A method and apparatus for preparing high-purity boron
By nesting large-sized boron oxide blocks with magnesium particles, using a stepped temperature-programmed reduction reaction and a multi-step non-oxidizing purification process, the problems of violent reaction, easy boiling, and impurity introduction in the magnesothermic reduction method were solved, the purity of amorphous boron powder was improved, and the stable preparation of high-purity boron was achieved.
Patent Information
- Application Number
- CN202611430210.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-17
AI Technical Summary
The existing magnesium thermal reduction method for preparing boron powder has problems such as violent reaction and easy boiling, easy introduction of impurities, and easy occurrence of secondary oxidation during post-processing, resulting in low product purity.
Large-sized boron oxide blocks and magnesium particles are nested together, combined with a stepped temperature-programmed reduction reaction and a multi-step non-oxidizing purification process, including initial acid leaching with hydrochloric acid solution, deep acid leaching with hydrofluoric acid, and ultrasonic washing with hot water. A pyrolytic boron nitride crucible is used to provide a sealing structure and argon protection to avoid high-temperature boiling and the introduction of impurities.
This method ensures the smooth progress of the magnesium thermal reduction reaction, improves the purity of amorphous boron powder, avoids secondary oxidation, and guarantees the preparation of high-purity boron powder.
Smart Images

Figure CN123105671A_ABST
Abstract
Description
Technical Field
[0002] This invention relates to the field of inorganic chemical technology, specifically to a method and apparatus for preparing high-purity boron. Background Technology
[0004] High-purity amorphous boron powder has significant applications in many cutting-edge industries. Currently, the magnesothermic reduction method is commonly used in industry to prepare boron powder, which utilizes elemental magnesium to reduce boron oxide at high temperatures. Traditional magnesothermic reduction processes typically involve directly mixing boron oxide powder and magnesium powder before heating. However, this powder mixing method results in an excessively large contact area between the materials. When the temperature reaches the reduction reaction trigger point, the reaction occurs rapidly and violently, releasing a large amount of heat. This easily causes boiling and splashing of the reactants, which not only reduces the reaction yield but also compromises the stability of the synthesized system.
[0005] Meanwhile, during the high-temperature reduction process, conventional reaction vessels easily introduce non-metallic or transition metal impurities such as silicon into the reactants at high temperatures, resulting in low initial purity of the crude product. In the subsequent purification stage, due to the high chemical reactivity of the newly generated amorphous boron powder, traditional acid washing purification processes often lack strict control over the acid composition and non-oxidizing environment. This leads to easy secondary oxidation of elemental boron during impurity removal, generating low-valence boron oxides that are difficult to remove through conventional washing. These problems—runaway high-temperature reaction, introduction of container impurities, and secondary oxidation during purification—combine to make it difficult for existing preparation processes to consistently obtain high-purity amorphous boron powder that meets the requirements. Summary of the Invention
[0007] To address the shortcomings of existing technologies, this invention provides a method and apparatus for preparing high-purity boron, which solves the problems of violent reaction and easy boiling during the preparation of boron powder by the existing magnesothermic reduction method, easy introduction of impurities, and easy occurrence of secondary oxidation during post-processing, resulting in low product purity.
[0008] To achieve the above objectives, the present invention provides a method for preparing high-purity boron, employing the following technical solution: Firstly, the present invention provides a method for preparing high-purity boron, using the following technical solution:
[0009] A method for preparing high-purity boron includes the following steps:
[0010] According to the ratio, high-purity magnesium particles and blocky high-purity boron oxide are sequentially loaded into a pretreated pyrolytic boron nitride crucible, so that the blocky high-purity boron oxide is completely located inside the high-purity magnesium particles. The pyrolytic boron nitride crucible is then sealed to obtain the reaction system.
[0011] The reaction system was placed under an inert atmosphere and subjected to a step-by-step temperature-programmed reduction reaction. After the first stage of temperature increase, the temperature was held constant. After the second stage of temperature increase, the temperature was held constant, and then cooled to room temperature to obtain the reaction product.
[0012] The cooled reaction product was mechanically crushed, and then subjected to initial acid leaching with hydrochloric acid solution, followed by deep acid leaching with a mixture of electronic-grade high-purity hydrochloric acid solution containing hydrofluoric acid or electronic-grade high-purity hydrochloric acid solution. After being ultrasonically washed with hot water until neutral, it was vacuum dried to obtain high-purity amorphous boron powder.
