A precision sheet metal extrusion molding device and molding process
By setting temperature difference zones and partitioned edge pressing devices on aluminum alloy slabs, the problems of forming force control and material flow in local large thickness ratio extrusion molding are solved, achieving high material utilization and streamline continuity while maintaining the mechanical properties of high-strength aluminum alloys.
Patent Information
- Application Number
- CN202611445378.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to simultaneously resolve the contradictions of controllable forming force, full cavity filling, and stable shape of non-thickened areas during extrusion molding with large local thickness ratios under uniform temperature fields. High-strength aluminum alloys are difficult to maintain their mechanical properties after warm forming, and it is difficult to balance material utilization and streamline continuity.
By adopting a temperature difference zone design, heating modules, cooling modules, and thermal insulation barriers are set on the aluminum alloy slab to establish a non-uniform temperature field within the slab surface. The temperature difference zone is used to control the material flow, and the active guidance and shape stabilization of the material are achieved through zoned edge pressing and back pressure devices.
It achieves controllable forming force, full cavity filling, and stable shape of non-thickened areas, while maintaining high material utilization, good streamline continuity, and the mechanical properties of high-strength aluminum alloys are restored after warm forming, avoiding strength loss caused by overall heating.
Smart Images

Figure CN123102774A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of sheet metal plastic forming technology, specifically to a precision sheet metal extrusion forming device and forming process. Background Technology
[0002] In the aerospace, rail transportation, and shipbuilding industries, many load-bearing components are structured as "a plate as a whole, with localized thickening," such as joints and lugs with localized bosses, and plate-type brackets with locally thickened mounting bases. The main body bears in-plane loads and stiffness, while the locally thickened areas bear concentrated loads, threaded connections, or bearing fits. The thickness increase ratio (i.e., the ratio of the thickened local thickness to the original plate thickness) is typically above 1.5. To balance load-bearing capacity and lightweight design, these components are often made of heat-treatable, high-strength aluminum alloys.
[0003] In the existing technology, there are three main manufacturing paths for such components.
[0004] The first category includes integral die forging, casting, and machining or welding of thick plates. Die forging produces a dense structure and continuous flow lines, but requires large-tonnage equipment. Due to flash, filler material, and draft angles, the material utilization rate of ordinary die forgings is only about 60% to 75% (this utilization rate is an industry-standard experience value), resulting in a large amount of subsequent machining. For complex components with I-beams or branched structures, ordinary open die forging is difficult to form. Casting can form complex shapes in one step, but the structure is loose, resulting in insufficient fatigue performance and plasticity. Machining of thick plates has extremely low material utilization, while welding results in flow line interruption and softening of the heat-affected zone. The common drawback of all three is low material utilization or discontinuous flow lines, making it difficult to balance load-bearing reliability and economy. Components with localized thickening features are particularly sensitive to material utilization. Therefore, directly forming components with varying thicknesses from slabs close to the component's outline has been a long-standing need in this field.
[0005] The second type is localized thickening of sheet metal, also known as sheet forging or sheet volume forming. It uses a slab as the blank, and the thickening process does not produce flash, offering advantages in material utilization and streamline continuity. The technical challenge lies in controlling material flow. Known methods include: using offset pressure blocks to maintain contact and suppress thickening buckling; employing flexible rolled blanks or oscillating forming to avoid thickening folding; having opposing surfaces move to reduce friction and lower forming force; and altering the force application sequence by changing the movement sequence of the punch and ejector pin. These methods all act on the boundary conditions of the deformed body, implicitly assuming that the material has uniform strength throughout, i.e., it is in a uniform temperature field. Therefore, material flow can only be passively contained and guided from the outside: insufficient constraint leads to material outflow and incomplete filling of the thickened area; excessive constraint leads to a sharp increase in forming force and induces instability. Furthermore, as the thickness increases, the contact area between the die and the slab continuously expands, and the forming force increases monotonically, requiring high-tonnage equipment.
[0006] The third category is zoned temperature control processes. High-strength steel variable-strength hot stamping uses zoned heating elements and cooling channels within a single mold, separated by insulating material. However, its application is to steel parts undergoing solid-state phase transformation. The temperature zoning applies to the cooling stage after forming, and it involves a single heating followed by quenching. The purpose is to control performance through phase transformation, not to control the material flow position within the sheet during forming. Hot forming and in-mold quenching, on the other hand, heats the entire slab to its solution temperature before forming and quenching. This is for deep-drawn thin-walled parts, involving almost no local thickening. It aims for the entire slab to enter a solution-soft state, which is technically opposite to the "local softening, local retention" required for local thickening.
[0007] As can be seen from the above path, the existing technology has not yet provided a solution that can simultaneously solve the following three technical problems.
[0008] First, the three indicators of localized large thickness increase compared to extrusion thickening are contradictory under any uniform temperature field. Controllable forming force and full filling of the thickened cavity require reducing material flow stress, while the stable shape of the non-thickened area requires increasing its flow resistance. In a uniform temperature field, flow stress is a single variable and cannot simultaneously possess two values. This contradiction is not due to improper selection of process parameters, but rather determined by the premise of a uniform temperature field itself. Furthermore, heat conduction causes the temperature gradient to decay over time and eventually degenerate into an overall warm state, and the allowable residence time of aluminum alloys in the high-temperature range is limited; temperature control must be coupled with time control. Existing technologies neither provide a device for maintaining the spatial temperature gradient within the sheet throughout the forming process, nor do they provide corresponding control methods.
[0009] Second, while achieving formability, high-strength aluminum alloys struggle to maintain or restore their mechanical properties. The warm forming temperature range of such alloys coincides with the precipitation phase transformation range. After warm forming, peak-aged plates exhibit changes in the precipitated strengthening phases and a decrease in strength, which is difficult to recover through conventional subsequent processes. Furthermore, overall heating methods cause the non-thickening areas to soften simultaneously and undergo regression or over-aging, resulting in strength losses that cannot be eliminated through subsequent heat treatment.
[0010] Third, existing forming methods struggle to balance material utilization and streamline continuity, and lack methods for controlling material flow through an in-plate temperature field for high-strength aluminum alloys. The former has already been discussed. Regarding the latter, the flow stress of steel in the low-to-medium temperature range changes very little with temperature; this difference can be directly derived from the difference in the slope of the flow stress versus temperature curves for high-strength steel and high-strength aluminum alloys. Therefore, the temperature gradient is insufficient to create an effective flow resistance difference in steel billets. Consequently, in existing technologies, temperature is always used as an overall process parameter—either heating the entire billet to reduce its overall deformation resistance, or not heating it to maintain the shape stability of non-thickening areas—and has never become a spatial variable within the plate surface. High-strength aluminum alloys exhibit highly temperature-sensitive flow stress within the warm forming temperature range. This property makes forming control in this range more difficult and has not yet been used by existing sheet metal forming technologies to limit material flow location. Furthermore, the temperature windows and parameter settings of existing processes are not suitable for high-strength aluminum alloys, and a process framework that can be calibrated and adapted for different grades such as 7-series, 6-series, and 5-series aluminum alloys has not been established. Summary of the Invention
[0011] The purpose of this application is to provide a precision sheet metal extrusion molding apparatus and molding process to solve the problems mentioned in the background art.
