A molecular sieve catalyst, its preparation method, and its application
Patent Information
- Application Number
- CN202611344998.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-17
Smart Images

Figure CN123102407A_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of catalyst technology, specifically relating to a molecular sieve catalyst, its preparation method, and its application. Background Technology
[0002] Molecular sieve catalysts play an irreplaceable role in petrochemical, coal chemical, and environmental catalysis fields due to their unique pore structure, tunable acidity, and good thermal stability. However, the micropore size in molecular sieve catalysts significantly restricts molecular diffusion during the reaction process, severely limiting further improvements in their catalytic performance.
[0003] To address the diffusion limitation problem of micropores in molecular sieve catalysts, related technologies generally employ a strategy of constructing hierarchical pore structures. By introducing mesopores, mass transfer efficiency can be improved. The main preparation methods include alkali treatment, acid treatment, fluoride treatment, and soft / hard template methods.
[0004] However, while introducing mesopores, the relevant methods generally suffer from the drawback of sacrificing micropores to achieve mesopores. While improving mass transfer capacity, they severely weaken the intrinsic microporous characteristics of molecular sieves, thus restricting their further application in the field of high-performance catalysis. Summary of the Invention
[0005] This application aims to provide a molecular sieve catalyst, its preparation method, and its application, in order to solve the problem that introducing mesopores may sacrifice micropores and weaken the intrinsic microporous properties of molecular sieves.
[0006] To solve the above-mentioned technical problems, this application is implemented as follows: In a first aspect, embodiments of this application disclose a method for preparing a molecular sieve catalyst, the preparation method comprising: The pretreated molecular sieve is mixed with an etching solution and etched to obtain a molecular sieve catalyst. The pore structure of the molecular sieve catalyst includes micropores and mesopores, and the mesopores diffuse outward regularly along the shape of the molecular sieve crystal; The etchant in the etching solution is selected from one or more of sodium carbonate, potassium carbonate, sodium bicarbonate, sodium carbonate-sodium bicarbonate, ethanolamine-hydrochloric acid, and triethanolamine-hydrochloric acid. The molecular sieve is selected from one of ZSM-5 molecular sieve, β molecular sieve, Y-type molecular sieve, mordenite, and MCM-22 molecular sieve; The solid-liquid ratio of the pretreated molecular sieve to the etching solution ranges from 1:5 g / mL to 1:50 g / mL.
[0007] Optionally, the concentration of the etching solution is 0.1 mol / L to 2.0 mol / L; and / or, The etching solution has a pH value of 10.5 to 12.0.
[0008] Optionally, the etching temperature is 10℃~40℃, and the etching time is 1 h~24 h.
[0009] Optionally, the preparation process of the pretreated molecular sieve includes: Molecular sieves are calcined to obtain pretreated molecular sieves, wherein the calcination temperature is 450℃~550℃, the calcination time is 3 h~8 h, and the heating rate is 1℃ / min~5℃ / min.
[0010] Optionally, the step of mixing the pretreated molecular sieve with an etching solution and performing etching to obtain a molecular sieve catalyst includes: The pretreated molecular sieve was mixed with an etching solution and etched. Then, it was separated, washed, and dried in sequence to obtain the precursor. The precursor is subjected to exchange and activation treatments to obtain a molecular sieve catalyst.
[0011] Optionally, the exchange process includes: The precursor was placed in an ammonium salt solution for ammonium ion exchange treatment. The ammonium salt solution is selected from ammonium nitrate solution or ammonium chloride solution; and / or, The concentration of the ammonium salt solution is 0.5 mol / L to 2.0 mol / L; and / or, The temperature for the exchange process is 25℃~80℃.
[0012] Optionally, the activation treatment temperature range is 450℃~600℃, and the activation time is 2 h~6 h.
[0013] Optionally, the silica-to-alumina ratio of the molecular sieve ranges from 20 to 200.
[0014] Secondly, embodiments of this application provide a molecular sieve catalyst, which is obtained according to the preparation method described above.
[0015] Thirdly, this application provides an application of a molecular sieve catalyst, which is used in the conversion reaction of syngas to produce aromatics. The reaction temperature in the conversion reaction is 300℃~500℃, and the space velocity in the conversion reaction is 500 h⁻¹. -1 ~3000h -1 ; The selectivity for aromatics is greater than 82%.
