A Pt-K-Ce@S-1 composite catalyst, its preparation method and application
By preparing the Pt-K-Ce@S-1 composite catalyst, the problems of low stability and toxic metal in existing catalysts were solved, achieving efficient alkane dehydrogenation and aromatization reactions, improving hexane conversion and olefin and aromatic yields, and making it suitable for industrial production.
Patent Information
- Application Number
- CN202611393664.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-09
- Publication Date
- 2026-11-17
AI Technical Summary
Existing catalysts exhibit low stability during alkane dehydrogenation and aromatization processes and contain toxic metal elements, leading to rapid catalyst deactivation and environmental pollution risks, making it difficult to meet the demand for efficient production of olefins and aromatics.
The Pt-K-Ce@S-1 composite catalyst is composed of an all-silica ZSM-5 molecular sieve and Pt metal and K additives confined within its pores. It is prepared by hydrothermal crystallization and calcination, avoiding the use of toxic metals. K and Ce are used to improve the dispersibility and adsorption capacity of Pt, and the pore confinement effect of ZSM-5 molecular sieve is fully utilized to prevent metal agglomeration.
It achieves high hexane conversion rate and high olefin and aromatic yield, improves catalyst stability, is suitable for industrial production, is green and environmentally friendly, and has low cost.
Smart Images

Figure CN123102405A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of catalyst technology, specifically relating to a Pt-K-Ce@S-1 composite catalyst, its preparation method, and its application. Background Technology
[0002] Coal gasification followed by Fischer-Tropsch synthesis to produce liquid fuels or methanol-to-hydrocarbons (MTH) to produce chemicals is an important technological pathway for clean, non-petroleum-dependent conversion. However, these processes often generate large amounts of low-value alkane byproducts (including both short-chain and long-chain alkanes), which lack economically viable utilization methods, resulting in significantly low carbon resource utilization rates.
[0003] Olefins and aromatics are key raw materials and platform molecules for the synthesis of various fine chemicals (such as rubber, polyester, fibers, and plastics), and market demand continues to grow. Currently, the production of olefins and aromatics is highly dependent on the catalytic reforming of petroleum fractions and the extraction of cracked gasoline. However, the increasing scarcity of petroleum resources and the uncertainty of the international geopolitical situation make it difficult for traditional supply models to meet medium- and long-term demand, necessitating the development of new processes for the production of olefins and aromatics that are not dependent on crude oil. Converting low-value alkanes into high-value-added olefins and aromatics through dehydrogenation and aromatization reactions provides a feasible solution that balances resource efficiency and raw material diversification.
[0004] Currently, extensive research has been conducted on the dehydrogenation of alkanes to olefins and the aromatization of olefins to aromatics, resulting in the development of various highly efficient metal-modified molecular sieve systems. For example, industrially used propane dehydrogenation catalysts are PtSn / Al₂O₃ and Cr₂O₃ / Al₂O₃, but these catalytic systems face challenges such as low stability and rapid catalyst deactivation requiring continuous regeneration. A PtCr@MFI catalyst has been developed for hexane aromatization, achieving hexane conversion of 70.4% and aromatic selectivity of 69.3% at 500℃. Despite significant progress, these catalytic systems often incorporate the toxic metal chromium during synthesis; although the Cr content is low, it still poses risks of environmental pollution and human health. Therefore, there is an urgent need to develop a catalytic system free of toxic metal elements that can effectively promote alkane dehydrogenation and aromatization reactions. Summary of the Invention
[0005] In view of this, the purpose of this invention is to provide a Pt-K-Ce@S-1 composite catalyst, its preparation method and application. The Pt-K-Ce@S-1 composite catalyst provided by this invention catalyzes the hexane dehydrogenation-aromatization reaction, which has the advantages of high hexane conversion, high olefin and aromatic yield, and high reaction stability, and does not contain any toxic metal elements.
[0006] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a Pt-K-Ce@S-1 composite catalyst, which consists of an all-silica ZSM-5 molecular sieve and Pt metal, K and Ce promoter confined within the pores of the all-silica ZSM-5 molecular sieve.
[0007] Preferably, the Pt-K-Ce@S-1 composite catalyst contains 0.2-2.0% Pt metal, 0.5-2.0% K promoter, and 0.1-3.0% Ce promoter.
[0008] This invention also provides a method for preparing the Pt-K-Ce@S-1 composite catalyst described in the above technical solution, comprising the following steps: A mixed salt solution containing Pt, K, and Ce elements is mixed with an organic amine ligand, and the resulting mixed solution is mixed with an initial gel for the synthesis of all-silica ZSM-5 molecular sieves to obtain a synthetic gel solution; the mixed salt solution containing Pt, K, and Ce elements includes soluble Pt salt, soluble K salt, and soluble Ce salt. The synthesized gel solution was subjected to hydrothermal crystallization, and the resulting hydrothermal crystallization product was subjected to solid-liquid separation. The resulting solid product was then dried and calcined to obtain the Pt-K-Ce@S-1 composite catalyst.
[0009] Preferably, the molar ratio of Pt, K and Ce in the mixed salt solution containing Pt, K and Ce is 1:1.3~50:0.1~20.
[0010] Preferably, the molar ratio of total metal ions to organic amine ligands in the mixed salt solution containing Pt, K and Ce elements is 1:2 to 50.
[0011] Preferably, the hydrothermal crystallization temperature is 150~200℃; the hydrothermal crystallization time is 30~120h.