[0012] To achieve the above objectives, this application provides the following technical solution: a precision sheet metal extrusion forming apparatus, comprising a punch, a die, and a pressing device arranged circumferentially around the thickening deformation zone of an aluminum alloy blank. The thickening deformation zone refers to a region on the aluminum alloy blank where a predetermined increase in thickness is expected. A temperature difference zone is also provided, consisting of a heating module, a cooling module, and a heat insulation partition arranged in pairs. The heating module is disposed within the punch and / or die corresponding to the thickening deformation zone, and is used to heat the thickening deformation zone to a set temperature T1, where T1 is the set temperature of the deformation zone in degrees Celsius. The cooling module is located within the punch and / or die, corresponding to the constraint area on the aluminum alloy slab other than the thickening deformation area. It cools the constraint area to a set constraint area temperature T2, where T2 is the set constraint area temperature in degrees Celsius, and T1 is greater than T2. The heat insulation barrier is located within the die between the heating module and the cooling module, its position on the plate surface corresponding to the boundary of the thickening deformation area. It blocks the heat conduction path from the heating module to the cooling module within the die. The set deformation area temperature T1 is greater than the lower limit of the forming window temperature of the sheet metal and less than the solution temperature of the sheet metal alloy. The heating module and the cooling module establish a temperature gradient from the thickening deformation area to the constraint area before the punch is loaded, and maintain this temperature gradient throughout the extrusion thickening process.
[0013] Furthermore, the heat insulation partition includes a heat insulation groove, a heat insulation pad embedded in the heat insulation groove, and a low thermal conductivity insert; the heat insulation groove is formed inside the mold body or on the back but does not extend to the cavity surface, and its upper end maintains a distance determined according to the strength check of the mold body; the heat insulation pad does not bear the molding load; the low thermal conductivity insert is disposed on the side of the cavity surface of the heating module facing the heat insulation groove, which blocks the heat conduction path in the plate surface direction, and keeps the heat transfer path unobstructed in the plate thickness direction; the cavity surface of the cooling module is composed of a high thermal conductivity insert; the punch and / or die are also provided with a deformation zone cooling channel on the side of the thickened deformation zone, which is independently provided or is combined by the channel integrated in the insert of the heating module.
[0014] Furthermore, the pressing device is a partitioned pressing unit, which is divided into at least two independent units along the circumference of the thickened deformation zone. The pressing gap gi of each unit is set independently and adjusted independently during the forming process. gi is the gap between the pressing surface and the surface of the blank, in millimeters. The pressing gap gi of each unit is set to an initial value according to the measured thickness of the aluminum alloy blank. The upper limit of gi is determined according to the critical condition that the constraint zone does not experience in-plane instability under the pressing surface, and the lower limit of gi is determined according to the condition that the material can flow from the constraint zone corresponding to the unit into the thickened deformation zone.
[0015] Furthermore, it also includes a back pressure unit, which applies a back pressure Fb to the free end of the thickened deformation zone. The back pressure Fb increases according to a set rule with the punch stroke. Fb is the back pressure, and its unit is kilonewtons. An exhaust structure is also provided on the bottom or side wall of the concave mold cavity. The exhaust structure is an exhaust hole or an exhaust gap opened on the parting surface. A temperature sensor and a control unit are also provided. The temperature sensor is embedded in the mold body at a distance of one to three millimeters from the surface of the cavity. At least one temperature sensor is arranged in each of the thickened deformation zone, the temperature transition zone, and the constraint zone. The temperature transition zone refers to the plate surface area where the temperature drops from T1 to T2. The control unit adjusts the heating power of the heating module and the cooling medium flow rate of the cooling module according to the temperature distribution measured by the temperature sensor, so that the attenuation of the difference between T1 and T2 during the entire molding process does not exceed the set threshold specified according to the alloy grade. The control unit also adjusts the blank holder gap gi and the back pressure Fb of each unit according to displacement and pressure feedback.
[0016] A precision sheet metal extrusion forming process includes the following steps: S1, cutting the blank according to the component outline and selecting the supply status of the blank; S2, applying a warm forming lubricant to the surface of the slab; S3, the blank is positioned and installed between the punch and the die, so that the thickened deformation area on the blank is aligned with the cavity of the die, and the initial pressing gap gi is set by the pressing device surrounding the thickened deformation area according to the actual measured thickness of the blank. S4, before loading, the thickened deformation zone is heated to the deformation zone set temperature T1, and the constraint zone on the slab other than the thickened deformation zone is cooled to the constraint zone set temperature T2. A temperature gradient from the thickened deformation zone to the constraint zone is established in the slab surface. T1 is greater than T2, greater than the lower limit temperature of the forming window of the plate, and less than the solution temperature of the plate alloy. S5, after the pressing device closes to the pressing gap gi, the punch moves downward at a set speed to compress and thicken the thickened deformation zone. gi is the gap between the pressing surface and the blank surface, in millimeters. Throughout the entire process of S5, heating and cooling are continuously performed to maintain the temperature gradient. A back pressure Fb is applied to the free end of the thickened deformation zone, i.e., the end where the material flows into the thickened deformation zone, which increases with the punch stroke according to a set rule. Fb is the back pressure, in kilonewtons. S6, after the thickened deformation zone is in place, pressure is maintained, and then the thickened deformation zone is forcibly and rapidly cooled to reduce its temperature below the process termination temperature; when the slab is a heat-treatable aluminum alloy, the process termination temperature is the lower limit of the alloy's return temperature range; when the slab is a non-heat-treatable aluminum alloy, the process termination temperature is a set temperature determined according to the measured flow stress-temperature relationship curve of the alloy, which is lower than the recrystallization temperature of the alloy. S7, Perform post-forming heat treatment according to the heat treatment route corresponding to the selected supply status; S8, remove the process allowance and perform machining.
[0017] Furthermore, the material source required for increasing the thickness of the thickened deformation zone is one or a combination of the following: firstly, a local compensation amount is reserved in the constraint zone adjacent to the thickened deformation zone when the slab is cut, and the local compensation amount is the excess slab area or local thickness increment; secondly, the material of the constraint zone flows into the thickened deformation zone from the boundary of the constraint zone under the control of the edge clamping gap gi, at which time the constraint zone undergoes controlled micro-thinning, and the thinning amount is limited to the constraint zone not experiencing in-plane instability.
[0018] Furthermore, the slab is supplied in T6 condition; T1 in S4 falls within the regression temperature range of the alloy; the cumulative time from when the temperature of the thickened deformation zone in S4 reaches T1 to when the temperature of the thickened deformation zone in S6 drops below the process termination temperature is tR, where tR is the cumulative residence time in seconds, and tR is within the regression window corresponding to T1. The regression window is the upper limit of the cumulative residence time allowed at T1 to restore the thickened deformation zone to its peak aged strength level after artificial aging in S7; the heat treatment in S7 is artificial aging to restore the thickened deformation zone to its peak aged strength level.
[0019] Furthermore, the heat treatment in S7 is a local re-aging process, which involves locally heating the thickened deformation zone after forming to the aging temperature, while simultaneously keeping the constrained zone on the slab, excluding the thickened deformation zone, cool, so that the temperature of the constrained zone is lower than the aging temperature, and the artificial aging only occurs in the thickened deformation zone; the aging temperature is 150 to 170 degrees Celsius, and the aging temperature is lower than the lower limit of the regression temperature range, and the holding time is two to six hours.
[0020] Furthermore, in S4, the criterion for the temperature gradient to reach the set state is: the temperature distribution of the mold body measured by the temperature sensor embedded in the mold body at a distance of one to three millimeters from the surface of the cavity reaches the set value determined according to the calibration relationship, wherein the calibration relationship is the correspondence between the pre-calibrated temperature distribution of the mold body and the temperature distribution of the slab; in S5, buckling precursors are identified based on the abrupt change in the slope of the load-displacement curve, and the blank holder gap gi and the back pressure Fb of each zone are adjusted accordingly.
[0021] Furthermore, the slab is made of a non-heat-treatable aluminum alloy, and no aging treatment is performed in S7. T1 and T2 are calibrated according to the measured flow stress-temperature relationship curve of the alloy.
