A microwave-assisted synthesis of molecular sieve @Ni / Al2O3 catalyst and its preparation method
The molecular sieve @Ni/Al2O3 catalyst was prepared by microwave-assisted synthesis, which solved the problems of nickel and aluminum component segregation and uneven distribution of active components in traditional methods, and achieved rapid and uniform heating of the catalyst and efficient catalytic biphenyl hydrogenation reaction.
Patent Information
- Application Number
- CN202611407480.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-10
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional methods for preparing molecular sieve @Ni/Al2O3 catalysts suffer from problems such as nickel and aluminum segregation, uneven distribution of active components, uneven heating, and long reaction times, which affect the activity and stability of the catalyst.
A microwave-assisted synthesis method was adopted, in which molecular sieve, urea and nickel-aluminum mixed salt solution were reacted under microwave conditions. The selective heating of microwave was used to achieve uniform dispersion of nickel and aluminum components on the surface of the support, thus preparing a molecular sieve@Ni/Al2O3 catalyst with uniform distribution of active components.
Rapid and uniform heating of molecular sieve@Ni/Al2O3 catalyst was achieved, shortening the reaction time, improving the uniformity of active component distribution and the activity and stability of the catalyst. It is suitable for hydrogenation catalysis of biphenyl hydrogenation reaction, with high conversion rate and good product selectivity.
Smart Images

Figure CN123102406A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of heterogeneous catalytic material preparation, specifically relating to a microwave-assisted synthesis of molecular sieve @Ni / Al2O3 catalyst and its preparation method. Background Technology
[0002] Molecular sieve @Ni / Al2O3 catalysts exhibit excellent catalytic performance in water-gas shift, electrocatalysis, hydrogenation, and dehydrogenation reactions. Currently, traditional preparation methods for molecular sieve @Ni / Al2O3 catalysts mainly include co-precipitation, impregnation, and hydrothermal methods. Among these, the precipitation process in the co-precipitation method is significantly affected by parameters such as pH and temperature, easily leading to the segregation of nickel and aluminum components; in the impregnation method, the active components are prone to migration and agglomeration after drying and calcination. While the traditional hydrothermal method commonly used in this field can improve the crystallinity of the product, its slow heating rate, uneven heating, and long reaction time result in uneven distribution of active components, ultimately affecting the activity and stability of the molecular sieve @Ni / Al2O3 catalyst. Summary of the Invention
[0003] The purpose of this invention is to provide a microwave-assisted synthesis method for molecular sieve @Ni / Al2O3 catalysts. The preparation method provided by this invention enables rapid and uniform heating, has a short reaction time, and produces molecular sieve @Ni / Al2O3 catalysts with uniform distribution of active components and good activity and stability.
[0004] To achieve the above objectives, the present invention provides the following technical solution: A method for preparing a microwave-assisted molecular sieve @Ni / Al2O3 catalyst includes the following steps: Molecular sieves, urea, and a nickel-aluminum mixed salt solution were mixed and reacted under microwave conditions to obtain a precursor. The precursor was activated in an activating atmosphere to obtain the molecular sieve@Ni / Al2O3 catalyst. The microwave power is 500~600W and the frequency is 2300~2500MHz; the reaction time is 1~2h.
[0005] Preferably, the molecular sieve includes MOR molecular sieve, HY molecular sieve or ZSM-5 molecular sieve; the molar ratio of silica to alumina in the MOR molecular sieve is 10~40:1; the molar ratio of silica to alumina in the ZSM-5 molecular sieve is 25~50:1.
[0006] Preferably, the concentration of nickel salt in the nickel-aluminum mixed salt solution is 0.15~0.25 mol / L, and the concentration of aluminum salt is 0.1~0.2 mol / L; the molar ratio of nickel to aluminum in the nickel-aluminum mixed salt solution is 1~7:1.
[0007] Preferably, the ratio of the molecular sieve, urea, and nickel-aluminum salt solution is 1~2g:4~6g:50~60mL.
[0008] Preferably, the reaction temperature is 95~100℃, the reaction is carried out under stirring conditions, and the stirring rate is 200~500 rpm.
[0009] Preferably, the activation atmosphere is a mixture of nitrogen and hydrogen, and the gas flow ratio of nitrogen to hydrogen is 1~1.2:1~1.2; the activation temperature is 480~520℃, and the holding time is 1~1.5h.
