A method for one-pot directional crystallization preparation of high-silicon Cu-SSZ-39 molecular sieve catalysts using high-silicon FAU and its application.

By using a one-pot directional crystallization method, a high-silicon Cu-SSZ-39 molecular sieve was formed by combining a high-silicon FAU molecular sieve with a copper complex. This solved the problems of activity and stability of the high-silicon Cu-SSZ-39 catalyst when treating tail gas containing NO and NO2, and achieved high-efficiency denitrification performance and low N2O generation.

CN123102410APending Publication Date: 2026-11-17HUAZHONG UNIV OF SCI & TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611321277.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to simultaneously achieve high silicon framework purity, difficulty in copper introduction, low-temperature activity, rapid SCR byproduct control, and hydrothermal aging stability in high-silicon Cu-SSZ-39 molecular sieve catalysts, especially when treating exhaust gases containing NO and NO2.

Method used

A one-pot directional crystallization method was adopted, using high-silicon FAU molecular sieve as a crystalline silicon-aluminum precursor, combined with copper complex, alkaline template agent and AEI structure directing agent, to form high-silicon Cu-SSZ-39 molecular sieve through hydrothermal crystallization. The framework charge density and copper content were controlled, avoiding copper anchoring mismatch and impurity phase formation in traditional methods.

Benefits of technology

It achieves efficient denitrification under both standard SCR and fast SCR conditions, while exhibiting good hydrothermal stability and low N2O generation. It is suitable for the purification of tail gas containing NO and NO2, and the catalyst maintains good structure and activity under high-temperature hydrothermal conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102410A_ABST
    Figure CN123102410A_ABST
Patent Text Reader

Abstract

This invention discloses a method and application for preparing a high-silicon Cu-SSZ-39 molecular sieve catalyst via one-pot directional crystallization of high-silicon FAU, belonging to the field of environmental catalytic materials and molecular sieve preparation technology. The method uses high-silicon FAU molecular sieve as a crystalline silicon-aluminum precursor and the sole aluminum source. A copper source is introduced in the form of a copper complex into an initial gel containing an inorganic base source, an organic structure directing agent, a supplementary silicon source, and AEI-structured molecular sieve seed crystals. After hydrothermal crystallization, ammonium exchange, and calcination, a high-silicon Cu-SSZ-39 molecular sieve catalyst with an AEI topology is obtained. By adjusting the silicon-aluminum ratio of the FAU precursor, the gel composition, and the amount of copper introduced, the formation of the high-silicon AEI framework and the simultaneous introduction of copper components are achieved, and the Si / Al ratio of the obtained catalyst is controlled. The obtained catalyst is suitable for the selective catalytic reduction of ammonia containing NO and NO2 tail gas, exhibiting good denitrification activity, hydrothermal stability, and N2O control performance under standard and rapid SCR conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of environmental catalytic materials and molecular sieve preparation technology, specifically relating to a method and application of one-pot directional crystallization of high-silicon FAU to prepare high-silicon Cu-SSZ-39 molecular sieve catalyst. In particular, it relates to a method for preparing AEI topological structure Cu-SSZ-39 by one-pot directional crystallization using high-silicon FAU molecular sieve as a crystalline silicon-aluminum precursor in the presence of copper complex, and the application of the obtained catalyst in the selective catalytic reduction reaction of ammonia in NO and NO2-containing tail gas, especially suitable for the purification of nitrogen oxide-containing tail gas. Background Technology

[0002] Nitrogen oxides emitted by diesel engines and other lean-burn combustion devices mainly include NO and NO2, which are important precursors to photochemical smog, fine particulate matter, and acid deposition. Ammonia selective catalytic reduction (ACR) technology uses NH3 as a reducing agent to reduce NO under oxygen-rich conditions. x Selective conversion to N2 and H2O is a widely used denitrification technology in the exhaust aftertreatment system of mobile source diesel engines. Depending on the ratio of NO to NO2 in the intake air, NH3-SCR typically includes standard SCR (i.e., SSCR) with NO as the main nitrogen oxide and fast SCR (i.e., FSCR) with both NO and NO2 participating.

[0003] Copper-based small-pore molecular sieves possess high low-temperature activity, a wide operating temperature window, and good N2 selectivity. Among them, Cu-SSZ-13, with its CHA topology, has been widely used. However, under conditions such as active regeneration of diesel particulate filters or other high-temperature, water-rich environments, the catalyst may experience high-temperature hydrothermal shock. Severe hydrothermal treatment can cause dealuminization of the molecular sieve framework, damage to the pore structure, and migration and aggregation of copper species, thereby reducing the low-temperature or high-temperature denitrification performance of Cu-SSZ-13.

[0004] Cu-SSZ-39 possesses the AEI topology. Both AEI and CHA belong to the category of small-pore molecular sieves with cage-like structures connected by eight-membered ring pores, but their double six-membered ring connection methods and local framework environments differ. These structural differences affect the spatial distribution of framework aluminum sites and exchangeable copper species, thus influencing framework evolution and copper species stability under hydrothermal conditions. The cage-like confined environment formed by the AEI framework provides a structural basis for the stable existence of the framework structure and exchangeable copper species under high-temperature, water-containing conditions. This structural and copper species stability helps Cu-SSZ-39 maintain its catalytic performance in long-term high-temperature, water-containing exhaust gas environments, making it an important candidate material for high-durability exhaust gas purification catalysts.

[0005] Existing Cu-SSZ-39 catalysts typically employ a two-step method: first preparing the SSZ-39 matrix, then introducing copper via liquid-phase ion exchange or impregnation. Some techniques directly add copper complexes to the initial gel, allowing copper introduction to occur simultaneously with AEI structure crystallization. Chinese patent application CN117427687A discloses an in-situ preparation route involving hydrothermal crystallization of an active metal salt, an auxiliary metal salt, a complexing agent, a silicon source, a Y-type molecular sieve, and SSZ-39 seed crystals. Its focus is on improving the SSCR catalytic performance and hydrothermal stability at 750°C of metal-supported SSZ-39 (a low-silicon catalyst) with a Si / Al ratio of approximately 8 through the auxiliary metal. However, this prior art does not discuss FSCR catalytic performance or N2O generation. Importantly, it is generally accepted in the art that molecular sieve catalysts with low Si / Al ratios are difficult to efficiently treat exhaust gases containing both NO and NO2.

[0006] However, existing in-situ synthesis routes mainly target Cu-SSZ-39 with high aluminum content (i.e., low-silicon Cu-SSZ-39). As the Si / Al ratio of the target AEI framework increases, the number of negatively charged sites in the initial gel that can be used to balance the cationic organic structure directing agent and stabilize copper ions decreases, making the formation of a pure AEI phase difficult and easily leading to the formation of impurities. In other words, simply increasing the amount of external silicon source can easily result in incomplete precursor transformation, reduced crystallization rate, impurity phase formation, or insufficient copper introduction, making it difficult to stably obtain Cu-SSZ-39 with both a high silicon framework and suitable copper content.

[0007] On the other hand, a lower or higher Si / Al ratio is not necessarily more advantageous for Cu-SSZ-39. A higher framework aluminum density provides more ion exchange sites, but it also increases the framework negative charge density and Brønsted acid site density, promoting strongly coordinated Cu. 2+ -2Al species and acidic site-related intermediates are formed. This composition favors some high-temperature reactions but may limit the [Cu(OH)] required for low-temperature reactions. + The Si / Al ratio increases the non-selective conversion of ammonium nitrate intermediates and N2O formation during rapid SCR. Conversely, while excessively increasing the Si / Al ratio can reduce acid site density, it may reduce the stable anchoring sites for copper ions, resulting in insufficient copper content or copper species migration during hydrothermal processes.

[0008] Therefore, there is a need for a one-pot directional crystallization method that can promote AEI formation using structural units of crystalline precursors and achieve controlled copper introduction even at low framework aluminum density, thereby obtaining high-silicon Cu-SSZ-39 that has activity, N2O selectivity and severe hydrothermal aging resistance under both standard SCR and fast SCR conditions. Summary of the Invention

[0009] The purpose of this invention is to overcome the problems in the prior art, such as the difficulty in simultaneously achieving high silicon Cu-SSZ-39 phase purity and copper introduction, insufficient control of low-temperature activity and rapid SCR byproducts in traditional aluminum-rich Cu-SSZ-39, and the difficulty in simultaneously maintaining the framework and copper species after severe hydrothermal aging. This invention provides a one-pot directional crystallization preparation method for high silicon Cu-SSZ-39 molecular sieve catalysts, the catalyst obtained by this method, and its application in NH3-SCR purification of NO and NO2-containing tail gas.

