A method for preparing a flower-shaped nitrogen-doped carbon-coated Mn-CdSe (Mn-CdSe@NC) photocatalyst

By preparing a flower-shaped nitrogen-doped carbon-coated Mn-CdSe photocatalyst, the problem of photogenerated electron-hole pair recombination in CdSe nanoparticles was solved, achieving highly efficient photocatalytic oxidation of benzylamine coupling and improving the activity and stability of the catalyst.

CN123102397APending Publication Date: 2026-11-17XUZHOU NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510629371.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The photocatalytic activity of existing CdSe nanoparticles is inhibited by the recombination of photogenerated electron-hole pairs. The impurity energy levels introduced by doping reduce the separation efficiency of photogenerated carriers, resulting in a decrease in catalytic activity.

Method used

A method for preparing Mn-CdSe (Mn-CdSe@NC) photocatalysts with a flower-like nitrogen-doped carbon coating was adopted. Using Mn/Cd-MOF as a precursor, nitrogen-doped carbon material was formed by high-temperature calcination and then combined with CdSe to improve the separation and migration efficiency of photogenerated carriers.

Benefits of technology

It exhibits excellent photocatalytic oxidation of benzylamine coupling performance under visible light, which significantly improves the activity and stability of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0005404882830000011
    Figure HDA0005404882830000011
  • Figure HDA0005404882830000012
    Figure HDA0005404882830000012
  • Figure HDA0005404882830000021
    Figure HDA0005404882830000021
Patent Text Reader

Abstract

This paper describes a method for preparing a flower-shaped nitrogen-doped carbon-coated Mn-CdSe (Mn-CdSe@N-C) photocatalyst. The method involves dissolving terephthalic acid in N,N-dimethylformamide solution and stirring until the solution becomes clear. Then, anhydrous ethanol, water, and ethylene glycol are added sequentially to the solution, and after thorough stirring, cadmium acetate dihydrate and manganese acetate tetrahydrate are added. After stirring for 4 hours, the mixture is transferred to a reactor and reacted at 150°C for 12 hours. After the reaction is complete, a white flower-shaped Mn / Cd-MOF precursor is obtained by centrifugation, washing, and drying. The Mn / Cd-MOF precursor and selenium powder are placed at both ends of a magnetic boat and calcined in a tube furnace to finally obtain the flower-shaped Mn-CdSe@N-C. The resulting nitrogen-doped carbon-coated Mn-CdSe (Mn-CdSe@N-C) porous structure exhibits excellent photocatalytic oxidation of benzylamine coupling performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of photocatalytic nanomaterial preparation technology, specifically to a method for preparing a flower-shaped nitrogen-doped carbon-coated Mn-CdSe (Mn-CdSe@NC) photocatalyst. Background Technology

[0002] Imines, as important precursors in the synthesis of fine chemicals and pharmaceuticals, play a significant role in fields such as medicine, agrochemicals, and synthetic chemistry. In recent years, the direct coupling of amines and imines catalyzed by photocatalysis has attracted widespread attention. Therefore, developing efficient and stable semiconductor photocatalysts is crucial for advancements in photocatalysis technology. Cadmium selenide (CdSe) is considered one of the most promising semiconductor materials due to its unique optical, electronic, and catalytic properties. CdSe nanoparticles possess semiconductor properties with narrow band gaps and high excitation energies, readily exciting electrons from the valence band to the conduction band under illumination. However, the recombination of photogenerated electron-hole pairs is suppressed; thus, photoinduced electrons and holes are neutralized before photocatalytic activity begins. To improve the photocatalytic activity of CdSe, transition metal ion doping is employed. Doping alters the band structure of semiconductor materials, reducing their band width and lowering the required excitation energy. However, the impurity levels introduced by doping often become recombination centers for photogenerated electrons and holes, reducing the separation efficiency of photogenerated carriers and consequently decreasing the photocatalytic activity of CdSe. Studies have shown that combining photocatalysts with carbon materials can effectively improve the electron mobility of photocatalysts, thereby enhancing the separation and migration efficiency of photogenerated carriers.

[0003] Therefore, this paper proposes a method for preparing flower-shaped nitrogen-doped carbon-coated Mn-CdSe (Mn-CdSe@NC) photocatalysts. These photocatalysts exhibit excellent photocatalytic oxidation of benzylamine coupling under visible light, providing an effective strategy for designing and developing highly efficient photocatalysts for future applications. Summary of the Invention

[0004] 1. Purpose of the invention: The purpose of this invention is to provide a method for preparing a flower-shaped nitrogen-doped carbon-coated Mn-CdSe (Mn-CdSe@NC) photocatalyst. This method uses Mn / Cd-MOF as a precursor and obtains a flower-shaped nitrogen-doped carbon-coated Mn-CdSe (Mn-CdSe@NC) photocatalyst by high-temperature calcination and selenization. This effectively improves the separation efficiency of photogenerated carriers and thus exhibits excellent photocatalytic oxidation of benzylamine coupling performance.