[0010] This invention provides a molecular sieve@Ni / Al2O3 catalyst prepared by the preparation method described above.
[0011] Preferably, the molecular sieve@Ni / Al2O3 catalyst comprises a molecular sieve support and an active component supported on the surface of the molecular sieve support. The active component is nickel and alumina, the molar ratio of nickel to alumina is 1~7:1, and the loading of the active component is 43~47%.
[0012] This invention provides the application of the molecular sieve@Ni / Al2O3 catalyst described above in the catalytic hydrogenation reaction of biphenyl.
[0013] Preferably, the mass ratio of the molecular sieve@Ni / Al2O3 catalyst to biphenyl is 2~2.5:1.
[0014] The microwave-assisted synthesis method for preparing molecular sieve @Ni / Al2O3 catalysts provided by this invention combines microwave radiation technology with chemical reaction synthesis methods. Utilizing the selective heating characteristic of microwaves, localized high temperatures are generated on the surface of the molecular sieve support, inducing rapid reactions of the active components on the overheated surface of the support. This achieves uniform dispersion and rapid deposition of nickel and aluminum components on the support surface, thereby efficiently constructing the molecular sieve @Ni / Al2O3 catalyst. The microwave-assisted synthesis method ensures uniform heating of the molecular sieve and active components, significantly shortening the reaction time and exhibiting energy-saving and consumption-reducing characteristics, aligning with the development concept of green chemistry. Compared with traditional methods, this invention, through microwave-assisted synthesis, can significantly shorten preparation time, reduce energy consumption, and achieve precise control over the crystal phase structure of the active components, thus obtaining a molecular sieve @Ni / Al2O3 catalyst with uniformly distributed active components.
[0015] The molecular sieve @Ni / Al2O3 catalyst prepared by this invention has good activity and stability, and can be used as a hydrogenation catalyst to catalyze the hydrogenation reaction of biphenyl, with high conversion rate and good product selectivity. Attached Figure Description
[0016] Figure 1 Transmission microscope image of the HY@Ni / Al2O3 catalyst prepared in Example 1; Figure 2 Transmission microscope image of the MOR@Ni / Al2O3 catalyst prepared in Example 2; Figure 3 Transmission microscope image of the ZSM-5@Ni / Al2O3 catalyst prepared in Example 4; Figure 4 Transmission microscope image of the MOR@Ni / Al2O3 catalyst-HT prepared in Comparative Example 1; Figure 5 Transmission microscope image of MOR@Ni / Al2O3 catalyst-HT prepared in Comparative Example 2; Figure 6 The histogram shows the particle size distribution of HY molecular sieves after ammonium exchange. Figures 7-9 This is a scanning electron microscope image of HY molecular sieve after ammonium exchange. Figure 10 The particle size distribution histogram of MOR molecular sieve (molar ratio of SiO2 to Al2O3 is 25:1); Figures 11-12 This is a scanning electron microscope image of MOR molecular sieve (the molar ratio of SiO2 to Al2O3 is 25:1). Figure 13 The particle size distribution histogram of MOR molecular sieve (molar ratio of SiO2 to Al2O3 is 10:1); Figures 14-16 This is a scanning electron microscope image of MOR molecular sieve (the molar ratio of SiO2 to Al2O3 is 10:1). Figure 17 The particle size distribution histogram of ZSM-5 molecular sieve (molar ratio of SiO2 to Al2O3 is 46:1); Figures 18-20 The image shows a scanning electron microscope image of ZSM-5 molecular sieve (with a molar ratio of SiO2 to Al2O3 of 46:1). Figure 21 The particle size distribution histogram of ZSM-5 molecular sieve (molar ratio of SiO2 to Al2O3 is 27:1); Figures 22-24 This is a scanning electron microscope image of ZSM-5 molecular sieve (the molar ratio of SiO2 to Al2O3 is 27:1). Detailed Implementation
[0017] This invention provides a method for preparing a microwave-assisted molecular sieve @Ni / Al2O3 catalyst, comprising the following steps: Molecular sieves, urea, and a nickel-aluminum mixed salt solution were mixed and reacted under microwave conditions to obtain a precursor. The precursor was activated in an activating atmosphere to obtain the molecular sieve@Ni / Al2O3 catalyst. The microwave power is 500~600W and the frequency is 2300~2500MHz; the reaction time is 1~2h.