[0010] To achieve the above objectives, the first aspect of the present invention provides a one-pot directional crystallization preparation method for a high-silicon Cu-SSZ-39 molecular sieve catalyst, comprising the following steps: (1) Preparation of copper complex solution: Dissolve copper source and complexing agent in water, stir to carry out complexation reaction, and obtain copper complex solution; (2) Preparation of alkaline template agent mixture: Inorganic alkali source, water and organic structure directing agent are mixed evenly to obtain alkaline template agent mixture; wherein, the metal element in the inorganic alkali source is an alkali metal element; (3) Mixing: Add the copper complex solution obtained in step (1) to the alkaline template agent mixture obtained in step (2) and stir until homogeneous; (4) Adding and crystallization: Add supplementary silicon source, high-silicon FAU molecular sieve and AEI structure molecular sieve seed crystals to the mixture obtained in step (3), mix evenly to obtain initial gel; perform hydrothermal crystallization on the initial gel to dissolve, recombine and directionally transform the high-silicon FAU molecular sieve to form copper-containing AEI structure molecular sieve; (5) Post-processing: The crystallized product obtained in step (4) is subjected to solid-liquid separation, washing and drying, and ion exchange is performed using ammonium salt solution. Then, it is dried and calcined to obtain the high-silicon Cu-SSZ-39 molecular sieve catalyst. The high-silica FAU molecular sieve has a SiO2 / Al2O3 molar ratio of 35 to 50 and serves as the crystalline silica-alumina precursor and the sole aluminum source in the initial gel. The SiO2 introduced by the high-silica FAU molecular sieve accounts for 60% to 80% of the total molar amount of SiO2 in the initial gel. The alkali metal element M in the inorganic base source, calculated as M2O, has a molar ratio of 0.15 to 0.18 with the SiO2 in the initial gel. The SiO2 / Al2O3 molar ratio of the obtained high-silicon Cu-SSZ-39 molecular sieve catalyst is 24 to 36.

[0011] As a further preferred embodiment of the present invention, the molar ratios of the components in the initial gel are: SiO2 / Al2O3 = 48 ~ 68; H2O / SiO2 = 7.1 ~ 8.6; OSDA / SiO2 = 0.11 ~ 0.15; Cu / Al = 0.50 ~ 0.90; complexing agent / Cu = 1.05 ~ 1.50; Wherein, the molar amount of SiO2 is the sum of the molar amounts of SiO2 introduced by the supplementary silicon source and the high-silicon FAU molecular sieve, and the molar amount of Al2O3 is the molar amount of Al2O3 introduced by the high-silicon FAU molecular sieve; OSDA is the organic structure directing agent.

[0012] As a further preferred embodiment of the present invention, the SiO2 / Al2O3 molar ratio of the high-silica FAU molecular sieve is 38 to 45, preferably 40; the SiO2 / Al2O3 molar ratio of the obtained Cu-SSZ-39 molecular sieve catalyst is preferably 26 to 32, and the Cu content is preferably 2.2 to 2.86 wt%.

[0013] As a further preferred embodiment of the present invention, the copper source is selected from one or more of copper sulfate, copper nitrate, copper chloride and copper acetate; the complexing agent is selected from one or two of EDTA-2Na·2H2O and EDTA-4Na·4H2O; preferably, the copper source is CuSO4·5H2O and the complexing agent is EDTA-4Na·4H2O.

[0014] As a further preferred embodiment of the present invention, the inorganic base source is selected from one or two of NaOH and KOH; the organic structure directing agent is 1,1,3,5-tetramethylpiperidine hydroxide; the supplementary silicon source is selected from one or more of silica sol, fumed silica and tetraethyl orthosilicate, preferably, the inorganic base source is NaOH and the supplementary silicon source is silica sol.

[0015] As a further preferred embodiment of the present invention, the AEI structured molecular sieve seed crystal is an SSZ-39 molecular sieve seed crystal, and its addition amount is 0.2% to 2.0% of the total mass of SiO2 and Al2O3 in the initial gel, preferably 0.5% to 1.0%.

[0016] As a further preferred embodiment of the present invention, in step (3), the copper complex solution is added to the alkaline template agent mixture and stirred for 0.5 to 3 h; in step (4), after adding the supplementary silicon source, the mixture is stirred for 0.5 to 2 h, and then high-silicon FAU molecular sieve and AEI structure molecular sieve seed crystals are added and stirred for another 0.5 to 3 h.

[0017] As a further preferred embodiment of the present invention, the hydrothermal crystallization temperature in step (4) is 160 ~ 185 ℃ and the crystallization time is 2 ~ 6 days; preferably, the hydrothermal crystallization temperature is 165 ~ 175 ℃ and the crystallization time is 3 ~ 5 days; more preferably, the hydrothermal crystallization temperature is 170 ℃ and the crystallization time is 4 days.

[0018] As a further preferred embodiment of the present invention, apart from the alkali metal element introduced by the inorganic alkali source and the alkali metal element optionally introduced in the complexing agent, no additional auxiliary salt is added to the initial gel; the metal elements in the auxiliary salt include alkaline earth metal elements, rare earth metals, and other transition metal elements other than copper.

[0019] As a further preferred embodiment of the present invention, the ammonium salt in step (5) is NH4Cl, the concentration of the ammonium salt solution is 0.5 ~ 1.5 mol / L, the ion exchange temperature is 60 ~ 90 ℃, and the number of ion exchanges is 1 ~ 4 times; the ion-exchanged product is dried at 100 ~ 120 ℃ and calcined in air at 550 ~ 650 ℃ for 4 ~ 8 h.

[0020] A second aspect of the present invention provides a Cu-SSZ-39 molecular sieve catalyst prepared by the above method, wherein the catalyst has an AEI topology and a SiO2 / Al2O3 molar ratio of 24 to 36.

[0021] As a further preferred embodiment of the present invention, the catalyst contains 1.99 to 3.0 wt% Cu and has a BET specific surface area of ​​680 to 820 m². 2 / g, total pore volume is 0.26 ~ 0.35 cm³ 3 / g; Preferably, the catalyst, after being hydrothermally treated at 800 °C for 16 h in an air atmosphere containing 10 vol% water vapor, retains a relative crystallinity of AEI of not less than 78% and a BET specific surface area of ​​not less than 82%.

[0022] The third aspect of this invention provides the application of the above-mentioned Cu-SSZ-39 molecular sieve catalyst in the selective catalytic reduction denitrification of ammonia containing NO and / or NO2 tail gas.

[0023] As a further preferred embodiment of the present invention, the exhaust gas and the catalyst are contacted at 150 ~ 550 °C to carry out a selective catalytic reduction denitrification reaction; Preferably, the exhaust gas contains both NO and NO2, with a molar ratio of NO to NO2 of 2:1 to 1:2, preferably 1:1; the exhaust gas also contains NH3, O2, water vapor and CO2.

[0024] As a further preferred embodiment of the present invention, the Cu-SSZ-39 molecular sieve catalyst, after being hydrothermally treated at 800 °C for 16 h in an air atmosphere containing 10 vol% water vapor, contains 250 ppm NO, 250 ppm NO2, 500 ppm NH3, 10 vol% O2, 8 vol% CO2, and 5 vol% H2O, with a gas hourly space velocity of 200,000 h⁻¹. -1 Under rapid ammonia selective catalytic reduction (SCR) conditions, the N2O formation concentration is no higher than 20 ppm; under standard SCR conditions, the NO concentration is maintained at no less than 90% within a temperature range of 225 ~ 500 ℃. x Conversion rate.

[0025] Compared with the prior art, the present invention has at least the following beneficial effects: (1) This invention does not directly crystallize amorphous aluminum-silicon species into AEI. Instead, it utilizes the characteristic that high-silicon FAU and AEI both contain double six-membered ring structural units. High-silicon FAU provides pre-organized crystalline structure information, and AEI seed crystals and organic structure directing agents (such as 1,1,3,5-tetramethylpiperidine cations) work together to improve the phase selectivity of directional crystallization, which is beneficial to forming AEI structure at a lower framework aluminum density.