[0012] Preferably, the molar ratio of the effective component SiO2, template agent and H2O in the initial gel of the all-silica ZSM-5 molecular sieve synthesis is 1:0.2~0.8:20~100.
[0013] Preferably, the calcination temperature is 500~650℃, and the holding time is 5~10h.
[0014] This invention also provides the application of the Pt-K-Ce@S-1 composite catalyst described in the above technical solution or the Pt-K-Ce@S-1 composite catalyst prepared by the preparation method described in the above technical solution in the catalytic aromatization of hexane.
[0015] This invention also provides a method for preparing aromatics by hexane dehydrogenation-aromatization, comprising the following steps: A hexane-nitrogen mixture is subjected to a catalytic hexane dehydrogenation-aromatization reaction in the presence of a catalyst to obtain olefins and aromatics; the catalyst is the Pt-K-Ce@S-1 composite catalyst described in the above technical solution or the Pt-K-Ce@S-1 composite catalyst prepared by the preparation method described in the above technical solution.
[0016] This invention provides a Pt-K-Ce@S-1 composite catalyst, which consists of an all-silica ZSM-5 molecular sieve (S-1) and Pt metal, K and Ce promoter confined within the pores of the all-silica ZSM-5 molecular sieve.
[0017] Beneficial effects: This invention provides a Pt-K-Ce@S-1 composite catalyst composed of an all-silica ZSM-5 molecular sieve (S-1) and Pt metal, K, and Ce promoters confined within its pores, containing no toxic metal elements. In this composite catalyst, Pt is the main active site for alkane dehydrogenation to olefins and olefin aromatization to aromatics, while K and Ce are important structural promoters. The introduction of K and Ce can improve the dispersion of Pt sites and enhance their ability to adsorb alkanes, thereby improving hexane conversion, olefin and aromatic yields. Furthermore, the molecular sieve-encapsulated metal catalyst designed in this invention can fully utilize the pore confinement effect of the ZSM-5 molecular sieve, limiting the rapid aggregation and sintering of metal sites, thus improving the stability of the composite catalyst. Example results show that the Pt-K-Ce@S-1 composite catalyst provided by this invention, when used to catalyze the hexane dehydrogenation-aromatization reaction, achieves an olefin and aromatic yield of 47.1%, a hexane conversion of 57.6%, and no significant deactivation of the catalyst after 24 hours of reaction.
[0018] This invention provides a method for preparing the above-mentioned Pt-K-Ce@S-1 composite catalyst. This preparation method is simple to operate, produces no secondary pollution, is green and environmentally friendly, has low production cost, and is suitable for industrial production applications. Attached Figure Description
[0019] Figure 1 The XRD pattern of the Pt-K-Ce@S-1 composite catalyst prepared in Example 1; Figure 2 TEM image of the Pt-K-Ce@S-1 composite catalyst prepared in Example 1; Figure 3 The figure shows the stability test results of the hexane dehydrogenation-aromatization reaction catalyzed by the Pt-K-Ce@S-1 composite catalyst prepared in Example 1, where a is the hexane conversion and b is the product selectivity. Detailed Implementation
[0020] This invention provides a Pt-K-Ce@S-1 composite catalyst, which consists of an all-silica ZSM-5 molecular sieve (S-1) and Pt metal, K and Ce promoter confined within the pores of the all-silica ZSM-5 molecular sieve.
[0021] Unless otherwise specified, the present invention does not have special requirements on the source of raw materials used, and commercially available products well known to those skilled in the art can be used.
[0022] As one embodiment, the Pt-K-Ce@S-1 composite catalyst does not contain any toxic metal elements.
[0023] In one embodiment, the mass fraction (x%) of Pt metal in the Pt-K-Ce@S-1 composite catalyst is 0.2~2.0%, in another embodiment it is 0.25~1.5%, and in a specific embodiment it is 0.30~1.0%; the mass fraction (y%) of K promoter is 0.5~2.0%, in another embodiment it is 1.0~2.0%, and in a specific embodiment it is 1.5~2.0%; and the mass fraction (z%) of Ce promoter is 0.1~3.0%, in another embodiment it is 0.2~2.5%, and in a specific embodiment it is 1.0~2.0%.
[0024] In one embodiment, the particle size of the Pt-K-Ce@S-1 composite catalyst is 10-60 mesh; in another embodiment, it is 20-50 mesh; and in a specific embodiment, it is 20-40 mesh. In this invention, controlling the particle size of the Pt-K-Ce@S-1 composite catalyst within the above range is beneficial for hexane dehydrogenation and aromatization to produce olefins and aromatics.
[0025] In the Pt-K-Ce@S-1 composite catalyst provided by this invention, Pt is the main active site for alkane dehydrogenation to olefins and olefin aromatization to aromatics, while K and Ce are important structural promoters. The introduction of K and Ce can improve the dispersion of Pt sites and enhance their ability to adsorb alkanes, thereby improving hexane conversion, olefin and aromatic yields. Furthermore, the molecular sieve-encapsulated metal catalyst designed in this invention can fully utilize the pore confinement effect of ZSM-5 molecular sieves, limiting the rapid aggregation and sintering of metal sites, thus improving the stability of the composite catalyst.