[0016] Compared with the prior art, the embodiments of this application have the following advantages: In the embodiments of this application, a pretreated molecular sieve is mixed with an etching solution and etched to obtain a molecular sieve catalyst. The pore structure of the molecular sieve catalyst includes micropores and mesopores, and the mesopores diffuse outward regularly along the shape of the molecular sieve crystal. The etchant in the etching solution is selected from one or more of sodium carbonate, potassium carbonate, sodium bicarbonate, sodium carbonate-sodium bicarbonate, ethanolamine-ethanolamine hydrochloride, and triethanolamine-hydrochloric acid. The molecular sieve is selected from one of ZSM-5 molecular sieve, β molecular sieve, Y-type molecular sieve, mordenite, and MCM-22 molecular sieve. The solid-liquid ratio of the pretreated molecular sieve to the etching solution is in the range of 1:5 to 1:50 g / mL.
[0017] Etching is performed using one or more of the following etchants: sodium carbonate, potassium carbonate, sodium bicarbonate, sodium carbonate-sodium bicarbonate, ethanolamine-ethanolamine hydrochloride, and triethanolamine-hydrochloric acid. These etchants provide a relatively mild and controllable etching process, preserving the integrity of the molecular sieve catalyst framework and minimizing damage to the microporous regions. The mild etching environment is far less aggressive on framework aluminum than strong alkalis. Ions in the etching solution form complexes with some free aluminum ions, slowing down aluminum loss and preventing rapid localized removal of framework aluminum due to pH abrupt changes. This helps maintain the number and uniform distribution of acidic sites in the molecular sieve catalyst. Simultaneously, the silicon species redeposition phenomenon (i.e., dissolution-reprecipitation equilibrium) during the etching process helps repair some framework defects, allowing the molecular sieve catalyst to introduce mesopores while retaining micropores.
[0018] Furthermore, the mesopores diffuse outward regularly along the shape of the molecular sieve crystals. This highly regular and ordered mesopore channel solves the problems of disorder and poor connectivity of traditional mesopores, and achieves a synergistic effect of rapid mass transfer, directional reaction, and anti-coking stability. Compared with existing disordered mesoporous molecular sieves, the molecular sieve catalyst of this application improves the selectivity of aromatics and extends the life of molecular sieve catalysts in the synthesis of aromatics from syngas, and solves the defects of sacrificing micropores for mesopores in related technologies.
[0019] Additional aspects and advantages of this application will be set forth in part in the description which follows, and in part will be obvious from the description, or may be learned by practice of this application. Attached Figure Description
[0020] The above and / or additional aspects and advantages of this application will become apparent and readily understood from the description of the embodiments taken in conjunction with the following drawings, in which: Figure 1 This paper shows a transmission electron microscope (TEM) image of the molecular sieve catalyst provided in Example 1 of this application; Figure 2The image shows a transmission electron microscope (TEM) image of the molecular sieve catalyst provided in Comparative Example 1 of this application; Figure 3 The image shown is a transmission electron microscope (TEM) image of the molecular sieve catalyst provided in Comparative Example 2 of this application; Figure 4 A comparison diagram of nitrogen adsorption-desorption isotherms of the molecular sieve catalysts provided in Example 1 and Comparative Example 1 of this application is shown. Detailed Implementation
[0021] The embodiments of this application will now be described in detail. Examples of these embodiments are illustrated in the accompanying drawings, wherein the same or similar reference numerals denote the same or similar elements or elements having the same or similar functions throughout. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain this application, and should not be construed as limiting this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without inventive effort are within the scope of protection of this application.
[0022] Molecular sieve catalysts, as a class of aluminosilicate crystal materials with regular microporous channels, occupy an irreplaceable core position in petrochemical, coal chemical, and environmental catalysis fields due to their tunable acidic site distribution, excellent hydrothermal stability, and unique shape-selective catalytic properties. Among them, ZSM-5 molecular sieve, with its 0.53×0.56 nm straight channels and 0.51×0.55 nm sinusoidal channels, exhibits excellent catalytic activity and product selectivity in reactions such as catalytic cracking, methanol-to-olefins / aromatics, and adsorption and removal of volatile organic compounds (VOCs), making it one of the most widely used molecular sieve catalysts in industrial catalysis. However, its narrow micropore size (approximately 0.55 nm) severely restricts the diffusion of larger molecules within the channels, leading to insufficient utilization of internal acidic sites, hindered mass transfer between reactants and products, susceptibility to secondary reactions, and carbon deposition and deactivation, especially when processing large molecular reactants.