[0026] (2) In this invention, high-silicon FAU, supplementary silicon source, gel basicity, OSDA, complexing agent and Cu are synergistically matched so that the introduction of copper occurs simultaneously with the formation of the high-silicon AEI structure, avoiding the mismatch of crystallization and copper anchoring caused by simply increasing the external silicon source. In the preparation method of this invention, the copper source is added to the initial gel in the form of a copper complex before hydrothermal crystallization, and the remaining SiO2 is provided by the supplementary silicon source.

[0027] (3) The high-silicon Cu-SSZ-39 obtained in this invention has a moderate framework charge density and acid site density, and can be reacted in highly reactive [Cu(OH)] reactions. + -Al species, stable Cu 2+ A relatively balanced distribution is formed between the -2Al species and Brønsted acid sites, thereby achieving a balance between low-temperature activity (200°C), hydrothermal stability, and rapid SCR byproduct (i.e., N2O) control under the catalyst series and evaluation conditions described in this invention.

[0028] Furthermore, the present invention yields a high-silicon catalyst. Because the SiO2 / Al2O3 molar ratio of the catalyst is 24-36, its acidity is lower, which inhibits the formation of intermediate ammonium nitrate during the rapid reaction process, keeping the ammonium nitrate within a suitable range and improving the catalytic efficiency of the rapid reaction. The SiO2 / Al2O3 molar ratio of the catalyst cannot exceed 36. This is mainly because while excessively increasing the SiO2 / Al2O3 ratio can reduce the acid site density, it may reduce the stable anchoring sites for copper ions, resulting in insufficient copper content or copper species migration during hydrothermal processes.

[0029] (4) The preferred catalyst can still maintain the long-range ordered structure of AEI, the microporous structure and the dispersed copper species well after hydrothermal treatment at 800 ℃, 10 vol% water vapor and 16 h, and maintain wide-temperature denitrification performance in standard SCR and fast SCR.

[0030] (5) In addition to the inorganic alkali source and the alkali metal element introduced by the complexing agent, no alkaline earth metal, other transition metals or rare earth metal additive salts other than copper are added to the initial gel in the method of the present invention. In this way, hydrothermal durability and low N2O generation can be achieved under the preferred composition without the need to introduce additional additive metals, reducing the complexity of multi-metal composition ratio and post-treatment control, and providing catalyst material for the purification of NO2 diesel engine exhaust gas.

[0031] In summary, based on the one-pot addition of a copper source, this invention uses high-silicon FAU with a specific silicon-to-aluminum ratio range as a crystalline precursor and the sole aluminum source. Through the synergistic matching of high-silicon FAU, supplementary silicon source, copper complex, AEI structure guiding system and gel alkalinity, a high-silicon Cu-SSZ-39 with controlled framework charge density and copper content is obtained, which can be used in particular for the purification of exhaust gases containing both NO and NO2. Attached Figure Description

[0032] Figure 1 The X-ray diffraction patterns are those of fresh samples obtained in Examples 1-9 and Comparative Examples 1-5, and the X-ray diffraction patterns of the preferred Cu-SSZ-39 molecular sieve catalyst obtained in Example 3 before and after hydrothermal aging; wherein, Figure 1 (a) in the figure is the X-ray diffraction pattern of the fresh samples obtained in Examples 1 to 9; Figure 1 (b) in the figure shows the X-ray diffraction patterns of the fresh samples obtained in Comparative Examples 1 to 5; Figure 1 (c) is the X-ray diffraction pattern of the preferred Cu-SSZ-39 molecular sieve catalyst obtained in Example 3 before and after hydrothermal aging.

[0033] Figure 2 The images shown are transmission electron microscope images of the preferred Cu-SSZ-39 molecular sieve catalyst obtained in Example 3 before and after hydrothermal aging; wherein, Figure 2(a) in the text corresponds to a fresh sample (i.e., one that has not undergone aging treatment); Figure 2 (b) in the text corresponds to the aged sample.

[0034] Figure 3 The figures show the N2 adsorption-desorption isotherms and pore size distribution of the preferred Cu-SSZ-39 molecular sieve catalyst obtained in Example 3 before and after hydrothermal aging; wherein, Figure 3 (a) in the figure corresponds to the N2 adsorption-desorption isotherm. Figure 3 (b) in the diagram corresponds to the aperture distribution.

[0035] Figure 4 NO levels before and after hydrothermal aging under standard SCR and fast SCR conditions for the preferred Cu-SSZ-39 molecular sieve catalyst and comparative catalyst obtained in Example 3. x Conversion rate curve; where, Figure 4 (a) in the text corresponds to SSCR. Figure 4 (b) in the text corresponds to FSCR.

[0036] Figure 5 The NO content of the preferred Cu-SSZ-39 molecular sieve catalyst obtained in Example 3 after hydrothermal treatment at 800 °C and 850 °C for different times under SSCR and FSCR reaction conditions. x Conversion rate. Detailed Implementation

[0037] The present invention will be further described below with reference to the embodiments and comparative examples. All raw material amounts are based on a single-batch experiment. Unless otherwise specified, the same general crystallization, ammonium exchange, and calcination conditions were used in each embodiment; the differences in formulation or process between the embodiments and comparative examples are used to verify the corresponding factors and their synergistic effects.

[0038] Unless otherwise stated, the atomic Si / Al ratio referred to in this invention is the molar ratio of silicon atoms to aluminum atoms, and the SiO2 / Al2O3 ratio is the molar ratio of oxides, numerically SiO2 / Al2O3 being twice the atomic Si / Al ratio. The molar amount of SiO2 in the initial gel is the sum of the molar amounts of supplementary silicon source and FAU molecular sieve-introduced SiO2, and the molar amount of Al2O3 is the molar amount of Al2O3-introduced by FAU molecular sieve. The amount of seed crystals added is calculated based on the total mass of SiO2 and Al2O3 in the initial gel. The molar amount of H2O in the initial gel is calculated based on the total amount of water introduced by each raw material, including added water, aqueous solutions, water in silica sol, and water of crystallization contained in hydrated raw materials (if silica sol and hydrated raw materials are used).

[0039] Unless otherwise specified, the same general crystallization, ammonium exchange, and calcination conditions were used in all embodiments as follows: The main raw materials used in each embodiment included NaOH, a 25% (w / w) aqueous solution of 1,1,3,5-tetramethylpiperidine hydroxide, EDTA-4Na·4H2O, a 30% (w / w) silica sol, CuSO4·5H2O, NH4Cl, high-silica FAU molecular sieve, and SSZ-39 seed crystals. Unless otherwise specified, hydrothermal crystallization was carried out in a stainless steel reactor with a polytetrafluoroethylene liner at 170 °C with dynamic rotation for 4 days; post-treatment involved three exchanges with 1.0 mol / L NH4Cl solution at 80 °C, followed by washing, drying at 110 °C overnight, and calcination at 600 °C for 6 h in air.

[0040] The fresh samples in the examples and comparative examples below are samples obtained after general crystallization, ammonium exchange and calcination treatment, without hydrothermal treatment; the aged samples are samples after the fresh samples have undergone standard hydrothermal aging treatment (i.e., at 800 °C for 16 h in an air atmosphere containing 10 vol% water vapor).

[0041] Example 1 This embodiment is used to verify the lower boundary of the target product's silicon-to-aluminum ratio range. 1.37 g of CuSO4·5H2O was dissolved in 5.0 g of deionized water, and 2.74 g of EDTA-4Na·4H2O was added and stirred for 1 h to obtain a copper complex solution. Separately, 2.45 g of NaOH was dissolved in 3.0 g of deionized water, and 17.84 g of a 25% (w / w) aqueous solution of 1,1,3,5-tetramethylpiperidine hydroxide was added and stirred for 1 h.

[0042] The copper complex solution was slowly added dropwise to the alkaline template agent mixture, and stirring was continued for 1.5 h after the addition was complete. 10.50 g of 30% silica sol was added and stirred for 1 h; subsequently, 8.80 g of FAU molecular sieve with a SiO2 / Al2O3 ratio of 35 was added, and after thorough mixing, 0.10 g of SSZ-39 seed crystals were added, and stirring was continued for 1 h. The resulting initial gel was crystallized and post-treated under general crystallization, ammonium exchange, and calcination conditions to obtain the Cu-SSZ-39 molecular sieve catalyst.

