An alcohol-based functional gel for gradient performance regulation of cemented carbide and a preparation method thereof

By utilizing the weak thixotropy and porous interconnected structure of alcohol-based functional gels, the problems of uneven coating and sedimentation and stratification of the binder phase on the surface of cemented carbide blanks are solved, achieving stable suspension and precise coating with high solids content, forming cemented carbide cutting tools with gradient properties, suitable for modern production.

CN123102992APending Publication Date: 2026-11-17SHAREATE TOOLS +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611258592.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, uneven coating on the surface of cemented carbide green blanks, easy sedimentation and stratification of the binder phase, poor adhesion of the coating agent, difficulty in achieving stable suspension with high solid content and precise local application, resulting in poor process stability during sintering and failing to meet the needs of modern production.

Method used

An alcohol-based functional gel is used, which contains alcohol solvents, gelling agents, binder phase pullers, promoters, dispersants and pore-forming agents. By constructing a weak thixotropic three-dimensional network structure and a porous interconnected structure, high solids content stable suspension, precise local coating and drying porous degassing are achieved, ensuring the directional redistribution of the binder phase during sintering.

Benefits of technology

It achieves high-solids-content stable suspension, dry porous degassing, and precise local coating of alcohol-based gel on the surface of cemented carbide blanks, forming a gradient hardness and toughness structure, which improves the service life and reliability of cemented carbide tools and is suitable for modern continuous sintering production lines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123102992A_ABST
    Figure CN123102992A_ABST
Patent Text Reader

Abstract

This invention discloses an alcohol-based functional gel for gradient performance regulation of cemented carbide and its preparation method. The alcohol-based functional gel comprises, by mass percentage: 40%–70% alcohol solvent, 0.5%–10.0% gelling agent, 0%–50% binder phase puller, 0%–50% binder phase promoter, 0.2%–2.0% dispersant, 1%–6% pore-forming aid, 0%–6% plasticizer, and the balance being deionized water; the total content of binder phase puller and promoter is 20%–50%. The gelling agent is selected from one or more of cellulose ethers, natural polymer gels, polyethylene oxide, polyvinylpyrrolidone, carbomer resins, and inorganic-organic composite thixotropic agents. This invention completely solves the gas blockage defect of dense carbon films, allows for precise local coating, and achieves gradient hardness and toughness after sintering, making it suitable for the industrial production of WC-Co cemented carbide mining tools and drilling tools.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of functional coating materials for cemented carbide surfaces, specifically relating to an alcohol-based functional gel for the surface of cemented carbide green blanks with adjustable redistribution of the binder phase and its preparation method, which is particularly suitable for gradient performance control of WC-Co type cemented carbide mining ball teeth and drilling tools. Background Technology

[0002] In the industrial production of cemented carbide (especially WC-Co cemented carbide), to achieve the comprehensive performance of "hard on the outside and tough on the inside" in cutting tools, it is usually necessary to apply a binder phase control material locally to the surface of the green blank. This causes the binder phases such as Co and Ni to redistribute directionally during sintering, thereby forming a gradient structure with high surface hardness and high wear resistance, and high core toughness and high impact resistance. Currently, many companies in the industry use a combination of binder phase puller and binder phase promoter to achieve this function, but the coating agent is in a suspension state rather than a gel.

[0003] The existing technology has the following insurmountable drawbacks: 1. In traditional aqueous or alcoholic suspensions, the density of the binder puller and propellant is about 7.5 to 8.5 g / cm3, which is much higher than the solvent density. They are very easy to settle, separate, and agglomerate quickly. The viscosity is not high, so they are easy to flow, resulting in uneven coating and making it impossible to achieve precise local application. 2. The suspension has poor adhesion and is prone to falling off, flowing and spreading during handling, loading, and pre-firing, resulting in poor process stability and difficulty in ensuring batch consistency. 3. It cannot simultaneously meet the four core requirements of high solids content (20-50 wt%), long-term stability without stratification, dry and porous degassing, and precise local coating, making it difficult to adapt to modern continuous sintering production lines. Summary of the Invention

[0004] The purpose of this invention is to provide an alcohol-based, multi-system compatible, high-solids-content, stable, non-stratified, dry, porous, and precisely localized functional gel for coating the surface of cemented carbide green blanks. During the sintering process, it can controllably drive the redistribution of the binder phase to obtain gradient hardness and gradient toughness, while ensuring smooth heating and venting of the green blank, defect-free sintering, and improving the service life and reliability of cemented carbide tools.

