A catalyst for selective hydrogenation of heavy aromatics to enhance the production of disproportionation feedstock and its application.
By constructing a spherical composite catalyst with an inner noble metal and an outer non-noble metal gradient distribution and a mild liquid-phase hydrogenation process, the problems of insufficient catalyst stability and selectivity in the processing of heavy aromatics were solved, achieving efficient conversion to light aromatics, reducing energy consumption and adapting to existing process flows.
Patent Information
- Application Number
- CN202611325751.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing heavy aromatics processing technologies suffer from problems such as insufficient stability of precious metal catalysts, insufficient activity and selectivity of non-precious metal catalysts, lack of suitable catalyst structures for liquid-phase hydrogenation processes, lengthy process flows, and high energy consumption, making it difficult to efficiently convert C10+ heavy aromatics into light aromatics.
A spherical composite catalyst structure with an inner noble metal and an outer non-noble metal spatial gradient distribution is adopted. Combined with a mild liquid-phase hydrogenation process, the catalyst is constructed through a two-step spherical molding process to achieve a gradient distribution of active metal and pores. Combined with hydrogen pre-dispersion and product recycling in the liquid-phase hydrogenation process, the mass transfer and diffusion process is optimized.
It achieves highly selective hydrogenation conversion of heavy aromatics, extends catalyst life, reduces energy consumption, improves the yield and stability of light aromatics, and is compatible with existing aromatics complex processes.
Abstract
Description
Technical Field
[0001] This invention relates to the field of heavy aromatics processing technology in the petrochemical industry, and in particular to a catalyst for selective hydrogenation of heavy aromatics to increase the production of disproportionation feedstock and its application. Background Technology
[0002] Petroleum processing produces a large amount of C9 and higher heavy aromatic hydrocarbon fractions as a byproduct. 10 + Heavy aromatics (such as methylnaphthalene and biphenyl) are difficult to convert efficiently due to their complex molecular structures and the difficulty in precisely controlling their reaction pathways. Industrially, they are mostly used only as low-value fuels or solvents, resulting in a significant waste of aromatic resources. Therefore, it is crucial to utilize heavy aromatics, especially C454... 10 + The selective conversion of heavy aromatics into light aromatics is of great significance for enhancing the comprehensive utilization value of aromatic resources.
[0003] Currently, converting heavy aromatics into light aromatics through lightening technology is a recognized efficient route. However, the industrial application of this technology still faces limitations at the catalyst and process levels.
[0004] At the process level, existing heavy aromatics processing technologies suffer from complex processes or insufficient compatibility. Some heavy aromatics processing technologies aim to directly convert heavy aromatics into BTX, such as the heavy aromatics processing methods disclosed in CN115141653B, CN115141651B, CN115141650B, CN116004284A, and CN112662428B. Although these methods can directly obtain light aromatics such as BTX, they usually require complex feedstock pretreatment and multi-stage hydrocracking, resulting in long process flows and high energy consumption. On the other hand, although there are liquid-phase hydrogenation processes for heavy aromatics that can improve mass transfer, they usually directly use traditional catalysts without synergistic design with the macroscopic gradient structure of the catalyst, thus failing to fully realize the process potential.
[0005] At the catalyst level, the contradiction between activity, selectivity, and stability is prominent. To improve hydrogenation conversion capacity, existing technologies often introduce noble metal components such as platinum (Pt) and palladium (Pd). For example, CN108940354B discloses a C 10 +While ring-opening catalysts for the hydrogenation of heavy aromatics are used, the precious metal active centers are directly exposed to complex heavy feedstocks. Despite requiring pre-purification of the feedstock, irreversible poisoning and deactivation due to trace sulfur and nitrogen impurities and deep condensation coking of polycyclic aromatic hydrocarbons are difficult to avoid during long-term operation, resulting in poor catalyst stability. To reduce production costs, non-precious metal catalytic systems have been extensively studied, such as the Ni2P-based composite support lightweight catalyst disclosed in CN106975515A and the alumina-supported Mo / W-Ni-P hydrogenation catalyst disclosed in CN117861695A. Non-precious metal catalysts have stronger resistance to impurities, but their hydrogenation activity and aromatic selectivity are significantly lower than those of precious metal catalysts; processing C 10 + Excessive hydrogenation cracking of heavy aromatics is highly likely to occur, generating large amounts of light alkanes and significantly reducing the yield of the target light aromatics. Furthermore, current research focuses primarily on the ratio of active metals and nanoscale acid modification of the support (e.g., CN117797859A, which regulates the aluminum content on the support surface), neglecting the macroscopic structural design of the catalyst particles. Under liquid-phase hydrogenation conditions, a significant concentration gradient exists between the reactants and products inside and outside the catalyst particles. Traditional catalysts with uniformly distributed active metals cannot adapt to this gradient environment, making precise control of the reaction pathway difficult, prone to localized overheating, and preventing the overall conversion efficiency from reaching its optimal level.