[0043] In the resulting initial gel, the SiO2 / Al2O3 molar ratio was 48.14, the M2O / SiO2 molar ratio was 0.159 (where M represents an alkali metal element, and M2O is calculated based on the content of alkali metal element M in the inorganic alkali source; the same applies below), the H2O / SiO2 molar ratio was 8.57, the OSDA / SiO2 molar ratio was 0.146, the Cu / Al molar ratio was 0.687, and the complexing agent / Cu molar ratio was 1.104. The SiO2 introduced by the high-silica FAU molecular sieve accounted for 72.7% of the total molar amount of SiO2 in the initial gel.

[0044] XRD results showed that the obtained product possessed an AEI topological structure, and no obvious FAU residual peaks or other crystalline impurities were observed. The SiO2 / Al2O3 ratio was 24.76; the Cu content was 2.51 wt%; and the BET specific surface area was 714 m². 2 / g, total pore volume is 0.29cm³ 3 / g. After hydrothermal aging at 800 ℃ for 16 h, the relative crystallinity of the AEI structure remained at 79%, the BET specific surface area was 617 m² / g, the BET specific surface area retention rate was 86.4%, and the total pore volume was 0.25 cm³. 3 / g.

[0045] Example 2 The preparation steps are the same as in Example 1, except that the amount of NaOH used is 2.65 g, the amount of silica sol is 11.50 g, and the amount of FAU molecular sieve is 9.40 g, with the SiO2 / Al2O3 ratio of the FAU molecular sieve being 38. This example is used to verify the purity of the AEI phase, the Si / Al ratio of the product, the pore structure, and the hydrothermal stability during the transition from a lower Si / Al ratio boundary to the preferred composition.

[0046] In the resulting initial gel, the molar ratio of SiO2 / Al2O3 was 52.57, the molar ratio of M2O / SiO2 was 0.160, the molar ratio of H2O / SiO2 was 8.13, the molar ratio of OSDA / SiO2 was 0.135, the molar ratio of Cu / Al was 0.696, and the molar ratio of complexing agent / Cu was 1.104. The SiO2 introduced by the high-silica FAU molecular sieve accounted for 72.3% of the total molar amount of SiO2 in the initial gel.

[0047] XRD results showed that the obtained product was a highly crystalline AEI-structured molecular sieve with no obvious FAU residue. The SiO2 / Al2O3 ratio was 26.34; the Cu content was 2.48 wt%; and the BET specific surface area was 736 m². 2 / g, total pore volume is 0.30 cm³ 3 / g. After hydrothermal aging at 800 ℃ for 16 h, the relative crystallinity retention rate of the AEI structure was 83%, and the BET specific surface area was 657 m².2 / g, BET specific surface area retention rate is 89.3%, and total pore volume is 0.27 cm³. 3 / g.

[0048] Example 3 This embodiment is a preferred central embodiment. 1.37 g of CuSO4·5H2O was dissolved in 5.0 g of deionized water, and 2.74 g of EDTA-4Na·4H2O was added and stirred for 1 h to obtain a copper complex solution. Separately, 2.80 g of NaOH was dissolved in 3.0 g of deionized water, and 17.84 g of a 25% (w / w) aqueous solution of 1,1,3,5-tetramethylpiperidine hydroxide was added and stirred for 1 h.

[0049] The copper complex solution was slowly added dropwise to the alkaline template agent mixture, and stirring was continued for 1.5 h after the addition was complete. 12.32 g of 30% silica sol was added and stirred for 1 h; then 9.90 g of FAU molecular sieve with a SiO2 / Al2O3 ratio of 40 was added, and after thorough mixing, 0.10 g of SSZ-39 seed crystals were added, and stirring was continued for 1 h. The resulting initial gel was transferred to a reactor and dynamically rotated for crystallization at 170 °C for 4 days. The crystallized product was filtered, washed with deionized water, and dried, and then exchanged three times with 1.0 mol / L NH4Cl solution at 80 °C. The exchanged product was washed, dried overnight at 110 °C, and calcined in air at 600 °C for 6 h to obtain a high-silica Cu-SSZ-39 molecular sieve catalyst.

[0050] In the resulting initial gel, the molar ratios of SiO2 / Al2O3 were 55.57, M2O / SiO2 were 0.159, H2O / SiO2 were 7.82, OSDA / SiO2 were 0.128, Cu / Al were 0.694, and the complexing agent / Cu were 1.104. The SiO2 introduced by the high-silica FAU molecular sieve accounted for 72.0% of the total molar amount of SiO2 in the initial gel.

[0051] XRD results showed that the obtained catalyst had a highly crystalline AEI topology, and no residual FAU peaks, other molecular sieve impurities, or obvious diffraction peaks attributable to crystalline CuO were observed. The SiO2 / Al2O3 ratio of the product was 27.86; the Cu content measured by AAS was 2.44 wt%; and the BET specific surface area was 751 m². 2 / g, total pore volume is 0.31 cm³ 3 / g, with a median pore width of 0.71 nm.

[0052] The obtained catalyst, after being treated at 800 °C for 16 h in an air atmosphere containing 10 vol% water vapor, still retained the AEI topology, with a relative crystallinity retention of 85%; the BET specific surface area was 682 m². 2 / g, BET specific surface area retention rate is 90.8%, and total pore volume is 0.28 cm³. 3 / g indicates that its microporous structure is well preserved after hydrothermal aging treatment.

[0053] Example 4 The preparation steps are the same as in Example 3, except that the amount of NaOH used is 3.10 g, the amount of silica sol is 12.00 g, and the amount of FAU molecular sieve is 10.50 g, with the SiO2 / Al2O3 ratio of the FAU molecular sieve being 45. This example is used to verify the phase purity, copper introduction amount, pore structure, and hydrothermal retention capability of the product when the atomic Si / Al ratio is around 15-16.

[0054] In the resulting initial gel, the molar ratio of SiO2 / Al2O3 was 61.01, the molar ratio of M2O / SiO2 was 0.170, the molar ratio of H2O / SiO2 was 7.47, the molar ratio of OSDA / SiO2 was 0.123, the molar ratio of Cu / Al was 0.733, and the molar ratio of complexing agent / Cu was 1.104. The SiO2 introduced by the high-silica FAU molecular sieve accounted for 73.8% of the total molar amount of SiO2 in the initial gel.

[0055] XRD results showed that the obtained product possessed an AEI topological structure, and no obvious impurity phases were observed. The SiO2 / Al2O3 ratio was 30.72; the Cu content was 2.31 wt%; and the BET specific surface area was 763 m². 2 / g, total pore volume is 0.32 cm³ 3 / g. After hydrothermal aging at 800 ℃ for 16 h, the relative crystallinity of the AEI structure was retained at 84%, and the BET specific surface area was 689 m². 2 / g, BET specific surface area retention rate is 90.3%, and total pore volume is 0.29 cm³. 3 / g.

[0056] Example 5 The preparation steps are the same as in Example 3, except that the amount of NaOH used is 3.30 g, the amount of silica sol is 12.50 g, and the amount of FAU molecular sieve is 11.00 g, with the SiO2 / Al2O3 ratio of the FAU molecular sieve being 50. This example is used to verify the upper boundary of Si / Al in the high-silicon FAU precursor and the obtained Cu-SSZ-39 product, and focuses on investigating the AEI phase purity, copper exchange capacity, low-temperature SCR activity, and structural retention ability after severe hydrothermal treatment.

[0057] In the resulting initial gel, the molar ratios of SiO2 / Al2O3 were 67.62, M2O / SiO2 were 0.172, H2O / SiO2 were 7.20, OSDA / SiO2 were 0.117, Cu / Al were 0.775, and the complexing agent / Cu were 1.104. The SiO2 introduced by the high-silica FAU molecular sieve accounted for 73.9% of the total molar amount of SiO2 in the initial gel.

[0058] XRD results showed that the obtained product was mainly composed of AEI structure, with no obvious FAU residue observed. The SiO2 / Al2O3 ratio was 34.28; the Cu content was 2.12 wt%; and the BET specific surface area was 708 m². 2 / g, total pore volume is 0.28 cm³ 3 / g. After hydrothermal aging at 800 ℃ for 16 h, the relative crystallinity of the AEI structure was retained at 78%, and the BET specific surface area was 612 m². 2 / g, BET specific surface area retention rate is 86.4%, and total pore volume is 0.24 cm³. 3 / g. Compared with Examples 3 and 4, further increasing the Si / Al ratio of the product resulted in a decrease in the amount of copper introduced and the micropore volume.