[0022] Compared with the prior art, the beneficial effects of this application are: 1) This invention utilizes a temperature difference zone structure, with heating and cooling modules paired along the thickness direction and arranged in zones along the surface direction, separated by thermal insulation. This transforms the forming temperature from a single process parameter into a spatial variable within the plate surface, establishing a steep temperature distribution within the slab: high temperature in the thickened deformation zone, low temperature in the constrained zone, and a steep temperature transition zone. Consequently, the material's flow stress becomes a function of position, achieving three effects: First, the low flow stress required to reduce forming force and the high flow stress required to increase flow resistance in the non-thickened zone are no longer constrained by the same variable, thus reducing the forming force. The three originally contradictory indicators of control, full cavity filling, and stable shape of non-thickened areas are achieved simultaneously; secondly, the material spontaneously gathers towards the thickened deformation area under the drive of the flow resistance difference, and the deformation is transformed from the passive constraint of boundary enclosure in the existing technology to the active guidance of the material's own property field, and the conditions for buckling, folding and incomplete filling are suppressed; thirdly, the hot zone continues to soften during the deformation process, and the rate at which the forming load increases with the expansion of the contact area is lower than that under uniform low temperature conditions; it should be noted that this effect relies on the strong temperature sensitivity of the flow stress of high-strength aluminum alloy within the warm forming temperature range.
[0023] 2) This invention utilizes a cooling module to keep the constrained area below the lower limit of the regression temperature range throughout the molding process, and combines this with a material state path of local regression and re-aging. The temperature difference area is further reused for local re-aging after molding, heating and aging only the thickened deformation area, while the constrained area continues to cool. This allows the thickened deformation area to recover to the peak aged strength level after molding and adds stress corrosion resistance. The non-thickened area does not undergo regression softening, and its strength loss is less than that of the overall heating scheme. In this embodiment, the Vickers hardness of the constrained area is maintained at 174, while that of the overall heating scheme drops to 152. When using local re-aging, the constrained area does not experience aging temperature, and its peak aged structure is not affected by heat treatment, thus enabling the plate-like components to have the mechanical properties to bear the main load-bearing function.
[0024] 3) This invention uses slabs as blanks and cuts them according to the component outline. No flash is generated during the thickening process, the material utilization rate is higher than that of die forgings, and the metal is continuously distributed along the component outline. There is no flow line interruption or heat-affected zone softening caused by welding joints. The cooling module has dual functions of flow control and microstructure protection. The temperature difference area can be reused as a tooling for forming and heat treatment when local re-aging is adopted. This achieves high material utilization and high flow line continuity manufacturing of plate components, thereby solving the problems of low material utilization in die forging, flow line interruption in welded structures, and heat-affected zone softening. Attached Figure Description
[0025] Figure 1 This is a schematic diagram of the overall structure of the device in this application; Figure 2 This is a cross-sectional structural diagram of the overall structure of the device in this application; Figure 3 This is a cross-sectional view of the device in this application, which uses an upper concave die and a lower convex die configuration. Figure 4 This is a schematic diagram showing the location of the slab and the thickened deformation zone in this application; Figure 5 This is a flowchart of the forming process of this application; Figure 6 This is a schematic diagram showing the change of flow stress in high-strength aluminum alloy with deformation temperature. Figure 7 This is a schematic diagram showing the comparison curves of forming force as a function of punch stroke; Figure 8 A schematic diagram of the temperature change over time in the thickened deformation zone. In the diagram: 1. Partitioned pressing unit; 2. Mold; 21. Punch; 22. Die; 3. Back pressure unit; 4. Heating module; 5. Cooling module; 6. Slab; 61. Thickened deformation zone; 7. Exhaust structure.
[0026] It should be noted that, since the processing object is an aluminum alloy slab blank, the types, contours and sizes of the workpieces vary, and the positions and structures of the punch, die, heating module, cooling module, heat insulation partition, partitioned pressing unit and back pressing unit are also different, which cannot be exhausted by a fixed view. Detailed Implementation
[0027] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0028] In the description of this application, it should be understood that the terms "upper", "lower", "front", "rear", "left", "right", "top", "bottom", "inner", "outer", etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this application.
[0029] Please see Figure 1-8 This application provides a technical solution: a precision sheet metal extrusion forming apparatus and forming process, including a punch, a die, and a pressing device arranged circumferentially around the thickened deformation zone of an aluminum alloy blank.
[0030] The thickening deformation zone refers to the area on the aluminum alloy slab where a predetermined increase in thickness is expected. The constraint zone refers to the area on the aluminum alloy slab, excluding the thickening deformation zone, that must maintain its original shape during the forming process and must not experience in-plane instability or wrinkling. Since the material is incompressible, the material required for the increased thickness of the thickening deformation zone must be available. The material source provided by this invention is one or a combination of the following: First, a local compensation amount is reserved in the constraint zone adjacent to the thickening deformation zone during slab blanking, i.e., reserving excess sheet area or local thickness increment; Second, the material in the constraint zone flows into the thickening deformation zone from its boundary under the control of the edge clamping gap. At this time, the constraint zone undergoes controlled micro-thinning, the amount of which is limited to preventing in-plane instability in the constraint zone.
[0031] A temperature difference zone is also provided. This zone consists of three paired sections: a heating module, a cooling module, and a thermal insulation partition. The heating and cooling modules are paired along the thickness direction and partitioned along the surface direction. The function of the temperature difference zone is to establish and maintain a spatially non-uniform temperature field within the slab surface, transforming temperature from a process parameter into a spatial variable. Furthermore, to force rapid cooling of the thickened deformation zone at the end of the forming process, the punch and / or die are equipped with a deformation zone cooling channel on the thickened deformation zone side. This channel can be set independently or can be integrated into the channel within the heating module's insert (in which case the heating module is energized or supplied with a heating medium during heating, and switches to a cooling medium during rapid cooling, forming a heating and cooling reuse module). This channel is labeled 11, Deformation Zone Cooling Channel, in the attached drawing.
[0032] The heating module, corresponding to the thickened deformation zone of the slab, is located within the punch and / or die. It is used to heat the thickened deformation zone to a set temperature T1 during the forming process (T1 is the set temperature of the deformation zone, which is greater than the lower limit of the forming window temperature of the slab and less than the solution temperature of the alloy of the slab, in degrees Celsius). The heating module can be a resistance heating rod embedded in the mold body, with its heat conducted to the cavity surface through the mold body, resulting in stable and controllable temperature. To meet the heating speed requirements of this invention, the heating module preferably uses a local induction heating coil or a direct contact rapid heating device, which has a fast response speed and can raise the deformation zone to the set temperature within twenty-five seconds, suitable for applications with strict temperature and time window requirements.
[0033] The cooling module, corresponding to the constraint area of the slab, is located within the punch and / or die. It consists of cooling medium channels positioned below the cavity surface and maintained at a distance determined by strength checks, or cooling medium channels within cooling inserts supported by a high-strength backing. The cooling medium can be water, oil mist, or compressed air, and the flow rate of each channel is independently adjustable. The deformation zone cooling channel located on the side of the thickened deformation zone is used for forced rapid cooling of the thickened deformation zone at the end of the forming process. It can be set independently or integrated into the heating module insert and shared with the heating module. It is important to note the functional positioning of the cooling module: its function is not simply to reduce the temperature of a certain area to a specific value, but rather to continuously resist heat conduction from the thickened deformation zone to the constraint zone throughout the forming process, thereby limiting the width w of the temperature transition zone within a set range. In this embodiment, this width is six millimeters, which is 1.5 times the slab thickness. The temperature transition zone refers to the area on the slab surface where the temperature drops from T1 to T2 (T2 is the set temperature of the constraint zone, in degrees Celsius). The smaller its width w, the steeper the temperature gradient, the higher the spatial resolution of the flow resistance difference, and the stronger the certainty that the material flow is confined within the thickened deformation zone. Because heat conduction is continuous, the cooling module must operate throughout the entire process, not just during the heating stage or the initial stage of forming.