[0023] Related technologies generally employ a strategy of constructing hierarchical porous structures to improve mass transfer efficiency by introducing mesopores. The main preparation methods include alkali treatment, acid treatment, fluoride treatment, and soft / hard template methods. Alkali treatment utilizes strong alkaline solutions such as sodium hydroxide and potassium hydroxide to selectively break the silicon-oxygen (Si-O-Si) bonds in the molecular sieve framework, removing silicon atoms to form mesopores. Acid treatment uses acid solutions such as HCl and HNO3 to remove aluminum atoms from the framework, constructing secondary channels within the molecular sieve. Fluoride treatment uses fluorine-containing reagents such as NH4F and HF-NH4F to etch the molecular sieve framework, introducing mesopores. Soft / hard template methods involve adding mesoporous templates such as hexadecyltrimethylammonium bromide (CTAB), carbon nanotubes, and polymers during molecular sieve synthesis to induce the simultaneous formation of mesoporous structures.
[0024] However, while introducing mesopores, these methods often come with significant structural and performance losses. Traditional strong base etching is a violent and difficult-to-control reaction, easily leading to large-area destruction of the microporous structure and a reduction in micropore area of more than 30%. Furthermore, etching often occurs randomly from defect sites, forming disordered "wormhole-like" mesopores with poor channel connectivity. Acid treatment, while capable of dealumination and pore creation, easily causes excessive dealumination, resulting in smaller mesopore sizes (typically less than 5 nm) and significant loss of acidic sites. Fluoride treatment is highly corrosive, posing high environmental and safety risks and making industrial implementation difficult. Soft / hard template methods face problems such as high template agent costs, complex synthesis steps, and poor mesopore-micropore connectivity. Overall, existing technologies generally suffer from the drawback of "sacrificing micropores for mesopores." While improving mass transfer capabilities, they severely weaken the intrinsic microporous characteristics, shape selectivity, and acid stability of molecular sieve catalysts, limiting their further application in high-performance catalysis and adsorption.
[0025] This application aims to address the problem that introducing mesopores sacrifices micropores, weakening the intrinsic microporous properties of molecular sieves. To address this issue, firstly, this application proposes a method for preparing a molecular sieve catalyst, the method comprising: The pretreated molecular sieve is mixed with an etching solution and etched to obtain a molecular sieve catalyst. The pore structure of the molecular sieve catalyst includes micropores and mesopores, and the mesopores diffuse outward regularly along the shape of the molecular sieve crystal; The etchant in the etching solution is selected from one or more of sodium carbonate, potassium carbonate, sodium bicarbonate, sodium carbonate-sodium bicarbonate, ethanolamine-hydrochloric acid, and triethanolamine-hydrochloric acid. The molecular sieve is selected from one of ZSM-5 molecular sieve, β molecular sieve, Y-type molecular sieve, mordenite, and MCM-22 molecular sieve; The solid-liquid ratio of the pretreated molecular sieve to the etching solution ranges from 1:5 g / mL to 1:50 g / mL.
[0026] It should be noted that the etching process requires magnetic or mechanical stirring, with a stirring speed range of 100 rpm to 500 rpm. For example, the speed can be one or any combination of 100 rpm, 150 rpm, 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm, 450 rpm, and 500 rpm.
[0027] It should be noted that ultrasonic-assisted etching can be used for etching. Applying ultrasonic waves during the etching process can accelerate mass transfer, shorten processing time, and maintain the characteristics of gentle etching.
[0028] Etching can also be performed in steps, such as pretreatment with a low concentration (0.1 mol / L ~ 0.5 mol / L) etching solution, followed by main etching with a slightly higher concentration (0.8 mol / L ~ 2 mol / L), which can achieve a gradient mesoporous structure.
[0029] It should be noted that after etching, a mild acid treatment (such as dilute hydrochloric acid) can be applied to further adjust the distribution of acidic sites; metals such as Zn, Ga, and La can also be introduced after etching to prepare functionalized hierarchical porous molecular sieve catalysts; phosphoric acid or phosphate modification can also be carried out after etching to improve the hydrothermal stability of the molecular sieve; these can be flexibly adjusted according to actual needs.