[0026] This invention provides a method for preparing the Pt-K-Ce@S-1 composite catalyst described above, comprising the following steps: A mixed salt solution containing Pt, K, and Ce elements is mixed with an organic amine ligand, and the resulting mixed solution is mixed with an initial gel for the synthesis of all-silica ZSM-5 molecular sieves to obtain a synthetic gel solution; the mixed salt solution containing Pt, K, and Ce elements includes soluble Pt salt, soluble K salt, and soluble Ce salt. The synthesized gel solution was subjected to hydrothermal crystallization, and the resulting hydrothermal crystallization product was subjected to solid-liquid separation. The resulting solid product was then dried and calcined to obtain the Pt-K-Ce@S-1 composite catalyst.
[0027] This invention involves mixing a mixed salt solution containing Pt, K, and Ce elements with an organic amine ligand, and then mixing the resulting mixed solution with an initial gel for the synthesis of all-silica ZSM-5 molecular sieves to obtain a synthetic gel solution.
[0028] In one embodiment, the mixed salt solution containing Pt, K, and Ce elements includes a soluble Pt salt, a soluble K salt, and a soluble Ce salt; the soluble Pt salt includes one or more of soluble platinum chloride, chloroplatinic acid, and tetraammineplatinum nitrate, with chloroplatinic acid being a specific example; the soluble K salt includes one or more of soluble potassium nitrate, potassium sulfate, and potassium chloride, with potassium nitrate being a specific example; the soluble Ce salt includes one or more of soluble cerium nitrate, cerium sulfate, and cerium chloride, with cerium nitrate being a specific example.
[0029] In one embodiment, the method for preparing the mixed salt solution containing Pt, K, and Ce elements is as follows: soluble Pt salt, soluble K salt, and soluble Ce salt are dissolved in water to obtain the mixed salt solution containing Pt, K, and Ce elements; the water is deionized water; the molar ratio of Pt, K, and Ce in the mixed salt solution containing Pt, K, and Ce elements is 1:1.3~50:0.1~20, another embodiment is 1:3.3~40:0.2~14, and a specific embodiment is 1:7.5~33:1~9.
[0030] In one embodiment, the organic amine ligand is ethylenediamine and / or triethylamine, with ethylenediamine being used in a specific embodiment; the molar ratio of total metal ions to organic amine ligand in the mixed salt solution containing Pt, K, and Ce elements is 1:2 to 50, with another embodiment being 1:2 to 50, and 1:4 being used in a specific embodiment; the mixing of the mixed salt solution containing Pt, K, and Ce elements with the organic amine ligand is carried out at room temperature.
[0031] As one embodiment, the preparation method of the initial gel for the synthesis of all-silica ZSM-5 molecular sieve is as follows: A silicon source, a template agent, and water are mixed and aged to obtain the initial gel for the synthesis of all-silica ZSM-5 molecular sieve; the silicon source includes one or more of tetraethyl orthosilicate, silica sol, and tetrabutyl orthosilicate, specifically tetraethyl or tetrabutyl orthosilicate in this embodiment; the template agent includes one or more of tetrapropylammonium hydroxide (TPAOH), tetraethylammonium hydroxide (TEAOH), and n-butylamine, specifically tetrapropylammonium hydroxide (TPAOH) in this embodiment; the template agent is used in the form of an aqueous template agent solution; the mass fraction of the aqueous template agent solution is 15-50%, specifically 20-45% in this embodiment. The present invention does not have any particular limitation on the mixing, as long as the raw materials are mixed evenly; the mixing temperature is room temperature; in the embodiments of the present invention, the mixing is: mixing the template agent aqueous solution with water until clear, and then adding the silicon source dropwise; the present invention does not have any particular limitation on the dropwise addition, as long as it is added dropwise at a uniform rate; the resulting mixed solution is mixed with the initial gel synthesized from all-silicon ZSM-5 molecular sieve under stirring conditions; the aging temperature is room temperature, and the aging time is 1~5h, another embodiment is 2~4h, and in a specific embodiment it is 3~4h; the aging is carried out under stirring conditions.
[0032] In one embodiment, the molar ratio of the effective component SiO2, template agent, and H2O in the initial gel synthesized from the all-silica ZSM-5 molecular sieve is 1:0.2~0.8:20~100; in another embodiment, it is 1:0.3~0.7:30~90; and in a specific embodiment, it is 1:0.4~0.6:40~80. The molar ratio of the total metal ions in the mixed salt solution containing Pt, K, and Ce elements to the effective component SiO2 in the initial gel synthesized from the all-silica ZSM-5 molecular sieve is 1:5~50; and in a specific embodiment, it is 1:10~35.
[0033] After obtaining the synthetic gel solution, the present invention performs hydrothermal crystallization on the synthetic gel solution, separates the obtained hydrothermal crystallization product into solid and liquid, and dries and calcines the obtained solid product in sequence to obtain the Pt-K-Ce@S-1 composite catalyst.
[0034] In one embodiment, the hydrothermal crystallization temperature is 150~200℃, another embodiment is 160~190℃, and a specific embodiment is 170~180℃; the hydrothermal crystallization time is 30~120h, another embodiment is 50~100h, and a specific embodiment is 60~80h. In this invention, the introduction of organic amine ligands can protect the soluble Pt source, soluble K source, and soluble Ce source during the hydrothermal crystallization process, promoting the confinement of Pt, K, and Ce metals within the pores of the all-silica ZSM-5 molecular sieve.
[0035] This invention does not impose any particular limitation on the method of solid-liquid separation; any solid-liquid separation method well-known to those skilled in the art can be used. In this embodiment, the solid-liquid separation is centrifugal separation. This invention also does not impose any particular requirements on the drying conditions; drying to constant weight can be achieved using drying conditions well-known to those skilled in the art.
