A porous ceramic catalytic material with synergistic photothermal and electrical conductivity enhancement and its preparation method

By introducing a CuO/Co3O4 photothermal-conductive functional layer and a BSO photocatalytic layer into a porous ceramic material, a three-dimensional interconnected framework structure was constructed, which solved the problem of low photogenerated carrier migration rate and achieved high-efficiency photocatalytic performance and organic pollutant degradation effect.

CN123102367APending Publication Date: 2026-11-17SHAANXI UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611456570.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing photocatalytic porous ceramic materials have low photogenerated carrier migration rates, resulting in high recombination rates and decreased catalytic efficiency. Furthermore, some preparation methods use highly toxic substances, affecting the stability and reproducibility of the materials.

Method used

A porous ceramic substrate based on sulfur-fixing ash is used, combined with a CuO/Co3O4 photothermal-conductive functional layer and a BSO photocatalytic functional layer. By constructing a three-dimensional interconnected porous framework structure, a photothermal-conductive network is formed by the synergistic effect of CuO and Co3O4, which promotes the rapid migration and separation of photogenerated carriers.

Benefits of technology

It improves the separation efficiency of photogenerated electron-hole pairs and the light energy utilization rate of photocatalytic materials, broadens the photocatalytic reaction pathway, enhances the degradation efficiency of organic pollutants, overcomes the problems of high carrier recombination rate and low light energy utilization rate, and can be applied to wastewater degradation and waste gas purification.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

This invention discloses a porous ceramic catalytic material with synergistic photothermal and electrical conductivity enhancement and its preparation method, belonging to the field of photocatalytic materials technology. The invention uses sulfur-fixing ash as raw material to prepare a porous ceramic matrix. A CuO / Co3O4 conductive functional layer and a bismuth silicate photocatalytic layer are sequentially constructed on the matrix surface using a vacuum impregnation method. This functional layer relies on the photothermal properties of the CuO / Co3O4 composite powder and the conductive structure of the Co3O4 spinel. The lattice thermal vibrations generated by photothermal activity lower the migration barrier of photogenerated carriers, increasing the migration rate of photogenerated carriers and thus improving the photocatalytic performance of the material. The material obtained by this invention combines the high specific surface area of ​​porous ceramics, the resource utilization of sulfur-fixing ash, and the synergistic photothermal and electrical conductivity enhancement of photocatalytic performance, showing broad application prospects in wastewater degradation, waste gas purification, and other fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of photocatalysis technology, specifically relating to a porous ceramic catalytic material with photothermal-electrical conductivity synergistic enhancement and its preparation method. Background Technology

[0002] Photocatalytic porous ceramic materials made from industrial waste have shown broad application potential in the environmental protection field, enabling diverse functions such as wastewater degradation, waste gas purification, and solid waste solidification. Currently, existing photocatalytic porous ceramic materials generally suffer from the problem of low photogenerated carrier migration rates on the supported catalyst leading to high recombination rates, which in turn reduces catalytic efficiency and limits the practical application of photocatalytic ceramics.

[0003] Co3O4, a stable conductive material under normal conditions, provides migration channels for charged substances such as ions and electrons through its spinel structure. CuO, a conductive metal oxide, lowers the carrier migration barrier and increases the carrier migration rate through lattice thermal vibrations, utilizing the properties of these two materials to prepare functional intercalated layers. This reduces the carrier migration barrier and improves the photocatalytic performance of the material.

[0004] Patent application CN118125860A discloses a method for preparing a porous titanium dioxide ceramic composite material with photothermal properties. The method involves mixing titanium dioxide, graphite powder, steel slag, starch, and a binder, then pressing and drying the mixture to obtain a composite. The mass ratio of titanium dioxide, graphite powder, steel slag, starch, and binder is 1:0.5:2:0.25 to 0.75:1.2, followed by reduction calcination. This process yields a titanium dioxide-based porous ceramic composite material with photothermal properties. However, because it is suitable for simple photothermal evaporation applications, it cannot degrade organic pollutants in water. Furthermore, different batches of steel slag can cause fluctuations in the physical properties during reduction sintering, making it difficult to guarantee the repeatability of the material's photothermal properties (absorption rate, evaporation rate).

[0005] Patent application CN120205227A discloses a titanium dioxide-based porous ceramic composite material with photothermal properties and its preparation method. The active component is porous MOFs (Metal-Oxide-Films) formed by the self-assembly of different metal salts and organic ligands, combined with foam ceramics such as alumina, zirconium oxide, and silicon carbide with pore sizes of 2 to 50 nm as a carrier. MOFs are synthesized through in-situ self-assembly and uniformly loaded into the pores of the foam ceramic using in-situ physical mixing and stirring, significantly improving the dispersibility and bonding strength of the MOFs with the substrate, ensuring its stability and durability under harsh conditions. However, due to the need for highly toxic substances such as hydrazine hydrate, there is a risk of residual highly toxic substances during the material's use. Summary of the Invention

[0006] To overcome the shortcomings of the prior art, the present invention aims to provide a porous ceramic catalytic material with photothermal-conductive synergistic enhancement and its preparation method. The method utilizes a single-component organic compound to gradually anchor a conductive material with photothermal properties and a catalytic material. Under the synergistic effect of the photothermal properties of CuO and the conductive metal oxide, the resulting composite material utilizes the lattice thermal vibration effect to promote the rapid migration of photogenerated carriers in the conductive network, thereby improving the photocatalytic performance of the material.