[0018] In this invention, unless otherwise specified, all raw materials / components used in the preparation are commercially available products well known to those skilled in the art.
[0019] This invention involves mixing molecular sieves, urea, and a nickel-aluminum mixed salt solution, and reacting them under microwave conditions to obtain a precursor. In one embodiment of this invention, the molecular sieve includes MOR molecular sieves, HY molecular sieves, or ZSM-5 molecular sieves, all purchased from Tianjin Nanhua Catalyst Co., Ltd.; the MOR molecular sieve includes microporous MOR molecular sieves or mesoporous MOR molecular sieves; the molar ratio of silica to alumina in the MOR molecular sieve is 10~40:1, more preferably 10~25:1; the molar ratio of silica to alumina in the ZSM-5 molecular sieve is 25~50:1, more preferably 27~46:1.
[0020] In one embodiment of the present invention, the HY molecular sieve further includes ammonium exchange and calcination before use. The ammonium exchange includes: mixing ammonium chloride and water to obtain an ammonium chloride solution with a concentration of 0.04~0.05 mol / mL; mixing the HY molecular sieve with the ammonium chloride solution at a material-to-liquid ratio of 1.5~2g:70~80mL; and performing ammonium exchange at a temperature of 80~85℃ for 3~4 hours in an oil bath. The ammonium exchange can be performed twice, preferably under the same conditions. Specifically, the material obtained after the first ammonium exchange is centrifuged, and the precipitate is collected and mixed with the ammonium chloride solution for the second ammonium exchange. In another embodiment of the present invention, post-treatment is included after ammonium exchange and before calcination. Specifically, the material obtained after the second ammonium exchange is naturally cooled to room temperature, the precipitate is collected by centrifugation, and then washed, dried, and ground sequentially. The washing is performed four times, 40mL each time. The drying is performed in a drying oven at a temperature of 55~60℃ for 10~12 hours. In one embodiment of the present invention, the calcination temperature is 500~600℃, specifically 550℃, and the time is 2~4h, specifically 3h. The heating rate to the calcination temperature is 2~3℃ / min, and the time is 250~260min. The particle size of the HY molecular sieve after calcination is 0.34343±0.11283μm.
[0021] In one embodiment of the present invention, the preparation method of the mesoporous MOR molecular sieve includes the following steps: mixing the MOR molecular sieve with a sodium hydroxide solution and reacting under microwave conditions to obtain the mesoporous MOR molecular sieve. In another embodiment of the present invention, the molar ratio of SiO2 to Al2O3 in the MOR molecular sieve is 25:1, the concentration of the sodium hydroxide solution is 0.15~0.2mol / L, and the volume ratio of the MOR molecular sieve to the sodium hydroxide solution is 3~4g:200~300mL; the microwave is provided by a microwave synthesizer with a power of 500~600W; the reaction is carried out under stirring conditions at a stirring rate of 200~500rpm; the reaction temperature is 80~85℃; and the reaction time is 0.5~1h. As one embodiment of the present invention, the reaction further includes: naturally cooling to room temperature, collecting the precipitate by centrifugation, and sequentially washing with water, drying and grinding to obtain a mesoporous MOR molecular sieve; the water washing is performed 4 times, 50 mL each time, the drying is carried out in a forced-air drying oven at a temperature of 55~60℃ for 10~12 h, and the particle size of the mesoporous MOR molecular sieve is 0.54±0.16096 μm.
[0022] In one embodiment of the present invention, the nickel-aluminum mixed salt solution comprises nickel salt and aluminum salt. The concentration of nickel salt in the nickel-aluminum mixed salt solution is 0.15~0.25 mol / L, specifically 0.2 mol / L, and the concentration of aluminum salt is 0.1~0.2 mol / L, specifically 0.12 mol / L. The nickel salt includes nickel nitrate hexahydrate, and the aluminum salt includes aluminum nitrate nonahydrate. The molar ratio of nickel to aluminum in the nickel-aluminum mixed salt solution is 1~7:1, more specifically 2~5:1, specifically 3:1.