[0006] In summary, existing heavy aromatics processing technologies suffer from four core contradictions: precious metal catalysts exhibit excellent hydrogenation activity but lack long-term operational stability; non-precious metal catalysts are low-cost and resistant to poisoning, but their hydrogenation activity and aromatics selectivity are insufficient; liquid-phase hydrogenation processes offer significant mass transfer advantages, but lack dedicated catalysts with suitable structures, hindering full efficiency release; and mainstream heavy aromatics conversion processes are lengthy, resulting in high energy consumption during plant operation. Therefore, there is an urgent need to develop a novel catalyst that balances high activity, high selectivity, and long-term stability, along with a corresponding low-energy, short-process technology to overcome existing processing bottlenecks and provide a technical solution for the efficient preparation of qualified disproportionated feedstocks from heavy aromatics. Summary of the Invention
[0007] The technical problem to be solved by this invention is to provide a catalyst for selective hydrogenation of heavy aromatics to increase the production of disproportionation feedstock and its application. By constructing a spherical composite catalyst structure with an inner noble metal and an outer non-noble metal spatial gradient distribution, and combining it with a mild liquid-phase hydrogenation process, a highly selective hydrogenation conversion of heavy aromatics is achieved. The resulting light components can be directly fed into the disproportionation unit. While taking into account the high hydrogenation activity, high aromatic selectivity and long-term stable operation of the catalyst, the processing flow is shortened and the overall production energy consumption of the unit is reduced.
[0008] The present invention solves the above-mentioned technical problems by adopting the following technical solutions: A catalyst for selective hydrogenation of heavy aromatics to increase the production of disproportionation feedstock is disclosed. The catalyst is a macroscopic spherical composite particle with a gradient distribution of active centers. It is formed by the agglomeration of primary microspheres with a particle size of 0.1-0.5 mm to form an overall structure with a particle size of 2-5 mm. The primary microspheres are based on a molecular sieve. The noble metal components are anchored in the molecular sieve channels in atomic or ionic states, while the oxides of non-noble metal components are enriched on the outer surface of the macroscopic spherical composite particles, forming a spatial gradient distribution structure of "inner noble metal and outer non-noble metal", thereby achieving the effect of gradient distribution of active metals and gradient distribution of channels.
[0009] As one of the preferred embodiments of the present invention, the molecular sieve is at least one of Y-type molecular sieve, Beta molecular sieve, ZSM-5 molecular sieve, and MWW-type molecular sieve.
[0010] As one of the preferred embodiments of the present invention, the primary microspheres are formed by molding molecular sieve-based powder and a first binder, and the macroscopic spherical composite particles are obtained by agglomeration of the primary microspheres and a second binder; the first binder and the second binder are independently selected from boehmite, aluminum sol or silica sol, and on a dry basis, the first binder accounts for 2% to 10% of the mass of the molecular sieve-based powder, more preferably 4% to 10%, and the second binder accounts for 2% to 10% of the mass of the primary microspheres, more preferably 5% to 10%; in addition, the particle size of the primary microspheres is more preferably 0.2 to 0.4 mm, and the particle size of the composite particles is more preferably 2.5 to 4 mm.
[0011] As one of the preferred embodiments of the present invention, the precious metal is at least one of platinum and palladium, and the content of the precious metal is 0.01% to 0.5% based on the total mass of the catalyst, more preferably 0.05% to 0.2%.
[0012] As one of the preferred embodiments of the present invention, the non-precious metal is at least one of chromium, molybdenum, cobalt, nickel, and tungsten, and the non-precious metal component accounts for 2% to 15% of the total mass of the catalyst, more preferably 8% to 15%, based on the mass of the oxide.
[0013] As one of the preferred embodiments of the present invention, the non-precious metal component is impregnated and loaded onto the outer surface of macroscopic spherical composite particles through a precursor solution with a pH value of 4.0 to 6.5, more preferably with a pH value of 4.0 to 5.8; the precursor is selected from at least one of metal salts of nickel, molybdenum, tungsten, cobalt, and chromium, citric acid complexes, or ethylenediaminetetraacetic acid complexes, more preferably phosphotungstic acid, silicotungstic acid, ammonium metatungstate, phosphomolybdic acid, silicotungstic acid, ammonium molybdate, and at least one of citric acid complexes of cobalt, nickel, and chromium or ethylenediaminetetraacetic acid complexes.
[0014] A method for preparing the above-mentioned catalyst includes the following steps: S1, Noble Metal Loading: A noble metal source is introduced into the molecular sieve system, and after drying and first calcination, a molecular sieve matrix powder with embedded noble metal is obtained; S2. Two-step spheroidizing: The molecular sieve-based powder is mixed with the first binder and granulated by rolling to obtain primary spheres with a particle size of 0.1~0.5mm, and then dried; the primary spheres are then mixed with the second binder and granulated by rolling to obtain spherical precursors with a particle size of 2~5mm, and after drying and a second calcination, a catalyst precursor is obtained. S3. Non-precious metal surface loading: Prepare a non-precious metal precursor solution, impregnate and load the catalyst precursor with it, and obtain the catalyst after drying and third calcination.