[0013] By adopting the above technical solution, due to the use of large-sized boron oxide blocks and magnesium particles nested together, liquid-solid interface penetration, and multi-step non-oxidizing purification, the effect of suppressing high-temperature boiling and improving the purity of amorphous boron is achieved.
[0014] The specific reaction mechanism of the reduction reaction stage in this invention is as follows:
[0015] During the first stage of heating and temperature control, the furnace temperature is maintained above the melting point of boron oxide and below the temperature at which the magnesian thermal reduction reaction occurs most violently. Solid, blocky high-purity boron oxide gradually melts into a liquid state from the surface inwards, penetrating downwards under gravity and capillary action to uniformly coat the surface of the bottom and surrounding high-purity magnesium particles, forming a liquid-solid contact reaction interface. This structure hinders the rapid diffusion of ions, avoiding the instantaneous overheating and reactant splashing / boiling that can occur in traditional powder mixing systems due to excessively rapid local reactions.
[0016] During the second stage of heating and isothermal control, the main reaction is triggered: B₂O₃ + 3Mg → 2B + 3MgO. Controlling the temperature during this stage ensures the complete completion of the magnesothermic reduction reaction. The pyrolytic boron nitride crucible exhibits chemical stability at high temperatures, and its closed internal cavity prevents the physical migration of external non-metallic and transition metal impurities into the reaction system.
[0017] The specific reaction mechanism of the post-treatment stage in this invention is as follows:
[0018] The initial acid leaching utilizes hydrochloric acid solution to extensively remove the byproduct magnesium oxide and excess elemental magnesium; the chemical reactions are: MgO + 2HCl → MgCl2 + H2O, and Mg + 2HCl → MgCl2 + H2↑. The deep acid leaching uses a mixed hydrochloric acid solution containing hydrofluoric acid to further dissolve deep-seated metallic impurity particles and low-valence boron oxides. This composite acid leaching system is non-oxidizing, preventing secondary oxidation of the newly formed highly reactive elemental boron during impurity removal. Finally, residual salts are removed by ultrasonic treatment with hot water, followed by vacuum drying to complete the preparation of high-purity amorphous boron powder.
[0019] Preferably, the theoretical stoichiometric molar ratio of boron oxide to magnesium in the reduction reaction is 1:3 as the basis for weighing and batching, and the actual added molar amount of high-purity magnesium particles is 3% to 15% in excess of the theoretical requirement; the characteristic size of the blocky high-purity boron oxide is 5 to 50 mm; the high-purity magnesium particles are irregular particles, and the particle size of the high-purity magnesium particles is 0.5 to 5 mm.
[0020] By adopting the above technical solution, excess magnesium can compensate for the trace amount of magnesium vapor volatilization loss at high temperatures, ensuring that boron oxide can be fully reduced and reducing the formation of low-valence boron oxides that are difficult to remove by acid washing. The differentiated size setting ensures that the gaps between magnesium particles are large enough to accommodate the liquid phase penetration of boron oxide during melting, preventing liquid boron oxide from directly contacting and adhering to the inner wall of the crucible.
[0021] Preferably, before loading the pyrolytic boron nitride crucible, the pyrolytic boron nitride crucible and the blocky high-purity boron oxide and high-purity magnesium particles used as reaction raw materials are pretreated as follows: the pyrolytic boron nitride crucible is completely immersed in aqua regia for 1-2 hours, then rinsed continuously with deionized water 3-5 times, and dried in a drying oven at 100°C for later use; the blocky high-purity boron oxide is placed in a vacuum drying oven and dried at 110-130°C for 1.5-3 hours, then removed and sealed; the high-purity magnesium particles are placed in a vacuum drying oven and dried at 70-90°C for 0.5-2 hours, then removed and sealed.
[0022] By employing the above technical solutions, aqua regia immersion removes the metal deposits on the surface of the crucible. Vacuum drying removes the moisture adsorbed inside the raw materials, preventing free moisture from reacting with magnesium at high temperatures to form magnesium oxide, thus avoiding additional consumption of reducing agent. It also eliminates pressure fluctuations inside the furnace caused by rapid moisture vaporization and side reaction gas production.