[0059] Example 6 To verify the lower limit of copper introduction, the high-silicon FAU, supplementary silicon source, inorganic base, organic structure directing agent, and seed crystal formulation of Example 3 were used. The difference was that the amount of CuSO4·5H2O was 1.12 g and the amount of EDTA-4Na·4H2O was 2.24 g, while the remaining steps and conditions were the same as in Example 3. This example was used to evaluate the effect of lower copper content on low-temperature ignition, N2O generation, and hydrothermal stability.

[0060] In the resulting initial gel, the molar ratios of SiO2 / Al2O3 were 55.57, M2O / SiO2 were 0.159, H2O / SiO2 were 7.78, OSDA / SiO2 were 0.128, Cu / Al were 0.568, and the complexing agent / Cu were 1.104. The SiO2 introduced by the high-silica FAU molecular sieve accounted for 72.0% of the total molar amount of SiO2 in the initial gel.

[0061] XRD results showed that the obtained product possessed an AEI topological structure, and no obvious impurity phases were observed. The SiO2 / Al2O3 ratio was 27.74; the Cu content was 1.99 wt%; and the BET specific surface area was 772 m². 2 / g, total pore volume is 0.32 cm³ 3 / g. After hydrothermal aging at 800 ℃ for 16 h, the relative crystallinity of the AEI structure was retained at 82%, and the BET specific surface area was 686 m².2 / g, BET specific surface area retention rate is 88.9%, and total pore volume is 0.28 cm³. 3 / g. Reducing the copper introduction amount did not significantly change the Si / Al and AEI phase composition of the product, but it increased the proportion of accessible pore structures in fresh samples.

[0062] Example 7 To verify the upper limit of copper introduction, the formulation and preparation method of Example 3 were used, except that the amount of CuSO4·5H2O was 1.62 g and the amount of EDTA-4Na·4H2O was 3.24 g, while the remaining steps and conditions were the same as in Example 3. This example was used to evaluate whether a higher copper content caused copper species aggregation, decreased pore accessibility, enhanced non-selective oxidation by NH3, or decreased selectivity of N2 at high temperatures.

[0063] In the resulting initial gel, the molar ratio of SiO2 / Al2O3 was 55.57, the molar ratio of M2O / SiO2 was 0.159, the molar ratio of H2O / SiO2 was 7.86, the molar ratio of OSDA / SiO2 was 0.128, the molar ratio of Cu / Al was 0.821, and the molar ratio of complexing agent / Cu was 1.104. The SiO2 introduced by the high-silica FAU molecular sieve accounted for 72.0% of the total molar amount of SiO2 in the initial gel.

[0064] XRD results showed that the obtained product possessed an AEI topological structure, and no obvious crystalline CuO diffraction peaks were observed. The SiO2 / Al2O3 ratio was 27.58; the Cu content was 2.86 wt%; and the BET specific surface area was 697 m². 2 / g, total pore volume is 0.27 cm³ 3 / g. After hydrothermal aging at 800 ℃ for 16 h, the relative crystallinity of the AEI structure was retained at 77%, and the BET specific surface area was 581 m². 2 / g, BET specific surface area retention rate is 83.4%, and total pore volume is 0.22 cm³. 3 / g. Compared to Example 3, the higher copper content resulted in a decrease in the accessibility of the pore structure and the ability to retain the structure after hydrothermal treatment.

[0065] Example 8 To verify the lower limit of the seed crystal addition amount, the preparation method of Example 3 was used, except that the amount of SSZ-39 seed crystals was 0.05 g, while all other conditions remained the same. This example was used to investigate the effect of a lower seed crystal amount on the degree of FAU conversion, AEI nucleation induction period, crystallization time, and product phase purity.

[0066] XRD results showed that the obtained product possessed the AEI topology, but the intensity of the characteristic AEI diffraction peaks was lower than that of Example 3, and it contained a small amount of incompletely converted FAU precursor. The SiO2 / Al2O3 ratio of the product was 27.80; the Cu content was 2.42 wt%; and the BET specific surface area was 681 m². 2 / g, total pore volume is 0.27 cm³ 3 / g. After hydrothermal aging at 800 ℃ for 16 h, the relative crystallinity of the AEI structure was retained at 76%, and the BET specific surface area was 558 m². 2 / g, BET specific surface area retention rate is 81.9%, and total pore volume is 0.21 cm³. 3 / g.

[0067] Example 9 To verify the upper limit of the seed crystal addition amount, the preparation method of Example 3 was used, except that the amount of SSZ-39 seed crystals was 0.25 g, while other conditions remained unchanged. This example was used to investigate the effect of increasing the amount of seed crystals on the purity of the AEI phase, crystal size, Si / Al ratio of the product, and pore structure.

[0068] XRD results showed that the obtained product was a highly crystalline AEI-structured molecular sieve, with no obvious FAU residue or other crystalline impurities observed. The SiO2 / Al2O3 ratio was 27.92; the Cu content was 2.46 wt%; and the BET specific surface area was 766 m². 2 / g, total pore volume is 0.32 cm³ 3 / g. After hydrothermal aging at 800 ℃ for 16 h, the relative crystallinity retention rate of the AEI structure was 83%, and the BET specific surface area was 680 m². 2 / g, BET specific surface area retention rate is 88.8%, and total pore volume is 0.28 cm³. 3 / g.

[0069] Example 10 The raw material formulation, feeding sequence, and post-processing method of Example 3 were used, with the only difference being that the hydrothermal crystallization temperature was 160 °C and the crystallization time was 4 days. After crystallization, the crystallized product was subjected to solid-liquid separation, washing, drying, ammonium exchange, and calcination to obtain the corresponding molecular sieve catalyst. XRD results showed that the obtained product had characteristic diffraction peaks of the AEI topological structure.

[0070] Example 11 The raw material formulation, feeding sequence, and post-processing method of Example 3 were used, with the only difference being that the hydrothermal crystallization temperature was 185 °C and the crystallization time was 4 days. After crystallization, the crystallized product was subjected to solid-liquid separation, washing, drying, ammonium exchange, and calcination to obtain the corresponding molecular sieve catalyst. XRD results showed that the obtained product had characteristic diffraction peaks of the AEI topological structure.

[0071] Example 12 The raw material formulation, feeding sequence, and post-processing method of Example 3 were used, with the only difference being that the hydrothermal crystallization temperature was 165 °C and the crystallization time was 4 days. After crystallization, the crystallized product was subjected to solid-liquid separation, washing, drying, ammonium exchange, and calcination to obtain the corresponding molecular sieve catalyst. XRD results showed that the obtained product had characteristic diffraction peaks of the AEI topology.

[0072] Example 13 The raw material formulation, feeding sequence, and post-processing method of Example 3 were used, with the only difference being that the hydrothermal crystallization temperature was 175 °C and the crystallization time was 4 days. After crystallization, the crystallized product was subjected to solid-liquid separation, washing, drying, ammonium exchange, and calcination to obtain the corresponding molecular sieve catalyst. XRD results showed that the obtained product had characteristic diffraction peaks of the AEI topological structure.

[0073] Example 14 The raw material formulation, feeding sequence, and post-processing method of Example 3 were used, with the only difference being that the hydrothermal crystallization temperature was 170 °C and the crystallization time was 2 days. After crystallization, the crystallized product was subjected to solid-liquid separation, washing, drying, ammonium exchange, and calcination to obtain the corresponding molecular sieve catalyst. XRD results showed that the obtained product had characteristic diffraction peaks of the AEI topological structure.

[0074] Example 15 The raw material formulation, feeding sequence, and post-processing method of Example 3 were used, with the only difference being that the hydrothermal crystallization temperature was 170 °C and the crystallization time was 6 days. After crystallization, the crystallized product was subjected to solid-liquid separation, washing, drying, ammonium exchange, and calcination to obtain the corresponding molecular sieve catalyst. XRD results showed that the obtained product had characteristic diffraction peaks of the AEI topology.