[0015] As one of the preferred embodiments of the present invention, step S1 is performed in any of the following ways: (1) In the hydrothermal crystallization synthesis stage of molecular sieve, a noble metal source is introduced into the synthesis system to participate in the crystallization process, and molecular sieve-based powder with embedded noble metal is obtained after post-processing. (2) First, complete the hydrothermal crystallization synthesis of molecular sieves. In the washing stage of the crystallization product, introduce the noble metal source into the washing medium. Load the noble metal through solid-liquid contact. Recycle the washing medium and obtain molecular sieve-based powder with embedded noble metals after post-processing.
[0016] As one of the preferred embodiments of the present invention, in steps S1, S2, and S3, the drying temperature is independently 80~150℃, and the drying time is independently 2~6h; the first calcination temperature is 350~500℃, the second calcination temperature is 400~600℃, the third calcination temperature is 350~600℃, and the calcination time is independently 2~6h.
[0017] A method for selective hydrogenation of heavy aromatics to increase the production of disproportionation feedstock involves using the aforementioned catalyst to mix hydrogen with heavy aromatic feedstock to form a liquid-phase feed, which is then introduced into a fixed-bed reactor for liquid-phase hydrogenation reaction. The light components obtained after separation of the reaction products are directly used as feedstock for the disproportionation unit, thereby increasing the production of disproportionation feedstock.
[0018] As one of the preferred embodiments of the present invention, the liquid-phase hydrogenation reaction conditions are: reaction temperature 150~320℃, reaction pressure 2.0~6.0MPa, and mass hourly space velocity (MHV) of the heavy aromatic feedstock 0.5~2.5h. -1 The hydrogen-to-oil volume ratio is 50:1 to 300:1; more preferably, the reaction temperature is 160 to 280°C, the reaction pressure is 4.0 to 5.0 MPa, and the mass hourly space velocity (MHV) of the heavy aromatic feedstock is 0.8 to 1.5 h⁻¹. -1 The hydrogen-to-oil volume ratio is 150:1 to 250:1.
[0019] As one of the preferred embodiments of the present invention, the hydrogen gas is fully dispersed and dissolved in the liquid feed through a mixer to form a homogeneous liquid system, which is then introduced into a fixed-bed reactor.
[0020] As one of the preferred embodiments of the present invention, after the reaction is completed, part of the reaction product is returned to the reactor inlet for recycling. The mass ratio of the recycled material to the extracted material is 10:90~80:20, more preferably 30:70~80:20. By regulating the reaction concentration and bed temperature rise through product recycling, the liquid-solid phase mass transfer effect is enhanced.
[0021] As one of the preferred embodiments of the present invention, the light aromatic components obtained after separation of the reaction products are directly fed into the disproportionation and alkyl transfer reaction unit in the disproportionation device; based on the total mass of the reaction products, the yield of the light components that can be used as disproportionation feed is not less than 75%; after the light aromatic components enter the disproportionation and alkyl transfer reaction unit, the total yield of benzene, toluene and xylene is not less than 60%.
[0022] As one of the preferred embodiments of the present invention, the disproportionation device can be stably operated using a conventional disproportionation catalyst. The mass percentage of the selective hydrogenation product of heavy aromatics obtained by the present invention in the total feed of the disproportionation device is 1% to 40%, more preferably 10% to 20%, which can be directly adapted to the process flow of existing aromatics complex units.
[0023] The advantages of this invention compared to the prior art are: (1) The catalyst active centers are rationally distributed and the performance of multiple components is highly synergistic: This invention constructs a macroscopic core-shell and multi-level interconnected channel structure through a unique two-step spherical process, realizing the spatial gradient distribution and functional zoning synergy of noble metal and non-noble metal oxides; the outer non-noble metal can preferentially complete the depurification and pre-hydrogenation treatment of heavy aromatic macromolecules, and the inner embedded noble metal active centers can perform highly selective deep hydrogenation of hydrogenation intermediates; at the same time, the outer structure can effectively shield sulfur and nitrogen impurities and coking precursors in the raw materials, forming physical protection for the inner noble metal active sites, significantly improving the catalyst's resistance to poisoning and coking, and effectively extending the long-term service life of the catalyst.
[0024] (2) Excellent mass transfer efficiency, mild reaction conditions and low energy consumption: The present invention is equipped with a dedicated liquid phase hydrogenation process and feed mixing structure. Combined with the diffusion advantages of the multi-level through-pore channels of the catalyst, the dispersion and dissolution effect of hydrogen in the liquid phase is greatly enhanced, and the mass transfer and diffusion process of reactants and products is optimized. The reaction can be carried out stably and efficiently under mild conditions of low hydrogen partial pressure and low hydrogen-oil ratio, which significantly reduces the energy consumption of the unit. Moreover, the overall process is compatible with the existing aromatic hydrocarbon complex process. More than 75% of the components in the product can be directly used as feed for the disproportionation unit. The unit has strong integration and low modification cost.