[0030] It should be noted that the solid-liquid ratio of the pretreated molecular sieve to the etching solution ranges from 1:5 g / mL to 1:50 g / mL. For example, the solid-liquid ratio can be any one or both of the following: 1:5 g / mL, 1:8 g / mL, 1:10 g / mL, 1:15 g / mL, 1:20 g / mL, 1:25 g / mL, 1:30 g / mL, 1:35 g / mL, 1:40 g / mL, 1:45 g / mL, and 1:50 g / mL. In a specific implementation, the mass of the pretreated molecular sieve is 5g, and the volume of the etching solution is 100mL; in this case, the solid-liquid ratio is 1:20 g / mL.
[0031] In this embodiment, etching is performed using one or more of sodium carbonate, potassium carbonate, sodium bicarbonate, sodium carbonate-sodium bicarbonate, ethanolamine-ethanolamine hydrochloride, and triethanolamine-hydrochloric acid. These etching agents are relatively mild during the etching process, which keeps the framework of the molecular sieve catalyst intact and prevents damage to the microporous region. The mild etching environment is far less aggressive to the aluminum framework than strong alkalis. Ions in the etching solution form complexes with some free aluminum ions, which slows down the loss of aluminum and avoids the rapid local removal of framework aluminum caused by pH changes. This helps to maintain the number and uniform distribution of acidic sites in the molecular sieve catalyst. At the same time, the silicon species redeposition phenomenon (i.e., dissolution-reprecipitation equilibrium) that occurs during the etching process helps to repair some framework defects. Thus, the molecular sieve catalyst can introduce mesopores while retaining micropores.
[0032] Furthermore, the mesopores diffuse outward regularly along the shape of the molecular sieve crystals. This highly regular and ordered mesopore channel solves the problems of disorder and poor connectivity of traditional mesopores, and achieves a synergistic effect of rapid mass transfer, directional reaction, and anti-coking stability. Compared with existing disordered mesoporous molecular sieves, the molecular sieve catalyst of this application improves the selectivity of aromatics and extends the life of molecular sieve catalysts in the synthesis of aromatics from syngas, and solves the defects of sacrificing micropores for mesopores in related technologies.
[0033] Optionally, in one embodiment, the concentration of the etching solution is 0.1 mol / L to 2.0 mol / L; Optionally, in one embodiment, the pH value of the etching solution is 10.5 to 12.0.
[0034] It should be noted that the concentration of the etching solution is 0.1 mol / L to 2.0 mol / L. For example, the concentration of the etching solution can be one or any two of the following: 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.5 mol / L, 0.6 mol / L, 0.8 mol / L, 0.9 mol / L, 1.0 mol / L, 1.2 mol / L, 1.5 mol / L, 1.8 mol / L, and 2.0 mol / L.
[0035] It should be noted that the pH value of the etching solution is 10.5~12.0. For example, the pH value of the etching solution is one or any two of the following: 10.5, 10.7, 10.9, 11.0, 11.3, 11.6, 11.8, and 12.0.
[0036] For example, when the etching solution is a sodium carbonate-sodium bicarbonate solution, CO3 is present in the solution. 2- With HCO3 - The hydrolysis equilibrium. When etching consumes hydroxide ions (OH-), the process... - When OH- is added, the equilibrium shifts to the right.- ; Local OH - When the concentration is too high, the equilibrium shifts to the left, consuming OH-. - This self-buffering mechanism maintains the pH of the etching solution within the range of 10.5-12.0 (compared to pH≈14 for NaOH), and the hydroxide concentration in this application remains relatively constant, thereby achieving a uniform, mild, and controllable etching process.
[0037] For example, when the etching solution is a sodium bicarbonate solution, its alkalinity is weaker (pKa≈8.3), which is suitable for scenarios requiring milder etching conditions, and the etching solution concentration can be increased to 2 mol / L ~ 3 mol / L.
[0038] When the etching solution is a potassium carbonate solution, the potassium ion has a large radius, which produces different regulatory effects on the etching process.
[0039] When the etching solution is an organic buffer system such as ethanolamine-hydrochloric acid or triethanolamine-hydrochloric acid, it has an adjustable buffer range and template effect.
[0040] In this embodiment, by controlling the etching solution concentration to 0.1 mol / L~2.0 mol / L and the pH value to 10.5~12.0, selective and mild etching of the molecular sieve catalyst is achieved. This ensures that the etching reaction preferentially breaks the silicon-oxygen bonds in the framework, and directional desilication forms highly regular and ordered mesoporous channels that diffuse outward regularly along the shape of the molecular sieve crystal, while preserving the original microporous structure and framework aluminum sites to the maximum extent.
