obtain a high-strength catalyst support. The specific preparation method of the PEG mixture is as follows: PEG is heated to 40℃, added to 50wt% deionized water preheated to 40℃, and stirred for 10 min to obtain the PEG mixture; gradient drying includes: drying at 40℃ and 80% humidity for 6 h; then heating to 80℃ at a rate of 1℃ / min and drying at 50% humidity for 8 h; then heating to 115℃ at a rate of 1℃ / min and drying for 4 h; gradient calcination includes: heating to 480℃ at a rate of 1℃ / min and holding for 2 h; then heating to 650℃ at a rate of 2℃ / min and holding for 3 h; then heating to 890℃ at a rate of 1.5℃ / min and holding for 4 h.
[0028] Example 5 A high-strength catalyst support comprises the following raw materials: aluminum source, lanthanum nitrate, silica sol, modified guar gum powder, hydroxypropyl methylcellulose ether, PEG, glyceryl monostearate, and deionized water; based on the total mass of the aluminum source; the aluminum source includes boehmite and gibbsite, with boehmite accounting for 80% and gibbsite accounting for 20% of the total mass of the aluminum source; lanthanum nitrate accounting for 0.30% of the total mass of the aluminum source; silica sol accounting for 0.7% of the total mass of the aluminum source; and the modified guar gum powder, hydroxypropyl methylcellulose ether, and PEG obtained in Example 2. The total mass of the modified guar gum powder, hydroxypropyl methylcellulose ether, PEG and glyceryl monostearate accounted for 2.4% of the total mass of the aluminum source. The mass ratio of the modified guar gum powder, hydroxypropyl methylcellulose ether, PEG and glyceryl monostearate obtained in Example 2 was 1.0:0.5:0.20:0.15. The PEG was obtained by mixing PEG1000 (supplier: Jiangsu Haian Petrochemical Plant, packaging specification: 50kg) and PEG4000 (supplier: Jiangsu Haian Petrochemical Plant, packaging specification: 25kg) in a mass ratio of 2:1.1. The mass of deionized water accounted for 33.0% of the total mass of the aluminum source.
[0029] A method for preparing a high-strength catalyst support includes the following steps: Step (1): Mix aluminum source and lanthanum nitrate, stir at room temperature and 550 rpm for 16 min, add silica sol (supplier: Tengyi Material Supply Station, Xigong District, Luoyang City, model: XH5170EHC5TD) by spraying, control the nozzle pressure at 0.20 MPa and the feed rate at 11 mL / min. After spraying, continue stirring at room temperature for 33 min, and dry at 83℃ for 1.8 h to obtain mixed powder 1; Step (II): Mix powder 1, modified guar gum powder obtained in Example 2, hydroxypropyl methylcellulose ether (supplier: Hebei Chuangzhiyuan Biotechnology Co., Ltd., packaging specification: 25kg), and glyceryl monostearate. Stir at room temperature and 300 rpm for 13 min. Spray 50 wt% deionized water in three batches, with an interval of 2.0 min between each spray. The amount of water sprayed each time is equal. After spraying, mix PEG with deionized water and stir to obtain a PEG mixture. Then spray the PEG mixture. After spraying, stir at room temperature and 200 rpm for 21 min, and then stir at room temperature and 100 rpm for 43 min. Seal and let stand for 12.5 h. Extrude and shape, control the extrusion rate at 35 rpm, perform gradient drying, then perform gradient heating calcination, and finally cool naturally to room temperature to obtain a high-strength catalyst support. The specific preparation method of the PEG mixture is as follows: PEG is heated to 43℃, and 50wt% deionized water preheated to 43℃ is added and stirred for 13 min to obtain the PEG mixture; gradient drying includes: drying at 41℃ and 83% humidity for 6.3 h; then heating to 81℃ at a rate of 1.5℃ / min and drying at 53% humidity for 8.3 h; then heating to 118℃ at a rate of 1.5℃ / min and drying for 4.3 h; gradient calcination includes: heating to 483℃ at a rate of 1.5℃ / min and holding for 2 h; then heating to 653℃ at a rate of 2.5℃ / min and holding for 3 h; then heating to 895℃ at a rate of 2.0℃ / min and holding for 4 h.