[0025] (3) The preparation process is novel and controllable, and has both economic and green environmental protection features: This invention provides two feasible preparation routes for precious metal loading, both of which can accurately realize the gradient spatial construction of catalyst active centers; among them, the scheme of loading precious metals in the molecular sieve washing stage can realize the recycling of washing filtrate, greatly improve the utilization rate of precious metal raw materials, reduce process wastewater discharge, reduce preparation costs, and fit the concept of green chemical manufacturing; the overall preparation steps are simple, the structure is highly controllable, and the prospects for industrial scale-up and practical application are excellent. Detailed Implementation
[0026] The embodiments of the present invention are described in detail below. These embodiments are implemented based on the technical solution of the present invention, and provide detailed implementation methods and specific operation processes. However, the scope of protection of the present invention is not limited to the following embodiments. In the following embodiments and comparative examples, the raw materials used, unless otherwise specified, are all industrial-grade raw materials; the equipment used, unless otherwise specified, are all conventional chemical equipment in the art, and those skilled in the art can reasonably select, assemble, and use them according to process requirements; the process methods and testing methods used, unless otherwise specified, are all conventional process methods and conventional testing methods in the art, and will not be described in detail again.
[0027] Example 1 The catalyst for selective hydrogenation of heavy aromatics to enhance the production of disproportionation feedstock in this embodiment is prepared by the following method: S1. Noble Metal Support: Hydrothermal Synthesis of Beta Molecular Sieves. An alcoholic solution of platinum acetylacetonate (catalyst loading: Pt 0.1%) was added to a silica-alumina gel, and the mixture was crystallized at 170℃ for 72 h. The product was washed, dried at 120℃ for 6 h, and calcined at 450℃ for 4 h to obtain Pt-Beta powder.
[0028] S2. Two-step spheroidizing: The above powder is spheroidized with boehmite (6% by dry weight) to form primary spheres with a particle size of 0.3 mm, and dried at 120°C for 4 hours. Then, the spheres are spheroidized with aluminum sol (5% by dry weight) to form composite spheres with a particle size of 3 mm, dried at 120°C for 6 hours, and calcined at 550°C for 4 hours to obtain the precursor.
[0029] S3. Non-precious metal surface loading: The precursor was impregnated with an equal volume of a mixture of phosphotungstic acid, nickel nitrate and ethylenediaminetetraacetic acid (pH=5.5, loading based on catalyst: WO3 10%, NiO 2%), dried at 120℃ for 4h, and calcined at 450℃ for 4h to obtain the catalyst.
[0030] Using reformed heavy aromatics from a certain refinery as the heavy aromatic feedstock (44.2 wt% monocyclic aromatics, 48.6 wt% bicyclic aromatics, 6.5 wt% tricyclic aromatics, and a small amount of non-aromatics), the catalyst prepared in this embodiment was used to carry out the liquid-phase hydrogenation reaction of heavy aromatics. Hydrogen and heavy aromatic feedstock were fed together into a mixer. The hydrogen was fully dispersed and dissolved in the liquid phase material by the mixer. After forming a liquid phase feed, it was fed into a fixed-bed reactor to complete the hydrogenation reaction.
[0031] Liquid-phase hydrogenation reaction conditions: reaction temperature 260℃, reaction pressure 4.0 MPa, heavy aromatic feedstock mass hourly space velocity 1.0 h⁻¹. -1 The hydrogen-to-oil volume ratio is 200:1. After the reaction is completed, some of the product is returned to the reactor inlet for recycling. The mass ratio of the recycled material to the extracted material is 50:50. The product recycling is used to regulate the material concentration in the reactor, slow down the bed temperature rise, and enhance the liquid-solid phase mass transfer effect.
[0032] After separation, the reactants yielded light aromatic hydrocarbons, with a yield of 76.8% based on the total mass of the reaction products. These light aromatic hydrocarbons were directly fed into the disproportionation and alkyl transfer reaction unit within the disproportionation apparatus. The disproportionation apparatus operated stably using a commercially available conventional disproportionation catalyst.
[0033] The hydrogenated light aromatics obtained in this embodiment were incorporated into the total feed of the disproportionation unit at a mass ratio of 20%, directly matching the process flow of the existing aromatics complex unit. Under standard disproportionation reaction conditions, the total initial yield of benzene, toluene, and xylene was 61.8%. After continuous and stable operation for 500 hours, the BTX yield retention rate (relative to the initial value) was 99.2%, demonstrating the excellent long-term stability of the catalyst.
[0034] Example 2 The catalyst for selective hydrogenation of heavy aromatics to enhance the production of disproportionation feedstock in this embodiment is prepared by the following method: S1. Noble metal loading: ZSM-5 was synthesized, crystallized, filtered, and washed with tetraamminepalladium nitrate solution (loading based on catalyst: Pd 0.05%) (filtrate was recovered for the next batch). After washing, it was dried at 110℃ for 5h and calcined at 400℃ for 3h to obtain Pd-ZSM-5 powder.