[0034] A thermal insulation partition is installed within the mold body between the heating and cooling modules, corresponding to the boundary of the thickened deformation zone. It blocks the heat conduction path within the mold body from the heating module side to the cooling module side, effectively preventing a thermal short circuit. Without insulation, heat from the heating module will be directly conducted to the cooling module via the mold body steel components, making it difficult to establish a temperature difference. Maintaining this difference would require extremely high heating power and cooling flow rate, which is neither economically viable nor controllable. The thermal insulation partition may include a thermal insulation groove on the mold body, a thermal insulation pad embedded within the groove, and a low thermal conductivity insert. The thermal insulation groove is located inside or on the back of the mold body and does not extend to the cavity surface. Its upper end maintains a distance from the cavity surface determined by mold strength checks to avoid weakening the mold body in high-stress areas at cavity corners. The thermal insulation pad only provides insulation and does not bear molding loads. In this embodiment, zirconia ceramic material is used; in other embodiments, other ceramic materials, mica materials, or aerogel materials may be used.
[0035] The directionality of the thermal insulation partition needs further explanation here. The thermal insulation partition blocks the lateral heat flow along the surface of the plate, i.e., from the heating module to the cooling module. However, the heat transfer path from the heating module to the slab is along the thickness direction. Since these two directions are different, the thermal requirements for the inserts are also directional: low thermal conductivity inserts can be made of titanium alloy or heat-resistant stainless steel and are positioned on the side of the heating module cavity facing the thermal insulation groove to increase lateral thermal resistance while maintaining the cavity surface strength. Their heat transfer path in the thickness direction should remain unobstructed to avoid hindering the heating module's heating of the slab and prolonging the heating time due to excessive cavity surface thermal resistance. Correspondingly, the cooling module cavity surface is composed of high thermal conductivity inserts to improve cooling response. When the heating module uses an induction heating coil, the coil should preferably be embedded on the side close to the cavity surface, making the slab itself the object of induction heating to increase the heating rate.
[0036] The edge-pressing device is a partitioned edge-pressing unit, divided into at least two independent units along the circumference of the thickening deformation zone. The edge-pressing gap gi (gi is the gap between the edge-pressing surface and the slab surface, in millimeters) of each unit is set independently and can be adjusted independently during the forming process. Considering that the slab thickness tolerance and the gap control accuracy are of the same order of magnitude, each partitioned edge-pressing unit should adaptively set its initial gap according to the actual measured thickness of the slab, and adopt a hybrid control method with gap as the main factor and edge-pressing pressure as a secondary factor. The key difference between this invention and known passive follow-up pressing schemes is that the edge-pressing gap determines whether the material can flow into the thickening deformation zone and the order in which the material flows into each partition, which is a control quantity of the nature of a flow valve; while the edge-pressing pressure mainly determines the magnitude of frictional resistance, which is a control quantity of the nature of a friction knob. Through the differentiated setting and dynamic adjustment of the gaps of each partition, the material supply sequence and supply amount can be actively arranged, thereby avoiding folding caused by local over-supply and incomplete filling caused by local under-supply. The value of the blanking gap gi for each zone should fall within the following range: its upper limit is determined according to the critical condition that the constraint zone does not experience in-plane instability under the blanking surface, and its lower limit is determined according to the need for material to flow from the zone into the thickening deformation zone. In this embodiment, the upper limit is 0.4 mm and the lower limit is 0.08 mm, which are 10% and 2% of the plate thickness, respectively. Within this range, the larger the value of gi, the stronger the material supply capacity and the weaker the constraint on the constraint zone, and vice versa.
[0037] This device also has an exhaust structure at the bottom or side wall of the concave mold cavity. The exhaust structure is an exhaust hole or an exhaust gap opened on the parting surface, which is used to discharge the gas in the mold cavity when the thickened material fills the cavity, to prevent incomplete filling and local burn-out caused by air entrapment.
[0038] This device also includes a back pressure unit, which applies a back pressure Fb (Fb is the back pressure, measured in kilonewtons) to the free end of the thickened deformation zone, i.e., the end of material flow, according to a set rule and varying with the punch stroke. The back pressure unit can be located within the die cavity and consists of an ejector rod, an anti-ejector block, or a hydraulic cushion, with its force directed towards the thickened deformation zone. The free end of the thickened deformation zone is the final position where material flows into it. The function of the back pressure is to transform the free upsetting at the thickened end into controlled upsetting, suppressing buckling and folding of the free end during the upsetting process. The back pressure must increase progressively with the punch stroke according to a set rule: if the back pressure is constant, its effect is no different from a passive elastic element, and it cannot adapt to changes in contact area and deformation resistance during the thickening process.
[0039] This device also includes temperature sensors and a control unit. The temperature sensors are embedded within the mold body at a distance of one to three millimeters from the cavity surface, with at least one sensor placed in each of the thickening deformation zone, temperature transition zone, and constraint zone. An infrared thermometer can be used to monitor the slab surface. The control unit adjusts the heating power of the heating module and the cooling medium flow rate of the cooling module based on temperature feedback, ensuring that the temperature difference ΔT = T1 - T2 does not exceed a set threshold throughout the molding process. This threshold is calibrated according to the alloy grade and is taken as 10% of the initial temperature difference. Simultaneously, it adjusts the edge clearance gi and back pressure Fb of each zone based on displacement and pressure feedback.
[0040] In this device, the deformation zone temperature T1 is set higher than the lower limit of the warm forming window of the sheet metal and lower than the solution temperature of the alloy. The lower limit of the warm forming window is defined as the temperature corresponding to when the flow stress of the alloy drops to 60% of the room temperature value. For VII series aluminum alloys, this lower limit is 180 degrees Celsius, and for V series aluminum alloys, it is 200 degrees Celsius. The technical rationale for setting this upper limit is that once high-strength aluminum alloys enter the solution temperature range, a large amount of precipitated phases dissolve back, and the material as a whole enters a supersaturated soft state. The strength difference between the deformation zone and the constrained zone disappears, which contradicts the purpose of this invention to create a flow resistance difference. Moreover, after forming, it is necessary to re-solution and aging treatment, and the deformation risk of thick plates is high during quenching. Therefore, this invention deliberately stays within the warm forming window and avoids the solution zone to retain the strength difference while softening appropriately.
[0041] A precision sheet metal extrusion molding process includes the following steps.
[0042] Step S1: Blanking and Selecting Material Condition. Blanks are cut according to the component outline to obtain aluminum alloy blanks, and the supply condition of the blanks is selected according to the material condition route described later.
[0043] Step S2, Surface treatment and lubrication. Apply a warm forming lubricant to the surface of the slab, thicken the cavity surface to accommodate the lubrication, and prevent surface scratches caused by lubrication film failure under warm forming conditions.
[0044] Step S3, mold installation and positioning. Position the slab between the punch and die, aligning the thickened deformation zone with the cavity. Set the initial blanking gap gi for each section's blanking unit according to the actual measured thickness of the slab.
[0045] Step S4: Quickly establish a temperature gradient within the plate surface. Before loading, activate the heating and cooling modules. A thermal insulation barrier blocks the heat conduction path from the heating module to the cooling module within the mold. Induction heating or direct contact rapid heating is used to heat the thickened deformation zone to temperature T1 within 25 seconds, while the constrained area is cooled and stabilized to temperature T2. The difference between T1 and T2 is not less than a set temperature difference, which is between 120 and 160 degrees Celsius depending on the alloy grade. In this embodiment, 140 degrees Celsius is used. T1 is higher than the lower limit of the forming window of the plate material and lower than the solution temperature of the alloy. Wait until the temperature field reaches the set state. Reaching the set state means that the temperature distribution measured by the temperature sensor embedded in the mold reaches the set value determined by the calibration relationship. At this point, the width w of the temperature transition zone tends to stabilize. The method for determining the width of the temperature transition zone is explained in detail in a later section. This step must precede loading; that is, the temperature gradient precedes plastic loading. This is the fundamental difference in timing between this invention and existing technologies such as "forming after overall heating." This step also marks the starting point for time measurement: starting from when the temperature of the thickened deformation zone reaches T1, the time that the zone spends within the regression temperature range is accumulated.