[0023] Preferably, high-purity magnesium particles and blocky high-purity boron oxide are sequentially loaded into a pretreated pyrolytic boron nitride crucible. Specifically, a layer of high-purity magnesium particles with a thickness of 2-5 mm is laid flat at the bottom of the pyrolytic boron nitride crucible; the blocky high-purity boron oxide is placed in the center of the bottom layer of high-purity magnesium particles; the remaining high-purity magnesium particles are poured into the pyrolytic boron nitride crucible, completely filling the gap between the blocky high-purity boron oxide and the inner wall of the pyrolytic boron nitride crucible and covering the top of the blocky high-purity boron oxide.
[0024] By adopting the above technical solution, it is ensured that there is a sufficient bed of magnesium particles at the bottom as a buffer and reaction carrier during the melting and downward flow of the blocky boron oxide, so that the solid-liquid interface reaction can proceed stably.
[0025] Preferably, before placing the reaction system under an inert atmosphere for a step-by-step temperature-programmed reduction reaction, the following operations are also included: connecting the inlet of the quartz tube to an argon gas source, opening the tail gas outlet, and introducing argon gas into the quartz tube at a flow rate of 400-600 mL / min for 10-15 min; placing the sealed pyrolytic boron nitride crucible in the quartz boat and pushing it entirely into the quartz tube; after sealing the system, continuing to introduce argon gas at a flow rate of 400-600 mL / min for 20-30 min.
[0026] By adopting the above technical solution, high-flow-rate argon cleaning can fully remove residual air from inside the quartz tube, providing a pure background atmosphere that isolates oxygen and nitrogen for the high-temperature reduction reaction.
[0027] Preferred process parameters for the stepped temperature-programmed reduction reaction are as follows: the argon flow rate in the quartz tube is reduced to 50–100 mL / min to maintain a slightly positive pressure in the furnace cavity; the tubular furnace heating program is started, and in the first stage, the furnace temperature is increased from room temperature to 450–550°C at a heating rate of 10–15°C / min, and held at 450–550°C for 30–60 min; in the second stage, the furnace temperature is increased to 800–1000°C at a heating rate of 10–15°C / min, and held at 800–1000°C for 1.5–3 h.
[0028] By adopting the above technical solution, the slightly positive pressure state can prevent external air from seeping back into the furnace cavity. The isothermal platform of 450 to 550°C matches the melting point of boron oxide, providing sufficient time for solid-liquid interface reconstruction; the isothermal platform of 800 to 1000°C ensures that the reduction reaction has sufficient kinetic rate, while avoiding boron powder crystallization growth and deep solid solution of impurities caused by excessive temperature, thereby obtaining products with amorphous morphology.
[0029] Preferably, the specific operation of the initial acid leaching is as follows: the reaction product after mechanical crushing is added to an excess of hydrochloric acid solution with a concentration of 2-4 mol / L, and the reaction is mechanically stirred at room temperature for 2-4 hours. After the reaction stops, the solid phase of the initial filter residue is separated by vacuum filtration.
[0030] By adopting the above technical solution, excess hydrochloric acid is used to stably remove large amounts of magnesium oxide matrix at room temperature, exposing the porous framework structure of the reaction product and providing a physical diffusion channel for subsequent deep purification.
[0031] Preferably, the specific steps of deep acid leaching are as follows: the initial filter residue is transferred to a polytetrafluoroethylene beaker, an electronic grade high-purity hydrochloric acid solution or an electronic grade high-purity hydrochloric acid mixed solution containing no more than 5% hydrofluoric acid by mass is added, and the mixture is soaked and slowly stirred for 1 to 2 hours under water bath heating conditions of 30 to 50°C. After the process is completed, the mixture is filtered again to obtain the solid powder after deep acid leaching.
[0032] By adopting the above technical solution, the micro-heating environment combined with the strong complexing effect of fluoride ions can specifically dissolve trace amounts of insoluble metal oxide impurities, thereby improving the intrinsic purity of the material while ensuring boron yield.
[0033] Preferably, the specific steps of hot water ultrasonic washing and vacuum drying are as follows: the solid powder after deep acid leaching is added to deionized water at 60-80°C, placed in an ultrasonic cleaner for ultrasonic oscillation for 10-20 minutes, filtered, and the hot water ultrasonic washing step is repeated 3-5 times until the pH value of the filtrate is neutral; the washed powder is placed in a vacuum drying oven and dried at 80-100°C for 2-6 hours until the powder quality is constant.