[0005] To achieve the above objectives, the functional gel technology of the present invention is as follows: an alcohol-based functional gel for gradient performance regulation of cemented carbide, comprising the following components by mass percentage: 40%–70% alcohol solvent, 0.5%–10.0% gelling agent, 0%–50% binder phase pull-out agent, 0%–50% binder phase promoter, 0.2%–2.0% dispersant, 1%–6% pore-forming aid, 0%–6% plasticizer, with the balance being deionized water, the content of which does not exceed 15%. The total content of the binder puller and the binder pusher is 20% to 50%; the gelling agent is selected from one or more of the following: cellulose ether gelling agents, natural polymer gelling agents, polyethylene oxide gelling agents, polyvinylpyrrolidone gelling agents, carbomer resin gelling agents, and inorganic-organic composite thixotropic agent gelling agents.

[0006] In the above scheme, preferably, the cellulose ether gelling agent is selected from one or more of hydroxypropyl methylcellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose; the natural polymer gelling agent is selected from one or more of sodium alginate, guar gum, xanthan gum, and gellan gum; the polyvinylpyrrolidone gelling agent is selected from one or two of polyvinylpyrrolidone K30 and polyvinylpyrrolidone K90; the carbomer resin gelling agent is selected from one or more of carbomer 940, carbomer 980, and carbomer Ultraz, and is used in conjunction with triethanolamine for neutralization; the inorganic-organic composite thixotropic agent gelling agent is fumed silica.

[0007] In the above scheme, the alcohol solvent is selected from ethanol, isopropanol or a mixture thereof, and serves as the main dispersion medium to quickly wet the surface of the cemented carbide green blank, evaporate completely without residue, and does not form a carbon film or contaminate the alloy.

[0008] In the above scheme, the binder phase pull-out agent is selected from one or more of metal oxides, metal hydroxides, metal carbonates, metal nitrates, organometallic salts (acetates, oxalates, etc.), metal nitrides, and metal binder phases, wherein the metal refers to Cr, V, Ti, Ta, Nb, Mo, Mn, Co, Ni, or Fe; the particle size of the binder phase pull-out agent is 0.1 to 10 μm.

[0009] Furthermore, the binder phase pull-out agent is one or more selected from Cr2O3, V2O5, V2O3, MnO2, MnCO3, FeCO3, NiO, NbO2, and metallic Co.

[0010] In the above scheme, the binder phase propellant is selected from one or more of metal carbides, carbon powder, and mixed powders that can react to generate metal carbides, wherein the metal refers to Cr, V, Ti, Ta, Nb, Mo, Mn, Co, Ni or Fe, and the particle size of the binder phase propellant is 0.1 to 10 μm.

[0011] Furthermore, the binder phase promoter is Cr3C2, VC, graphite, Cr7C3, Cr 23 One or more of the following: C6, NbC, TaC, TiC, WC powder, carbon black, organic carbon and its precursor powder, and mixed powders that can react to form metal carbides.

[0012] In the above scheme, the dispersant is selected from at least one of polyethylene glycol, Span series, Tween series, and ammonium polyacrylate, which reduces the surface energy of the powder, improves wetting and dispersibility, and inhibits the agglomeration and sedimentation of high-density particles.

[0013] In the above scheme, the pore-forming agent is selected from one or more of PEG-2000, PEG-4000, and PEG-6000. It decomposes and volatilizes during the drying and low-temperature sintering stages to form continuous through pores, ensuring that gas can be freely discharged.

[0014] In the above scheme, the plasticizer is selected from one or both of glycerol and propylene glycol.

[0015] In the above scheme, the viscosity of the alcohol-based functional gel at 25°C is 2000-8000 mPa·s, and there is no sedimentation or stratification after standing for 72 hours; after drying, it forms a porous interconnected structure and does not form a dense carbon film.

[0016] To achieve the above objectives, the technical solution of the preparation method of the functional gel of the present invention is: a method for preparing the above-mentioned alcohol-based functional gel for gradient property regulation of cemented carbide, characterized by comprising the following steps: (1) Add the alcohol solvent to the mixing tank, turn on the stirring, slowly add the gelling agent, and stir until completely dissolved or evenly dispersed; (2) Add dispersant, pore-forming aid, and plasticizer, and continue stirring for 5-10 minutes until homogeneous; (3) Add the binder phase puller and binder phase propellant powder in steps, stir at high speed and disperse ultrasonically for 10-20 minutes; (4) Adjust the viscosity of the system to 2000-8000 mPa·s, and degas under vacuum for 10 minutes; (5) A uniform and stable alcohol-based functional gel was obtained.