[0075] Example 16 The raw material formulation, feeding sequence, and post-processing method of Example 3 were used, with the only difference being that the hydrothermal crystallization temperature was 170 °C and the crystallization time was 3 days. After crystallization, the crystallized product was subjected to solid-liquid separation, washing, drying, ammonium exchange, and calcination to obtain the corresponding molecular sieve catalyst. XRD results showed that the obtained product had characteristic diffraction peaks of the AEI topological structure.

[0076] Example 17 The raw material formulation, feeding sequence, and post-processing method of Example 3 were used, with the only difference being that the hydrothermal crystallization temperature was 170 °C and the crystallization time was 5 days. After crystallization, the crystallized product was subjected to solid-liquid separation, washing, drying, ammonium exchange, and calcination to obtain the corresponding molecular sieve catalyst. XRD results showed that the obtained product had characteristic diffraction peaks of the AEI topological structure.

[0077] Example 18 The raw material formulation, feeding sequence, crystallization conditions, and post-treatment method of Example 3 were used, with the only difference being that the amount of NaOH was adjusted to 2.64 g. In the resulting initial gel, the molar ratio of Na (calculated as Na2O) to SiO2 in the inorganic alkali source was 0.150. After crystallization and post-treatment, the resulting product exhibited characteristic diffraction peaks of the AEI topological structure as detected by XRD.

[0078] Example 19 The raw material formulation, feeding sequence, crystallization conditions, and post-treatment method of Example 3 were used, with the only difference being that the amount of NaOH was adjusted to 3.16 g. In the resulting initial gel, the molar ratio of Na (calculated as Na2O) to SiO2 in the inorganic alkali source was 0.180. After crystallization and post-treatment, the resulting product exhibited characteristic diffraction peaks of the AEI topological structure as detected by XRD.

[0079] Example 20 The raw material formulation, feeding sequence, crystallization conditions, and post-treatment method of Example 3 were used, with the only difference being that the amount of EDTA-4Na·4H2O was adjusted to 2.61 g. The molar ratio of complexing agent to Cu in the resulting initial gel was 1.05. After crystallization and post-treatment, the obtained product exhibited characteristic diffraction peaks of the AEI topological structure as detected by XRD.

[0080] Example 21 The raw material formulation, feeding sequence, crystallization conditions, and post-treatment method of Example 3 were used, with the only difference being that the amount of EDTA-4Na·4H2O was adjusted to 3.72 g. The molar ratio of complexing agent to Cu in the resulting initial gel was 1.50. After crystallization and post-treatment, the obtained product exhibited characteristic diffraction peaks of the AEI topological structure as detected by XRD.

[0081] Example 22 The raw materials, feeding sequence, crystallization conditions, and post-treatment methods of Example 3 were used, with the difference being that the amount of silica sol (30% by mass) was 17.59 g, the amount of FAU molecular sieve with a SiO2 / Al2O3 ratio of 40 was 8.25 g, and the amount of deionized water used to dissolve NaOH was adjusted from 3.0 g to 2.39 g. In the resulting initial gel, SiO2 introduced by the high-silica FAU molecular sieve accounted for 60.0% of the total molar amount of SiO2 in the initial gel. After crystallization and post-treatment, the resulting product exhibited characteristic diffraction peaks of the AEI topology as detected by XRD.

[0082] Example 23 The raw materials, feeding sequence, crystallization conditions, and post-treatment methods of Example 3 were used, with the difference being that the amount of silica sol (30% by mass) was 8.80 g, and the amount of FAU molecular sieve with a SiO2 / Al2O3 ratio of 40 was 11.00 g. In the resulting initial gel, SiO2 introduced by the high-silica FAU molecular sieve accounted for 80.0% of the total molar amount of SiO2 in the initial gel. After crystallization and post-treatment, the resulting product exhibited characteristic diffraction peaks of the AEI topological structure as detected by XRD.

[0083] Comparative Example 1 A FAU molecular sieve with a SiO2 / Al2O3 ratio of 30 was used instead of the high-silica FAU molecular sieve in Example 3, and the amount of NaOH was adjusted to 2.10 g according to the target gel composition. Other preparation steps were the same as in Example 3. This comparative example was used to investigate the effects of the low-silica FAU precursor on the charge density of the obtained Cu-SSZ-39 framework, copper species distribution, rapid SCR N2O formation, and hydrothermal stability.

[0084] XRD results showed that the obtained product possessed an AEI topological structure. The SiO2 / Al2O3 ratio was 16.08; the Cu content was 2.45 wt%; and the BET specific surface area was 638 m². 2 / g, total pore volume is 0.26 cm³ 3 / g. After hydrothermal aging at 800 ℃ for 16 h, the relative crystallinity of the AEI structure was retained at 71%, and the BET specific surface area decreased to 428 m². 2 / g, the BET specific surface area retention rate is 67.1%, and the total pore volume is reduced to 0.17 cm³. 3 The / g indicates that a lower SiO2 / Al2O3 content is detrimental to the maintenance of the AEI microporous structure under severe hydrothermal aging conditions.

[0085] Comparative Example 2 The preparation steps were the same as in Example 3, except that SSZ-39 seed crystals were not added to the initial gel. This comparative example was used to investigate the effect of AEI-structured seed crystals on the directional crystallization of high-silicon FAU precursors, and to compare FAU residue, AEI crystallinity, and impurity phase formation under the same crystallization time.

[0086] XRD results showed that the product mainly contained AEI structure and contained impurities. The SiO2 / Al2O3 ratio was 27.42; the Cu content was 2.37 wt%; and the BET specific surface area was 518 m². 2 / g, total pore volume is 0.19 cm³ 3 / g. After hydrothermal aging at 800 ℃ for 16 h, the specific surface area of ​​BET is 352 m². 2 / g, total pore volume is 0.12 cm³ 3 / g. Since the fresh sample is a mixture of AEI and FAU phases with impurities, the discussion of its relative crystallinity retention rate is meaningless.

[0087] Comparative Example 3 The preparation steps were the same as in Example 3, except that the amount of NaOH used was reduced from 2.80 g to 1.80 g. This comparative example was used to verify the lower boundary of gel basicity and to investigate the effect of insufficient basicity on FAU dissolution and reconstruction, AEI nucleation, and the degree of crystallization.

[0088] XRD results showed that the obtained product was mainly composed of residual FAU precursor, with only low-intensity AEI characteristic diffraction peaks, indicating that FAU dissolution and reconstruction and AEI crystallization were insufficient when the basicity was inadequate. The SiO2 / Al2O3 ratio of the product was 28.63; the Cu content was 2.28 wt%; and the BET specific surface area was 436 m². 2 / g, total pore volume is 0.14 cm³ 3 / g. After hydrothermal aging at 800 ℃ for 16 h, the specific surface area of ​​BET decreased to 278 m². 2 / g, total pore volume decreased to 0.08 cm³. 3 / g.

[0089] Comparative Example 4 The preparation steps were the same as in Example 3, except that the amount of NaOH was increased from 2.80 g to 3.80 g. This comparative example was used to verify the upper boundary of gel basicity and to investigate the effects of excessively high basicity on the over-dissolution of silica-alumina species, crystal defects, product yield, and the formation of competing crystal phases.

[0090] XRD results showed that the obtained product was mainly composed of AEI structure, but the diffraction peaks were broadened, background scattering was enhanced, and a small number of competing crystalline phases appeared, indicating that excessively high basicity reduced the phase purity and crystal integrity of the product. The SiO2 / Al2O3 ratio of the product was 24.18; the Cu content was 2.56 wt%; and the BET specific surface area was 526 m². 2 / g, total pore volume is 0.20 cm³ 3 / g. After hydrothermal aging at 800 ℃ for 16 h, the relative crystallinity retention rate of the AEI structure was 54%, and the BET specific surface area was 337 m². 2 / g, BET specific surface area retention rate is 64.1%, and total pore volume is 0.11 cm³. 3 / g.