[0034] By employing the above technical solution, the ultrasonic cavitation effect disrupts the residual liquid film within the micropores of the powder, and combined with the diffusivity of hot water, removes adhering acid and soluble chlorides. Vacuum drying isolates external oxygen, preventing surface oxidation of the purified high-purity boron powder, which has a large specific surface area, during the heating and dehydration process.
[0035] Secondly, the present invention provides an apparatus for preparing high-purity boron, which adopts the following technical solution:
[0036] An apparatus for preparing high-purity boron includes: a quartz tube having an inlet and an outlet; a quartz boat disposed inside the quartz tube; and a pyrolytic boron nitride crucible placed inside the quartz boat, the pyrolytic boron nitride crucible having a sealed structure, the interior of the pyrolytic boron nitride crucible being used to contain bulk high-purity boron oxide and high-purity magnesium particles.
[0037] By adopting the above technical solution, the quartz tube and quartz boat form a large atmosphere protective chamber that isolates the external environment. The internal pyrolytic boron nitride crucible does not react with the boron and magnesium in the material at high temperatures. Its sealed structure can confine the magnesium vapor within the reaction area to maintain partial pressure, while preventing the external quartz tube from releasing silicon impurities into the interior at high temperatures. This dual-space isolation ensures the purity of the final boron powder product.
[0038] This invention provides a method and apparatus for preparing high-purity boron. It has the following beneficial effects:
[0039] 1. This invention completely embeds blocky boron oxide inside magnesium particles and uses a stepped temperature program to allow liquid boron oxide to penetrate and coat the surface of solid magnesium particles before the main reaction occurs. This pre-constructed liquid-solid interface restricts the rapid diffusion of ions, solving the problem of high-temperature boiling caused by excessively rapid local reactions due to direct mixing of traditional powder materials, and making the magnesium thermal reduction reaction process more stable.
[0040] 2. This invention employs a post-treatment process combining multi-step non-oxidizing composite acid leaching with hot water ultrasonic washing. The stepwise washing with hydrochloric acid and fluorine-containing mixed acids sequentially removes bulk magnesium oxide byproducts and deep-seated insoluble metal impurities. The non-oxidizing acid environment and the final vacuum drying step effectively prevent secondary oxidation of highly active amorphous boron powder during the purification and heating dehydration stages, thereby improving the intrinsic purity of the boron powder product.
[0041] 3. This invention uses a pyrolytic boron nitride crucible with a sealed structure and an outer quartz tube filled with argon gas to form a double protection system. Pyrolytic boron nitride does not undergo side reactions with boron and magnesium at high temperatures. Its sealed inner cavity maintains the local magnesium vapor partial pressure to ensure the complete reduction reaction, while physically preventing the migration of silicon and other environmental impurities released by the outer quartz tube at high temperatures to the reactants, thus ensuring the cleanliness of the synthesis environment from the equipment level. Attached Figure Description
[0043] Figure 1 This is a schematic diagram of the device structure of the present invention;
[0044] Figure 2 These are schematic diagrams of the gas pressure fluctuation curves during the heating process of various embodiments and comparative examples of the present invention;
[0045] Figure 3 These are schematic diagrams of the X-ray diffraction patterns of the final products of various embodiments and comparative examples of the present invention;
[0046] Figure 4 This is a schematic diagram showing the biaxial distribution trend of target product yield and splash loss in various embodiments and comparative examples of the present invention;
[0047] Figure 5 This is a logarithmic diagram showing the distribution of trace non-metallic and metallic impurities in the final products of each reaction system of the present invention;
[0048] Figure 6 This is a schematic diagram showing the depth profile distribution of oxygen content on the surface and inside of the final products of each system in this invention.
[0049] Among them, 1. Quartz tube; 2. Air inlet; 3. Exhaust outlet; 4. Quartz boat; 5. Pyrolytic boron nitride crucible. Detailed Implementation
[0051] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0052] See attached document Figure 1 The present invention provides an apparatus for preparing high-purity boron, comprising a quartz tube 1, wherein the quartz tube 1 is provided with an air inlet 2 and an exhaust outlet 3;
[0053] Quartz boat 4 is installed inside quartz tube 1;
[0054] The pyrolytic boron nitride crucible 5 is placed inside the quartz boat 4. The pyrolytic boron nitride crucible 5 has a sealed structure, and its interior is used to contain bulk high-purity boron oxide and high-purity magnesium particles.