[0017] To achieve the above objectives, the technical solution of the method for redistribution of cemented carbide binder phase of the present invention is as follows: a method for redistribution of cemented carbide binder phase, wherein the above-mentioned functional gel is applied to the surface of green cemented carbide, and after sintering, the binder phase undergoes directional migration to form a gradient hardness structure.

[0018] The alcohol-based functional gel of this invention can simultaneously achieve three major technical effects: high solids content and stable suspension, dry and porous degassing, and precise local coating. Its mechanism of action is as follows: 1. Differences in film-forming mechanisms of alcohol-based systems Traditional water-based organic gels or starch gels, after drying, cause the organic matrix (polysaccharides, proteins, starch, etc.) to carbonize at high temperatures, forming a continuous and dense carbon film. This acts like a "sealing layer" on the surface of the green body, hindering the release of internal gases during sintering and leading to defects such as bubbling, cracking, and porosity. In contrast, this invention uses alcohols as the main solvent (40-70%), with a gelling agent content of only 0.5-10%. After the alcohol solvent evaporates, only a loose three-dimensional framework structure formed by a low content of gelling agent remains, rather than a dense carbon film—gas can freely escape through the gaps in the framework, fundamentally solving the gas blockage problem of dense carbon films.

[0019] 2. Suspension mechanism of three-dimensional gel networks The density of the binder puller and the pusher is as high as 6-15 g / cm³. 3 The density of the granules is much higher than that of the solvent. In traditional suspensions, particles that are temporarily suspended by viscosity will quickly settle under gravity (clearly stratifying within 10 minutes). This invention constructs a weakly thixotropic three-dimensional network structure in an alcohol system using a gelling agent. This physically encapsulates high-density powder particles within the network nodes, forming a "spatial barrier"—the elastic recovery force of the gel network balances the particle gravity, thus achieving no settling or stratification after 72 hours of standing.

[0020] 3. Thixotropic properties enable precise coating. The alcohol-based gel of this invention has significant thixotropic properties: under shear force (during brushing, spraying, or spot coating), the gel network structure is temporarily destroyed, the viscosity decreases, and the fluidity improves, making it easier to coat evenly; after the shear force is removed (when the coating is completed and the area is left to stand), the gel network quickly recovers, the viscosity rises, and the gel no longer flows or spreads, thereby achieving precise spot coating on designated local areas such as the tip, edge, and side of the blade.

[0021] 4. Synergistic degassing of pore-forming agents After the alcohol solvent evaporates, it forms primary pores (skeleton gaps). The pore-forming aid (PEG series) further decomposes and volatilizes during the low-temperature sintering stage of 100-500℃, forming secondary pores (microchannels). The two levels of pores are interconnected to form a continuous pore network, ensuring that the gas inside the green body can be smoothly discharged throughout the sintering process, and eliminating defects such as bubbling and cracks.

[0022] The beneficial effects of this invention include: Compared with the prior art, this invention has the following beneficial effects: (1) The alcohol-based system does not form a dense carbon film during drying and sintering, thus completely solving the problem of exhaust blockage; (2) The total content of functional powder is 20-50%, which can achieve no stratification and no sedimentation after 72 hours of standing; (3) Drying forms a porous and interconnected structure, allowing for smooth air venting of the green body and eliminating bubbling, cracking, and pore defects; (4) It has excellent thixotropic properties, does not flow or spread, and can be precisely applied to areas such as the tip, edge, and side of the blade; (5) It is 100% compatible with existing cemented carbide sintering processes and can directly replace traditional suspensions; (6) The components are simple, the cost is low, and the preparation is convenient, making it suitable for large-scale and stable industrial production. Attached Figure Description