[0036] In one embodiment, the roasting temperature is 500~650℃, another embodiment is 530~620℃, a specific embodiment is 550~600℃, and the holding time is 5~10h, another embodiment is 6~9h, a specific embodiment is 7~8h; the roasting includes sequentially performing a first roasting and a second roasting; the temperature of the first roasting is 520~570℃, a specific embodiment is 550℃, and the holding time is 5~10h, a specific embodiment is 8h; the temperature of the second roasting is 580~600℃, a specific embodiment is 600℃, and the holding time is 1~3h, a specific embodiment is 2h; the roasting atmosphere is an air atmosphere.
[0037] In one embodiment, after the calcination is completed, the process further includes: sequentially pressing, pulverizing, and sieving the calcined product to obtain a Pt-K-Ce@S-1 composite catalyst; the particle size of the Pt-K-Ce@S-1 composite catalyst is 10-60 mesh, and in a specific embodiment, it is 20-40 mesh. This invention does not have specific limitations on the pressing, pulverizing, and sieving processes; any method that yields a Pt-K-Ce@S-1 composite catalyst with a particle size of 10-60 mesh is acceptable.
[0038] This invention also provides the application of the Pt-K-Ce@S-1 composite catalyst described in the above technical solution or the Pt-K-Ce@S-1 composite catalyst prepared by the preparation method described in the above technical solution in the catalytic aromatization of hexane.
[0039] This invention also provides a method for preparing aromatics by hexane dehydrogenation-aromatization, comprising the following steps: A hexane-nitrogen mixture is subjected to a catalytic hexane dehydrogenation-aromatization reaction in the presence of a catalyst to obtain olefins and aromatics; the catalyst is the Pt-K-Ce@S-1 composite catalyst described in the above technical solution or the Pt-K-Ce@S-1 composite catalyst prepared by the preparation method described in the above technical solution.
[0040] In one embodiment, the catalyst is subjected to a reduction treatment before use; the temperature of the reduction treatment is 400~700℃, another embodiment is 450~650℃, and a specific embodiment is 500~650℃; the time of the reduction treatment is 1~8h, another embodiment is 2~7h, and a specific embodiment is 3~6h; the reducing agent used in the reduction treatment is a mixture of hydrogen and protective gas, or hydrogen; the protective gas is nitrogen.
[0041] In this invention, the volume ratio of hexane to nitrogen in the hexane-nitrogen mixed gas is 1:0~20, another embodiment is 1:1~8, and a specific embodiment is 1:2; the flow rate of the hexane-nitrogen mixed gas is 10~50 sccm, and a specific embodiment is 15 sccm; the space velocity of the catalytic hexane dehydrogenation-aromatization reaction is 0.1~20 h⁻¹. -1 In specific embodiments, the time is 0.2~15 h. -1 The temperature for the catalytic hexane dehydrogenation-aromatization reaction is 400~600℃, specifically 520~580℃ in this embodiment; the pressure is 0.1~1MPa, specifically 0.1MPa in this embodiment; and the time is 2~100h, specifically 2~24h in this embodiment.
[0042] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments thereof, but they should not be construed as limiting the scope of protection of the present invention.
[0043] Example 1 13.02 g of TPAOH aqueous solution (mass fraction 25%) was added to 15 g of deionized water (H2O) and magnetically stirred until the solution became clear. Then, 8.24 g of tetraethyl orthosilicate (TEOS) was added dropwise. The mixture was aged at room temperature with stirring for 4 h to obtain the initial gel for the synthesis of all-silica ZSM-5 molecular sieve (molar ratio of H2O, TPAOH, and SiO2 was 35:0.4:1). At room temperature, 0.38 g of hexachloroplatinic acid hexahydrate solution (10 wt%), 0.99 g of potassium nitrate solution (10 wt%), and 1.28 g of cerium nitrate hexahydrate solution (10 wt%) were dissolved in 5 g of deionized water, and then mixed thoroughly with 0.32 g of ethylenediamine at room temperature. The molar ratio of Pt, K, and Ce was 1:13:4, and the molar ratio of total Pt, K, and Ce metal ions to ethylenediamine was 1:4. The resulting mixed solution containing Pt, K, Ce elements and organic amine ligands was added to the all-silicon ZSM-5 molecule. The mixture was stirred and homogenized in the initial gel, with a molar ratio of total metal ions (Pt, K, Ce) to SiO2 of 1:30. The mixture was then transferred to a 100 mL high-pressure reactor and hydrothermally crystallized at 175 °C for 96 h. After centrifugation, the resulting solid product was dried in an oven at 100 °C for 12 h, and then placed in a muffle furnace for calcination at 550 °C in air for 8 h, followed by calcination at 600 °C for 2 h. The product was then tableted, pulverized, and sieved to obtain a 0.6%Pt-1.6%K-1.72%Ce@S-1 composite catalyst with a particle size of 20-40 mesh.
[0044] Figure 1 The XRD pattern of the 0.6%Pt-1.6%K-1.72%Ce@S-1 composite catalyst prepared in Example 1 is shown. Figure 1 It can be seen that the prepared 0.6%Pt-1.6%K-1.72%Ce@S-1 composite catalyst mainly showed the typical diffraction peaks of ZSM-5 molecular sieve, and no obvious characteristic peaks of Pt, K or Ce were observed, indicating that these metal components are highly dispersed on ZSM-5 molecular sieve.