[0023] In one embodiment of the present invention, the ratio of the molecular sieve, urea, and nickel-aluminum salt solution is 1-2 g: 4-6 g: 50-60 mL, specifically 1 g: 4.95 g: 50 mL; the molecular sieve, urea, and nickel-aluminum mixed salt solution are mixed under ultrasonic conditions for 5 minutes at room temperature. The present invention utilizes ultrasound to fully disperse the molecular sieve, forming a homogeneous mixture.
[0024] After mixing molecular sieves, urea, and a nickel-aluminum mixed salt solution, the present invention reacts under microwave conditions to obtain a precursor. In this invention, the microwave power is 500-600W, the frequency is 2300-2500MHz (specifically 2450MHz), and the microwave is a constant power continuous microwave; the reaction time is 1-2 hours. In one embodiment, the reaction time can be 1.5 hours, the reaction temperature is 95-100℃, and the reaction is carried out under stirring at a stirring rate of 200-500 rpm. This invention, by reacting under microwave conditions, eliminates the need for additional auxiliary means (such as ultrasound) to ensure uniform heating of the molecular sieve and active components, and uniform dispersion and rapid deposition of the nickel and aluminum components on the carrier surface.
[0025] As one embodiment of the present invention, the reaction further includes: cooling the reaction system to room temperature, centrifuging to collect the precipitate, washing the precipitate with water and drying it sequentially to obtain the precursor; the water washing is performed 3 times, with 25 mL used for each wash, and the present invention removes unreacted salts by water washing; the drying is carried out in an oven at a temperature of 60°C for 12 hours.
[0026] After obtaining the precursor, the present invention activates the precursor in an activating atmosphere to obtain the molecular sieve@Ni / Al2O3 catalyst. In one embodiment of the present invention, the activating atmosphere is a mixture of nitrogen and hydrogen, with a nitrogen to hydrogen gas flow rate ratio of 1~1.2:1~1.2, specifically 1:1; the activation temperature is 480~520℃, specifically 500℃, and the holding time is 1~1.5h, specifically 1h.
[0027] This invention provides a molecular sieve@Ni / Al2O3 catalyst prepared by the preparation method described above.
[0028] In one embodiment of the present invention, the molecular sieve@Ni / Al2O3 catalyst comprises a molecular sieve support and an active component supported on the surface of the molecular sieve support. The active component is nickel and alumina, wherein the molar ratio of nickel to alumina is 1~7:1, specifically 3:1, and the loading of the active component is 43~47%, specifically 45.5%. In the molecular sieve@Ni / Al2O3 catalyst, the molecular sieve support is a sheet-like stacked block with a size of 100~1500 nm.
[0029] This invention provides the application of the molecular sieve@Ni / Al2O3 catalyst described above in the catalytic hydrogenation reaction of biphenyl.
[0030] In one embodiment of the present invention, the biphenyl hydrogenation reaction includes the following steps: Biphenyl, a catalyst, and n-hexane are mixed and hydrogenated under hydrogen conditions to obtain cyclohexylbenzene; the catalyst is the molecular sieve@Ni / Al2O3 catalyst described in the above technical solution.
[0031] In one embodiment of the present invention, the mass ratio of the molecular sieve@Ni / Al2O3 catalyst to biphenyl is 2~2.5:1, specifically 2.3:1; the mass ratio of biphenyl to n-hexane is 0.3~0.35g:35~40mL; the hydrogenation reaction includes purging nitrogen gas to replace the gas before the hydrogenation reaction; the hydrogenation reaction is carried out under stirring conditions, the stirring rate is 650~700rpm, the temperature of the hydrogenation reaction is 300~350℃, the pressure is 1~1.2MPa, and the time is 8~9h.
[0032] In one embodiment of the present invention, the conversion rate of the biphenyl is 80-90%, and the selectivity of the product is 85-90%.
[0033] To further illustrate the present invention, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments thereof. Obviously, the described embodiments are merely some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0034] The nickel nitrate hexahydrate, aluminum nitrate nonahydrate, urea, ammonium chloride, and n-hexane used in this invention were all analytical grade and purchased from Anhui Zesheng Technology Co., Ltd.; deionized water was prepared in the laboratory. Molecular sieves used for molecular screening included MOR molecular sieves (SiO2 to Al2O3 molar ratio of 25:1 or 10:1), ZSM-5 molecular sieves (SiO2 to Al2O3 molar ratio of 46:1 or 27:1), and HY molecular sieves.