[0041] Optionally, in one embodiment, the etching temperature is 10°C to 40°C, and the etching time is 1 h to 24 h.
[0042] It should be noted that the etching temperature is 10~40℃. For example, the etching temperature is one or any two of the following: 10℃, 15℃, 20℃, 25℃, 30℃, 35℃, and 40℃.
[0043] It should be noted that the etching time is 1 to 24 hours. For example, the etching time is one or any two of the following: 1 hour, 2 hours, 5 hours, 8 hours, 10 hours, 12 hours, 15 hours, 18 hours, 20 hours, 22 hours, and 24 hours.
[0044] In this embodiment, by controlling the etching temperature to be 10℃~40℃ and the etching time to be 1 h~24 h, mild and directional etching of molecular sieve catalysts can be achieved at room temperature or near room temperature, avoiding defects such as framework collapse and mesoporous disorder caused by high temperature and long time etching. Moreover, it has low energy consumption, simple equipment requirements, and is easy to scale up industrially. Ultimately, in the synthesis of aromatics from syngas, it is beneficial to improve the selectivity of molecular sieve catalysts for aromatics.
[0045] Optionally, in one embodiment, the preparation process of the pretreated molecular sieve includes: Molecular sieves are calcined to obtain pretreated molecular sieves, wherein the calcination temperature is 450℃~550℃, the calcination time is 3 h~8 h, and the heating rate is 1℃ / min~5℃ / min.
[0046] It should be noted that the roasting temperature is 450℃~550℃. For example, the roasting temperature is one or any two of the following: 450℃, 480℃, 500℃, 520℃, and 550℃.
[0047] It should be noted that the roasting time is 3 to 8 hours. For example, the roasting time is one or any two of the following: 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, and 8 hours.
[0048] It should be noted that the heating rate is 1℃ / min to 5℃ / min. For example, the heating rate is one or any two of the following: 1℃ / min, 2℃ / min, 3℃ / min, 4℃ / min, and 5℃ / min.
[0049] In this embodiment, by controlling the calcination temperature to 450℃~550℃, the calcination time to 3h~8h, and the heating rate to 1℃ / min~5℃ / min, precise pretreatment of molecular sieves can be achieved. The calcination process completely removes organic template agents and constructs open microporous channels while avoiding the collapse of the framework structure and the loss of acidic sites. The pretreated molecular sieve has a high surface cleanliness and sufficient exposure of active sites, providing a uniform reaction substrate for subsequent gentle etching.
[0050] Optionally, in one embodiment, the step of mixing the pretreated molecular sieve with an etching solution and performing etching to obtain a molecular sieve catalyst includes: The pretreated molecular sieve was mixed with an etching solution and etched. Then, it was separated, washed, and dried in sequence to obtain the precursor. The precursor is subjected to exchange and activation treatments to obtain a molecular sieve catalyst.
[0051] In practice, the pretreated molecular sieve is mixed with an etching solution and etched. After etching, the system is cooled to room temperature (if the etching temperature is higher than room temperature), and then separated by filtration or centrifugation at 3000 rpm to 8000 rpm for 5 to 15 minutes, during which time the solid and liquid are separated. The filtrate is washed with deionized water until it is neutral (pH 6.5 to 7.5), usually 3 to 6 times. Then, it is dried at 80℃ to 120℃ for 6 to 12 hours to obtain the precursor. The precursor is then exchanged to replace residual sodium / potassium ions, and then activated to obtain the molecular sieve catalyst.
[0052] In this embodiment, a refined post-processing procedure including etching, separation, washing, drying, exchange, and activation is used to achieve the precise preparation of multi-level porous molecular sieve catalysts. Separation and washing after etching can terminate the etching reaction, remove residual impurities, and avoid framework collapse and pore blockage. Ion exchange and activation can remove alkali metal ions, construct highly efficient active sites, and enhance catalytic synergy.
[0053] Optionally, in one embodiment, the exchange treatment includes: placing the precursor in an ammonium salt solution for ammonium ion exchange treatment; the ammonium salt solution is selected from ammonium nitrate solution or ammonium chloride solution.
[0054] Optionally, in one embodiment, the concentration of the ammonium salt solution is 0.5 mol / L to 2.0 mol / L.
[0055] Optionally, in one embodiment, the temperature of the exchange process is 25°C to 80°C.