[0045] Figure 2 TEM image of the 0.6%Pt-1.6%K-1.72%Ce@S-1 composite catalyst prepared in Example 1. Figure 2 It can be seen that no obvious metal particles were detected in the prepared 0.6%Pt-1.6%K-1.72%Ce@S-1 composite catalyst.
[0046] Example 2 13.02 g of TPAOH aqueous solution (mass fraction 25%) was added to 15 g of deionized water (H2O) and magnetically stirred until the solution became clear. Then, 8.24 g of tetraethyl orthosilicate (TEOS) was added dropwise. The mixture was aged at room temperature with stirring for 4 h to obtain the initial gel for the synthesis of all-silica ZSM-5 molecular sieve (molar ratio of H2O, TPAOH, and SiO2 was 35:0.4:1). At room temperature, 0.25 g of hexachloroplatinic acid hexahydrate solution (10 wt%), 0.99 g of potassium nitrate solution (10 wt%), and 1.28 g of cerium nitrate hexahydrate solution (10 wt%) were dissolved in 5 g of deionized water, and then mixed thoroughly with 0.32 g of ethylenediamine at room temperature. The molar ratio of Pt, K, and Ce was 1:20:6, and the molar ratio of total Pt, K, and Ce metal ions to ethylenediamine was 1:4. The resulting mixed solution containing Pt, K, Ce elements and organic amine ligands was added to the all-silicon ZSM-5 molecule. The mixture was stirred and homogenized in the initial gel, with a molar ratio of total metal ions (Pt, K, Ce) to SiO2 of 1:30. The mixture was then transferred to a 100 mL high-pressure reactor and hydrothermally crystallized at 175 °C for 96 h. After centrifugation, the resulting solid product was dried in an oven at 100 °C for 12 h, and then placed in a muffle furnace for calcination at 550 °C in air for 8 h, followed by calcination at 600 °C for 2 h. The product was then tableted, pulverized, and sieved to obtain a 0.4%Pt-1.6%K-1.72%Ce@S-1 composite catalyst with a particle size of 20-40 mesh.
[0047] Example 3 13.02 g of TPAOH aqueous solution (mass fraction 25%) was added to 15 g of deionized water (H2O) and magnetically stirred until the solution became clear. Then, 8.24 g of tetraethyl orthosilicate (TEOS) was added dropwise. The mixture was aged at room temperature with stirring for 4 h to obtain the initial gel for the synthesis of all-silica ZSM-5 molecular sieve (molar ratio of H2O, TPAOH, and SiO2 was 35:0.4:1). At room temperature, 0.38 g of hexachloroplatinic acid hexahydrate solution (10 wt%), 0.62 g of potassium nitrate solution (10 wt%), and 1.28 g of cerium nitrate hexahydrate solution (10 wt%) were dissolved in 5 g of deionized water, and then mixed thoroughly with 0.24 g of ethylenediamine at room temperature. The molar ratio of Pt, K, and Ce was 1:8:4, and the molar ratio of total Pt, K, and Ce metal ions to ethylenediamine was 1:4. The resulting mixed solution containing Pt, K, Ce elements and organic amine ligands was added to the all-silica ZSM-5 molecular sieve. The initial gel was stirred and mixed evenly, with a molar ratio of total metal ions of Pt, K, and Ce to SiO2 of 1:40. The mixture was then transferred to a 100 mL high-pressure reactor and hydrothermally crystallized at 175 °C for 96 h. After centrifugation, the resulting solid product was dried in an oven at 100 °C for 12 h, and then placed in a muffle furnace and calcined at 550 °C in air for 8 h, followed by calcination at 600 °C for 2 h. The product was then tableted, pulverized, and sieved to obtain a 0.6%Pt-1.0%K-1.72%Ce@S-1 composite catalyst with a particle size of 20-40 mesh.
[0048] Example 4 13.02 g of TPAOH aqueous solution (mass fraction 25%) was added to 15 g of deionized water (H2O) and magnetically stirred until the solution became clear. Then, 8.24 g of tetraethyl orthosilicate (TEOS) was added dropwise. The mixture was aged at room temperature with stirring for 4 h to obtain the initial gel for the synthesis of all-silica ZSM-5 molecular sieve (molar ratio of H2O, TPAOH, and SiO2 was 35:0.4:1). At room temperature, 0.38 g of hexachloroplatinic acid hexahydrate solution (10 wt%), 0.99 g of potassium nitrate solution (10 wt%), and 0.32 g of cerium nitrate hexahydrate solution (10 wt%) were dissolved in 5 g of deionized water, and then mixed thoroughly with 0.27 g of ethylenediamine at room temperature. The molar ratio of Pt, K, and Ce was 1:13:1, and the molar ratio of total Pt, K, and Ce metal ions to ethylenediamine was 1:4. The resulting mixed solution containing Pt, K, Ce elements and organic amine ligands was added to the all-silicon ZSM-5 molecule. The mixture was stirred and homogenized in the initial gel, with a molar ratio of total metal ions (Pt, K, Ce) to SiO2 of 1:12. The mixture was then transferred to a 100 mL high-pressure reactor and hydrothermally crystallized at 175 °C for 96 h. After centrifugation, the resulting solid product was dried in an oven at 100 °C for 12 h, and then placed in a muffle furnace for calcination at 550 °C in air for 8 h, followed by calcination at 600 °C for 2 h. The product was then tableted, pulverized, and sieved to obtain a 0.6%Pt-1.6%K-0.43%Ce@S-1 composite catalyst with a particle size of 20-40 mesh.