[0035] Figure 6 This is a histogram of the particle size distribution of HY molecular sieves after ammonium exchange; based on Figure 6 It can be seen that the average particle size of the HY molecular sieve after ammonium exchange is 0.34343±0.11283μm.
[0036] Figures 7-9 This is a scanning electron microscope image of HY molecular sieve after ammonium exchange; based on Figures 7-9 It can be seen that the surface roughness of the HY molecular sieve after ammonium exchange is slightly improved under high magnification, with no crystal fragmentation or pulverization.
[0037] Figure 10 The histogram of particle size distribution for MOR molecular sieves (SiO2 to Al2O3 molar ratio of 25:1); based on Figure 10It can be seen that the average particle size of MOR molecular sieve (the molar ratio of SiO2 to Al2O3 is 25:1) is 0.54±0.16096μm.
[0038] Figures 11-12 The image shows a scanning electron microscope (SEM) image of MOR molecular sieve (SiO2 to Al2O3 molar ratio of 25:1); based on... Figures 11-12 It can be seen that, at low magnification: the MOR molecular sieve (SiO2 to Al2O3 molar ratio of 25:1) has looser crystal aggregates, fewer large-sized aggregates, and slightly better particle dispersion than the MOR molecular sieve (SiO2 to Al2O3 molar ratio of 10:1); the overall particle size distribution is more uniform. At high magnification: the single crystal has a complete crystal form, smooth crystal faces, and sharp edges.
[0039] Figure 13 The histogram shows the particle size distribution of MOR molecular sieves (SiO2 to Al2O3 molar ratio of 10:1); based on... Figure 13 It can be seen that the average particle size of MOR molecular sieve (the molar ratio of SiO2 to Al2O3 is 10:1) is 0.29447±0.05863μm.
[0040] Figures 14-16 The image shows a scanning electron microscope (SEM) image of MOR molecular sieve (SiO2 to Al2O3 molar ratio of 10:1); based on... Figures 14-16 It can be seen that, under low magnification, the MOR molecular sieve (SiO2 to Al2O3 molar ratio of 10:1) crystals are mainly irregular blocks and aggregates, with obvious particle agglomeration and uneven particle distribution. Stacks of crystals of varying sizes are visible, and the overall agglomerate size is in the micrometer range. Under high magnification, the outline of individual MOR crystals is clear, the crystal surface is relatively flat, the crystal face is sharp, and there are no large amounts of amorphous impurities attached; the grain size is concentrated in the range of 200~500nm, and the crystal integrity is good.
[0041] Figure 17 The histogram of particle size distribution for ZSM-5 molecular sieve (SiO2 to Al2O3 molar ratio 46:1); based on Figure 17 It can be seen that the average particle size of ZSM-5 molecular sieve (the molar ratio of SiO2 to Al2O3 is 46:1) is 1.35771±0.23184μm.
[0042] Figures 18-20 The image shows a scanning electron microscope (SEM) image of ZSM-5 molecular sieve (SiO2 to Al2O3 molar ratio of 46:1); based on... Figures 18-20It can be seen that the ZSM-5 molecular sieve (with a molar ratio of SiO2 to Al2O3 of 46:1) retains the characteristic ellipsoidal crystal form of ZSM-5, and the framework structure remains unchanged. The grain size is further refined, the overall particle size is smaller, and the particle uniformity is further improved. The particle agglomeration phenomenon is extremely weak, and the dispersibility is better than that of ZSM-5 molecular sieve (with a molar ratio of SiO2 to Al2O3 of 27:1). The crystal surface remains smooth, without any crystal phase transformation or crystal breakage issues.
[0043] Figure 21 The histogram of particle size distribution for ZSM-5 molecular sieve (SiO2 to Al2O3 molar ratio of 27:1); based on Figure 21 It can be seen that the average particle size of ZSM-5 molecular sieve (the molar ratio of SiO2 to Al2O3 is 27:1) is 0.74842±0.1314μm.