[0091] Comparative Example 5 Without adding a copper source or complexing agent, a high-silica SSZ-39 molecular sieve matrix was prepared according to the high-silica FAU directional crystallization system in Example 3. The crystallized product was filtered, washed, and dried, then calcined in air at 600 °C for 6 h to remove the organic structure-directing agent. It was then exchanged three times with a 1.0 mol / L NH4Cl solution at 80 °C to obtain the NH4-SSZ-39 molecular sieve. A copper nitrate solution was prepared based on the saturated water absorption of the NH4-SSZ-39 molecular sieve, and copper was loaded using an equal-volume impregnation method to achieve a Cu content of 2.44 wt% in the resulting catalyst. The impregnated product was dried overnight at 110 °C and then calcined in air at 600 °C for 6 h to obtain the two-step Cu-SSZ-39 catalyst. This comparative example compares the effects of simultaneous introduction of copper during crystallization versus copper loading after crystallization on pore structure, copper species distribution, hydrothermal stability, SCR activity, and N2O generation under conditions of similar Si / Al and Cu content in the products.

[0092] XRD results showed that the obtained two-step catalyst possessed an AEI topology and no obvious FAU residue was observed. The SiO2 / Al2O3 ratio of the product was 27.81; the Cu content was 2.44 wt%; and the BET specific surface area was 716 m². 2 / g, total pore volume is 0.28 cm³ 3 / g. No obvious crystalline CuO diffraction peaks were observed by XRD. After hydrothermal aging at 800 °C for 16 h, the relative crystallinity of the AEI structure was retained at 75%, and the BET specific surface area was 584 m². 2 / g, BET specific surface area retention rate is 81.6%, and total pore volume is 0.22 cm³. 3 / g.

[0093] Structural and compositional characterization X-ray diffraction was used to determine the crystal phase composition of the products obtained in the examples and comparative examples to confirm the AEI topology, FAU precursor residues, and the formation of competing crystal phases; X-ray fluorescence spectroscopy was used to determine the SiO2 / Al2O3 ratio of the products; atomic absorption spectroscopy was used to determine the Cu content; N2 adsorption-desorption was used to determine the BET specific surface area, total pore volume, and pore size distribution; and transmission electron microscopy was used to observe the crystal morphology and copper species aggregation of representative catalysts before and after hydrothermal treatment.

[0094] The relative crystallinity retention rate of the AEI structure was calculated by the ratio of the integrated areas of the selected AEI characteristic diffraction peaks before and after hydrothermal aging of the same sample. The BET specific surface area retention rate was calculated by the ratio of the BET specific surface area after hydrothermal aging to that of the fresh sample. Additionally, the fresh catalyst obtained in Example 3 was treated at 850 °C for 10 h in an air atmosphere containing 10 vol% water vapor to evaluate its ability to retain structure and catalytic performance under stringent hydrothermal conditions.

[0095] Catalytic performance evaluation Catalytic performance was evaluated in a fixed-bed reactor. 0.25 g of catalyst with a particle size of 60–80 mesh was weighed and packed into a quartz reaction tube with an inner diameter of 10 mm. The standard SCR reaction atmosphere was 500 ppm NO, 500 ppm NH3, 10 vol% O2, 8 vol% CO2, and 5 vol% H2O, with N2 as the balance gas; the fast SCR reaction atmosphere was 250 ppm NO, 250 ppm NO2, 500 ppm NH3, 10 vol% O2, 8 vol% CO2, and 5 vol% H2O, with N2 as the balance gas. The total gas flow rate was 1670 mL / min, and the gas hourly space velocity (GHSV) was 200,000 h⁻¹. -1 .

[0096] Before testing, the inlet gas composition was stabilized to the target concentration via a bypass. The reactor was heated from room temperature at a rate of 5 °C / min. After reaching 120 °C, the reactant gas was switched to pass through the catalyst bed, and the catalytic performance was recorded within the range of 150–550 °C (catalytic data were collected for samples every 25 °C). The outlet concentrations of NO, NO2, NH3, and N2O were continuously measured using a Fourier transform infrared gas analyzer. x Conversion rate is calculated using the following formula: NO x Conversion rate = [1 - (NO)] x Export concentration / NO x [Inlet concentration] × 100% NO x It is the sum of the concentrations of NO and NO2.

[0097] Furthermore, the performance differences between fresh samples without hydrothermal aging treatment and aged samples treated at 800 °C with 10 vol% water vapor for 16 h are discussed. The NO content of samples obtained in Examples 1-9 and Comparative Examples 1-5 at 200 °C is also discussed. x The conversion rate and the peak N2O generation within the test range of 150 ~ 550 ℃ are shown in Table 1.

[0098] Table 1 Catalytic performance of the samples obtained in the examples and comparative examples

[0099] As shown in Table 1, the fresh samples of the catalysts obtained in Examples 1 to 5 all exhibited high NO content at 200 °C. xThe conversion rate was affected, but the Si / Al ratio of the product had a significant impact on the low-temperature activity after hydrothermal aging and the N2O generation under FSCR conditions. The Si / Al ratios of the products in Examples 1 and 2 were lower than those in Example 3, resulting in relatively lower low-temperature activity after aging and higher N2O peak values ​​under FSCR conditions. Although the N2O generation in Example 5 was lower, its 200 °C SSCR activity and activity after aging decreased due to the higher Si / Al ratio, lower Cu content, and reduced available exchange sites.

[0100] Example 3: SSCR and FSCR in fresh condition at 200 °C NO x The conversion rates were 97.4% and 98.5%, respectively, and remained at 78.9% and 91.6% after hydrothermal aging at 800 °C for 16 h. Combined with the complete temperature curve, it can be seen that the aged Example 3 maintained no less than 90% NO content within the range of 225 ~ 500 °C under SSCR conditions. x The conversion rate, with a peak N2O concentration of 19.4 ppm in FSCR, indicates that the catalyst achieves a good overall balance between low-temperature activity, wide-temperature activity, hydrothermal stability, and N2O control.

[0101] The lower Cu content in Example 6 resulted in a corresponding decrease in N2O generation, but also led to a decline in activity at 200 °C. The higher copper content in Example 7 improved the low-temperature conversion rate of the fresh sample, but significantly increased the N2O peak value, and resulted in lower activity and pore structure retention after aging compared to Example 3. This indicates that the copper content needs to be appropriate; too low a copper content would limit low-temperature redox cycling, while too high a copper content would increase the tendency for copper species aggregation and non-selective side reactions.

[0102] Example 8 had a small amount of residual FAU due to the low seed crystal amount, and its activity, both fresh and aged, was lower than that of Example 3. Example 9 had high AEI phase purity, and its catalytic performance was close to that of Example 3, but increasing the seed crystal amount did not bring a corresponding performance improvement. Comparative Example 2 formed a mixed phase of AEI and FAU without the addition of SSZ-39 seed crystals. Comparative Example 3 was dominated by unconverted FAU when the alkalinity was insufficient. Comparative Example 4 showed a decrease in crystal integrity and competition for crystal phases when the alkalinity was too high. The catalytic performance of all three was significantly reduced after aging.

[0103] The N2O peak values ​​of Comparative Examples 2 and 3 were relatively low, mainly due to their lower NO content. x The lower conversion rate and reduced effective reaction amount are related, and cannot be used to conclude that it has higher N2 selectivity. Although Comparative Example 1 showed high activity in its fresh SSCR, the NO content decreased after aging at 200 °C. xThe conversion rate dropped to 58.2%, while the peak value of fresh FSCR N2O reached 34.7 ppm and the peak value of by-product N2O was too high, indicating that the low Si / Al ratio of the product is not conducive to maintaining both hydrothermal stability and FSCR selectivity.

[0104] Comparative Example 5 and Example 3 have similar Si / Al and Cu contents, but their SSCR and FSCR after aging at 200℃ are significantly different. x The conversion rates were 60.5% and 78.3%, respectively, and the peak N2O concentration under FSCR reached 42.4 ppm, indicating an excessively high peak value for the byproduct N2O. These results suggest that, under similar overall compositions, the simultaneous introduction of copper during crystallization is beneficial for improving the dispersion of copper species and the accessibility of pores after hydrothermal treatment, while also suppressing N2O formation under FSCR conditions.

[0105] The catalyst obtained in Example 3, after being treated with 850 °C and 10 vol% steam for 10 h, showed that the activity loss was mainly located in the low-temperature ignition zone and the high-temperature zone, while it still maintained a high NO content in the medium-temperature range. x Conversion rate. NO content of the catalyst in Example 3 after hydrothermal aging at 800 °C for 16 h. x The fact that the conversion rate did not show a continuous decline indicates that it has good operational stability.