[0056] It should be noted that the concentration of the ammonium salt solution is 0.5 mol / L to 2.0 mol / L. For example, the concentration of the ammonium salt solution is one or any two of the following: 0.5 mol / L, 0.8 mol / L, 1.0 mol / L, 1.2 mol / L, 1.5 mol / L, 1.8 mol / L, and 2.0 mol / L.
[0057] It should be noted that the temperature of the exchange process is 25℃~80℃. For example, the temperature of the exchange process is one or any two of the following: 25℃, 30℃, 40℃, 50℃, 60℃, 70℃, and 80℃.
[0058] In this embodiment, an ammonium salt solution is used for exchange treatment. The concentration of the ammonium salt solution is 0.5 mol / L to 2.0 mol / L, and the exchange treatment temperature is 25℃ to 80℃. This synergistically achieves efficient removal of alkali metal cations and precise control of acidic sites. Compared with the defects of incomplete exchange of low-concentration ammonium salts and skeletal swelling caused by high concentrations in related technologies, the processing parameters of this application can ensure uniform distribution of acidic sites. The microporous-mesoporous molecular sieve catalyst obtained after subsequent calcination and activation exhibits excellent catalytic activity and stability in the synthesis of aromatics from syngas, which is beneficial to improving CO conversion rate and aromatic selectivity.
[0059] Optionally, in one embodiment, the activation treatment temperature range is 450℃~600℃, and the activation time is 2~6h.
[0060] It should be noted that the activation treatment temperature range is 450℃~600℃. For example, the activation treatment temperature range is one or any two of the following: 450℃, 480℃, 500℃, 520℃, 550℃, 580℃, and 600℃.
[0061] It should be noted that the activation time is 2 to 6 hours. For example, the activation time is one or any two of the following: 2 hours, 3 hours, 4 hours, 5 hours, and 6 hours.
[0062] In this embodiment, by controlling the activation temperature range to 450℃~600℃ and the activation time to 2~6h, the directional conversion of ammonium-type molecular sieves to highly active molecular sieves is achieved, ensuring complete decomposition to generate acidic active sites, while avoiding the collapse of the molecular sieve framework and the loss of acidic sites. Ultimately, in the synthesis of aromatics from syngas, this is beneficial for improving the selectivity of molecular sieve catalysts for aromatics.
[0063] Optionally, in one embodiment, the silica-to-alumina ratio of the molecular sieve is in the range of 20 to 200.
[0064] It should be noted that molecular sieves include silicon dioxide (SiO2) and aluminum oxide (Al2O3). The molar ratio of silicon dioxide to aluminum oxide is called the silicon-aluminum ratio, which ranges from 20 to 200. For example, the silicon-aluminum ratio can be one or any two of the following values: 20, 24, 30, 36, 40, 44, 48, 50, 52, 56, 60, 64, 66, 70, 72, 76, 78, 80, 82, 86, 90, 92, 96, 100, 120, 140, 160, 180, and 200.
[0065] In this embodiment, the silica-to-alumina ratio of the molecular sieve is controlled between 20 and 200 to balance the acidity, pore structure stability, catalytic selectivity, and resistance to coking. Specifically, controlling the silica-to-alumina ratio between 20 and 200 helps improve the stability of the molecular sieve framework while preserving the microporous structure. In the syngas-to-aromatics reaction, this helps to improve CO conversion and enhance aromatics selectivity.
[0066] Secondly, embodiments of this application provide a molecular sieve catalyst, which is obtained according to the preparation method described above.
[0067] Thirdly, this application provides an application of a molecular sieve catalyst, which is used in the conversion reaction of syngas to produce aromatics. The reaction temperature in the conversion reaction is 300℃~500℃, and the space velocity in the conversion reaction is 500 h⁻¹. -1 ~3000h -1 ; The selectivity for aromatics is greater than 82%.
[0068] It should be noted that the reaction temperature in the conversion reaction is 300℃~500℃. For example, the reaction temperature in the conversion reaction is one or any two of the following: 300℃, 330℃, 350℃, 380℃, 400℃, 420℃, 450℃, and 500℃.
[0069] It should be noted that space velocity (GHSV) represents the amount of feed gas processed per unit mass of catalyst per unit time.
[0070] It should be noted that the space velocity in the conversion reaction is 500 h⁻¹. -1 ~3000h -1 For example, the space velocity in the conversion reaction is 500 h⁻¹. -1 600 h -1 700 h -1 800 h -1 900 h -1 1000 h -1 1500 h -1 2000 h -1 2500 h -1 3000 h -1 The range of one or any two of them.