[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A porous ceramic catalytic material with synergistic photothermal-electrical conductivity enhancement is characterized by comprising: a porous ceramic substrate based on sulfur-fixing ash, a CuO / Co3O4 photothermal-electrical conductivity functional layer, and a BSO photocatalytic functional layer, and having an overall three-dimensional interconnected porous framework structure.

[0008] The porous ceramic framework based on sulfur-fixing ash has a rough surface and a continuous open pore structure, which facilitates the adhesion of functional components. The CuO / Co3O4 photothermal-conductive functional layer is adhered to the outer surface and part of the inner wall of the pores of the porous ceramic framework based on sulfur-fixing ash through epoxy resin, and is tightly bonded to the framework. Inside the CuO / Co3O4 photothermal-conductive functional layer, smaller Co3O4 particles are dispersed around and at the edges of the blocky CuO particles, connecting adjacent CuO particles to form a photothermal-conductive network with blocky CuO as nodes and Co3O4 particles as bridging branches. Flower-shaped BSO particles are further fixed above the CuO / Co3O4 photothermal-conductive functional layer through epoxy resin to form a BSO photocatalytic active layer.

[0009] A method for preparing a porous ceramic catalytic material with synergistic photothermal and electrical conductivity enhancement includes the following steps: Step 1: The polyurethane foam is pretreated with sodium hydroxide solution and then soaked in carboxymethyl cellulose solution. After drying, the modified polyurethane foam is obtained. Step 2: Mix and ball-mill the sulfur-fixing ash, sulfur-fixing slag, zirconium oxide, calcium lignosulfonate, carboxymethyl cellulose, silica sol, polyvinyl alcohol solution, and deionized water to obtain a ceramic slurry; then immerse the modified polyurethane foam in the ceramic slurry and sinter it to obtain foam ceramic. Step 3: Dissolve bismuth nitrate pentahydrate and sodium metasilicate nonahydrate, stir evenly and mix thoroughly, then perform hydrothermal treatment and washing to obtain bismuth silicate powder; Step 4: Ball mill and mix copper oxide and cobalt oxide to obtain CuO / Co3O4 powder; Step 5: Mix epoxy resin with anhydrous ethanol, stir at a constant temperature until uniform, add CuO / Co3O4 powder obtained in step 4 and disperse evenly, then immerse the foam ceramic obtained in step 2 in it, dry it, and obtain CuO / Co3O4 foam ceramic sample. Step 6: Dissolve the bismuth silicate powder obtained in step 3 and epoxy resin in anhydrous ethanol to obtain a bismuth silicate suspension. Step 7: Place the CuO / Co3O4 foam ceramic sample obtained in Step 5 into the bismuth silicate suspension obtained in Step 6 for vacuum impregnation, and then dry to obtain the CuO / Co3O4-BSO foam ceramic sample.

[0010] The specific method of step 1 includes: The polyurethane foam is immersed in a 15-30 wt% sodium hydroxide solution and pretreated at 60-70℃ for 2-3 h. After washing and drying, it is immersed in a 1.5-2.5 wt% carboxymethyl cellulose solution at room temperature for 2-3 h. The excess carboxymethyl cellulose solution is removed and squeezed out, and the foam is dried for 8-10 h to obtain the modified polyurethane foam.

[0011] The specific method for step 2 includes: In a ball mill jar, 16–32 parts by weight of desulfurization ash, 9–20 parts by weight of desulfurization slag, 1–2 parts by weight of zirconium oxide, 1–2 parts by weight of calcium lignosulfonate, 0.04–0.2 parts by weight of carboxymethyl cellulose, 2.5–5 parts by weight of 3–8 wt% polyvinyl alcohol solution, 5–8 parts by weight of silica sol, and an appropriate amount of deionized water are added to prepare a mixture with a solid content of 50–60 wt%. Then, a ball milling stone is added at a mass ratio of 1:(2–2.2) of the mixture to the ball milling stone, and the mixture is ball milled for 3–5 hours to obtain a ceramic slurry. The modified polyurethane foam obtained in step 1 is immersed in the ceramic slurry, then removed and excess slurry is taken out. This process is repeated 2 to 3 times, followed by drying for 8 to 10 hours to obtain a ceramic green body. The green body is then sintered in a high-temperature box-type resistance furnace at 1000 to 1200°C and held at the sintering temperature for 1 to 2 hours to obtain foam ceramic.

[0012] The specific method for step 3 includes: Deionized water and ethylene glycol were mixed at a volume ratio of 1:(1-3), and bismuth nitrate pentahydrate was added to form solution A with a concentration of 0.5-0.7 mol / L. Sodium metasilicate nonahydrate was dissolved in deionized water to form solution B with a concentration of 0.8–1.5 mol / L; According to the volume ratio of solution A to solution B of (1-1.5):1, solution B is slowly added dropwise to solution A and stirred for 20-30 min to obtain a white emulsion-like bismuth silicate precursor solution. The bismuth silicate precursor solution is loaded into a reaction vessel at a filling ratio of 60%-80% and reacted at 160-180℃ for 10-12 h. After cooling to room temperature with the furnace, the mixture is washed and centrifuged several times with deionized water and anhydrous ethanol alternately. It is then dried in an oven at 50-70℃ and ground to obtain bismuth silicate powder.