[0049] Comparative Example 1 13.02 g of TPAOH aqueous solution (mass fraction 25%) was added to 15 g of deionized water (H2O) and magnetically stirred until the solution became clear. Then, 8.24 g of tetraethyl orthosilicate (TEOS) was added dropwise. The mixture was aged at room temperature with stirring for 4 h to obtain the initial gel for the synthesis of all-silica ZSM-5 molecular sieve (molar ratio of H2O, TPAOH, and SiO2 was 35:0.4:1). At room temperature, 0.38 g of hexachloroplatinic acid hexahydrate solution (10 wt%) and 0.99 g of potassium nitrate solution (10 wt%) were dissolved in 5 g of deionized water, and then mixed thoroughly with 0.25 g of ethylenediamine at room temperature. The molar ratio of Pt to K was 1:13, and the molar ratio of total Pt and K metal ions to ethylenediamine was 1:4. The resulting mixed solution containing Pt, K, and organic amine ligands was added to the initial gel for the synthesis of the all-silica ZSM-5 molecular sieve and stirred. The mixture was homogeneous, with a molar ratio of total Pt and K metal ions to SiO2 of 1:38. It was transferred to a 100 mL high-pressure reactor and hydrothermally crystallized at 175 °C for 96 h. After centrifugation, the resulting solid product was dried in an oven at 100 °C for 12 h, and then placed in a muffle furnace and calcined at 550 °C in air for 8 h, followed by calcination at 600 °C for 2 h. The product was then pressed into tablets, pulverized, and sieved to obtain a 0.6%Pt-1.6%K@S-1 composite catalyst with a particle size of 20-40 mesh.
[0050] Comparative Example 2 13.02 g of TPAOH aqueous solution (mass fraction 25%) was added to 15 g of deionized water (H2O) and magnetically stirred until the solution became clear. Then, 8.24 g of tetraethyl orthosilicate (TEOS) was added dropwise. The mixture was aged at room temperature with stirring for 4 h to obtain the initial gel for the synthesis of all-silica ZSM-5 molecular sieve (molar ratio of H2O, TPAOH, and SiO2 was 35:0.4:1). At room temperature, 0.38 g of hexachloroplatinic acid hexahydrate solution (10 wt%) and 1.28 g of cerium nitrate hexahydrate solution (10 wt%) were dissolved in 5 g of deionized water, and then mixed thoroughly with 0.089 g of ethylenediamine at room temperature. The molar ratio of Pt to Ce was 1:4, and the molar ratio of total Pt and Ce metal ions to ethylenediamine was 1:4. The resulting mixed solution containing Pt, Ce, and organic amine ligands was added to the initial gel for the synthesis of the all-silica ZSM-5 molecular sieve and stirred. The mixture was thoroughly mixed, with a molar ratio of total Pt and Ce metal ions to SiO2 of 1:108. The mixture was then transferred to a 100 mL high-pressure reactor and hydrothermally crystallized at 175 °C for 96 h. After centrifugation, the resulting solid product was dried in an oven at 100 °C for 12 h. It was then placed in a muffle furnace and calcined at 550 °C in air for 8 h, followed by calcination at 600 °C for 2 h. The product was then pressed into tablets, pulverized, and sieved to obtain a 0.6%Pt-1.72%Ce@S-1 composite catalyst with a particle size of 20-40 mesh.
[0051] Comparative Example 3 13.02 g of TPAOH aqueous solution (mass fraction of 25%) was added to 15 g of deionized water (H2O) and magnetically stirred until the solution was clear. Then, 8.24 g of tetraethyl orthosilicate (TEOS) was added dropwise. The mixture was aged for 4 h at room temperature with stirring to obtain the initial gel for the synthesis of all-silica ZSM-5 molecular sieve (molar ratio of H2O, TPAOH, and SiO2 was 35:0.4:1).
[0052] At room temperature, 0.99 g of potassium nitrate solution (10 wt%) and 1.28 g of cerium nitrate hexahydrate solution (10 wt%) were dissolved in 5 g of deionized water, and then mixed thoroughly with 4.5 g of ethylenediamine at room temperature. The molar ratio of K to Ce was 1:3.3, and the molar ratio of total K and Ce metal ions to ethylenediamine was 1:4. The resulting mixed solution containing K, Ce, and organic amine ligands was added to the initial gel for the synthesis of the all-silica ZSM-5 molecular sieve and stirred. The homogeneous K, Ce total metal ions to SiO2 molar ratio was 1:31. The mixture was transferred to a 100 mL high-pressure reactor and hydrothermally crystallized at 175 °C for 96 h. After centrifugation, the resulting solid product was dried in an oven at 100 °C for 12 h, and then placed in a muffle furnace and calcined at 550 °C in air for 8 h, followed by calcination at 600 °C for 2 h. The product was then pressed into tablets, pulverized, and sieved to obtain a 1.6% K-1.72% Ce@S-1 composite catalyst with a particle size of 20-40 mesh.