[0044] Figures 22-24 The image shows a scanning electron microscope (SEM) image of ZSM-5 molecular sieve (SiO2 to Al2O3 molar ratio of 27:1); based on... Figures 22-24 As can be seen, the ZSM-5 molecular sieve (with a SiO2 to Al2O3 molar ratio of 27:1) exhibits the classic hexagonal / quasi-ellipsoidal crystals characteristic of this molecular sieve, distinct from the bulk crystal form of MOR, demonstrating high crystal form recognition. Low magnification: good grain dispersion, with a small amount of slight agglomeration, and overall uniform particle size. High magnification: clean and smooth crystal surface, clear grain boundaries, no obvious defects, cracks, or impurities, and high crystallinity. The ZSM-5 molecular sieve (with a SiO2 to Al2O3 molar ratio of 27:1) exhibits a standard crystal form, ideal crystallization effect, and good particle state, representing a typical high-quality ZSM-5 molecular sieve morphology.
[0045] Example 1 (1) Weigh 4.289g of ammonium chloride, add 80mL of deionized water to prepare an ammonium chloride solution, add the ammonium chloride solution and 2g of HY molecular sieve to a three-necked flask, stir and react in an oil bath at 85℃ for 4h to carry out the first ammonium exchange, centrifuge after the reaction is completed and collect the precipitate; Weigh another 4.289g of ammonium chloride, add 80mL of deionized water to prepare an ammonium chloride solution, add the precipitate, stir and react in an oil bath at 85℃ for 4h to carry out the second ammonium exchange, cool naturally to room temperature after the reaction is completed, centrifuge and wash the obtained precipitate 4 times with deionized water (40mL each time), place the washed precipitate in a drying oven and dry at 60℃ for 12h, grind the obtained dried HY molecular sieve, then heat at a heating rate of 2℃ / min for 260min, calcine at 550℃ for 3h to obtain the calcined HY molecular sieve (particle size of 0.34343±0.11283μm).
[0046] (2) Weigh 10.905g of nickel nitrate hexahydrate and 4.68g of aluminum nitrate nonahydrate, add deionized water to make up to 100mL to obtain a mixed salt solution (the molar ratio of Ni to Al is 3:1); take 50mL of the mixed salt solution and add it to a three-necked flask, then add 4.95g of urea and 1g of calcined HY molecular sieve, and sonicate at 25℃ for 5min; transfer the three-necked flask to a microwave synthesizer, set the microwave power to 600W, the frequency to 2450MHz, and the stirring speed to 200rpm, and react at 98℃ for 1.5h in a closed system under normal pressure; after the reaction is completed, cool naturally to room temperature, centrifuge to remove the supernatant, wash the obtained precipitate three times with deionized water (25mL each time), place the washed precipitate in a forced-air drying oven, dry at 60℃ for 12h, and then grind to obtain the HY@Ni / Al2O3 precursor.
[0047] (3) Take 0.35g of the HY@Ni / Al2O3 precursor and place it in a tube furnace. Set the heating rate of the instrument from room temperature to 500℃ to 5℃ to 5℃ / min and the heating time to 95min. Introduce N2 (volume flow rate of 60mL / min) and H2 (volume flow rate of 60mL / min) and carry out the activation reaction at 500℃ for 1h to obtain 0.0661g of HY@Ni / Al2O3 catalyst with a yield of 18.84%. The loading of Ni / Al2O3 in the HY@Ni / Al2O3 catalyst is 45.5%.
[0048] Figure 1 Transmission microscopy image of the HY@Ni / Al2O3 catalyst prepared in Example 1. According to... Figure 1 The black particles are nickel particles with obvious agglomeration, while the light gray matrix is HY molecular sieve and alumina support with a core-shell structure outline.
[0049] Example 2 (1) The MOR molecular sieve was heated at a heating rate of 2℃ / min for 260min and calcined at 550℃ for 3h to obtain the calcined MOR molecular sieve (the molar ratio of SiO2 to Al2O3 was 25:1).
[0050] Step (2) uses the calcined MOR molecular sieve prepared in step (1) and other conditions are the same as in Example 1 to obtain the MOR@Ni / Al2O3 precursor.
[0051] Step (3) uses MOR@Ni / Al2O3 precursor, and other conditions are the same as in Example 1 to obtain 0.0676 g of MOR@Ni / Al2O3 catalyst with a yield of 19.31%; the loading of Ni / Al2O3 in the MOR@Ni / Al2O3 catalyst is 45.5%.
[0052] Figure 2 Transmission microscopy image of the MOR@Ni / Al2O3 catalyst prepared in Example 2. According to... Figure 2 It can be seen that the nickel particles in the sample agglomerated under low-magnification TEM, and the surface of the MOR molecular sieve matrix was coated with a large number of two-dimensional nanosheets. Medium and high-magnification TEM showed that the coating layer was composed of a large number of ultrathin, wrinkled and curled Ni-Al based nanosheets interwoven with each other, exhibiting a flower-like morphology, and some free nanosheet aggregates could also be observed.