[0013] The specific method for step 4 includes: Weigh 10-20 parts by weight of copper oxide and 1-2 parts by weight of cobalt oxide and place them in a ball mill jar. Add a ball mill stone at a mass ratio of 1:(1-2) of mixed powder to ball mill stone. After ball milling for 4-5 hours, a uniform CuO / Co3O4 powder is obtained.

[0014] The specific method for step 5 includes: Weigh 1-2 parts by weight of epoxy resin and 16-32 parts by weight of anhydrous ethanol, stir at 60-70℃ for 10-20 min to obtain a uniformly dispersed mixed solution, denoted as solution C. Add 0.1-0.2 parts by weight of CuO / Co3O4 powder obtained in step 4 to solution C, sonicate for 25-30 min, denoted as solution D. Immerse the foam ceramic obtained in step 2 in solution D for 5-10 min to form an adhesive layer, and dry for 1-3 h to obtain a CuO / Co3O4 foam ceramic sample.

[0015] The specific method for step 6 includes: Dissolve 1-1.4 parts by weight of bismuth silicate powder obtained in step 3 and 1.8-3.5 parts by weight of epoxy resin in 23-48 parts by weight of anhydrous ethanol, and ultrasonically stir for 10-40 min to obtain a bismuth silicate suspension with a solid content of 2-5 wt%.

[0016] The specific method for step 7 includes: The CuO / Co3O4 foam ceramic sample obtained in step 5 is placed in the bismuth silicate suspension obtained in step 6 and vacuum impregnated on both sides 1-2 times for 5-10 min each, and then dried for 1-3 h to obtain the CuO / Co3O4-BSO foam ceramic sample.

[0017] Compared with the prior art, the present invention has the following beneficial effects: This invention provides a porous ceramic catalytic material with synergistic photothermal and conductive enhancement, and its preparation method. The method uses industrial desulfurization ash as the main raw material, and sintersing at a relatively low temperature to obtain a porous ceramic matrix with a rough surface, well-developed pores, and a three-dimensional interconnected structure. Through multiple vacuum impregnation processes, a CuO / Co3O4 intermediate photothermal and conductive layer and a bismuth silicate outer photocatalytic layer are sequentially constructed on its surface and within its internal pores. The intermediate functional layer uses refined CuO / Co3O4 composite powder. Utilizing the density difference between CuO and Co3O4 and the surface tension generated during epoxy resin drying and curing, some of the smaller Co3O4 nanoparticles are deposited on the surface of CuO particles, while others are distributed in the gaps between CuO particles, thus spontaneously forming a continuous, exposed conductive network with multi-level conductive paths. This intermediate layer possesses both dark-color photothermal conversion and spinel structure electronic conduction characteristics, efficiently absorbing visible light and even near-infrared light and converting it into lattice thermal energy, while simultaneously providing a low-resistance transport channel for photogenerated electrons.

[0018] Based on the above structure, a gradient synergistic relationship is formed between the porous ceramic framework, the CuO / Co3O4 intermediate photothermal-conductive layer, and the bismuth silicate outer photocatalytic layer in this invention. This synergistic effect is mainly reflected in the enhanced coupling between the photothermal effect and conductive transport. On the one hand, both CuO and Co3O4 have a dark appearance, enabling them to efficiently absorb visible light and even near-infrared light, converting it into lattice thermal energy. Simultaneously, the spinel structure of Co3O4 endows the functional layer with excellent electronic conductivity. Under illumination, the enhanced lattice thermal vibration caused by the photothermal effect effectively reduces the migration barrier of photogenerated carriers at the interface between bismuth silicate and the conductive layer, as well as within the conductive layer. This makes it easier for photogenerated carriers to cross the interface barrier and be rapidly extracted, thereby significantly improving the separation efficiency of photogenerated electron-hole pairs and the light energy utilization rate. On the other hand, this conductive functional layer can rapidly capture excess photogenerated electrons generated by the photoexcitation of the bismuth silicate photocatalytic layer and efficiently transport them along the low-migration-barrier CuO / Co3O4 conductive path, suppressing the recombination of photogenerated carriers inside the bismuth silicate and extending carrier lifetime. Simultaneously, the excess photogenerated electrons exported through the conductive functional layer can also be transported to the surface of other catalyst particles, reacting with dissolved oxygen molecules adsorbed on the material surface to generate highly oxidizing superoxide radicals (·O2). - This active species can directly act on the main organic pollutants and participate in the oxidative degradation process of pollutants together with photogenerated holes, hydroxyl radicals, etc., thereby adding a reduction activation pathway in addition to the original photocatalytic oxidation pathway, broadening the photocatalytic reaction pathway, and further improving the degradation efficiency of materials for organic pollutants in wastewater and exhaust gas.

[0019] Thus, the resulting composite material combines the high specific surface area of ​​porous ceramics, the photothermal conversion and electron transport capabilities of the conductive functional layer, and the photocatalytic activity of bismuth silicate. Through the synergistic coupling of photothermal effect and conductivity, it effectively overcomes the defects of high carrier recombination rate and low light energy utilization of single photocatalytic materials, and has broad application prospects in environmental governance fields such as wastewater degradation, waste gas purification, antibacterial and deodorizing. Attached Figure Description

[0020] Figure 1 These are SEM images from Embodiment 2 of the present invention; wherein, Figure 1 (a) in the text is CuO. Figure 1 (b) in the text represents Co3O4. Figure 1 (c) in the figure represents a porous ceramic surface. Figure 1 (d) in the figure represents the surface of CuO / Co3O4-BSO foam ceramic. Figure 1 (e) in the text represents CuO / Co3O4 powder.