[0030] Example 6 A high-strength catalyst support comprises the following raw materials: aluminum source, lanthanum nitrate, silica sol, modified guar gum powder, hydroxypropyl methylcellulose ether, PEG, glyceryl monostearate, and deionized water; based on the total mass of the aluminum source; the aluminum source includes boehmite and gibbsite, with boehmite accounting for 85% and gibbsite accounting for 15% of the total mass of the aluminum source; lanthanum nitrate accounts for 0.35% of the total mass of the aluminum source, and silica sol accounts for 0.8% of the total mass of the aluminum source; the modified guar gum powder, hydroxypropyl methylcellulose ether, and PEG obtained in Example 3 are also included. The total mass of the modified guar gum powder, hydroxypropyl methylcellulose ether, PEG and glyceryl monostearate accounted for 2.8% of the total mass of the aluminum source. The mass ratio of the modified guar gum powder, hydroxypropyl methylcellulose ether, PEG and glyceryl monostearate obtained in Example 3 was 1.2:0.6:0.25:0.2. The PEG was obtained by mixing PEG1000 (supplier: Jiangsu Haian Petrochemical Plant, packaging specification: 50kg) and PEG4000 (supplier: Jiangsu Haian Petrochemical Plant, packaging specification: 25kg) in a mass ratio of 2:1.2. The mass of deionized water accounted for 33.5% of the total mass of the aluminum source.
[0031] A method for preparing a high-strength catalyst support includes the following steps: Step (1): Mix aluminum source and lanthanum nitrate, stir at room temperature and 600 rpm for 17 min, add silica sol (supplier: Tengyi Material Supply Station, Xigong District, Luoyang City, model: XH5170EHC5TD) by spraying, control the nozzle pressure at 0.22 MPa and the feed rate at 14 mL / min. After spraying, continue stirring at room temperature for 35 min, and dry at 85℃ for 2.0 h to obtain mixed powder 1; Step (II): Mix powder 1, modified guar gum powder obtained in Example 3, hydroxypropyl methylcellulose ether (supplier: Hebei Chuangzhiyuan Biotechnology Co., Ltd., packaging specification: 25kg), and glyceryl monostearate. Stir at room temperature and 320 rpm for 15 min. Spray 50 wt% deionized water in three batches, with an interval of 2.5 min between each spray. The amount of water sprayed in each batch is equal. After spraying, mix PEG with deionized water and stir to obtain a PEG mixture. Spray the PEG mixture in. After spraying, stir at room temperature and 220 rpm for 22 min, then stir at room temperature and 120 rpm for 45 min. Seal and let stand for 13 h. Extrude and shape the mixture. Control the extrusion rate at 40 rpm. Perform gradient drying, then gradient heating calcination, and finally cool naturally to room temperature to obtain a high-strength catalyst support. The specific preparation method of the PEG mixture is as follows: PEG is heated to 45℃, and 50wt% deionized water preheated to 45℃ is added and stirred for 15 min to obtain the PEG mixture; gradient drying includes: drying at 42℃ and 85% humidity for 6.5 h; then heating to 82℃ at a rate of 2℃ / min and drying at 55% humidity for 8.5 h; then heating to 120℃ at a rate of 2℃ / min and drying for 4.5 h; gradient calcination includes: heating to 485℃ at a rate of 2℃ / min and holding for 2 h; then heating to 655℃ at a rate of 3℃ / min and holding for 3 h; then heating to 900℃ at a rate of 2.5℃ / min and holding for 4 h.