[0055] Preparation Example 1:
[0056] This preparation example provides a method for preparing a reaction system for preparing high-purity boron, including the following steps:
[0057] Pretreatment stage: The pyrolytic boron nitride crucible 5 was completely immersed in aqua regia for 1 hour, then rinsed three times with deionized water and dried in a drying oven at 100°C for later use. High-purity boron oxide lumps with a characteristic size of 20 mm were selected and dried in a vacuum drying oven at 120°C for 2 hours, then removed and sealed. Irregular high-purity magnesium particles with a particle size of 2 mm were selected and dried in a vacuum drying oven at 80°C for 1 hour, then removed and sealed. The above materials were transferred to an argon-filled glove box for storage.
[0058] Loading stage: Weighing and batching are based on the theoretical stoichiometric ratio (molar ratio 1:3) for the reduction reaction of boron oxide and magnesium, with the actual added molar amount of high-purity magnesium particles exceeding the theoretical requirement by 6%. Inside the glove box, a layer of high-purity magnesium particles with a thickness of 3 mm is first laid flat at the bottom of the pyrolytic boron nitride crucible 5; blocky high-purity boron oxide is placed in the center of the bottom layer of high-purity magnesium particles; the remaining high-purity magnesium particles are poured into the pyrolytic boron nitride crucible 5, completely filling the gap between the blocky high-purity boron oxide and the inner wall of the pyrolytic boron nitride crucible 5 and covering the top of the blocky high-purity boron oxide, and the pyrolytic boron nitride crucible 5 is sealed.
[0059] Atmosphere replacement: Connect the inlet 2 of quartz tube 1 to an argon gas source and open the outlet 3. Introduce argon gas into quartz tube 1 at a flow rate of 500 mL / min for 10 min. Place the sealed pyrolytic boron nitride crucible 5 inside the quartz boat 4 and push it entirely into quartz tube 1. After sealing the system, continue to introduce argon gas at a flow rate of 500 mL / min for 20 min.
[0060] Preparation Example 2:
[0061] This preparation example provides a method for preparing a reaction system for preparing high-purity boron, including the following steps:
[0062] Pretreatment stage: The pyrolytic boron nitride crucible 5 was completely immersed in aqua regia for 1 hour, then rinsed three times with deionized water and dried in a drying oven at 100°C for later use. Blocky high-purity boron oxide with a characteristic size of 5 mm was selected and dried in a vacuum drying oven at 110°C for 1.5 hours, then removed and sealed. Irregular high-purity magnesium particles with a particle size of 0.5 mm were selected and dried in a vacuum drying oven at 70°C for 0.5 hours, then removed and sealed. The above materials were transferred to an argon-filled glove box for storage.
[0063] Loading stage: Weighing and batching are based on the theoretical stoichiometric molar ratio of 1:3 for the reduction reaction of boron oxide and magnesium, with the actual added molar amount of high-purity magnesium particles exceeding the theoretical requirement by 3%. Inside the glove box, a layer of high-purity magnesium particles with a thickness of 2 mm is first laid flat at the bottom of the pyrolytic boron nitride crucible 5; blocky high-purity boron oxide is placed in the center of the bottom layer of high-purity magnesium particles; the remaining high-purity magnesium particles are poured into the pyrolytic boron nitride crucible 5, completely filling the gap between the blocky high-purity boron oxide and the inner wall of the pyrolytic boron nitride crucible 5 and covering the top of the blocky high-purity boron oxide, and the pyrolytic boron nitride crucible 5 is sealed.
[0064] Atmosphere replacement: Connect the inlet 2 of quartz tube 1 to an argon gas source and open the outlet 3. Introduce argon gas into quartz tube 1 at a flow rate of 400 mL / min for 10 min. Place the sealed pyrolytic boron nitride crucible 5 inside the quartz boat 4 and push the entire crucible into quartz tube 1. After sealing the system, continue to introduce argon gas at a flow rate of 400 mL / min for 20 min.