[0046] Step S5, edge clamping and extrusion thickening. The edge clamping unit closes to the set gap, establishing a constraint on the constrained area; then the punch descends at a set speed, which in this embodiment is 0.5 mm per second, to extrude and thicken the thickened deformation area. Continuous heating and cooling are applied throughout the process to maintain the temperature gradient; simultaneously, a back pressure Fb is applied to the free end of the thickened deformation area, increasing with the stroke according to a set rule. During the forming process, buckling precursors can be identified based on the characteristics of the load-displacement curve, especially the abrupt change in the slope of the load curve, and the gaps and back pressures of each section can be finely adjusted accordingly. The criterion for this abrupt change in slope is that within a 0.5 mm stroke window, the load increment decreases by more than 30% compared to the previous window.
[0047] Step S6, Pressure Holding and Forced Cooling. After the thickness is achieved, pressure is held for 15 seconds, followed by forced rapid cooling of the thickened deformation area by the cooling channels on the punch and / or die, reducing it to below the process termination temperature within 5 seconds at a rate of not less than 40 degrees Celsius per second. When the slab is a heat-treatable aluminum alloy, the process termination temperature is the lower limit of the alloy's return temperature range. In this embodiment, the lower limit is 190 degrees Celsius, and the value of the lower limit for different grades is approximately 180 to 200 degrees Celsius. When the slab is a non-heat-treatable aluminum alloy, the process termination temperature is a set temperature determined according to the measured flow stress-temperature relationship curve of the alloy, which is lower than the recrystallization temperature of the alloy. In this embodiment, the set temperature is 150 degrees Celsius. The cumulative time tR (tR is the cumulative dwell time in seconds) from when the temperature of the deformation zone reaches T1 in step S4 until the deformation zone is cooled below the process termination temperature in this step must be within the regression window corresponding to T1. If this cannot be met due to limitations of the component and process conditions, the workpiece will be processed according to the T6 state temperature forming route (i.e., route A) described later, which means acknowledging that the material has been aged and correspondingly reducing the expected strength level.
[0048] Step S7, post-forming heat treatment. Perform heat treatment according to the material state route: Route A: no special heat treatment is performed, or only low-temperature supplementary aging is implemented; Route B: the entire component is re-aged, or the thickened deformation area is locally re-aged using the temperature difference region as described in the preferred method below.
[0049] Step S8, trimming and machining. Remove the excess material, machine the thickened end face and connecting parts, and perform surface treatment.
[0050] To address the issue of changes in precipitated phases and loss of peak aged strength in heat-treatable high-strength aluminum alloys within the warm forming temperature range, this invention provides two optional material state routes, and recommends the second one.
[0051] Route A involves temperature forming at T6. The slab is supplied in the T6 state and undergoes no special heat treatment after temperature forming, or only low-temperature supplementary aging. This route has the simplest process, but the thickened deformation zone is over-aged due to its residence in the temperature range of temperature forming, resulting in a strength reduction to the T7 state level that cannot be fully recovered. In this embodiment, the tensile strength is reduced from 570 MPa to 505 MPa. This route is suitable for non-load-bearing components with low strength requirements, and also for situations where the cumulative high-temperature residence time cannot be compressed within the recovery window due to limitations in component size and process cycle.
[0052] Route B, a combination of local re-aging and re-aging, is the recommended route of this invention. The slab is still supplied in the T6 condition, but the deformation zone setting temperature T1 is selected within the re-aging temperature range of the alloy, and the cumulative residence time tR of the thickened deformation zone within the re-aging temperature range is within the corresponding re-aging window. Re-aging refers to the phenomenon where, after a short heating of an alloy in its peak-aged state, the precipitated phase partially dissolves, resulting in a temporary decrease in strength. This phenomenon is reversible, and the strength can be restored through subsequent artificial aging treatment. Since the re-aging softening window and the warm forming window highly overlap in temperature, this route unifies softening for forming and performance restoration within the same temperature band.
[0053] The success of this route depends on the dual control of temperature and time: the higher the temperature, the more complete the softening, but the shorter the allowed dwell time. The two constitute a process window that can be specified according to the alloy grade. Based on this, the present invention gives a coupling limit to T1 and tR, and requires rapid heating, forming and forced rapid cooling, so that the entire process is completed within this window. In this embodiment, the regression window for the 7-series aluminum alloy is tR not exceeding 90 seconds at 240 degrees Celsius and not exceeding 45 seconds at 260 degrees Celsius.
[0054] The lower limit of the aforementioned regression temperature range, i.e., the temperature at which the regression effect of the alloy basically disappears, is determined by calibrating the alloy grade through tests on the change of hardness or electrical conductivity with temperature. Correspondingly, "below the lower limit of the regression temperature range" in step S6 is the endpoint criterion for forced rapid cooling and the source of the process termination temperature. This lower limit corresponds to the 7-series aluminum alloy. In this embodiment, the lower limit is 190 degrees Celsius. The range of the lower limit for different grades is approximately 180 to 200 degrees Celsius. It should be noted that the lower limit of the regression temperature range also constitutes the upper limit of the aging temperature during local re-aging: the aging temperature should be lower than the lower limit, and the temperature of the constrained area during the local re-aging process should be lower than the aging temperature, so as to maintain a positive temperature difference between the thickened deformation area and the constrained area. The upper limit of the regression temperature range coincides with the upper limit of the warm forming window, and its correspondence with tR (i.e., the higher the temperature, the shorter the allowable dwell time) is also calibrated according to the grade and filled into the process card.
[0055] There are two implementation methods for post-forming re-aging treatment. One is overall re-aging: the entire component is artificially aged to restore the thickened deformation zone to its peak aged strength level. Due to the regression re-aging effect, it achieves stress corrosion resistance superior to the conventional T6 state. In this embodiment, the electrical conductivity of the thickened deformation zone is increased from 32% of the international annealed copper standard to 38.5%. Since the constrained area did not enter the regression range during the forming process and its peak aged structure was not damaged by regression, the additional strength reduction of the constrained area caused by overall re-aging is less than that of the overall heating method. In this embodiment, the Vickers hardness of the constrained area is reduced from 174 after forming to about 171, a reduction of about 1.7%, while the overall heating method reduces it to 152.
[0056] Secondly, local re-aging: After molding, the temperature difference area of this device is used to locally heat the thickened deformation area to the aging temperature by the heating module, while the cooling module continues to keep the constrained area at a low temperature, so that re-aging only occurs in the thickened deformation area; thus, the peak aged microstructure of the constrained area is not affected by heat treatment, and the non-thickened area does not suffer strength loss due to heat treatment after molding. The local re-aging method also expands the temperature difference area from the molding tooling to a tooling that can be reused for both molding and heat treatment, eliminating the need for additional heat treatment equipment.
[0057] Considering that the temperature difference region is occupied during local re-aging, local re-aging should preferably adopt a short-time aging regime with a temperature higher than that of conventional single-stage aging, such as 150 to 170 degrees Celsius depending on the alloy grade, and holding for two to six hours, to shorten the tooling occupation time. For components with higher performance requirements, a two-stage aging regime can also be used. It should be noted that the above-mentioned short-time aging regime must be coordinated with the local re-aging method: if the regime is applied to the component as a whole, the unrecovered constraint area will be over-aged as a result; therefore, when using a short-time high-temperature regime, it should be implemented using a local re-aging method, while the overall re-aging should preferably adopt a conventional single-stage aging regime. The above-mentioned aging regime is determined by actual measurement according to the alloy grade, and this invention does not limit it.