[0053] Comparative Example 4 13.02 g of TPAOH aqueous solution (mass fraction 25%) was added to 15 g of deionized water (H2O) and magnetically stirred until the solution became clear. Then, 8.24 g of tetraethyl orthosilicate (TEOS) was added dropwise. The mixture was aged at room temperature with stirring for 4 h to obtain the initial gel for the synthesis of all-silica ZSM-5 molecular sieve (molar ratio of H2O, TPAOH, and SiO2 was 35:0.4:1). At room temperature, 0.38 g of hexachloroplatinic acid hexahydrate solution (10 wt%), 0.99 g of potassium nitrate solution (10 wt%), and 1.27 g of zirconium nitrate pentahydrate solution (10 wt%) were dissolved in 5 g of deionized water, and then mixed thoroughly with 0.32 g of ethylenediamine at room temperature. The molar ratio of Pt, K, and Zr was 1:13:4, and the molar ratio of total Pt, K, and Zr metal ions to ethylenediamine was 1:4. The resulting mixed solution containing Pt, K, Zr elements and organic amine ligands was added to the all-silicon ZSM-5 molecule. The Pt, K, and Zr total metal ions were stirred and mixed evenly in the initial gel. The molar ratio of Pt, K, and Zr to SiO2 was 1:30. The mixture was transferred to a 100 mL high-pressure reactor and hydrothermally crystallized at 175 °C for 96 h. After centrifugation, the resulting solid product was dried in an oven at 100 °C for 12 h. Then, it was placed in a muffle furnace and calcined at 550 °C in air for 8 h, followed by calcination at 600 °C for 2 h. The product was then tableted, pulverized, and sieved to obtain a 0.6%Pt-1.6%K-1.12%Zr@S-1 composite catalyst with a particle size of 20-40 mesh.
[0054] Comparative Example 5 13.02 g of TPAOH aqueous solution (mass fraction 25%) was added to 15 g of deionized water (H2O) and magnetically stirred until the solution became clear. Then, 8.24 g of tetraethyl orthosilicate (TEOS) was added dropwise. The mixture was aged at room temperature with stirring for 4 h to obtain the initial gel for the synthesis of all-silica ZSM-5 molecular sieve (molar ratio of H2O, TPAOH, and SiO2 was 35:0.4:1). At room temperature, 0.38 g of hexachloroplatinic acid hexahydrate solution (10 wt%), 0.99 g of potassium nitrate solution (10 wt%), and 0.76 g of gallium nitrate hydrate solution (10 wt%) were dissolved in 5 g of deionized water, and then mixed thoroughly with 0.32 g of ethylenediamine at room temperature. The molar ratio of Pt, K, and Ga was 1:13:4, and the molar ratio of total Pt, K, and Ga metal ions to ethylenediamine was 1:4. The resulting mixed solution containing Pt, K, Ga elements and organic amine ligands was added to the all-silica ZSM-5 molecular sieve. The initial gel was stirred and mixed evenly, with a molar ratio of total metal ions of Pt, K, and Ga to SiO2 of 1:30. The mixture was then transferred to a 100 mL high-pressure reactor and hydrothermally crystallized at 175 °C for 96 h. After centrifugation, the resulting solid product was dried in an oven at 100 °C for 12 h, and then placed in a muffle furnace for calcination at 550 °C in air for 8 h, followed by calcination at 600 °C for 2 h. The product was then tableted, pulverized, and sieved to obtain a 0.6%Pt-1.6%K-0.86%Ga@S-1 composite catalyst with a particle size of 20-40 mesh.
[0055] Comparative Example 6 13.02 g of TPAOH aqueous solution (25% by mass) was added to 15 g of deionized water (H2O) and magnetically stirred until the solution became clear. Then, 8.24 g of tetraethyl orthosilicate (TEOS) was added dropwise. The mixture was aged for 4 h at room temperature with stirring to obtain the initial gel for the synthesis of all-silica ZSM-5 molecular sieve (molar ratio of H2O, TPAOH, and SiO2 was 35:0.4:1). At room temperature, 0.38 g of hexachloroplatinic acid hexahydrate solution (10 wt%), 0.99 g of potassium nitrate solution (10 wt%), and 1.13 g of iridium nitrate hexahydrate solution (10 wt%) were dissolved in 5 g of deionized water, and then mixed thoroughly with 0.32 g of ethylenediamine at room temperature. The molar ratio of Pt, K, and Y was 1:13:4, and the molar ratio of total Pt, K, and Y metal ions to ethylenediamine was 1:4. The resulting mixed solution containing Pt, K, Y elements and organic amine ligands was added to the all-silicon ZSM-5 molecule. The Pt, K, and Y total metal ions were stirred and mixed evenly in the initial gel. The molar ratio of Pt, K, and Y to SiO2 was 1:30. The mixture was transferred to a 100 mL high-pressure reactor and hydrothermally crystallized at 175 °C for 96 h. After centrifugation, the resulting solid product was dried in an oven at 100 °C for 12 h. Then, it was placed in a muffle furnace and calcined at 550 °C in air for 8 h, followed by calcination at 600 °C for 2 h. The product was then tableted, pulverized, and sieved to obtain a 0.6%Pt-1.6%K-1.1%Y@S-1 composite catalyst with a particle size of 20-40 mesh.
[0056] Comparative Example 7 The only difference from Example 1 is that 1.28g of cerium nitrate hexahydrate solution (10wt%) was replaced with 1.77g of chromium nitrate nonahydrate solution (10wt%) to obtain a 0.6%Pt-1.6%K-0.96%Cr@S-1 composite catalyst.
[0057] Application Example 1 The catalysts prepared in Examples 1-4 and Comparative Examples 1-7 were subjected to catalytic performance tests.
[0058] The catalysts prepared in Examples 1-4 and Comparative Examples 1-7 were reduced at 600°C under a hydrogen atmosphere for 1 h to obtain activated catalysts. A hexane-nitrogen mixture (hexane to nitrogen volume ratio = 1:2) was introduced at 15 sccm into a reactor containing 0.15 g of activated catalyst to carry out a catalytic alkane dehydrogenation-aromatization reaction, with a hexane mass hourly space velocity (HHSV) of 7 h⁻¹. -1 The temperature was 500℃, the pressure was 0.1MPa, and the time was 2h, yielding olefins and aromatics.