[0021] Figure 2 This is a graph showing the degradation performance of CuO / Co3O4-BSO foam ceramic sample from Example 3 of this invention on tetracycline hydrochloride and rhodamine B; wherein, Figure 2 (a) in the figure is the degradation performance diagram of 20 mg / L tetracycline; Figure 2 (b) in the figure shows the degradation performance of 10 mg / L Rhodamine B.

[0022] Figure 3 This is a graph showing the photothermal properties of the CuO / Co3O4-BSO foam ceramic sample from Example 1 of this invention.

[0023] Figure 4 These are performance images of the CuO / Co3O4-BSO foam ceramic sample from Example 3 of this invention; wherein, Figure 4 In the figure, (a) represents the photocurrent. Figure 4 (b) in the diagram is the impedance diagram. Detailed Implementation

[0024] The technical solution adopted by the present invention will be further described below with reference to the accompanying drawings and specific embodiments.

[0025] This embodiment provides a porous ceramic catalytic material with photothermal-electrical synergistic enhancement, comprising: a porous ceramic substrate based on sulfur-fixing ash, a CuO / Co3O4 photothermal-electrical functional layer, and a BSO photocatalytic functional layer, and the whole having a three-dimensional interconnected porous framework structure.

[0026] The porous ceramic framework based on sulfur-fixing ash has a rough surface and a continuous open pore structure, which facilitates the attachment of functional components. The CuO / Co3O4 photothermal-conductive functional layer is adhered to the outer surface and part of the inner wall of the pores of the porous ceramic framework based on sulfur-fixing ash through epoxy resin, and is tightly bonded to the framework. Inside the CuO / Co3O4 photothermal-conductive functional layer, smaller Co3O4 particles are dispersed around and at the edges of the blocky CuO particles, connecting adjacent CuO particles to form a photothermal-conductive network with blocky CuO as nodes and Co3O4 particles as bridging branches. Flower-shaped BSO particles are further fixed above the CuO / Co3O4 photothermal-conductive functional layer through epoxy resin to form a BSO photocatalytic active layer. Thus, the CuO / Co3O4-BSO foam ceramic integrates a photothermal-conductive intermediate layer and a photocatalytic outer layer on a three-dimensional porous framework, and has the characteristics of a blocky multifunctional photocatalytic material with porous framework support, photothermal-conductive synergy, and photocatalytic activity.

[0027] Example 1 A method for preparing a porous ceramic catalytic material with synergistic photothermal and electrical conductivity enhancement includes the following steps: Step 1: Immerse polyurethane foam in a 30 wt% sodium hydroxide solution and pretreat it at 70°C for 3 h; then wash and dry it and immerse it in a 2.5 wt% carboxymethyl cellulose solution at 40°C for 3 h; remove and squeeze out excess carboxymethyl cellulose solution, and dry it for 10 h to obtain modified polyurethane foam. Step 2: In a ball mill jar, 32 g of desulfurization ash, 20 g of desulfurization slag, 2 g of zirconium oxide, 2 g of calcium lignosulfonate, 0.2 g of carboxymethyl cellulose, 5 g of polyvinyl alcohol solution (8 wt%), 8 g of silica sol, and 20.8 mL of deionized water are added sequentially to prepare a mixture with a solid content of 60 wt%. Then, grinding stones are added at a mass ratio of 1:2.2 (mixture:grinding stone). The mixture is ball-milled for 5 h to obtain a ceramic slurry. The solid components are desulfurization ash, desulfurization slag, and zirconium oxide; the solutes are calcium lignosulfonate, carboxymethyl cellulose, polyvinyl alcohol, and silica sol; and the solvent is deionized water.