[0058] This approach also endows the cooling module with a second technical function. Because the constrained area is cooled below the lower limit of the regression temperature range throughout the entire molding process, it does not enter the regression range, and the peak aging microstructure is not damaged by regression. Therefore, the cooling module not only maintains the flow resistance gradient during molding but also protects the original strength of the non-thickening area in terms of performance. Continuous cooling throughout the molding process thus becomes a necessary process condition.
[0059] For non-heat-treatable aluminum alloys such as the five-series (aluminum-magnesium series), there are no aging or regression issues. The temperature difference zone extrusion thickening process of this invention can be directly used for warm forming. The temperature window is separately calibrated according to the measured flow stress-temperature relationship curve of the alloy. In this embodiment, the warm forming window for the five-series aluminum alloy is 200 to 300 degrees Celsius, with T1 at 260 degrees Celsius and T2 at 120 degrees Celsius. Since this type of alloy has no regression temperature range, the process termination temperature is not based on the lower limit of regression, but is determined according to the measured flow stress-temperature relationship curve of the alloy, taking a set temperature lower than the recrystallization temperature of the alloy. The criterion for this value is that continuing to hold at this temperature will not cause further changes in the alloy's microstructure and properties. This criterion is calibrated through the measured flow stress-temperature relationship curve combined with hardness testing. In this embodiment, the recrystallization temperature of the alloy is approximately 320 degrees Celsius, and the set temperature is 150 degrees Celsius.
[0060] The method for determining the width of the temperature transition zone is explained below. The temperature transition zone is located inside the slab and is difficult to measure directly online. This invention uses two methods to determine it: First, the temperature distribution of the mold body, measured by a temperature sensor embedded in the mold body, is estimated by combining this with a pre-calibrated correspondence between the mold body temperature distribution and the slab temperature distribution. This correspondence is obtained through offline thermal imaging measurement or slab sectioning temperature calibration. Second, the calibration results are solidified into process parameters, i.e., the cooling medium flow rate, heating power, and insulation structure are set according to the calibration relationship, so that the width of the temperature transition zone is controlled in the process. During production, the control unit maintains the above process parameters in a closed loop according to the mold body temperature measurement.
[0061] Example 1 (7-series high-strength aluminum alloy, material condition route B) The component in this embodiment is a plate joint with a local boss. The slab material is 7075-T6 aluminum alloy, supplied in T6 condition, with a planar dimension of 300 mm x 200 mm. The original thickness of the constraint zone, i.e., the plate thickness t0, is 4.0 mm. The thickening deformation zone is a circular area located in the middle of the slab, with a diameter of 30 mm and an area of approximately 707 square millimeters. During blanking, a local thickness increment of 0.3 mm is reserved in the annular constraint zone adjacent to the thickening deformation zone (inner diameter 30 mm, outer diameter 70 mm, area 3142 square millimeters), i.e., the blanking thickness of this ring is 4.3 mm.
[0062] The target thickness after thickening is 6.4 mm, with a thickness increase ratio of 1.6. Based on volume balance calculations, the additional material volume required for the thickened deformation zone is approximately 707 x 2.4, or about 1697 cubic millimeters. Of this, 3142 x 0.3, or about 943 cubic millimeters, is provided by the local compensation allowance reserved during blanking; the remaining approximately 754 cubic millimeters is provided by the controlled micro-thinning of the annular constraint zone during the forming process. The thickness of this annular zone is correspondingly reduced from 4.3 mm during blanking to 3.76 mm after forming, meaning a thinning of 0.24 mm relative to the original plate thickness of 4.0 mm, a thinning rate of 6.0%, which does not exceed the limit for preventing in-plane instability in the constraint zone.
[0063] The alloy has a solution temperature of 477 degrees Celsius, a warm forming window of 180 to 320 degrees Celsius, and a return temperature range of 190 to 320 degrees Celsius, with its upper limit coinciding with the upper limit of the warm forming window. Based on this, the deformation zone temperature T1 is set at 240 degrees Celsius, and the constraint zone temperature T2 is set at 100 degrees Celsius, with a difference ΔT of 140 degrees Celsius. T1 is greater than the lower limit of the warm forming window (180 degrees Celsius), less than the solution temperature of 477 degrees Celsius, and falls within the return temperature range.
[0064] The heating module uses a local induction heating coil, which raises the temperature of the thickened deformation zone from room temperature to 240 degrees Celsius within 25 seconds after power-on. The cooling module simultaneously heats the thickened deformation zone and circulates a cooling medium through the constrained zone, stabilizing it at 100 degrees Celsius. The width w of the temperature transition zone is 6 millimeters, which is 1.5 times the plate thickness. Temperature sensors are placed in the thickened deformation zone, the temperature transition zone, and the constrained zone, embedded within the mold body at a distance of 2 millimeters from the cavity surface. The temperature difference ΔT decreases by 8.4 degrees Celsius throughout the molding process, accounting for 6% of the initial temperature difference, which does not exceed the set threshold of 10% of the initial temperature difference.
[0065] The edge-pressing device is divided into four zoned edge-pressing units. The two zones located in the supply direction have an edge-pressing gap gi of 0.3 mm, which is 7.5% of the plate thickness. This gap is between the upper limit of 0.4 mm (10% of the plate thickness) and the lower limit of 0.08 mm (2% of the plate thickness), allowing material to flow into the thickening deformation zone from these two zones. The other two zones have an edge-pressing gap gi of 0.04 mm, which is 1% of the plate thickness. This gap is less than the lower limit, preventing material from flowing in and serving only as a constraint.
[0066] The punch descends at a speed of 0.5 mm / s, with a stroke of 2.4 mm, corresponding to an extrusion time of 4.8 seconds, to extrude and thicken the thickened deformation zone. The back pressure unit applies a back pressure Fb to the free end of the thickened deformation zone, with Fb increasing linearly from 15 kN to 55 kN as the punch stroke progresses. Continuous heating and cooling are applied throughout the entire process to maintain the aforementioned temperature gradient.
[0067] After the thickness is achieved, the pressure is held for 15 seconds. Then, the cooling medium is switched from the deformation zone cooling channel integrated in the heating module insert to the forced rapid cooling of the thickened deformation zone. Within 5 seconds, the temperature is reduced to 150 degrees Celsius at a rate of not less than 40 degrees Celsius per second. This temperature is lower than the process termination temperature, i.e., the lower limit of the return temperature range of 190 degrees Celsius. The cumulative residence time tR from when the temperature of the thickened deformation zone reaches 240 degrees Celsius until it drops below 190 degrees Celsius is approximately 21 seconds. Among them, the extrusion thickening takes 4.8 seconds, the pressure holding takes 15 seconds, and the rapid cooling from 240 degrees Celsius to below 190 degrees Celsius at a rate of not less than 40 degrees Celsius per second takes approximately 1.3 seconds, which is less than the upper limit of the 90-second return window for the alloy at 240 degrees Celsius. The temperature rises from 190 degrees Celsius to 240 degrees Celsius in about six seconds. During this period, the temperature is constantly changing and is not included in tR according to the unified standard of the process card in this embodiment. If it is conservatively included, tR is about 27 seconds, which is still less than the upper limit of the 90-second regression window.
[0068] After molding, local re-aging is performed according to route B: the heating module locally heats the thickened deformation area to 160 degrees Celsius and holds it at that temperature for four hours. During the holding period, the cooling module continues to maintain the constraint area at 90 degrees Celsius, which is lower than the constraint area set temperature of 100 degrees Celsius during molding, in order to avoid aging of the constraint area during the holding period. This temperature is lower than the aging temperature of 160 degrees Celsius, so artificial aging only occurs in the thickened deformation area. The aforementioned aging temperature of 160 degrees Celsius is lower than the lower limit of the regression temperature range of 190 degrees Celsius.