[0032] Comparative Example 1 Compared with Example 6, the order of adding anhydrous ethanol and 30% sodium hydroxide solution in the preparation process of modified guar gum powder was interchanged, while the rest was exactly the same as in Example 6, to obtain a high-strength catalyst support. Specifically: Guaranteed sesame powder and a 30% sodium hydroxide solution were mixed and stirred at 600 rpm for 20 min at room temperature. Anhydrous ethanol was added, and stirring continued at 600 rpm for 45 min at room temperature. Nitrogen gas was introduced, and the mixture was heated to 42°C. 30 wt% epoxide was added, and the mixture was stirred for 35 min. The temperature was raised to 52°C, and 70 wt% epoxide was added. The mixture was stirred for 1.4 h, cooled to 37°C, and a 10% acetic acid solution was added. The mixture was stirred for 15 min, dried at 55°C for 6 h, and pulverized through an 180-mesh sieve to obtain modified guaranteed sesame powder. The mass ratio of guaranteed sesame powder, anhydrous ethanol, a 30% sodium hydroxide solution, epoxide, and a 10% acetic acid solution was 11:31:3.8:5.4:5.5.
[0033] Comparative Example 2 Compared with Example 6, the modified guar gum powder was directly mixed with a 30% sodium hydroxide solution during the preparation process, without the addition of anhydrous ethanol, and the rest was exactly the same as in Example 6, to obtain a high-strength catalyst support. Specifically: Guaranteed sesame powder and a 30% sodium hydroxide solution were mixed and stirred at 600 rpm for 65 min at room temperature. Nitrogen gas was introduced, and the mixture was heated to 42°C. 30 wt% epoxide was added, and the mixture was stirred for 35 min. The temperature was raised to 52°C, and 70 wt% epoxide was added. The mixture was stirred for 1.4 h, cooled to 37°C, and a 10% acetic acid solution was added. The mixture was stirred for 15 min, dried at 55°C for 6 h, and pulverized through an 180-mesh sieve to obtain modified guaranteed sesame powder. The mass ratio of guaranteed sesame powder, 30% sodium hydroxide solution, epoxide, and 10% acetic acid solution was 11:3.8:5.4:5.5.
[0034] Comparative Example 3 Compared with Example 6, without the addition of glycerol monostearate, the mass ratio of modified guar gum powder, hydroxypropyl methylcellulose ether, and PEG was 1.2:0.6:0.45, and the rest was exactly the same as in Example 6, to obtain a high-strength catalyst support.
[0035] Comparative Example 4 Compared with Example 6, without the addition of PEG, the mass ratio of modified guar gum powder, hydroxypropyl methylcellulose ether, and glyceryl monostearate was 1.2:0.6:0.45, and the rest was exactly the same as in Example 6, to obtain a high-strength catalyst support.
[0036] Comparative Example 5 Compared with Example 6, without the addition of hydroxypropyl methylcellulose ether, the mass ratio of modified guar gum powder, PEG, and glyceryl monostearate was 1.2:0.55:0.5, and the rest was exactly the same as in Example 6, thus obtaining a high-strength catalyst support.
[0037] Comparative Example 6 Compared with Example 6, the PEG mixture in the preparation of the high-strength catalyst support was sprayed in before the deionized water, and the rest was exactly the same as in Example 6, to obtain the high-strength catalyst support; Specifically: Step (II): Mix powder 1, modified guar gum powder obtained in Example 3, hydroxypropyl methylcellulose ether (supplier: Hebei Chuangzhiyuan Biotechnology Co., Ltd., packaging specification: 25kg), and glyceryl monostearate. Stir at room temperature and 320 rpm for 15 min. Mix PEG with deionized water and stir to obtain a PEG mixture. Spray the PEG mixture into the mixture. After spraying, spray 50wt% deionized water in three separate sprays, with an interval of 2.5 min between each spray and an equal amount each time. After spraying, stir at room temperature and 220 rpm for 22 min, then stir at room temperature and 120 rpm for 45 min. Seal and let stand for 13 h. Extrude and shape the mixture, controlling the extrusion rate at 40 rpm. Perform gradient drying, then gradient heating calcination, and finally cool naturally to room temperature to obtain a high-strength catalyst support. The specific preparation method of the PEG mixture is as follows: PEG is heated to 45℃, and 50wt% deionized water preheated to 45℃ is added and stirred for 15 min to obtain the PEG mixture; gradient drying includes: drying at 42℃ and 85% humidity for 6.5 h; then heating to 82℃ at a rate of 2℃ / min and drying at 55% humidity for 8.5 h; then heating to 120℃ at a rate of 2℃ / min and drying for 4.5 h; gradient calcination includes: heating to 485℃ at a rate of 2℃ / min and holding for 2 h; then heating to 655℃ at a rate of 3℃ / min and holding for 3 h; then heating to 900℃ at a rate of 2.5℃ / min and holding for 4 h.