[0053] Example 3 (1) Take 300 mL of 0.2 mol / L NaOH solution and add it to a three-necked flask. Add 4 g of MOR molecular sieve (SiO2 to Al2O3 molar ratio of 25:1). Transfer the three-necked flask to a microwave synthesizer, set the stirring speed to 200 rpm and the microwave power to 600 W, and react at 85 °C for 1 h. After the reaction is completed, cool naturally to room temperature, centrifuge and discard the supernatant. Wash the obtained precipitate four times with deionized water (50 mL each time). Place the washed precipitate in a forced-air drying oven and dry at 60 °C for 12 h. After grinding, heat at a rate of 2 °C / min for 260 min and calcine at 550 °C for 3 h to obtain the calcined mesoporous MOR molecular sieve (particle size of 0.54 ± 0.16096 μm).
[0054] Step (2) uses the mesoporous MOR molecular sieve prepared in step (1) and other conditions are the same as in Example 1 to obtain the mesoporous MOR@Ni / Al2O3 precursor.
[0055] Step (3) uses MOR@Ni / Al2O3 precursor, and other conditions are the same as in Example 1 to obtain 0.0614 g of mesoporous MOR@Ni / Al2O3 catalyst with a yield of 17.51%; the loading of Ni / Al2O3 in the mesoporous MOR@Ni / Al2O3 catalyst is 45.5%.
[0056] Example 4 (1) ZSM-5 molecular sieve (molar ratio of SiO2 to Al2O3 of 46:1) was purchased from Tianjin Nanhua Catalyst Co., Ltd.
[0057] Step (2) uses the ZSM-5 molecular sieve prepared in step (1) and other conditions are the same as in Example 1 to obtain the ZSM-5@Ni / Al2O3 precursor.
[0058] Step (3) uses ZSM-5@Ni / Al2O3 precursor, and other conditions are the same as in Example 1, to obtain 0.1293 g of ZSM-5@Ni / Al2O3 catalyst with a yield of 36.91%; the loading of Ni / Al2O3 in the ZSM-5@Ni / Al2O3 catalyst is 45.5%.
[0059] Figure 3 This is a transmission microscope image of the ZSM-5@Ni / Al2O3 catalyst prepared in Example 4. According to... Figure 3 Low-magnification TEM results show that the ZSM-5 molecular sieve particles are completely coated with a large number of nanosheets, and the nickel particles are aggregated. Medium- and high-magnification TEM results show that the Ni-Al based nanosheets of the coating layer grow radially outward in a manner perpendicular to the surface of the ZSM-5 support, exhibiting a sea urchin-like cluster morphology; the nanosheets are ultrathin, and the layers are interwoven to form abundant mesopores.
[0060] Comparative Example 1 Step (1) is the same as in Example 2.
[0061] Step (2) is basically the same as in Example 2, except that the amount of urea added is 4.95g, microwave-assisted synthesis is omitted, and only the reaction system is subjected to hydrothermal reaction to obtain MOR@Ni / Al2O3 precursor-HT.
[0062] In step (3), the MOR@Ni / Al2O3 precursor-HT was used, and other conditions were the same as in Example 2. 0.0343 g of MOR@Ni / Al2O3 catalyst-HT was obtained with a yield of 9.8%. The loading of Ni / Al2O3 in the MOR@Ni / Al2O3 catalyst-HT was 45.5%.
[0063] Figure 4 Transmission microscopy image of the MOR@Ni / Al2O3 catalyst-HT prepared in Comparative Example 1. According to... Figure 4 It can be seen that the nickel particles are severely agglomerated under low magnification TEM, while under high magnification TEM, the lamellae are short and thick, stacked and compressed in large quantities, and the gaps between the lamellae are blocked. There are many fine and dispersed particles in some areas, indicating that the nucleation is uneven and some metal species have not grown into complete two-dimensional lamellae, but have precipitated as small particles.
[0064] Comparative Example 2 Step (1) is basically the same as in Example 2, except that the molar ratio of SiO2 to Al2O3 in the MOR molecular sieve is 10:1.