[0106] The above results indicate a matching relationship between the high-silicon FAU precursor, the supplementary silicon source, the gel basicity, the copper complex, and the SSZ-39 seed crystals. By synergistically controlling these factors, the directional formation of the high-silicon AEI structure and the simultaneous introduction of the copper component can be achieved in the same hydrothermal crystallization process, and the resulting Cu-SSZ-39 molecular sieve catalyst can achieve a comprehensive balance of activity, selectivity, and structural stability under SSCR, FSCR, and severe hydrothermal treatment conditions.

[0107] The above embodiments are used to illustrate the technical concept of the present invention and are not intended to limit the scope of protection of the present invention. Any equivalent substitutions or reasonable adjustments made by those skilled in the art to the types of raw materials, component ratios, order of addition, and process conditions without departing from the technical concept of the present invention shall fall within the scope of protection of the present invention.

Claims

1. A one-pot directional crystallization preparation method for a high-silicon Cu-SSZ-39 molecular sieve catalyst, characterized in that, Includes the following steps: (1) Preparation of copper complex solution: Dissolve copper source and complexing agent in water, stir to carry out complexation reaction, and obtain copper complex solution; (2) Preparation of alkaline template agent mixture: Inorganic alkali source, water and organic structure directing agent are mixed evenly to obtain alkaline template agent mixture; wherein, the metal element in the inorganic alkali source is an alkali metal element; (3) Mixing: Add the copper complex solution obtained in step (1) to the alkaline template agent mixture obtained in step (2) and stir until homogeneous; (4) Adding and crystallization: Add supplementary silicon source, high-silicon FAU molecular sieve and AEI structure molecular sieve seed crystals to the mixture obtained in step (3), mix evenly to obtain initial gel; perform hydrothermal crystallization on the initial gel to dissolve, recombine and directionally transform the high-silicon FAU molecular sieve to form copper-containing AEI structure molecular sieve. (5) Post-processing: The crystallized product obtained in step (4) is subjected to solid-liquid separation, washing and drying, and ion exchange is performed using ammonium salt solution. Then, it is dried and calcined to obtain the high-silicon Cu-SSZ-39 molecular sieve catalyst. The high-silica FAU molecular sieve has a SiO2 / Al2O3 molar ratio of 35 to 50 and serves as the crystalline silica-alumina precursor and the sole aluminum source in the initial gel. The SiO2 introduced by the high-silica FAU molecular sieve accounts for 60% to 80% of the total molar amount of SiO2 in the initial gel. The alkali metal element M in the inorganic base source, calculated as M2O, has a molar ratio of 0.15 to 0.18 with the SiO2 in the initial gel. The SiO2 / Al2O3 molar ratio of the obtained high-silicon Cu-SSZ-39 molecular sieve catalyst is 24 to 36.

2. The method according to claim 1, characterized in that, The molar ratios of the components in the initial gel are as follows: SiO2 / Al2O3 = 48 ~ 68; H2O / SiO2 = 7.1 ~ 8.6; OSDA / SiO2 = 0.11 ~ 0.15; Cu / Al = 0.50 ~ 0.90; complexing agent / Cu = 1.05 ~ 1.50; Wherein, the molar amount of SiO2 is the sum of the molar amounts of SiO2 introduced by the supplementary silicon source and the high-silicon FAU molecular sieve, and the molar amount of Al2O3 is the molar amount of Al2O3 introduced by the high-silicon FAU molecular sieve; OSDA is the organic structure directing agent.

3. The method according to claim 1, characterized in that, The SiO2 / Al2O3 molar ratio of the high-silica FAU molecular sieve is 38 to 45, preferably 40; the SiO2 / Al2O3 molar ratio of the obtained Cu-SSZ-39 molecular sieve catalyst is preferably 26 to 32, and the Cu content is preferably 2.2 to 2.86 wt%.

4. The method according to claim 1, characterized in that, The copper source is selected from one or more of copper sulfate, copper nitrate, copper chloride, and copper acetate; the complexing agent is selected from one or two of EDTA-2Na·2H2O and EDTA-4Na·4H2O; preferably, the copper source is CuSO4·5H2O and the complexing agent is EDTA-4Na·4H2O.

5. The method according to claim 1, characterized in that, The inorganic base source is selected from one or two of NaOH and KOH; the organic structure directing agent is 1,1,3,5-tetramethylpiperidine hydroxide; the supplementary silicon source is selected from one or more of silica sol, fumed silica and tetraethyl orthosilicate, preferably, the inorganic base source is NaOH and the supplementary silicon source is silica sol.

6. The method according to claim 1, characterized in that, The AEI structured molecular sieve seed crystal is SSZ-39 molecular sieve seed crystal, and its addition amount is 0.2% to 2.0% of the total mass of SiO2 and Al2O3 in the initial gel, preferably 0.5% to 1.0%.

7. The method according to claim 1, characterized in that, In step (3), the copper complex solution is added to the alkaline template agent mixture and stirred for 0.5 to 3 hours; in step (4), after adding the supplementary silicon source, the mixture is stirred for 0.5 to 2 hours, and then high-silicon FAU molecular sieve and AEI structure molecular sieve seed crystals are added and stirred for another 0.5 to 3 hours.

8. The method according to claim 1, characterized in that, The hydrothermal crystallization temperature in step (4) is 160~185 ℃ and the crystallization time is 2~6 days; preferably, the hydrothermal crystallization temperature is 165~175 ℃ and the crystallization time is 3~5 days; more preferably, the hydrothermal crystallization temperature is 170 ℃ and the crystallization time is 4 days.

9. The method according to claim 1, characterized in that, Except for the alkali metal elements introduced by the inorganic alkali source and the optional alkali metal elements introduced in the complexing agent, no additional auxiliary salts are added to the initial gel; the metal elements in the auxiliary salts include alkaline earth metals, rare earth metals, and other transition metal elements except copper.

10. The method according to claim 1, characterized in that, The ammonium salt mentioned in step (5) is NH4Cl, the concentration of the ammonium salt solution is 0.5 ~ 1.5 mol / L, the ion exchange temperature is 60 ~ 90 ℃, and the number of ion exchanges is 1 ~ 4 times; the product after ion exchange is dried at 100 ~ 120 ℃ and calcined in air at 550 ~ 650 ℃ for 4 ~ 8 h.

11. A Cu-SSZ-39 molecular sieve catalyst prepared by the method according to any one of claims 1 to 10, characterized in that, The catalyst has an AEI topology and a SiO2 / Al2O3 molar ratio of 24 to 36.

12. The Cu-SSZ-39 molecular sieve catalyst according to claim 11, characterized in that, The catalyst contains 1.99 to 3.0 wt% Cu and has a BET specific surface area of ​​680 to 820 m². 2 / g, total pore volume is 0.26 ~ 0.35 cm³ 3 / g; Preferably, the catalyst, after being hydrothermally treated at 800 °C for 16 h in an air atmosphere containing 10 vol% water vapor, retains a relative crystallinity of AEI of not less than 78% and a BET specific surface area of ​​not less than 82%.

13. The application of the Cu-SSZ-39 molecular sieve catalyst according to claim 11 or 12 in the selective catalytic reduction denitrification of ammonia containing NO and / or NO2 tail gas.

14. The application according to claim 13, characterized in that, The exhaust gas is contacted with the catalyst at 150 ~ 550 ℃ to carry out a selective catalytic reduction denitrification reaction; Preferably, the exhaust gas contains both NO and NO2, with a molar ratio of NO to NO2 of 2:1 to 1:2, preferably 1:1; the exhaust gas also contains NH3, O2, water vapor and CO2.

15. The application according to claim 13 or 14, characterized in that, The Cu-SSZ-39 molecular sieve catalyst, after being hydrothermally treated at 800 °C for 16 h in an air atmosphere containing 10 vol% water vapor, was then subjected to a gas hourly space velocity (GHSV) of 200,000 h⁻¹ containing 250 ppm NO, 250 ppm NO₂, 500 ppm NH₃, 10 vol% O₂, 8 vol% CO₂, and 5 vol% H₂O. -1 Under rapid ammonia selective catalytic reduction (SCR) conditions, the N2O concentration generated is no higher than 20 ppm; under standard SCR conditions, the NO concentration is maintained at no less than 90% within a temperature range of 225 ~ 500 ℃. x Conversion rate.

Citation Information

Patent Citations

  • Auxiliary agent metal modified active metal loaded SSZ-39 molecular sieve, preparation and application

    CN117427687A