[0023] Figure 1 Comparison of the appearance of the alcohol-based gels prepared in Examples 3 and 4 and after standing for 18 hours; Figure 2 SEM images of the microstructure of the alcohol-based gel membranes after drying in Examples 3 and 4; Figure 3 The image shows the morphology and energy dispersive spectroscopy (EDS) analysis of the gel after drying in Example 4. Figure 4 This is a hardness distribution diagram of the entire cross-section of the tooth head after the gel of Example 4 was coated and sintered on the WC-6%Co alloy ball tooth head. Figure 5 This is a diagram showing the distribution of Cr content in cobalt in the cross-section of a WC-6%Co alloy ball tooth after the gel from Example 4 is coated and sintered, extending from the tooth tip along the central axis inwards. Figure 6 This is a cobalt content distribution diagram of the cross section of a WC-6%Co alloy ball tooth after the gels of Example 2 (drawing agent only) and Example 4 (propelling agent only) are coated and sintered, from the tooth tip along the central axis inward (tooth diameter 9mm, coated tooth tip only). Detailed Implementation

[0024] Example 1 (General Stable Type): Component mass percentage: Isopropanol 52%, Hydroxypropyl cellulose (HPC) 1.2%, Cr2O3 (pulling agent) 20%, Cr3C2 and graphite mixture (1:1) 12%, Dispersant PEG-4000 1.0%, Pore-forming aid PEG-6000 3.0%, Deionized water 10.8%.

[0025] Preparation steps: ① Add isopropanol to the reaction vessel, start stirring, add HPC and stir until a clear solution is obtained; ② Add dispersant PEG-4000 and pore-forming aid PEG-6000, and stir until homogeneous; ③ Add Cr2O3, Cr3C2, and graphite, disperse at high speed, and sonicate for 15 minutes; ④ Vacuum degassing for 10 minutes to obtain a uniform alcohol-based functional gel.

[0026] Performance results: The total content of functional powder is 32%, and there is no stratification or sedimentation after standing at 25℃ for 72 hours; the dry film is porous and breathable; after coating the green body and sintering, there is no bubbling, cracking, or porosity, and the hardness gradient is clear and controllable.

[0027] Example 2 (Carbomer system): Component mass percentage: ethanol 55%, carbomer 980 0.8%, triethanolamine 1.0%, PEG-4000 4%, glycerol 3%, Cr2O3 (pulling agent) 32%, deionized water balance.

[0028] Preparation steps: ① Add deionized water and ethanol to the container, stir at low speed until well mixed, and leave at room temperature until a clear solution is obtained; ② While stirring the alcohol-water mixture at low speed, slowly sprinkle in Carbomer 980 powder while stirring. Seal and let stand for 30-40 minutes to allow it to swell until it is completely transparent and free of small white lumps. ③ Slowly add triethanolamine while stirring at low speed. The system gradually thickens and becomes a uniform, transparent alcohol gel. ④ Add dispersant PEG-4000 and glycerin, and stir until homogeneous; ⑤ While stirring the gel system, slowly add Cr2O3 powder in batches, and stir at high speed for 15-20 minutes after the addition is complete; ⑥ Allow to stand or degas under vacuum for 10-20 minutes to obtain a uniform alcohol-based functional gel.

[0029] Performance results: The total content of functional powder is 32%, and there is no stratification or sedimentation after standing at 25℃ for 72 hours; the dry film is porous and breathable; after coating the green body and sintering, there is no bubbling, cracking, or porosity, and the hardness gradient is clear and controllable.

[0030] Example 2 is an instance where only a binder phase puller is used, but no binder phase pusher is used.

[0031] Example 3 (PEG-free system): Component mass percentage: ethanol 66%, carbomer 980 0.8%, triethanolamine 1.0%, mixture of Cr3C2 and carbon 22%, deionized water balance.

[0032] Preparation steps: ① Add deionized water and ethanol to the container and stir at low speed until well mixed; ② While stirring the alcohol-water mixture at low speed, slowly sprinkle in Carbomer 980 powder while stirring. Seal and let stand for 30-40 minutes to allow it to swell until it is completely transparent and free of small white lumps. ③ Slowly add triethanolamine while stirring at low speed. The system gradually thickens and becomes a uniform, transparent alcohol gel. ④ While stirring the gel system, slowly add the mixture of Cr3C2 and carbon powder in batches, and stir at high speed for 15-20 minutes after the addition is complete; ⑤ Allow to stand or degas under vacuum for 10-20 minutes to obtain a uniform alcohol-based functional gel.

[0033] Performance Results: The freshly prepared alcohol gel had a suitable viscosity, and after standing for 18 hours, no obvious stratification or sedimentation occurred, indicating strong anti-settling ability. A small number of pores were visible under 1000x magnification; these pores are left after alcohol evaporation. Figure 1 and Figure 2 .