[0035] S2. Two-step spheroidizing: The above powder is spheroidized with silica sol (4% by dry weight) into primary spheres (0.2 mm); then spheroidized with aluminum sol (5% by dry weight) into composite spheres (2.5 mm); dried at 120°C for 6 h, and calcined at 550°C for 4 h to obtain the precursor.
[0036] S3. Non-precious metal surface loading: The catalyst was obtained by impregnation with an equal volume of a mixture of molybdenum trioxide, phosphoric acid and basic nickel carbonate (based on catalyst loading: MoO 38%, NiO 1.5%) at pH=4.0, drying at 100℃ for 6 h, and calcining at 500℃ for 3 h.
[0037] Using reformed heavy aromatics from a certain refinery as the heavy aromatic feedstock (44.2 wt% monocyclic aromatics, 48.6 wt% bicyclic aromatics, 6.5 wt% tricyclic aromatics, and a small amount of non-aromatics), the catalyst prepared in this embodiment was used to carry out the liquid-phase hydrogenation reaction of heavy aromatics. Hydrogen and heavy aromatic feedstock were fed together into a mixer. The hydrogen was fully dispersed and dissolved in the liquid phase material by the mixer. After forming a liquid phase feed, it was fed into a fixed-bed reactor to complete the hydrogenation reaction.
[0038] Liquid-phase hydrogenation reaction conditions: reaction temperature 235℃, reaction pressure 5.0MPa, heavy aromatic feedstock mass hourly space velocity 1.5h⁻¹. -1 The hydrogen-to-oil volume ratio is 150:1. After the reaction is completed, some of the product is returned to the reactor inlet for recycling. The mass ratio of the recycled material to the extracted material is 30:70. The product recycling is used to regulate the material concentration in the reactor, slow down the bed temperature rise, and enhance the liquid-solid phase mass transfer effect.
[0039] After separation, the reactants yield light aromatic hydrocarbons, with a yield of 78.5% based on the total mass of the reaction products. These light aromatic hydrocarbons are directly fed into the disproportionation and alkyl transfer reaction unit within the disproportionation apparatus. The disproportionation apparatus operates stably using a commercially available conventional disproportionation catalyst.
[0040] The hydrogenated light aromatics obtained in this embodiment were incorporated into the total feed of the disproportionation unit at a mass ratio of 20%, directly matching the process flow of the existing aromatics complex unit. Under standard disproportionation reaction conditions, the total initial yield of benzene, toluene, and xylene was 61.5%. After continuous and stable operation for 500 hours, the BTX yield retention rate (relative to the initial value) was 99.0%, demonstrating the excellent long-term stability of the catalyst.
[0041] Example 3 The catalyst for selective hydrogenation of heavy aromatics to enhance the production of disproportionation feedstock in this embodiment is prepared by the following method: S1. Noble metal loading: MCM-22 (MWW) molecular sieve was hydrothermally synthesized, and palladium acetylacetone was introduced in the washing step (loading based on catalyst: Pd 0.08%, filtrate was reused), dried at 130℃ for 4h, and calcined at 480℃ for 3h to obtain Pd-MWW powder.
[0042] S2. Two-step spheroidizing: The above powder is spheroidized with boehmite (8% by dry weight) to form primary spheres (0.4 mm); then spheroidized with silica sol (7% by dry weight) to form composite spheres (4 mm); dried at 120°C for 6 h, and calcined at 500°C for 5 h to obtain the precursor.
[0043] S3. Non-precious metal surface loading: The catalyst was impregnated with an equal volume of a mixture of ammonium metatungstate and cobalt nitrate (pH=5.8, loading based on catalyst: WO3 12%, CoO 3%), dried at 100℃ for 6 h, and calcined at 480℃ for 4 h to obtain the catalyst.
[0044] Using reformed heavy aromatics from a certain refinery as the heavy aromatic feedstock (44.2 wt% monocyclic aromatics, 48.6 wt% bicyclic aromatics, 6.5 wt% tricyclic aromatics, and a small amount of non-aromatics), the catalyst prepared in this embodiment was used to carry out the liquid-phase hydrogenation reaction of heavy aromatics. Hydrogen and heavy aromatic feedstock were fed together into a mixer. The hydrogen was fully dispersed and dissolved in the liquid phase material by the mixer. After forming a liquid phase feed, it was fed into a fixed-bed reactor to complete the hydrogenation reaction.
[0045] Liquid-phase hydrogenation reaction conditions: reaction temperature 280℃, reaction pressure 4.5MPa, heavy aromatic feedstock mass hourly space velocity 1.2h⁻¹. -1 The hydrogen-to-oil volume ratio is 180:1. After the reaction is completed, some of the product is returned to the reactor inlet for recycling. The mass ratio of the recycled material to the extracted material is 80:20. The product recycling is used to regulate the material concentration in the reactor, slow down the bed temperature rise, and enhance the liquid-solid phase mass transfer effect.
[0046] After separation, the reactants yield light aromatic hydrocarbons, with a yield of 80.2% based on the total mass of the reaction products. These light aromatic hydrocarbons are directly fed into the disproportionation and alkyl transfer reaction unit within the disproportionation apparatus. The disproportionation apparatus operates stably using a commercially available conventional disproportionation catalyst.