[0005] 2. Technical Solution

[0006] Synthesis of Mn / Cd-MOF precursors

[0007] Terephthalic acid was dissolved in N,N-dimethylformamide solution and stirred until the solution became clear. Then, anhydrous ethanol, water, and ethylene glycol were added sequentially to the solution, and the mixture was stirred thoroughly. Cadmium acetate dihydrate and manganese acetate tetrahydrate were then added to the mixture, and the mixture was stirred for 4 hours. The mixture was then transferred to a reaction vessel and reacted at 150°C for 12 hours. After the reaction was complete, the product was centrifuged, washed, and dried to obtain a white, flower-shaped Mn / Cd-MOF precursor.

[0008] Preparation of nitrogen-doped carbon-coated Mn-CdSe (Mn-CdSe@NC) photocatalyst

[0009] The Mn / Cd-MOF precursor and selenium powder were placed at both ends of a magnetic boat and calcined in a tube furnace under an Ar / H2 atmosphere for 2 hours to finally obtain Mn-CdSe@NC.

[0010] 3. Beneficial effects

[0011] This study successfully synthesized nitrogen-doped carbon-coated Mn-CdSe (Mn-CdSe@NC) with a flower-like structure using a bimetallic MOF as a precursor. A series of theoretical and experimental studies showed that undoped CdSe nanoparticles exhibited low catalytic efficiency for benzylamine coupling. Optimal Mn... 2+ The doping level significantly improved the photocatalytic performance of CdSe. Mn ion doping generates impurity energy levels, promoting light absorption. Furthermore, compositing with nitrogen-doped carbon materials not only further enhances electron transport capabilities, but the polarization effect induced by nitrogen doping also results in a high positron density in the carbon materials, further improving their conductivity and effectively addressing the problem of easy recombination of photogenerated carriers. Photocatalytic testing results show that the Mn-CdSe@NC photocatalyst exhibits excellent photocatalytic activity in the benzylamine coupling reaction under blue light and air conditions. This study provides a new research method for the development of highly efficient visible light catalysts, promoting future applications in organic reactions. Attached Figure Description

[0012] Figure 1 Here are the elemental distribution diagrams (af) of the Mn / Cd-MOF precursor prepared in the embodiments of the present invention, (a) being a scanning electron microscope image of Mn / Cd-MOF; and (bf) being an elemental distribution diagram.

[0013] Figure 2 This is the X-ray powder diffraction (XRD) pattern of the Mn / Cd-MOF precursor prepared in the embodiments of the present invention;

[0014] Figure 3The following are elemental distribution diagrams (af) and (bf) of the flower-shaped nitrogen-doped carbon-coated Mn-CdSe (Mn-CdSe@NC) photocatalyst prepared in the embodiments of the present invention. (a) is a scanning electron microscope image of Mn-CdSe@NC; (bf) is an elemental distribution diagram.

[0015] Figure 4 This is an X-ray powder diffraction (XRD) pattern of the flower-shaped nitrogen-doped carbon-coated Mn-CdSe (Mn-CdSe@NC) photocatalyst prepared in the embodiments of the present invention;

[0016] Figure 5 The Raman spectrum of the flower-shaped nitrogen-doped carbon-coated Mn-CdSe (Mn-CdSe@NC) photocatalyst prepared in the embodiments of the present invention is shown.

[0017] Figure 6 This is a benzylamine coupling performance test diagram of the flower-shaped nitrogen-doped carbon-coated Mn-CdSe (Mn-CdSe@NC) photocatalyst prepared in the embodiments of the present invention. Detailed Implementation

[0018] Example 1: Synthesis of Mn / Cd-MOF precursor

[0019] 240 mg of terephthalic acid was dissolved in 10 mL of N,N-dimethylformamide solution and stirred until the solution became clear. Then, 10 mL of anhydrous ethanol, 5 mL of water, and 5 mL of ethylene glycol were added sequentially to the solution, and the mixture was stirred thoroughly. Next, 550 mg of cadmium acetate dihydrate and 24.5 mg of manganese acetate tetrahydrate were added to the mixture, and the mixture was stirred for 4 hours. The mixture was then transferred to a reaction vessel and reacted at 150 °C for 12 hours. After the reaction was complete, the product was centrifuged, washed, and dried to obtain a white, flower-shaped Mn / Cd-MOF precursor.