[0028] The modified polyurethane foam obtained in step 1 is immersed in the ceramic slurry, then removed and excess slurry is taken out. This process is repeated 3 times, followed by drying for 10 hours to obtain a ceramic green body. The green body is then sintered in a high-temperature box-type resistance furnace at 1200℃ and held at the sintering temperature for 2 hours to obtain foam ceramic. Step 3: Weigh 14 mmol of bismuth nitrate pentahydrate and dissolve it in a mixed solution of 10 mL of deionized water and 10 mL of ethylene glycol. Stir for 20 min to form solution A with a concentration of 0.7 mol / L. Weigh 7.5 mmol of sodium metasilicate nonahydrate and dissolve it in 5 mL of deionized water to form solution B with a concentration of 1.5 mol / L; According to the volume ratio of solution A to solution B of 1.5:1, solution B was slowly added dropwise to solution A and stirred for 30 min to obtain a white emulsion-like bismuth silicate precursor solution. The bismuth silicate precursor solution was loaded into the reaction vessel at a filling ratio of 80% and reacted at 180℃ for 12 h. After cooling to room temperature with the furnace, the mixture was washed three times alternately with deionized water and anhydrous ethanol, centrifuged, dried in an oven at 70℃, and ground to obtain bismuth silicate powder. Step 4: Weigh 20 g of copper oxide and 2 g of cobalt oxide and put them into a ball mill jar. Add a ball mill stone at a mass ratio of 1:2 for the mixed powder and the ball mill stone. After ball milling for 5 hours, a uniform CuO / Co3O4 powder is obtained. Step 5: Weigh 2 g of epoxy resin and 32 g of anhydrous ethanol, stir at 70℃ for 20 min to obtain a uniformly dispersed mixed solution, denoted as solution C. Add 0.2 g of CuO / Co3O4 powder obtained in step 4 to solution C, sonicate for 30 min, denoted as solution D. Immerse the foam ceramic obtained in step 2 in solution D for 10 min to form an adhesive layer, dry for 3 h to obtain CuO / Co3O4 foam ceramic sample. Step 6: Dissolve 1.4 g of bismuth silicate powder obtained in Step 3 and 3.5 g of epoxy resin in 23.1 g of anhydrous ethanol, and ultrasonically stir for 40 min to obtain a bismuth silicate suspension with a solid content of 5 wt%. The solid component is bismuth silicate powder, the solute is epoxy resin, and the solvent is anhydrous ethanol. Step 7: Place the CuO / Co3O4 foam ceramic sample obtained in Step 5 into the bismuth silicate suspension obtained in Step 6 and perform vacuum impregnation on both sides twice for 10 min each, and dry for 3 h to obtain the CuO / Co3O4-BSO foam ceramic sample.

[0029] Example 2 A method for preparing a porous ceramic catalytic material with synergistic photothermal and electrical conductivity enhancement includes the following steps: Step 1: Immerse polyurethane foam in a 15 wt% sodium hydroxide solution and pretreat it at 60°C for 2 h; then wash and dry it and immerse it in a 1.5 wt% carboxymethyl cellulose solution at 10°C for 2 h; remove and squeeze out excess carboxymethyl cellulose solution, and dry for 8 h to obtain modified polyurethane foam. Step 2: In a ball mill jar, 16 g of desulfurization ash, 9 g of desulfurization slag, 1 g of zirconium oxide, 1 g of calcium lignosulfonate, 0.04 g of carboxymethyl cellulose, 2.5 g of polyvinyl alcohol solution (3 wt%), 5 g of silica sol, and 17.4 mL of deionized water are added sequentially to prepare a mixture with a solid content of 50 wt%. Then, grinding stones are added at a mass ratio of 1:2 for the mixture, and the mixture is ball-milled for 3 hours to obtain a ceramic slurry. The solid components are desulfurization ash, desulfurization slag, and zirconium oxide; the solutes are calcium lignosulfonate, carboxymethyl cellulose, polyvinyl alcohol, and silica sol; and the solvent is deionized water.

[0030] The modified polyurethane foam obtained in step 1 is immersed in the ceramic slurry, then removed and excess slurry is taken out. This process is repeated twice, followed by drying for 8 hours to obtain a ceramic green body. The green body is then sintered in a high-temperature box-type resistance furnace at 1000℃ and held at the sintering temperature for 1 hour to obtain foam ceramic. Step 3: Weigh 7.5 mmol of bismuth nitrate pentahydrate and dissolve it in a mixed solution of 7.5 mL of deionized water and 7.5 mL of ethylene glycol. Stir for 20 min to form solution A with a concentration of 0.5 mol / L. Weigh 12 mmol of sodium metasilicate nonahydrate and dissolve it in 15 mL of deionized water to form solution B with a concentration of 0.8 mol / L; According to the volume ratio of solution A to solution B of 1:1, solution B was slowly added dropwise to solution A and stirred for 20 min to obtain a white emulsion-like bismuth silicate precursor solution. The bismuth silicate precursor solution was loaded into a reaction vessel at a filling ratio of 60% and reacted at 160℃ for 10 h. After cooling to room temperature with the furnace, the mixture was washed three times alternately with deionized water and anhydrous ethanol, centrifuged, dried in an oven at 50℃, and ground to obtain bismuth silicate powder. Step 4: Weigh 10 g of copper oxide and 1 g of cobalt oxide and put them into a ball mill jar. Add a ball mill stone at a mass ratio of 1:1 for the mixed powder and the ball mill stone. After ball milling for 4 hours, a uniform CuO / Co3O4 powder is obtained. Step 5: Weigh 1 g of epoxy resin and 16 g of anhydrous ethanol, stir at 60℃ for 10 min to obtain a uniformly dispersed mixed solution, denoted as solution C. Add 0.1 g of CuO / Co3O4 powder obtained in step 4 to solution C, sonicate for 25 min, denoted as solution D. Immerse the foam ceramic obtained in step 2 in solution D for 5 min to form an adhesive layer, dry for 1 h to obtain the CuO / Co3O4 foam ceramic sample. Step 6: Dissolve 1 g of bismuth silicate powder obtained in Step 3 and 1.8 g of epoxy resin in 47.2 g of anhydrous ethanol, and ultrasonically stir for 10 min to obtain a bismuth silicate suspension with a solid content of 2 wt%. The solid component is bismuth silicate powder, the solute is epoxy resin, and the solvent is anhydrous ethanol.