[0047] The hydrogenated light aromatics obtained in this embodiment were incorporated into the total feed of the disproportionation unit at a mass ratio of 10%, directly matching the process flow of the existing aromatics complex unit. Under standard disproportionation reaction conditions, the total initial yield of benzene, toluene, and xylene was 61.0%. After continuous and stable operation for 500 hours, the BTX yield retention rate (relative to the initial value) was 99.1%, demonstrating the excellent long-term stability of the catalyst.
[0048] Example 4 The catalyst for selective hydrogenation of heavy aromatics to enhance the production of disproportionation feedstock in this embodiment is prepared by the following method: S1. Noble metal loading: Beta molecular sieves were synthesized by hydrothermal method. After crystallization and solid-liquid separation, the sieves were washed multiple times with an aqueous solution of tetraamminepalladium dichloride (calculated as catalyst: Pd 0.2%). The filtrates from the first two washes were collected and recycled. The sieves were dried at 130℃ for 5 hours and calcined in air at 500℃ for 3 hours to obtain Pd-Beta powder.
[0049] S2. Two-step spheroidizing: The above powder is spheroidized with boehmite (10% by dry weight) to form primary spheres (0.3 mm); the spheres are spheroidized with aluminum sol (10% by dry weight) to form composite spheres (3 mm); dried at 120°C for 6 h and calcined at 600°C for 3 h to obtain the precursor.
[0050] S3. Non-precious metal surface loading: Prepare a citric acid-complexed ammonium molybdate-nickel nitrate mixed solution, adjust the pH to 5.0 (loading based on catalyst: MoO 36%, NiO 2%), impregnate with equal volume, dry at 120℃ for 4h, and calcine at 500℃ for 4h to obtain the catalyst.
[0051] Using reformed heavy aromatics from a certain refinery as the heavy aromatic feedstock (44.2 wt% monocyclic aromatics, 48.6 wt% bicyclic aromatics, 6.5 wt% tricyclic aromatics, and a small amount of non-aromatics), the catalyst prepared in this embodiment was used to carry out the liquid-phase hydrogenation reaction of heavy aromatics. Hydrogen and heavy aromatic feedstock were fed together into a mixer. The hydrogen was fully dispersed and dissolved in the liquid phase material by the mixer. After forming a liquid phase feed, it was fed into a fixed-bed reactor to complete the hydrogenation reaction.
[0052] Liquid-phase hydrogenation reaction conditions: reaction temperature 160℃, reaction pressure 5.0 MPa, heavy aromatic feedstock mass hourly space velocity 0.8 h⁻¹ -1 The hydrogen-to-oil volume ratio is 250:1. After the reaction is completed, some of the product is returned to the reactor inlet for recycling. The mass ratio of the recycled material to the extracted material is 60:40. The product recycling is used to regulate the material concentration in the reactor, slow down the bed temperature rise, and enhance the liquid-solid phase mass transfer effect.
[0053] After separation, the reactants yield light aromatic hydrocarbons, with a yield of 78.8% based on the total mass of the reaction products. These light aromatic hydrocarbons are directly fed into the disproportionation and alkyl transfer reaction unit within the disproportionation apparatus. The disproportionation apparatus operates stably using a commercially available conventional disproportionation catalyst.
[0054] The hydrogenated light aromatics obtained in this embodiment were incorporated into the total feed of the disproportionation unit at a mass ratio of 20%, directly matching the process flow of the existing aromatics complex unit. Under standard disproportionation reaction conditions, the total initial yield of benzene, toluene, and xylene was 60.5%. After continuous and stable operation for 500 hours, the BTX yield retention rate (relative to the initial value) was 99.0%, demonstrating the excellent long-term stability of the catalyst.
[0055] Comparative Example 1 This comparative example catalyst follows the same overall preparation process and total metal loading as Example 1. The main difference lies in the elimination of the two-step granulation process to construct the gradient distribution structure. Instead, Beta powder, binder, Pt source, and tungsten-nickel metal source are blended and impregnated simultaneously in a single step, resulting in a uniform distribution of the active metal within the support. It does not possess an "inner noble metal, outer non-noble metal" gradient structure. The hydrogenation evaluation process conditions and raw materials remain consistent with Example 1.
[0056] Results: The yield of light aromatics was 71.0%, the initial BTX yield of the disproportionation unit was 58.2%, and the BTX yield retention rate was 90.1% after 500 h of operation.
[0057] Comparative Example 2 This comparative example catalyst uses the same two-step spheroidizing and non-precious metal surface loading processes as Example 1. The main difference is that in step S1, no precious metal Pt is introduced during the preparation of the molecular sieve powder; only the non-precious metal active component is loaded on the surface, and the catalyst does not contain precious metal hydrogenation centers. The hydrogenation evaluation process conditions and raw materials are consistent with those of Example 1.
[0058] Results: The yield of light aromatics was 55.3%, the initial BTX yield of the disproportionation unit was 50.0%, and the BTX yield retention rate was 80.3% after 500 h of operation.