[0038] The effects of the high-strength catalyst supports prepared in Examples 4-6 and Comparative Examples 1-6 of the present invention were further tested below, and the test results are shown below.
[0039] Referring to GB / T 19587-2017, the nitrogen adsorption BET method was used, and 0.5 g of catalyst support was placed under a vacuum of 10... - 4 The sample was kept at 300℃ for 4 hours and then naturally cooled to room temperature. Nitrogen adsorption was measured at 77K liquid nitrogen temperature to calculate the specific surface area and total pore volume.
[0040] Referring to GB / T 44750-2024 and HG / T 2782-2024, 30 parallel samples of 6mm catalyst carrier with intact appearance and no crack defects were selected. The fracture pressure of each sample was measured using a particle strength tester. The lateral compressive strength of a single sample was calculated based on the sample length. The average lateral compressive strength of the 30 parallel samples was calculated as the average mechanical strength.
[0041] The results are recorded in Table 1.
[0042] Table 1: Performance test results of high-strength catalyst supports According to the data in Table 1, the high-strength catalyst supports prepared in Examples 4-6 of the present invention have high average mechanical strength while retaining good specific surface area and total pore volume.
[0043] Comparing Example 6 with Comparative Example 1, it can be seen that by reversing the order of adding anhydrous ethanol and 30% sodium hydroxide solution in the preparation process of modified guar gum powder, the method of the present invention, which first pre-disperses and stirs anhydrous guar gum powder and then adds 30% sodium hydroxide solution, makes it easier for guar gum powder to graft with epoxide butane, which is more conducive to forming a flexible polymer network to improve the overall plasticity and molding toughness of the mixture system, alleviate the stress concentration effect during the extrusion molding process, and thus improve the average mechanical strength, specific surface area and total pore volume of the catalyst support.
[0044] Comparing Example 6 with Comparative Example 2, it can be seen that directly mixing the modified guar powder with a 30% sodium hydroxide solution during the preparation process, without adding anhydrous ethanol, indicates that the method of first pre-dispersing and stirring the guar powder with anhydrous ethanol and then adding a 30% sodium hydroxide solution makes the guar powder easier to graft onto butane oxide, which is more conducive to forming a flexible polymer network to improve the overall plasticity and molding toughness of the mixture system, alleviate the stress concentration effect during extrusion molding, and thus improve the average mechanical strength, specific surface area and total pore volume of the catalyst support.
[0045] Comparing Example 6 with Comparative Examples 3-5, it can be seen that without the addition of glyceryl monostearate, PEG, and hydroxypropyl methylcellulose ether, respectively, the present invention uses a specific ratio of hydroxypropyl methylcellulose ether, PEG, glyceryl monostearate, and modified guar gum powder to form a flexible polymer network, thereby improving the overall plasticity and molding toughness of the mixture system, alleviating the stress concentration effect during the extrusion molding process, and thus improving the average mechanical strength, specific surface area, and total pore volume of the catalyst support.
[0046] Comparing Example 6 with Comparative Example 6, it can be seen that spraying the PEG mixture in the preparation of the high-strength catalyst support before the deionized water indicates that the present invention sprays the deionized water first and then the PEG mixture, which helps to uniformly disperse the mixture and is more conducive to forming a flexible polymer network to improve the overall plasticity and molding toughness of the mixture system, alleviate the stress concentration effect during the extrusion molding process, and thus improve the average mechanical strength, specific surface area and total pore volume of the catalyst support.