[0059] The catalytic performance of the catalysts prepared in Examples 1-4 and Comparative Examples 1-7 under different catalytic reaction conditions is shown in Table 1: Table 1 Catalytic performance of the catalysts prepared in Examples 1-4 and Comparative Examples 1-7
[0060] As shown in Table 1, the Pt-K-Ce@S-1 composite catalyst prepared in this invention, when used in the catalytic dehydrogenation-aromatization of hexane to aromatics reaction, achieves a hexane conversion of 57.6% and an olefin and aromatic yield of 47.1% after 2 hours of reaction. In contrast, without the promoter Ce, the hexane conversion and the yields of olefins and aromatics decrease to 34.6% and 29.4%, respectively; without the promoter K, the hexane conversion and the yields of olefins and aromatics decrease to 37.3% and 27.2%, respectively; and without the presence of metal Pt, the above reactions are almost impossible to occur, with a hexane conversion as low as 1.1%. If the promoter Ce is replaced with Zr, Ga, Y, Cr, etc., the hexane conversion and the yields of olefins and aromatics also significantly decrease to 33.2%, 37.4%, 44.2%, and 42.7%, respectively. These results demonstrate that the Pt-K-Ce@S-1 composite catalyst prepared in this invention exhibits both high hexane conversion and yields of olefins and aromatics in the catalytic hexane dehydrogenation-aromatization reaction, and the catalyst does not contain any toxic metal elements.
[0061] Application Example 2 The catalytic stability of the Pt-K-Ce@S-1 composite catalyst prepared in Example 1 was tested. The catalytic reaction conditions were: reaction temperature 500℃, pressure 0.1 MPa, and hexane space velocity 7 h⁻¹. -1 The catalytic stability test results of the Pt-K-Ce@S-1 composite catalyst are as follows: Figure 3 As shown.
[0062] Depend on Figure 3 It is evident that the Pt-K-Ce@S-1 composite catalyst prepared in this invention exhibits good reaction stability when used in the catalytic dehydrogenation-aromatization reaction of hexane. After 24 hours of reaction, the hexane conversion and olefin + aromatics yield of the Pt-K-Ce@S-1 composite catalyst remained at 52.5% and 43.3%, respectively.
[0063] Although the above embodiments have provided a detailed description of the present invention, they are only some embodiments of the present invention and not all embodiments. People can obtain other embodiments based on these embodiments without creative effort, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A Pt-K-Ce@S-1 composite catalyst, characterized in that, It consists of an all-silica ZSM-5 molecular sieve and Pt metal, K and Ce additives confined within the pores of the all-silica ZSM-5 molecular sieve.
2. The Pt-K-Ce@S-1 composite catalyst according to claim 1, characterized in that, The Pt-K-Ce@S-1 composite catalyst contains 0.2-2.0% Pt metal, 0.5-2.0% K promoter, and 0.1-3.0% Ce promoter.
3. The method for preparing the Pt-K-Ce@S-1 composite catalyst according to claim 1 or 2, characterized in that, Includes the following steps: A mixed salt solution containing Pt, K, and Ce elements is mixed with an organic amine ligand, and the resulting mixed solution is mixed with an initial gel for the synthesis of all-silica ZSM-5 molecular sieves to obtain a synthetic gel solution; the mixed salt solution containing Pt, K, and Ce elements includes soluble Pt salt, soluble K salt, and soluble Ce salt. The synthesized gel solution was subjected to hydrothermal crystallization, and the resulting hydrothermal crystallization product was subjected to solid-liquid separation. The resulting solid product was then dried and calcined to obtain the Pt-K-Ce@S-1 composite catalyst.
4. The preparation method according to claim 3, characterized in that, The molar ratio of Pt, K, and Ce in the mixed salt solution containing Pt, K, and Ce is 1:1.3~50:0.1~20.
5. The preparation method according to claim 3, characterized in that, The molar ratio of total metal ions to organic amine ligands in the mixed salt solution containing Pt, K, and Ce elements is 1:2 to 50.
6. The preparation method according to claim 3, characterized in that, The hydrothermal crystallization temperature is 150~200℃; the hydrothermal crystallization time is 30~120h.
7. The preparation method according to claim 3, characterized in that, The molar ratio of the active ingredient SiO2, template agent and H2O in the initial gel synthesized from the all-silica ZSM-5 molecular sieve is 1:0.2~0.8:20~100.
8. The preparation method according to claim 3, characterized in that, The roasting temperature is 500~650℃, and the holding time is 5~10h.
9. The application of the Pt-K-Ce@S-1 composite catalyst according to claim 1 or 2 or the Pt-K-Ce@S-1 composite catalyst prepared by the preparation method according to any one of claims 3 to 8 in the catalytic aromatization of hexane.
10. A method for preparing aromatics by hexane dehydrogenation-aromatization, characterized in that, Includes the following steps: A hexane-nitrogen mixture is subjected to a catalytic hexane dehydrogenation-aromatization reaction in the presence of a catalyst to obtain olefins and aromatics; the catalyst is the Pt-K-Ce@S-1 composite catalyst according to claim 1 or 2 or the Pt-K-Ce@S-1 composite catalyst prepared by any one of the preparation methods of claims 3 to 8.