[0071] In the embodiments of this application, the obtained molecular sieve catalyst is applied at 300℃~500℃ for 500 h. -1 ~3000h -1In the synthesis of aromatics from syngas, the excellent performance of achieving an aromatic selectivity of >82% is attributed to the microporous-highly ordered mesoporous structure of the molecular sieve catalyst and the mild etching process, which ensures the efficient activation and aromatization of syngas, while suppressing side reactions such as alkane formation and aromatic oligomerization, and has significant industrial application value.
[0072] To make the inventive objectives, technical solutions, and beneficial effects of this application clearer, the application is further described below with reference to embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of this application.
[0073] The present application will be described in detail below through embodiments.
[0074] Example 1 (1) Preparation of pretreated molecular sieves Take 5g of ZSM-5 molecular sieve, wherein the silicon-to-aluminum ratio of ZSM-5 molecular sieve is 76, and calcine the ZSM-5 molecular sieve to obtain pretreated molecular sieve. The calcine temperature is 550℃, the calcine time is 4 hours, and the heating rate is 5℃ / min.
[0075] (2) Preparation of molecular sieve catalysts Sodium carbonate was used as the etching agent, and 100 mL of sodium carbonate aqueous solution with a concentration of 1 mol / L was prepared as the etching solution. The pH value of the etching solution was 11.0, and the solid-liquid ratio of the pretreated molecular sieve to the etching solution was 1:20 g / mL.
[0076] The pretreated molecular sieve was mixed with an aqueous sodium carbonate solution and etched. The etching temperature was 25°C, the etching time was 6 hours, and the stirring rate was 300 rpm.
[0077] After the etching reaction is completed, the sample is cooled and then subjected to separation, washing until neutral, and drying to obtain the precursor. The drying temperature is 100°C and the drying time is 10 hours.
[0078] The aforementioned precursor was subjected to two exchange treatments with a 1.0 mol / L ammonium nitrate solution at 25°C, each lasting 6 hours. After exchange, the catalyst was filtered, washed, dried, and then activated to obtain the molecular sieve catalyst. The activation temperature was 500°C, and the activation time was 4 hours.
[0079] The molecular sieve catalyst obtained in Example 1 was observed by TEM, as follows: Figure 1 As shown, in the molecular sieve catalyst obtained in Example 1, the mesopores diffuse outward regularly along the shape of the molecular sieve crystal, which can also be understood as the formation of regular strip-shaped mesopores radiating outward from the center inside the crystal.
[0080] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is as follows: No etching process was performed in Comparative Example 1.
[0081] The remaining steps and dosages are the same as in Example 1, to obtain the molecular sieve catalyst.
[0082] The molecular sieve catalyst obtained in Comparative Example 1 was observed by TEM, such as... Figure 2 As shown, its internal crystal structure is dense and lacks obvious mesopores.
[0083] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is as follows: In Comparative Example 2, the etching solution in the preparation of the molecular sieve catalyst in step (2) was changed to sodium hydroxide.
[0084] The remaining steps and dosages are the same as in Example 1, to obtain the molecular sieve catalyst.
[0085] The molecular sieve catalyst obtained in Comparative Example 2 was observed by TEM, such as... Figure 3 As shown.
[0086] Depend on Figure 3 It is evident that the morphology of ZSM-5 molecular sieves undergoes significant changes after etching with sodium hydroxide. Scanning electron microscopy (SEM) images show that the molecular sieve no longer exhibits a regular grain morphology, but rather forms an aggregated structure composed of irregularly broken particles. The particle edges are broken, the surface is rough, and there are obvious local fragmentation and collapse phenomena. Transmission electron microscopy (TEM) images further show that the etched molecular sieve particles are irregularly flaky or fragmented, with blurred crystal boundaries, uneven internal contrast distribution, and severe damage to the original continuous framework structure. These results indicate that sodium hydroxide has a strong etching effect on ZSM-5 molecular sieves. Under this treatment condition, the molecular sieve undergoes severe desilication and framework collapse, resulting in the near loss of its original crystal structure and regular morphology.
[0087] The molecular sieve catalysts obtained in Example 1 and Comparative Example 1 were subjected to nitrogen adsorption-desorption tests, and the results are as follows: Figure 4 As shown in Table 1.