[0047] The above description is merely an example and illustration of the concept of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described or use similar methods to replace them, as long as they do not deviate from the concept of the invention or exceed the scope defined in the claims, they should all fall within the protection scope of the present invention.
Claims
1. A high-strength catalyst support, characterized in that: The raw materials include: aluminum source, lanthanum nitrate, silica sol, modified guar gum powder, hydroxypropyl methylcellulose ether, PEG, glyceryl monostearate, and deionized water; Based on the total mass of the aluminum source; The lanthanum nitrate accounts for 0.25-0.35% of the total mass of the aluminum source; The silica sol accounts for 0.6-0.8% of the total mass of the aluminum source; The total mass of the modified guar gum powder, hydroxypropyl methylcellulose ether, PEG and glyceryl monostearate accounts for 2.0-2.8% of the total mass of the aluminum source; the mass ratio of the modified guar gum powder, hydroxypropyl methylcellulose ether, PEG and glyceryl monostearate is 0.8-1.2:0.4-0.6:0.15-0.25:0.1-0.
2.
2. The high-strength catalyst support according to claim 1, characterized in that: The aluminum source includes boehmite and gibbsite, with the boehmite accounting for 75-85% of the total mass of the aluminum source and the gibbsite accounting for 15-25% of the total mass of the aluminum source.
3. The high-strength catalyst support according to claim 1, characterized in that: The PEG is obtained by mixing PEG1000 and PEG4000 in a mass ratio of 2:1-1.
2.
4. The high-strength catalyst support according to claim 1, characterized in that: The modified guar gum powder is prepared by the following steps: Mix guar gum powder and anhydrous ethanol, stir, add sodium hydroxide solution, continue stirring, introduce protective gas, heat, add epoxide butane, continue stirring, heat up, add more epoxide butane, stir, cool down, add acetic acid solution, stir, dry, pulverize and sieve to obtain modified guar gum powder.
5. A high-strength catalyst support according to claim 4, characterized in that: The mass ratio of the guar gum powder, anhydrous ethanol, sodium hydroxide solution, epoxide butane, and acetic acid solution is 10-11:30-31:3.6-3.8:5.2-5.4:5.3-5.
5.
6. A method for preparing a high-strength catalyst support according to any one of claims 1-5, characterized in that: Includes the following steps: Step (1): Mix aluminum source and lanthanum nitrate, stir, and then add silica sol by spraying. After spraying is complete, continue stirring and dry to obtain mixed powder 1. Step (2): Mix powder 1, modified guar gum powder, hydroxypropyl methylcellulose ether, and glyceryl monostearate. After stirring, spray in deionized water. Mix PEG with deionized water and stir to obtain a PEG mixture. Then spray in the PEG mixture and stir. After sealing and standing, extrusion molding, gradient drying, gradient heating calcination, and cooling, a high-strength catalyst support is obtained.
7. The method for preparing a high-strength catalyst support according to claim 6, characterized in that: In step (i), the spray control nozzle pressure is 0.18-0.22 MPa and the feed rate is 8-14 mL / min.
8. The method for preparing a high-strength catalyst support according to claim 6, characterized in that: In step (ii), the specific preparation method of the PEG mixture is as follows: heat PEG to 40-45℃, add it to deionized water preheated to 40-45℃, stir for 10-15 minutes to obtain the PEG mixture.
9. The method for preparing a high-strength catalyst support according to claim 6, characterized in that: In step (ii), the gradient drying includes: drying at 40-42℃ and 80-85% humidity for 6-6.5h; then heating to 80-82℃ at a rate of 1-2℃ / min and drying at 50-55% humidity for 8-8.5h; then heating to 115-120℃ at a rate of 1-2℃ / min and drying for 4-4.5h.
10. The method for preparing a high-strength catalyst support according to claim 6, characterized in that: In step (ii), the gradient heating calcination includes: heating to 480-485℃ at a rate of 1-2℃ / min and holding for 2h; then heating to 650-655℃ at a rate of 2-3℃ / min and holding for 3h; and then heating to 890-900℃ at a rate of 1.5-2.5℃ / min and holding for 4h.