[0034] Example 4 (System containing PEG pore-forming agent): Component mass percentage: ethanol 51%, carbomer 980 0.8%, triethanolamine 1.0%, PEG-2000 1%, mixture of Cr3C2 and carbon (propellant) 22%, deionized water balance.

[0035] Preparation steps: ① First, mix and dissolve 10% deionized water with 1% PEG-2000; ② Add the remaining deionized water and ethanol to the container and stir at low speed until well mixed; ③ While stirring the alcohol-water mixture at low speed, slowly sprinkle in Carbomer 980 powder while stirring. Seal and let stand for 30-40 minutes to allow it to swell until it is completely transparent and free of small white lumps. ④ Slowly add triethanolamine while stirring at low speed. The system will gradually thicken and become a uniform, transparent alcohol gel. ⑤ Add the aqueous solution of PEG-2000 and stir until well mixed; ⑥ While stirring the gel system, slowly add the mixture of Cr3C2 and carbon powder in batches, and stir at high speed for 15-20 minutes after the addition is complete; ⑦ Let stand or degas under vacuum for 10-20 minutes to obtain a uniform alcohol-based functional gel.

[0036] Performance results: The dried gel film consisted of loose aggregates, and the aggregates themselves had many pores, see... Figure 1 and Figure 2 In practical use, Example 4 dries quickly, has a uniform thickness, and does not drip after coating. After coating the tip of the WC-6%Co alloy ball tooth, a clear hardness gradient and Cr content gradient can be formed after sintering using conventional processes.

[0037] Figure 3The image shows the morphology after gel drying. To more intuitively and accurately distinguish the carbon particles in the Cr3C2 / carbon mixture powder, carbon particles with a size of 10-200 μm were used. In practical applications, the finer the carbon particles, the more uniform their distribution, resulting in a more uniform coating thickness and a more stable effect. The energy dispersive spectroscopy (EDS) results show that the fine powder particles in the image are Cr3C2, while the larger particles are carbon powder.

[0038] The alcohol-based functional gel of this embodiment is applied to the surface of a green cemented carbide blank. After sintering, the binder phase undergoes directional migration to form a gradient hardness structure. Specifically, it is used for WC-6%Co alloy ball teeth. The hardness distribution across the entire cross-section of the WC-6%Co alloy ball tooth tip after sintering is as follows: Figure 4 As shown, the distribution of Cr content in cobalt along the central axis from the tooth tip in the cross-section is as follows: Figure 5 As shown.

[0039] Example 4 is an instance where only a binder phase pusher is used and no binder phase puller is used.

[0040] Effect verification comparison The alcohol-based functional gel of this invention was compared and verified with a traditional suspension system. The results are shown in the table below: As can be seen from the table above, the alcohol-based functional gel of the present invention is significantly superior to the traditional suspension system in terms of functional powder stability, dry film structure, green body venting, sintering defect control and coating precision. It can effectively solve the technical defects of the prior art such as easy sedimentation, easy flow, poor venting and low coating precision of the suspension.

[0041] Example 5: Component mass percentage: Isopropanol 50%, HPC 1.0%, CrN / Cr2N 16%, Graphite 14%, Dispersant 1.0%, Pore-forming aid 3.0%, Deionized water 15.0%.

[0042] Example 6: Component mass percentage: Isopropanol 50%, Carbomer + Triethanolamine 1.5%, Cr3C2 and Carbon Black mixture 35%, Dispersant 1.0%, PEG 10000 3.0%, Glycerin 3%, Deionized Water 6.5%.

[0043] The functional powder of the present invention can use a binder phase puller alone, a binder phase pusher alone, or a combination of both. When the puller is used alone, unidirectional migration of the binder phase toward the application area can be achieved; when the pusher is used alone, unidirectional migration of the binder phase away from the application area can be achieved.

[0044] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. An alcohol-based functional gel for gradient property regulation of cemented carbide, characterized in that: By weight percentage, it comprises the following components: 40%–70% alcohol solvent, 0.5%–10.0% gelling agent, 0%–50% binder puller, 0%–50% binder promoter, 0.2%–2.0% dispersant, 1%–6% pore-forming aid, 0%–6% plasticizer, and the balance being deionized water, with the deionized water content not exceeding 15%. The total content of the binder puller and the binder pusher is 20% to 50%; the gelling agent is selected from one or more of the following: cellulose ether gelling agents, natural polymer gelling agents, polyethylene oxide gelling agents, polyvinylpyrrolidone gelling agents, carbomer resin gelling agents, and inorganic-organic composite thixotropic agent gelling agents.