[0059] Comparative Example 3 The catalyst in this comparative example follows the same molecular sieve powder synthesis, noble metal loading, and two-step spheroidizing steps as in Example 1. The main difference is that, although step S3 uses the same phosphotungstic acid, nickel nitrate, and ethylenediaminetetraacetic acid mixed impregnation solution as in Example 1, the pH of the precursor solution is adjusted to 7.0 with alkali. The remaining impregnation, drying, and calcination process parameters remain unchanged. The hydrogenation evaluation process conditions and raw materials are consistent with those in Example 1.
[0060] Results: The yield of light aromatics was 73.2%, the initial BTX yield of the disproportionation unit was 56.3%, and the BTX yield retention rate was 91.8% after 500 h of operation.
[0061] Comparative Example 4 This comparative example uses the gradient catalyst prepared in Example 1. The main difference is that the hydrogen dissolution operation of the pre-mixer is eliminated, and the traditional gas-liquid co-flow trickle bed process is adopted. There is no product circulation process, and the hydrogen-to-oil volume ratio is increased to 1000:1. The remaining temperature, pressure, space velocity, and raw materials are the same as in Example 1.
[0062] Results: The yield of light aromatics was 72.1%, the initial BTX yield of the disproportionation unit was 60.5%, and the BTX yield retention rate was 96.0% after 500 h of operation.
[0063] Comparing the data results of Examples 1-4 with those of Comparative Examples 1-4, it can be seen that: 1. Compared with the catalyst with uniform metal component distribution in Comparative Example 1, the catalyst constructed in this invention with a gradient structure of "inner noble metal and outer non-noble metal" significantly improves the yield of light aromatic hydrocarbons, and the BTX yield retention rate is significantly improved after 500 hours of long-term operation. This proves that the spatial distribution mode of the active center with inner and outer layers can achieve functional synergy. The outer non-noble metal completes the pre-hydrogenation of heavy aromatic macromolecules and the interception of impurities, while the inner noble metal achieves highly selective hydrogenation of intermediates, effectively inhibiting coking and delaying the deactivation of noble metals, thus balancing reaction activity and catalyst stability.
[0064] 2. In Comparative Example 2, the yield of light aromatics decreased significantly after the complete removal of the precious metal component. This indicates that the precious metal active center is an indispensable key component for ensuring the hydrogenation conversion depth of heavy aromatics and improving the selectivity of light aromatics. It is difficult to achieve C2000 by relying solely on a non-precious metal system. 10 + Highly efficient conversion of heavy aromatics to prepare disproportionated feedstock.
[0065] 3. In Comparative Example 3, when the pH of the non-precious metal impregnation solution was increased to 7.0, the catalytic performance showed a significant decline. This indicates that an impregnation solution with suitable acidity can regulate the adsorption behavior of non-precious metal precursors and promote the uniform enrichment of active components on the outer surface of particles. A deviation from pH will cause the dispersion state of active components to deteriorate and weaken the surface pre-hydrogenation function.
[0066] 4. Comparative Example 4 uses a traditional gas-liquid co-flow trickle bed process, eliminating the liquid-phase premixing hydrogen dissolution and product recycling process. Even with a significant increase in the hydrogen-to-oil volume ratio to 1000:1, the yield of light aromatics is still lower than that of the liquid-phase hydrogenation process of this invention. This confirms that the mixed hydrogen dissolution + product recycling process of this invention enhances the liquid-phase hydrogen dissolution and bed mass transfer, achieving high-efficiency reaction under low hydrogen-to-oil ratio conditions, and has significant energy-saving advantages.
[0067] In Examples 1-4, under different molecular sieve matrices, noble metal types, active metal ratios, and process operating ranges, the yield of light aromatic hydrocarbons can be stably reached 76.8%-80.2%, the initial yield of the disproportionation unit BTX is higher than 60%, and the stability retention rate after 500 hours is higher than 99.0%, indicating that the catalyst composition, structure, and supporting process of the present invention have a certain applicable range, and the technical solution can be stably repeated.
[0068] In summary, this invention constructs a spherical composite catalyst with a gradient distribution of "inner noble metal and outer non-noble metal" through a two-step spherical molding process, and rationally designs two types of active centers. Simultaneously, it is equipped with a low-energy liquid-phase hydrogenation process involving liquid-phase hydrogen pre-dispersion and product recycling. This effectively solves the problems of existing heavy aromatic hydrocarbon hydrogenation catalysts struggling to balance activity, selectivity, and stability, as well as the high hydrogen-to-oil ratio and high energy consumption of traditional hydrogenation processes. It can also reduce C...10 + The efficient conversion of heavy aromatics into light aromatic components suitable for disproportionation unit feedstock is easy to integrate with existing aromatics complexes and has good prospects for industrial application.