[0031] Step 7: Place the CuO / Co3O4 foam ceramic sample obtained in Step 5 into the bismuth silicate suspension obtained in Step 6 and vacuum impregnate both sides once for 5 min, then dry for 1 h to obtain the CuO / Co3O4-BSO foam ceramic sample.

[0032] Example 3 A method for preparing a porous ceramic catalytic material with synergistic photothermal and electrical conductivity enhancement includes the following steps: Step 1: Immerse polyurethane foam in a 20 wt% sodium hydroxide solution and pretreat it at 60°C for 2 h; then wash and dry it and immerse it in a 1.75 wt% carboxymethyl cellulose solution at 25°C for 2 h; remove and squeeze out excess carboxymethyl cellulose solution, and dry it for 10 h to obtain modified polyurethane foam. Step 2: In a ball mill jar, 16 g of desulfurization ash, 9 g of desulfurization slag, 1 g of zirconium oxide, 1 g of calcium lignosulfonate, 0.04 g of carboxymethyl cellulose, 5 g of polyvinyl alcohol solution (5 wt%), 5 g of silica sol, and 10.2 mL of deionized water are added sequentially to prepare a mixture with a solid content of 55 wt%. Then, grinding stones are added at a mass ratio of 1:2 for the mixture, and the mixture is ball-milled for 5 hours to obtain a ceramic slurry. The solid components are desulfurization ash, desulfurization slag, and zirconium oxide; the solutes are calcium lignosulfonate, carboxymethyl cellulose, polyvinyl alcohol, and silica sol; and the solvent is deionized water.

[0033] The modified polyurethane foam obtained in step 1 is immersed in the ceramic slurry, then removed and excess slurry is taken out. This process is repeated twice, followed by drying for 8 hours to obtain a ceramic green body. The green body is then sintered in a high-temperature box-type resistance furnace at 1100℃ and held at the sintering temperature for 1.5 hours to obtain foam ceramic. Step 3: Weigh 6 mmol of bismuth nitrate pentahydrate and dissolve it in a mixed solution of 4 mL of deionized water and 5.5 mL of ethylene glycol. Stir for 20 min to form solution A with a concentration of 0.63 mol / L. Weigh 6 mmol of sodium metasilicate nonahydrate and dissolve it in 7 mL of deionized water to form solution B with a concentration of 0.86 mol / L; According to the volume ratio of solution A to solution B of 1.36:1, solution B was slowly added dropwise to solution A and stirred for 30 min to obtain a white emulsion-like bismuth silicate precursor solution. The bismuth silicate precursor solution was loaded into a 25 mL polytetrafluoroethylene reactor at a filling ratio of 66% and reacted at 180℃ for 12 h. After cooling to room temperature in the furnace, the mixture was washed three times alternately with deionized water and anhydrous ethanol, centrifuged, dried in an oven at 50℃, and ground to obtain bismuth silicate powder. Step 4: Weigh 20 g of copper oxide and 1 g of cobalt oxide and put them into a ball mill jar. Add a ball mill stone at a mass ratio of 1:1.5 for the mixed powder and the ball mill stone. After ball milling for 5 hours, a uniform CuO / Co3O4 powder is obtained. Step 5: Weigh 1.5 g of epoxy resin and 23.7 g of anhydrous ethanol, stir at 60℃ for 15 min to obtain a uniformly dispersed mixed solution, denoted as solution C. Add 0.1 g of CuO / Co3O4 powder obtained in step 4 to solution C, sonicate for 30 min, denoted as solution D. Immerse the foam ceramic obtained in step 2 in solution D for 10 min to form an adhesive layer, dry for 2 h to obtain CuO / Co3O4 foam ceramic sample. Step 6: Dissolve 0.6 g of bismuth silicate powder obtained in Step 3 and 1.5 g of epoxy resin in 23.7 g of anhydrous ethanol, and ultrasonically stir for 30 min to obtain a bismuth silicate suspension with a solid content of 2.3 wt%. The solid component is bismuth silicate powder, the solute is epoxy resin, and the solvent is anhydrous ethanol.

[0034] Step 7: Place the CuO / Co3O4 foam ceramic sample obtained in Step 5 into the bismuth silicate suspension obtained in Step 6 and vacuum impregnate both sides once for 10 min. Then dry for 2 h to obtain the CuO / Co3O4-BSO foam ceramic sample.

[0035] Figure 1 These are SEM images from Embodiment 2 of the present invention, wherein, Figure 1 (a) in the text is CuO. Figure 1 (b) in the text represents Co3O4. Figure 1 (c) in the figure represents a porous ceramic surface. Figure 1 (d) in the figure represents the surface of CuO / Co3O4-BSO foam ceramic. Figure 1 (e) in the text represents CuO / Co3O4 powder. For example... Figure 1 As shown in (a), CuO exhibits a flower-like structure overall; for example... Figure 1 As shown in (b), Co3O4 has a broccoli-like structure; Figure 1 As shown in (c), the rough surface of porous ceramics with numerous tiny pores enhances the adhesion of the functional layer to the porous ceramic surface; for example... Figure 1As shown in (d), the microstructure of the CuO / Co3O4 photothermal-conductive functional layer consists of small Co3O4 nanoparticles deposited on and around the CuO surface, forming an exposed, dark-colored photothermal-conductive network on the porous ceramic surface; for example... Figure 1 As shown in (e), the flower-shaped BSO in the catalyst layer is in direct contact with the CuO / Co3O4 photothermal-conductive functional layer, forming a multi-layered, multifunctional porous block photocatalytic material.