[0065] Preparation Example 3:
[0066] This preparation example provides a method for preparing a reaction system for preparing high-purity boron, including the following steps:
[0067] Pretreatment stage: The pyrolytic boron nitride crucible 5 was completely immersed in aqua regia for 2 hours, then rinsed five times with deionized water and dried in a drying oven at 100°C for later use. Blocky high-purity boron oxide with a characteristic size of 50 mm was selected and dried in a vacuum drying oven at 130°C for 3 hours, then removed and sealed. Irregular high-purity magnesium particles with a particle size of 5 mm were selected and dried in a vacuum drying oven at 90°C for 2 hours, then removed and sealed. The above materials were transferred to an argon-filled glove box for storage.
[0068] Loading stage: Weighing and batching are based on the theoretical stoichiometric molar ratio of 1:3 for the reduction reaction of boron oxide and magnesium, with the actual added molar amount of high-purity magnesium particles exceeding the theoretical requirement by 15%. Inside the glove box, a layer of high-purity magnesium particles with a thickness of 5 mm is first laid flat at the bottom of the pyrolytic boron nitride crucible 5; blocky high-purity boron oxide is placed in the center of the bottom layer of high-purity magnesium particles; the remaining high-purity magnesium particles are poured into the pyrolytic boron nitride crucible 5, completely filling the gap between the blocky high-purity boron oxide and the inner wall of the pyrolytic boron nitride crucible 5 and covering the top of the blocky high-purity boron oxide, and the pyrolytic boron nitride crucible 5 is sealed.
[0069] Atmosphere replacement: Connect the inlet 2 of quartz tube 1 to an argon gas source and open the outlet 3. Introduce argon gas into quartz tube 1 at a flow rate of 600 mL / min for 15 min. Place the sealed pyrolytic boron nitride crucible 5 inside the quartz boat 4 and push it entirely into quartz tube 1. After sealing the system, continue to introduce argon gas at a flow rate of 600 mL / min for 30 min.
[0070] Example 1:
[0071] This embodiment provides a method for preparing high-purity boron, including the following steps:
[0072] A stepped temperature-programmed reduction reaction was carried out using the atmosphere-purified reaction system obtained in Preparation Example 1: the argon flow rate in quartz tube 1 was reduced to 75 mL / min to maintain a slightly positive pressure in the furnace cavity. The tube furnace heating program was started. In the first stage, the furnace temperature was increased from room temperature to 500°C at a heating rate of 14°C / min and held at this temperature for 45 min. In the second stage, the furnace temperature was increased to 900°C at a heating rate of 14°C / min and held at 900°C for 2 h. After the holding period, the heating power was cut off, and the pyrolytic boron nitride crucible 5 was allowed to cool naturally to room temperature with the furnace while argon gas was continuously introduced at a rate of 75 mL / min.
[0073] Multi-step non-oxidative composite post-treatment: The cooled reaction product was mechanically crushed and added to an excess of 3 mol / L hydrochloric acid solution. The mixture was mechanically stirred at room temperature for 3 hours. After the reaction stopped, the solid residue was separated by vacuum filtration. The initial residue was transferred to a polytetrafluoroethylene beaker and a mixed solution of electronic-grade high-purity hydrochloric acid containing 3% hydrofluoric acid was added. The mixture was soaked in a water bath at 40°C and slowly stirred for 1.5 hours. After the reaction, it was filtered again. The solid powder after deep acid leaching was added to deionized water at 70°C and ultrasonically oscillated for 15 minutes in an ultrasonic cleaner. After filtration, this hot water ultrasonic washing step was repeated 4 times until the pH value of the filtrate was neutral. The finally washed powder was placed in a vacuum drying oven and dried at 90°C for 4 hours until the powder mass was constant, resulting in high-purity amorphous boron powder.
[0074] Example 2:
[0075] This embodiment provides a method for preparing high-purity boron, including the following steps:
[0076] A stepped temperature-programmed reduction reaction was carried out using the atmosphere-purified reaction system obtained in Preparation Example 2: the argon flow rate in quartz tube 1 was reduced to 50 mL / min to maintain a slightly positive pressure in the furnace cavity. The tube furnace heating program was started. In the first stage, the furnace temperature was increased from room temperature to 450°C at a heating rate of 10°C / min and held at this temperature for 30 min. In the second stage, the furnace temperature was increased to 800°C at a heating rate of 10°C / min and held at 800°C for 1.5 h. After the holding period, the heating power was cut off, and the pyrolytic boron nitride crucible 5 was allowed to cool naturally to room temperature with the furnace while argon gas was continuously supplied at a rate of 50 mL / min.