[0069] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A catalyst for selective hydrogenation of heavy aromatics to increase the production of disproportionation feedstock, characterized in that, The catalyst is a macroscopic spherical composite particle with a gradient distribution of active centers. It is formed by the agglomeration of primary microspheres with a particle size of 0.1~0.5 mm to form an overall structure with a particle size of 2~5 mm. The primary microspheres are based on molecular sieves, with noble metal components anchored inside the molecular sieve channels and oxides of non-noble metal components enriched on the outer surface of the macroscopic spherical composite particles, forming a spatial gradient distribution structure of inner noble metal and outer non-noble metal.
2. The catalyst according to claim 1, characterized in that, The molecular sieve is at least one of Y-type molecular sieve, Beta molecular sieve, ZSM-5 molecular sieve, and MWW-type molecular sieve.
3. The catalyst according to claim 1, characterized in that, The primary microspheres are formed by molding molecular sieve-based powder and a first binder, and the macroscopic spherical composite particles are obtained by agglomeration of primary microspheres and a second binder. The first binder and the second binder are independently selected from boehmite, aluminum sol or silica sol. On a dry basis, the first binder accounts for 2% to 10% of the mass of molecular sieve-based powder, and the second binder accounts for 2% to 10% of the mass of primary microspheres.
4. The catalyst according to claim 1, characterized in that, The precious metal is at least one of platinum and palladium, and the content of the precious metal is 0.01% to 0.5% based on the total mass of the catalyst.
5. The catalyst according to claim 1, characterized in that, The non-precious metal is at least one of chromium, molybdenum, cobalt, nickel, and tungsten, and the non-precious metal component accounts for 2% to 15% of the total mass of the catalyst based on the mass of oxides.
6. The catalyst according to claim 1, characterized in that, The non-precious metal component is impregnated and loaded onto the outer surface of macroscopic spherical composite particles by a precursor solution with a pH of 4.0 to 6.5; the precursor is selected from at least one of the metal salts of nickel, molybdenum, tungsten, cobalt, and chromium, citric acid complexes, or ethylenediaminetetraacetic acid complexes.
7. A method for preparing a catalyst as described in any one of claims 1 to 6, characterized in that, Includes the following steps: S1, Noble Metal Loading: A noble metal source is introduced into the molecular sieve system, and after drying and first calcination, a molecular sieve matrix powder with embedded noble metal is obtained; S2. Two-step spheroidizing: The molecular sieve-based powder is mixed with the first binder and granulated by rolling to obtain primary spheres with a particle size of 0.1~0.5mm, and then dried; the primary spheres are then mixed with the second binder and granulated by rolling to obtain spherical precursors with a particle size of 2~5mm, and after drying and a second calcination, a catalyst precursor is obtained. S3. Non-precious metal surface loading: Prepare a non-precious metal precursor solution, impregnate and load the catalyst precursor with it, and obtain the catalyst after drying and third calcination.
8. The preparation method according to claim 7, characterized in that, Step S1 can be performed in any of the following ways: (1) In the hydrothermal crystallization synthesis stage of molecular sieve, a noble metal source is introduced into the synthesis system to participate in the crystallization process, and molecular sieve-based powder with embedded noble metal is obtained after post-processing. (2) First, complete the hydrothermal crystallization synthesis of molecular sieves. In the washing stage of the crystallization product, introduce the noble metal source into the washing medium. Load the noble metal through solid-liquid contact. Recycle the washing medium and obtain molecular sieve-based powder with embedded noble metals after post-processing.
9. The preparation method according to claim 7, characterized in that, In steps S1, S2, and S3, the drying temperature is independently 80~150℃, and the drying time is independently 2~6h; the first calcination temperature is 350~500℃, the second calcination temperature is 400~600℃, the third calcination temperature is 350~600℃, and the calcination time is independently 2~6h.
10. A method for selective hydrogenation of heavy aromatics to increase the production of disproportionation feedstock, characterized in that, Using the catalyst described in any one of claims 1 to 6, hydrogen is mixed with heavy aromatic hydrocarbon feedstock to form a liquid-phase feed, which is then introduced into a fixed-bed reactor for liquid-phase hydrogenation. The light components obtained after separation of the reaction products are directly used as feedstock for the disproportionation unit, thereby increasing the production of disproportionation feedstock. The liquid-phase hydrogenation reaction conditions are: reaction temperature 150~320℃, reaction pressure 2.0~6.0MPa, and mass hourly space velocity (MHV) of the heavy aromatic hydrocarbon feedstock 0.5~2.5h. -1 The hydrogen-to-oil volume ratio is 50:1 to 300:1.
Citation Information
Patent Citations
Non-noble metal catalyst for conversion of heavy aromatic hydrocarbons to lightweight aromatic hydrocarbons, and preparation method thereof
CN106975515A
A type of C 10 + Selective hydrogenation ring-opening catalysts for heavy aromatics and their preparation methods
CN108940354B
C10 + Method and System for Hydrogenation and Lightening of Heavy Aromatic Hydrocarbons
CN112662428B
A system and method for producing light aromatics from distillate oil
CN115141650B
A system and method for zoning-enhanced production of chemical raw materials using aromatic fraction oil
CN115141651B