[0036] Figure 2 This is a graph showing the degradation performance of CuO / Co3O4-BSO foam ceramic sample from Example 3 of this invention on tetracycline hydrochloride and rhodamine B; wherein, Figure 2 (a) in the figure is the degradation performance diagram of 20 mg / L tetracycline; Figure 2 (b) shows the degradation performance of 10 mg / L Rhodamine B. After 150 min of light exposure, as shown... Figure 2 As shown in (a), the degradation rates of TC for the sample loaded with BSO alone and the CuO / Co3O4-BSO foam ceramic sample were 66.7% and 88.1%, respectively; Figure 2 As shown in (b), the degradation rates of TC by the BSO-loaded sample and the CuO / Co3O4-BSO foam ceramic sample were 84.3% and 88.6%, respectively. The results indicate that the CuO / Co3O4 functional layer can effectively improve the photocatalytic performance of the foam ceramic sample.

[0037] Figure 3 This is a photothermal performance diagram of the CuO / Co3O4-BSO foam ceramic sample from Example 1 of this invention. After irradiation for 25 min, the K of the CuO / Co3O4 foam ceramic sample increased from 293 K to 323 K, the K of the CuO / Co3O4-BSO foam ceramic sample increased from 293 K to 315 K, while the K of the BSO foam ceramic sample only increased to 300 K. The results indicate that the CuO / Co3O4 functional layer can effectively improve the photothermal performance of the foam ceramic samples.

[0038] Figure 4 These are performance images of the CuO / Co3O4-BSO foam ceramic sample from Example 3 of this invention; wherein, Figure 4 In the figure, (a) represents the photocurrent. Figure 4 (b) in the diagram is an impedance diagram. From... Figure 4 As shown in (a), the photocurrent generated by loading a CuO / Co3O4 functional layer is 3 times that of loading pure BSO and 1.5 times that of loading a CuO functional layer. Figure 4 As shown in (b), the impedance after loading with the CuO / Co3O4 functional layer is 1 / 2 that of the impedance after loading with pure BSO and 3 / 4 that of the impedance after loading with the CuO functional layer. The results indicate that the CuO / Co3O4 functional layer can effectively enhance the photocurrent and conductivity of the material.

Claims

1. A porous ceramic catalytic material with synergistic photothermal and electrical conductivity enhancement, characterized in that, include: The porous ceramic substrate based on sulfur-fixing ash slag, the CuO / Co3O4 photothermal-conductive functional layer, and the BSO photocatalytic functional layer together form a three-dimensional interconnected porous framework structure.

2. The porous ceramic catalytic material with photothermal-conductive synergistic enhancement according to claim 1, characterized in that, The porous ceramic framework based on sulfur-fixing ash has a rough surface and a continuous open pore structure, which facilitates the adhesion of functional components. The CuO / Co3O4 photothermal-conductive functional layer is adhered to the outer surface and part of the inner wall of the pores of the porous ceramic framework based on sulfur-fixing ash through epoxy resin, and is tightly bonded to the framework. Inside the CuO / Co3O4 photothermal-conductive functional layer, Co3O4 particles are dispersed around and at the edges of the blocky CuO particles, connecting adjacent CuO particles to form a photothermal-conductive network with blocky CuO as nodes and Co3O4 particles as bridging branches. The flower-shaped BSO particles are further fixed above the CuO / Co3O4 photothermal-conductive functional layer through epoxy resin to form a BSO photocatalytic active layer.

3. A method for preparing a porous ceramic catalytic material with synergistic photothermal and electrical conductivity enhancement, characterized in that, Includes the following steps: Step 1: The polyurethane foam is pretreated with sodium hydroxide solution and then soaked in carboxymethyl cellulose solution. After drying, the modified polyurethane foam is obtained. Step 2: Mix and ball-mill the sulfur-fixing ash, sulfur-fixing slag, zirconium oxide, calcium lignosulfonate, carboxymethyl cellulose, silica sol, polyvinyl alcohol solution, and deionized water to obtain a ceramic slurry; then immerse the modified polyurethane foam in the ceramic slurry and sinter it to obtain foam ceramic. Step 3: Dissolve bismuth nitrate pentahydrate and sodium metasilicate nonahydrate, stir evenly and mix thoroughly, then perform hydrothermal treatment and washing to obtain bismuth silicate powder; Step 4: Ball mill and mix copper oxide and cobalt oxide to obtain CuO / Co3O4 powder; Step 5: Mix epoxy resin with anhydrous ethanol, stir at a constant temperature until uniform, add CuO / Co3O4 powder obtained in step 4 and disperse evenly, then immerse the foam ceramic obtained in step 2 in it, dry it, and obtain CuO / Co3O4 foam ceramic sample. Step 6: Dissolve the bismuth silicate powder obtained in step 3 and epoxy resin in anhydrous ethanol to obtain a bismuth silicate suspension. Step 7: The CuO / Co3O4 foam ceramic sample obtained in Step 5 is placed in the bismuth silicate suspension obtained in Step 6 for vacuum impregnation, and then dried to obtain the CuO / Co3O4-BSO foam ceramic sample.