[0069] The molding results of this embodiment are as follows: peak molding force of 126 kN; thickened cavity filling rate of 99.2%; maximum thinning rate of the constrained area of 6.0%, consistent with the above-mentioned volume balance calculation value, and no in-plane instability or wrinkling occurred; the Vickers hardness of the constrained area after molding is 174, which is basically consistent with the original T6 state of 175; the Vickers hardness of the thickened deformation area before local reaging is 138, which recovers to 171 after local reaging, which is 97.7% of the original T6 state; the electrical conductivity of the thickened deformation area increases from 32% of the original T6 state, equivalent to the international annealed copper standard, to 38.5%; and the material utilization rate is 92%.
[0070] Example 2 (5-series aluminum alloy, without aging treatment) The slab material in this embodiment is 5083-H321 aluminum alloy, which is a non-heat-treatable aluminum alloy. It is supplied in H321 condition. The slab's planar dimensions are 300 mm x 200 mm, and the thickness t0 is 5.0 mm. The thickening deformation zone is a circular area located in the center of the slab, with a diameter of 40 mm. The target thickness after thickening is 8.0 mm, with a thickness increase ratio of 1.6. Based on volume balance calculations, the area of the thickening deformation zone is approximately 1257 square millimeters, and the material volume required to increase its thickness is approximately 1257 x 3.0 mm, or approximately 3771 cubic millimeters. During blanking, a local thickness increment of 0.45 mm is reserved in the annular constraint area (inner diameter 40 mm, outer diameter 90 mm, area approximately 5,105 square millimeters) adjacent to the thickened deformation area. That is, the blanking thickness of the ring is 5.45 mm, which can provide approximately 2,297 cubic millimeters. The remaining approximately 1,474 cubic millimeters are provided by the controlled micro-thinning of the annular constraint area during the forming process. The thickness of the ring is correspondingly reduced from 5.45 mm during blanking to 4.71 mm after forming, which is a reduction of 0.29 mm relative to the original plate thickness of 5.0 mm. The thinning rate is 5.8%, which is consistent with the forming results described later and does not exceed the limit of the constraint area not experiencing in-plane instability.
[0071] This alloy does not have aging or regression issues, and its recrystallization temperature is 320 degrees Celsius. The warm forming window is calibrated to 200-300 degrees Celsius based on the measured flow stress-temperature relationship curve of this alloy. The solution temperature of this alloy is higher than the upper limit of the warm forming window of 300 degrees Celsius, so T1 is set to 260 degrees Celsius to meet the requirement of being lower than the solution temperature of the alloy in this sheet material. Accordingly, the set temperature T1 for the deformation zone is 260 degrees Celsius, and the set temperature T2 for the constraint zone is 120 degrees Celsius, with a difference ΔT of 140 degrees Celsius; the width w of the temperature transition zone is 7.5 millimeters, which is 1.5 times the thickness of the sheet.
[0072] The heating module uses a local induction heating coil to raise the temperature of the thickened deformation zone to 260 degrees Celsius within 30 seconds. The edge-pressing device is divided into four zoned edge-pressing units. The edge-pressing gap gi of the two zones located in the feeding direction is 0.38 mm, approximately 7.5% of the plate thickness; the gap gi of the other two zones is 0.05 mm, approximately 1% of the plate thickness, which is less than the lower limit of 0.1 mm determined according to 2% of the plate thickness, preventing material flow and only serving a restraining function. In this embodiment, the upper and lower limits of the edge-pressing gap are 0.5 mm and 0.1 mm, respectively. The punch descends at a speed of 0.5 mm per second, with a stroke of 3.0 mm; the back pressure Fb increases linearly from 20 kN to 70 kN. After the thickening is in place, the pressure is held for 15 seconds, followed by forced rapid cooling, reducing the temperature to 140 degrees Celsius within 6 seconds. This temperature is lower than the process termination temperature of 150 degrees Celsius in this embodiment.
[0073] Since the alloy cannot be strengthened by heat treatment, no aging treatment is performed in S7. Instead, a stabilization annealing at 150 degrees Celsius for one hour is carried out to eliminate residual stress. The stabilization annealing is for the purpose of eliminating residual stress and is not an aging treatment. Its temperature is consistent with the process termination temperature of this embodiment. Continuing to leave the process will not cause further changes in the microstructure and properties of the alloy.
[0074] The molding results of this embodiment are as follows: peak molding force of 95 kN; filling rate of thickened cavity of 98.6%; maximum thinning rate of constrained area of 5.8%, with no in-plane instability or wrinkling; Vickers hardness of constrained area of 94, which is basically consistent with the original 95; Vickers hardness of thickened deformation area of 84; and material utilization rate of 93%.
[0075] Test case Using the same components, molds, and slabs as in Example 1, only the temperature conditions and heating methods were changed to conduct three sets of comparative tests.
[0076] Comparative Example 1: Room temperature molding under a uniform temperature field: The heating and cooling modules are not activated, and the slab is at room temperature. The results are: peak molding force of 268 kN, filling rate of the thickened cavity of 72%, folding at the free end of the thickened area, maximum thinning rate of the constrained area of 11.2%, and Vickers hardness of 175 in the constrained area.
[0077] Comparative Example 2: Overall heating and forming under a uniform temperature field: Without activating the temperature difference zone, the entire slab was placed in the heating device and heated to 240 degrees Celsius. It was then transferred to the mold and formed. During the forming process, neither the heating nor cooling modules were operational. The results showed a peak forming force of 132 kN, a cavity filling rate of 98%, but a maximum thinning rate of 18.5% in the constrained area, accompanied by in-plane instability and wrinkling. The Vickers hardness of the constrained area decreased to 152, a reduction of 13.1%.
[0078] The present invention is a zoned temperature control scheme for Example 1: the peak molding force is 126 kN, which is 53.0% less than that of Comparative Example 1 and comparable to that of Comparative Example 2; the thickened cavity filling rate is 99.2%, which is higher than that of Comparative Example 1 and Comparative Example 2; the maximum thinning rate of the constrained area is 6.0%, and no wrinkling occurs; the Vickers hardness of the constrained area is 174, with basically no loss.
[0079] As can be seen from the above comparison, although Comparative Example 1 can maintain the strength of the constrained area, the forming force is high, the filling is insufficient, and folding occurs; although Comparative Example 2 has low forming force and full filling, the constrained area becomes unstable and its strength decreases. Only when a temperature gradient is established and maintained throughout the process within the plate can the four indicators of controllable forming force, full cavity filling, stable shape of non-thickening area, and maintained strength of constrained area be achieved simultaneously.
[0080] The foregoing has shown and described the basic principles, main features, and advantages of this application. It will be apparent to those skilled in the art that this application is not limited to the details of the exemplary embodiments described above, and that this application can be implemented in other specific forms without departing from the spirit or basic characteristics of this application. Therefore, the embodiments should be regarded as exemplary and non-limiting in all respects. The scope of this application is defined by the appended claims rather than the foregoing description. Therefore, it is intended to encompass all variations falling within the meaning and scope of equivalents of the claims within this application, and no reference numerals in the claims should be regarded as limiting the scope of the claims.