[0065] Step (2) is basically the same as in Example 2, except that the amount of urea added is 4.95g and the reaction time is 0.5h, to obtain the MOR@Ni / Al2O3 precursor-HT.
[0066] In step (3), the MOR@Ni / Al2O3 precursor-HT was used, and other conditions were the same as in Example 2, to obtain 0.0094 g of MOR@Ni / Al2O3 catalyst-HT, with a yield of 2.69%.
[0067] Figure 5 Transmission microscopy image of the MOR@Ni / Al2O3 catalyst-HT prepared in Comparative Example 2. According to... Figure 5 It can be seen that under low-magnification TEM, aggregates can be observed. Under medium- and high-magnification TEM, most molecular sieve crystal surfaces are exposed, with only a few particles showing a very small amount of indistinct flocculent deposits. No continuous and complete two-dimensional nanosheet shells have formed; only a very small amount of sporadic spot-like deposits remain on the surface, and no intricately folded two-dimensional LDH sheets have developed. Metal species only undergo weak, localized deposition and have not completed lamellar construction.
[0068] Application Example 1 Weigh 0.35g of the catalyst prepared in Example 4 and add it to a high-pressure reactor along with 0.15g of biphenyl and 40mL of n-hexane. First, pressurize with N2 and purge the air, then introduce H2 until the pressure reaches 1MPa. Heat to 300℃ and react at 300℃ for 9h with a stirring rate of 700rpm.
[0069] This document uses specific examples to illustrate the principles and implementation methods of the present invention. The descriptions of the above embodiments are only for the purpose of helping to understand the method and core ideas of the present invention. Furthermore, those skilled in the art will recognize that, based on the ideas of the present invention, there will be changes in the specific implementation methods and application scope. Therefore, the content of this specification should not be construed as a limitation of the present invention.
Claims
1. A method for preparing a microwave-assisted molecular sieve@Ni / Al2O3 catalyst, comprising the following steps: Molecular sieves, urea, and a nickel-aluminum mixed salt solution were mixed and reacted under microwave conditions to obtain a precursor. The precursor was activated in an activating atmosphere to obtain the molecular sieve@Ni / Al2O3 catalyst. The microwave power is 500~600W and the frequency is 2300~2500MHz; the reaction time is 1~2h.
2. The preparation method according to claim 1, characterized in that, The molecular sieve includes MOR molecular sieve, HY molecular sieve or ZSM-5 molecular sieve; the molar ratio of silica to alumina in the MOR molecular sieve is 10~40:1; the molar ratio of silica to alumina in the ZSM-5 molecular sieve is 25~50:
1.
3. The preparation method according to claim 1, characterized in that, The nickel-aluminum mixed salt solution has a nickel salt concentration of 0.15~0.25 mol / L and an aluminum salt concentration of 0.1~0.2 mol / L; the molar ratio of nickel to aluminum in the nickel-aluminum mixed salt solution is 1~7:
1.
4. The preparation method according to claim 3, characterized in that, The ratio of molecular sieve, urea, and nickel-aluminum salt solution is 1~2g:4~6g:50~60mL.
5. The preparation method according to claim 1, characterized in that, The reaction is carried out at a temperature of 95~100℃ and under stirring conditions at a stirring rate of 200~500 rpm.
6. The preparation method according to claim 1, characterized in that, The activation atmosphere is a mixture of nitrogen and hydrogen, with a nitrogen to hydrogen gas flow rate ratio of 1~1.2:1~1.2; the activation temperature is 480~520℃, and the holding time is 1~1.5h.
7. The molecular sieve@Ni / Al2O3 catalyst prepared by the preparation method according to any one of claims 1 to 6.
8. The molecular sieve@Ni / Al2O3 catalyst according to claim 7, characterized in that, The molecular sieve@Ni / Al2O3 catalyst includes a molecular sieve support and an active component supported on the surface of the molecular sieve support. The active component is nickel and alumina, the molar ratio of nickel to alumina is 1~7:1, and the loading of the active component is 43~47%.
9. The application of the molecular sieve@Ni / Al2O3 catalyst according to claim 7 or 8 in the catalytic hydrogenation reaction of biphenyl.
10. The application according to claim 9, characterized in that, The mass ratio of the molecular sieve@Ni / Al2O3 catalyst to biphenyl is 2~2.5:1.