[0088] Table 1
[0089] according to Figure 4 As shown in Table 1, the molecular sieve catalysts obtained in the examples have significantly increased specific surface area and mesopore volume. At the same time, the molecular sieve catalysts have introduced mesopores while retaining micropores, that is, they do not sacrifice micropores for mesopores.
[0090] Catalytic performance test The molecular sieve catalysts obtained in Examples 1 and Comparative Example 1 were subjected to catalytic performance testing. The specific testing process is as follows: Molecular sieve catalyst was pressed into tablets, sieved to 40-60 mesh, and placed in a fixed-bed reactor for the conversion reaction of syngas to aromatics. The reaction conditions were: atmospheric pressure, reaction temperature of 350℃, and space velocity of 600 h⁻¹. -1 The results are shown in Table 2.
[0091] Table 2
[0092] As shown in Table 2, the molecular sieve catalyst obtained in this application exhibits excellent CO conversion and aromatic selectivity in the conversion reaction of syngas to aromatics.
[0093] In the description of this specification, the references to terms such as "one embodiment," "some embodiments," "illustrative embodiment," "example," "specific example," or "some examples," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of this application. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0094] Although embodiments of this application have been shown and described, those skilled in the art will understand that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of this application, the scope of which is defined by the claims and their equivalents.
Claims
1. A method for preparing a molecular sieve catalyst, characterized in that, The preparation method includes: The pretreated molecular sieve is mixed with an etching solution and etched to obtain a molecular sieve catalyst. The pore structure of the molecular sieve catalyst includes micropores and mesopores, and the mesopores diffuse outward regularly along the shape of the molecular sieve crystal; The etchant in the etching solution is selected from one or more of sodium carbonate, potassium carbonate, sodium bicarbonate, sodium carbonate-sodium bicarbonate, ethanolamine-hydrochloric acid, and triethanolamine-hydrochloric acid. The molecular sieve is selected from one of ZSM-5 molecular sieve, β molecular sieve, Y-type molecular sieve, mordenite, and MCM-22 molecular sieve; The solid-liquid ratio of the pretreated molecular sieve to the etching solution ranges from 1:5 g / mL to 1:50 g / mL.
2. The preparation method according to claim 1, characterized in that, The concentration of the etching solution is 0.1 mol / L to 2.0 mol / L; and / or, The etching solution has a pH value of 10.5 to 12.
0.
3. The preparation method according to claim 1, characterized in that, The etching process is performed at a temperature of 10°C to 40°C for 1 hour to 24 hours.
4. The preparation method according to claim 1, characterized in that, The preparation process of the pretreated molecular sieve includes: Molecular sieves are calcined to obtain pretreated molecular sieves, wherein the calcination temperature is 450℃~550℃, the calcination time is 3 h~8 h, and the heating rate is 1℃ / min~5℃ / min.
5. The preparation method according to claim 1, characterized in that, The process of mixing the pretreated molecular sieve with an etching solution and performing etching to obtain a molecular sieve catalyst includes: The pretreated molecular sieve was mixed with an etching solution and etched. Then, it was separated, washed, and dried in sequence to obtain the precursor. The precursor is subjected to exchange and activation treatments to obtain a molecular sieve catalyst.
6. The preparation method according to claim 5, characterized in that, The exchange process includes: The precursor was placed in an ammonium salt solution for ammonium ion exchange treatment. The ammonium salt solution is selected from ammonium nitrate solution or ammonium chloride solution; and / or, The concentration of the ammonium salt solution is 0.5 mol / L to 2.0 mol / L; and / or, The temperature for the exchange process is 25℃~80℃.
7. The preparation method according to claim 5, characterized in that, The activation treatment temperature range is 450℃~600℃, and the activation time is 2 h~6 h.
8. The preparation method according to any one of claims 1-7, characterized in that, The silica-to-alumina ratio of the molecular sieve ranges from 20 to 200.
9. A molecular sieve catalyst, characterized in that, The molecular sieve catalyst is obtained by the preparation method according to any one of claims 1-8.
10. An application of a molecular sieve catalyst, characterized in that, The molecular sieve catalyst obtained in claim 9 is used in the conversion reaction of syngas to produce aromatics; The reaction temperature in the conversion reaction is 300℃~500℃, and the space velocity in the conversion reaction is 500 h⁻¹. -1 ~3000h -1 ; The selectivity for aromatics is greater than 82%.