4. The method for preparing a porous ceramic catalytic material with synergistic photothermal-electrical conductivity enhancement according to claim 3, characterized in that, The specific method of step 1 includes: The polyurethane foam is immersed in a 15-30 wt% sodium hydroxide solution and pretreated at 60-70℃ for 2-3 h. After washing and drying, it is immersed in a 1.5-2.5 wt% carboxymethyl cellulose solution at room temperature for 2-3 h. The excess carboxymethyl cellulose solution is removed and squeezed out, and the foam is dried for 8-10 h to obtain the modified polyurethane foam.

5. The method for preparing a porous ceramic catalytic material with synergistic photothermal-electrical conductivity enhancement according to claim 3, characterized in that, The specific method for step 2 includes: In a ball mill jar, 16–32 parts by weight of desulfurization ash, 9–20 parts by weight of desulfurization slag, 1–2 parts by weight of zirconium oxide, 1–2 parts by weight of calcium lignosulfonate, 0.04–0.2 parts by weight of carboxymethyl cellulose, 2.5–5 parts by weight of 3–8 wt% polyvinyl alcohol solution, 5–8 parts by weight of silica sol, and an appropriate amount of deionized water are added to prepare a mixture with a solid content of 50–60 wt%. A ball mill stone is added at a mass ratio of 1:(2–2.2) of the mixture to the ball mill stone, and the mixture is ball milled for 3–5 h to obtain a ceramic slurry. The modified polyurethane foam obtained in step 1 is immersed in the ceramic slurry, then removed and excess slurry is taken out. This process is repeated 2 to 3 times, followed by drying for 8 to 10 hours to obtain a ceramic green body. The green body is then sintered in a high-temperature box-type resistance furnace at 1000 to 1200°C and held at the sintering temperature for 1 to 2 hours to obtain foam ceramic.

6. The method for preparing a porous ceramic catalytic material with synergistic photothermal-electrical conductivity enhancement according to claim 3, characterized in that, The specific method for step 3 includes: Deionized water and ethylene glycol were mixed at a volume ratio of 1:(1-3), and bismuth nitrate pentahydrate was added to form solution A with a concentration of 0.5-0.7 mol / L. Sodium metasilicate nonahydrate was dissolved in deionized water to form solution B with a concentration of 0.8–1.5 mol / L; According to the volume ratio of solution A to solution B of (1-1.5):1, solution B is slowly added dropwise to solution A and stirred for 20-30 min to obtain a white emulsion-like bismuth silicate precursor solution. The bismuth silicate precursor solution is loaded into a reaction vessel at a filling ratio of 60%-80% and reacted at 160-180℃ for 10-12 h. After cooling to room temperature with the furnace, the mixture is washed and centrifuged several times with deionized water and anhydrous ethanol alternately. It is then dried in an oven at 50-70℃ and ground to obtain bismuth silicate powder.

7. The method for preparing a porous ceramic catalytic material with synergistic photothermal-electrical conductivity enhancement according to claim 3, characterized in that, The specific method for step 4 includes: Weigh 10-20 parts by weight of copper oxide and 1-2 parts by weight of cobalt oxide and place them in a ball mill jar. Add a ball mill stone at a mass ratio of 1:(1-2) of mixed powder to ball mill stone. After ball milling for 4-5 hours, a uniform CuO / Co3O4 powder is obtained.

8. The method for preparing a porous ceramic catalytic material with synergistic photothermal-electrical conductivity enhancement according to claim 3, characterized in that, The specific method for step 5 includes: Weigh 1-2 parts by weight of epoxy resin and 16-32 parts by weight of anhydrous ethanol, stir at 60-70℃ for 10-20 min to obtain a uniformly dispersed mixed solution, denoted as solution C. Add 0.1-0.2 parts by weight of CuO / Co3O4 powder obtained in step 4 to solution C, sonicate for 25-30 min, denoted as solution D. Immerse the foam ceramic obtained in step 2 in solution D for 5-10 min to form an adhesive layer, and dry for 1-3 h to obtain a CuO / Co3O4 foam ceramic sample.

9. The method for preparing a porous ceramic catalytic material with synergistic photothermal-electrical conductivity enhancement according to claim 3, characterized in that, The specific method for step 6 includes: Dissolve 1-1.4 parts by weight of bismuth silicate powder obtained in step 3 and 1.8-3.5 parts by weight of epoxy resin in 23-48 parts by weight of anhydrous ethanol, and ultrasonically stir for 10-40 min to obtain a bismuth silicate suspension with a solid content of 2-5 wt%.

10. The method for preparing a porous ceramic catalytic material with synergistic photothermal-electrical conductivity enhancement according to claim 3, characterized in that, The specific method for step 7 includes: The CuO / Co3O4 foam ceramic sample obtained in step 5 is placed in the bismuth silicate suspension obtained in step 6 and vacuum impregnated on both sides 1-2 times for 5-10 min each, and then dried for 1-3 h to obtain the CuO / Co3O4-BSO foam ceramic sample.

Citation Information

Patent Citations

  • Titanium dioxide-based porous ceramic composite material with photo-thermal performance and preparation method of titanium dioxide-based porous ceramic composite material

    CN118125860A

  • Preparation method of foamed ceramic-metal organic framework composite catalytic material and application of foamed ceramic-metal organic framework composite catalytic material in photo-thermal catalytic elimination of nitro compound

    CN120205227A