[0081] Although embodiments of this application have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and variations can be made to these embodiments without departing from the principles and spirit of this application, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A precision sheet metal extrusion forming apparatus, comprising a punch, a die, and a pressing device arranged circumferentially around a thickening deformation zone of an aluminum alloy blank, wherein the thickening deformation zone refers to a region on the aluminum alloy blank where a predetermined increase in thickness is to be generated, characterized in that: A temperature difference zone is also provided, which is composed of a heating module, a cooling module and a heat insulation partition arranged in pairs. The heating module is located in the punch and / or die corresponding to the thickening deformation zone, and is used to heat the thickening deformation zone to the set temperature T1 of the deformation zone. T1 is the set temperature of the deformation zone. The cooling module is located within the punch and / or die, corresponding to the constraint area on the aluminum alloy slab other than the thickening deformation area. It is used to cool the constraint area to a set temperature T2, where T2 is the set temperature and T1 is greater than T2. The heat insulation partition is located within the mold between the heating module and the cooling module, and its position on the plate surface corresponds to the boundary of the thickening deformation area. It is used to block the heat conduction path from the heating module to the cooling module inside the mold. The set temperature T1 of the deformation area is greater than the lower limit of the forming window temperature of the sheet metal and less than the solution temperature of the alloy of the sheet metal. The heating module and the cooling module establish a temperature gradient from the thickening deformation area to the constraint area before the punch is loaded, and maintain the temperature gradient throughout the extrusion thickening process.
2. The precision sheet metal extrusion forming apparatus according to claim 1, characterized in that: The heat insulation partition includes a heat insulation groove, a heat insulation pad embedded in the heat insulation groove, and a low thermal conductivity insert; the heat insulation groove is formed inside the mold body or on the back and does not extend to the cavity surface, and its upper end maintains a distance determined according to the strength check of the mold body. The heat insulation pad does not bear the molding load; the low thermal conductivity insert is set on the side of the cavity surface of the heating module facing the heat insulation groove, which blocks the heat conduction path in the plate surface direction, and keeps the heat transfer path in the plate thickness direction unobstructed; the cavity surface of the cooling module is composed of a high thermal conductivity insert; the punch and / or die are also provided with a deformation zone cooling channel on the thickened deformation zone side, which is independently set or is combined by the channel integrated in the insert of the heating module.
3. The precision sheet metal extrusion forming apparatus according to claim 1, characterized in that: The edge-pressing device is a partitioned edge-pressing unit, which is divided into at least two independent units along the circumference of the thickened deformation zone. The edge-pressing gap gi of each unit is set independently and adjusted independently during the forming process. gi is the gap between the edge-pressing surface and the surface of the blank. The edge-pressing gap gi of each unit is set to an initial value according to the measured thickness of the aluminum alloy blank. The upper limit of gi is determined according to the critical condition that the constraint zone does not experience in-plane instability under the edge-pressing surface, and the lower limit of gi is determined according to the condition that the material can flow from the constraint zone corresponding to the unit into the thickened deformation zone.
4. The precision sheet metal extrusion forming apparatus according to claim 1, characterized in that: It also includes a back pressure unit, which applies back pressure Fb to the free end of the thickened deformation zone. Fb increases according to a set rule as the punch stroke progresses. An exhaust structure is also provided on the bottom or sidewall of the cavity, which is an exhaust hole or an exhaust gap opened on the parting surface. A temperature sensor and control unit are also provided. The temperature sensor is embedded in the mold body at a distance of one to three millimeters from the cavity surface, with at least one sensor arranged in each of the thickened deformation zone, the temperature transition zone, and the constraint zone. The temperature transition zone refers to the plate surface area where the temperature drops from T1 to T2. The control unit adjusts the heating power of the heating module and the cooling medium flow rate of the cooling module according to the temperature distribution measured by the temperature sensor, ensuring that the attenuation of the difference between T1 and T2 throughout the molding process does not exceed a set threshold specified according to the alloy grade. The control unit also adjusts the edge clearance gi and the back pressure Fb of each unit based on displacement and pressure feedback.
5. A precision sheet metal extrusion forming process, wherein the precision sheet metal extrusion forming apparatus according to claims 1-5 is characterized in that: Includes the following steps: S1, cut the slab according to the component outline and select the supply status of the slab; S2, applying a warm forming lubricant to the surface of the slab; S3, the blank is positioned and installed between the punch and the die, so that the thickened deformation area on the blank is aligned with the cavity of the die, and the initial pressing gap gi is set by the pressing device surrounding the thickened deformation area according to the actual measured thickness of the blank. S4, before loading, the thickened deformation zone is heated to the deformation zone set temperature T1, and the constraint zone on the slab other than the thickened deformation zone is cooled to the constraint zone set temperature T2. A temperature gradient from the thickened deformation zone to the constraint zone is established in the slab surface. T1 is greater than T2, greater than the lower limit temperature of the forming window of the plate, and less than the solution temperature of the plate alloy. S5, after the pressing device closes to the pressing gap gi, the punch moves downward at a set speed to press and thicken the thickened deformation zone. gi is the gap between the pressing surface and the blank surface. Throughout the entire process of S5, heating and cooling are continuously performed to maintain the temperature gradient. A back pressure Fb is applied to the free end of the thickened deformation zone, i.e. the end where the material flows into the thickened deformation zone, which increases with the punch stroke according to a set rule. S6, after the thickened deformation zone is in place, pressure is maintained, and then the thickened deformation zone is forcibly and rapidly cooled to reduce its temperature below the process termination temperature; when the slab is a heat-treatable aluminum alloy, the process termination temperature is the lower limit of the alloy's return temperature range; when the slab is a non-heat-treatable aluminum alloy, the process termination temperature is a set temperature determined according to the measured flow stress-temperature relationship curve of the alloy, which is lower than the recrystallization temperature of the alloy. S7, Perform post-forming heat treatment according to the heat treatment route corresponding to the selected supply status; S8, remove the process allowance and perform machining.
6. The precision sheet metal extrusion forming process according to claim 5, characterized in that: The material source required to increase the thickness of the thickened deformation zone is one or a combination of the following: First, a local compensation amount is reserved in the constraint zone adjacent to the thickened deformation zone when the slab is cut, and the local compensation amount is the excess slab area or local thickness increment; Second, the material of the constraint zone flows into the thickened deformation zone from the boundary of the constraint zone under the control of the edge clamping gap gi, at which time the constraint zone undergoes controlled thinning, and the thinning amount is limited to the constraint zone not experiencing in-plane instability.
7. The precision sheet metal extrusion forming process according to claim 5, characterized in that: In S4, T1 falls within the regression temperature range of the alloy; the cumulative time from when the temperature of the thickened deformation zone in S4 reaches T1 to when the temperature of the thickened deformation zone in S6 drops below the process termination temperature is tR, and tR is within the regression window corresponding to T1. The regression window is the upper limit of the cumulative residence time allowed at T1 so that the thickened deformation zone can be restored to the peak aging strength level by the artificial aging in S7; the heat treatment in S7 is artificial aging to restore the thickened deformation zone to the peak aging strength level.
8. The precision sheet metal extrusion forming process according to claim 7, characterized in that: The heat treatment in S7 is local re-aging, which involves locally heating the thickened deformation area after forming to the aging temperature, while the constrained area on the slab other than the thickened deformation area continues to be cooled, so that the temperature of the constrained area is lower than the aging temperature, and the artificial aging only occurs in the thickened deformation area; the aging temperature is 150 to 170 degrees Celsius, and the aging temperature is lower than the lower limit of the regression temperature range, and the holding time is two to six hours.
9. The precision sheet metal extrusion forming process according to claim 5, characterized in that: In S4, the criterion for the temperature gradient to reach the set state is: the temperature distribution of the mold body measured by the temperature sensor embedded in the mold body at a distance of one to three millimeters from the surface of the cavity reaches the set value determined by the calibration relationship, wherein the calibration relationship is the correspondence between the pre-calibrated temperature distribution of the mold body and the temperature distribution of the slab; in S5, buckling precursors are identified based on the abrupt change in the slope of the load-displacement curve, and the blank holder gap gi and the back pressure Fb of each zone are adjusted accordingly.