2. The alcohol-based functional gel for gradient property regulation of cemented carbide according to claim 1, characterized in that: The cellulose ether gelling agent is selected from one or more of hydroxypropyl methylcellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose; the natural polymer gelling agent is selected from one or more of sodium alginate, guar gum, xanthan gum, and gellan gum; the polyvinylpyrrolidone gelling agent is selected from one or two of polyvinylpyrrolidone K30 and polyvinylpyrrolidone K90; the carbomer resin gelling agent is selected from one or more of carbomer 940, carbomer 980, and carbomer Ultraz, and is used in combination with triethanolamine for neutralization; the inorganic-organic composite thixotropic agent gelling agent is fumed silica.

3. The alcohol-based functional gel for gradient property regulation of cemented carbide according to claim 1, characterized in that: The alcohol solvent is selected from ethanol, isopropanol, or mixtures thereof.

4. The alcohol-based functional gel for gradient property regulation of cemented carbide according to claim 1, characterized in that: The binder phase drawing agent is selected from one or more of the following: metal oxides, metal hydroxides, metal carbonates, metal nitrates, organometallic salts, metal nitrides, and metal binder phases, wherein the metal refers to Cr, V, Ti, Ta, Nb, Mo, Mn, Co, Ni, or Fe; the particle size of the binder phase drawing agent is 0.1–10 μm.

5. The alcohol-based functional gel for gradient property regulation of cemented carbide according to claim 4, characterized in that: The binder phase pull-out agent is one or more of Cr2O3, V2O5, V2O3, MnO2, MnCO3, FeCO3, NiO, NbO2, and metallic Co.

6. The alcohol-based functional gel for gradient property regulation of cemented carbide according to claim 1, characterized in that: The binder phase propellant is selected from one or more of metal carbides, carbon powder, and mixed powders that can react to generate metal carbides, wherein the metal refers to Cr, V, Ti, Ta, Nb, Mo, Mn, Co, Ni or Fe, and the particle size of the binder phase propellant is 0.1 to 10 μm.

7. The alcohol-based functional gel for gradient property regulation of cemented carbide according to claim 6, characterized in that: The binder phase promoter is Cr3C2, VC, graphite, Cr7C3, Cr 23 One or more of the following: C6, NbC, TaC, TiC, WC powder, carbon black, organic carbon and its precursor powder, and mixed powders that can react to form metal carbides.

8. The alcohol-based functional gel for gradient property regulation of cemented carbide according to claim 1, characterized in that: The dispersant is selected from at least one of polyethylene glycol, Span series, Tween series, and ammonium polyacrylate; the pore-forming aid is selected from one or more of PEG-2000, PEG-4000, and PEG-6000; and the plasticizer is selected from one or two of glycerol and propylene glycol.

9. The alcohol-based functional gel for gradient property regulation of cemented carbide according to claim 1, characterized in that, The alcohol-based functional gel has a viscosity of 2000–8000 mPa·s at 25°C, and shows no sedimentation or stratification after standing for 72 hours. After drying, it forms a porous, interconnected structure without forming a dense carbon film.

10. A method for preparing an alcohol-based functional gel for gradient property regulation of cemented carbide as described in any one of claims 1 to 8, characterized in that: Includes the following steps: (1) Add the alcohol solvent to the mixing tank, turn on the stirring, slowly add the gelling agent, and stir until completely dissolved or evenly dispersed; (2) Add dispersant, pore-forming aid, and plasticizer, and continue stirring for 5-10 minutes until homogeneous; (3) Add the binder phase puller and binder phase propellant powder in steps, stir at high speed and disperse ultrasonically for 10-20 minutes; (4) Adjust the viscosity of the system to 2000-8000 mPa·s, and degas under vacuum for 10 minutes; (5) A uniform and stable alcohol-based functional gel was obtained.

11. A method for redistributing the binder phase in a cemented carbide alloy, characterized in that: The functional gel as described in any one of claims 1 to 9 is applied to the surface of a green cemented carbide, and after sintering, the binder phase undergoes directional migration to form a gradient hardness structure.