[0020] Figures 1-2 The images show the SEM, XRD, and elemental analysis results of the sample prepared in Example 1. Figure 1 As can be seen, the Mn / Cd-MOF precursor synthesized in this embodiment has a flower-like structure composed of rods, and is composed of five elements: Mn, Cd, C, O, and N, with uniform elemental distribution. According to... Figure 2 The phase of the synthesized sample can be identified as Mn / Cd-MOF.

[0021] Example 2: Preparation of nitrogen-doped carbon-coated Mn-CdSe (Mn-CdSe@NC) photocatalyst

[0022] 30 mg of Mn / Cd-MOF precursor and 120 mg of selenium powder were placed at both ends of a magnetic boat and calcined in a tube furnace at 500 °C for 2 h under an Ar / H2 atmosphere to finally obtain nitrogen-doped carbon-coated Mn-CdSe (Mn-CdSe@NC) photocatalyst.

[0023] Figures 3-4 The images show the SEM, elemental analysis chromatogram, and XRD of the Mn-CdSe@NC sample prepared in Example 2. Figure 3 It can be seen that the prepared Mn-CdSe@NC has a flower-like morphology, and the Mn-CdSe@NC synthesized in this embodiment is composed of five elements: Mn, Cd, Se, N, and C, with uniform element distribution. According to... Figure 4 The X-ray powder diffraction peak positions of nitrogen-doped carbon-coated Mn-CdSe (Mn-CdSe@NC) photocatalyst match those of CdSe, proving that the material Mn-CdSe@NC has been successfully synthesized.

[0024] Figure 5 This is the Raman spectrum of the Mn-CdSe@NC sample prepared in Example 2. According to... Figure 5 This proves that Mn-CdSe@NC was successfully coated with a carbon layer.

[0025] Figure 6 This is a performance diagram of the photocatalytic oxidation of benzylamine coupling reaction using Mn-CdSe@NC. From... Figure 6 As can be seen, the catalyst has good catalytic efficiency. Furthermore, after five cycles, the conversion rate of benzylamine can reach over 90%, thus demonstrating the catalyst's good stability.

Claims

1. A method for preparing a flower-shaped nitrogen-doped carbon-coated Mn-CdSe (Mn-CdSe@NC) photocatalyst, characterized in that, Includes the following steps: (a) Synthesis of Mn / Cd-MOF precursors: Terephthalic acid was dissolved in N,N-dimethylformamide solution and stirred until the solution became clear. Then, anhydrous ethanol, water, and ethylene glycol were added sequentially to the solution, and the mixture was stirred thoroughly. Cadmium acetate dihydrate and manganese acetate tetrahydrate were then added to the mixture, and after stirring for 4 hours, the solution was transferred to a reaction vessel and reacted at 150°C for 12 hours. After the reaction was complete, the product was centrifuged, washed, and dried to obtain a white, flower-shaped Mn / Cd-MOF precursor. (b) Synthesis of Mn-CdSe@NC photocatalyst: The Mn / Cd-MOF precursor and selenium powder were placed at both ends of a magnetic boat and calcined in a tube furnace under an Ar / H2 atmosphere for 2 hours to finally obtain Mn-CdSe@NC.

2. The preparation method according to claim 1, characterized in that, In the synthesis of the Mn / Cd-MOF, cadmium acetate dihydrate and manganese acetate tetrahydrate are used as Cd... 2+ and Mn 2+ The source is terephthalic acid as the organic ligand, and N,N-dimethylformamide, anhydrous ethanol, water and ethylene glycol as the reaction solution.

3. The preparation method according to claim 1, characterized in that, In the synthesis of Mn / Cd-MOF, the heating temperature was 150℃ and the reaction time was 12h.

4. The preparation method according to claim 1, characterized in that, In the synthesis of Mn / Cd-MOF, Mn 2+ with cd 2+ The molar ratio is 1:

20.

5. The preparation method according to claim 1, characterized in that, In the synthesis of Mn / Cd-MOF, the volume ratio of N,N-dimethylformamide, anhydrous ethanol, water, and ethylene glycol is 2:2:1:

1.

6. The preparation method according to claim 1, characterized in that, In the synthesis of Mn-CdSe@NC, the mass ratio of Mn / Cd-MOF precursor to selenium powder is 1:

4.

7. The preparation method according to claim 1, characterized in that, In the synthesis of Mn-CdSe@NC, the calcination conditions were as follows: under an Ar / H2 atmosphere, at 5 °C·min. -1 The heating rate was increased to 500℃, and calcination was carried out for 2 hours.