[0077] Multi-step non-oxidative composite post-treatment: The cooled reaction product was mechanically crushed and added to an excess of 2 mol / L hydrochloric acid solution. The mixture was mechanically stirred at room temperature for 2 hours. After the reaction stopped, the solid residue was separated by vacuum filtration. The initial residue was transferred to a polytetrafluoroethylene beaker, and electronic-grade high-purity hydrochloric acid solution was added. The mixture was soaked in a water bath at 30°C and slowly stirred for 1 hour. After the reaction, it was filtered again. The deeply acid-soaked solid powder was added to deionized water at 60°C and ultrasonically oscillated for 10 minutes in an ultrasonic cleaner. After filtration, this hot water ultrasonic washing step was repeated 3 times until the pH value of the filtrate was neutral. The finally washed powder was placed in a vacuum drying oven and dried at 80°C for 2 hours until the powder mass was constant, resulting in high-purity amorphous boron powder.
[0078] Example 3:
[0079] This embodiment provides a method for preparing high-purity boron, including the following steps:
[0080] A step-temperature programmed reduction reaction was carried out using the reaction system obtained in Preparation Example 3 after complete atmosphere replacement:
[0081] The argon flow rate in quartz tube 1 was reduced to 100 mL / min to maintain a slightly positive pressure within the furnace cavity. The tubular furnace heating program was started. In the first stage, the furnace temperature was increased from room temperature to 550°C at a heating rate of 15°C / min and held at this temperature for 60 min. In the second stage, the furnace temperature was increased to 1000°C at a heating rate of 15°C / min and held at 1000°C for 3 h. After the holding period, the heating power was cut off, and the pyrolytic boron nitride crucible 5 was allowed to cool naturally to room temperature with the furnace while continuously supplying argon at a rate of 100 mL / min.
[0082] Multi-step non-oxidative composite post-treatment: The cooled reaction product was mechanically crushed and added to an excess of 4 mol / L hydrochloric acid solution. The mixture was mechanically stirred at room temperature for 4 hours. After the reaction stopped, the solid residue was separated by vacuum filtration. The initial residue was transferred to a polytetrafluoroethylene beaker and a mixed solution of electronic-grade high-purity hydrochloric acid containing 5% hydrofluoric acid was added. The mixture was soaked in a water bath at 50°C and slowly stirred for 2 hours. After the reaction, it was filtered again. The solid powder after deep acid leaching was added to deionized water at 80°C and ultrasonically oscillated for 20 minutes in an ultrasonic cleaner. After filtration, this hot water ultrasonic washing step was repeated 5 times until the pH value of the filtrate was neutral. The finally washed powder was placed in a vacuum drying oven and dried at 100°C for 6 hours until the powder mass was constant, resulting in high-purity amorphous boron powder.
[0083] Comparative Example 1:
[0084] Compared with Example 1, the difference is that in the pretreatment and loading stages, high-purity boron oxide powder is used instead of blocky high-purity boron oxide, and high-purity magnesium powder is used instead of high-purity magnesium particles. The two are mixed evenly and then directly filled into the pyrolytic boron nitride crucible 5. The sandwich-embedded loading structure is not used. All other aspects are the same.
[0085] Comparative Example 2:
[0086] Compared with Example 1, the difference is that in the stepped temperature-programmed reduction reaction stage, the first stage of heating and constant temperature holding is cancelled, and the furnace temperature is directly raised from room temperature to 900°C at a heating rate of 14°C / min, and then held at 900°C for 2 hours. All other aspects are the same.
[0087] Comparative Example 3:
[0088] Compared with Example 1, the difference is that in the deep acid leaching step of the multi-step non-oxidizing composite post-treatment, the electronic-grade high-purity hydrochloric acid mixed solution containing 3% hydrofluoric acid by mass is replaced with an equal volume of superior-grade pure nitric acid aqueous solution with a mass fraction of 65% to 68%, and the rest are the same.
[0089] Comparative Example 4:
[0090] Compared with Example 1, the difference is that a conventional high-purity quartz crucible is used instead of the pyrolytic boron nitride crucible 5 for the reaction vessel, and the quartz crucible is only washed and dried with water during the pretreatment stage, without soaking in aqua regia. All other aspects are the same.
[0091] Test Example 1:
[0092] The reaction systems in Examples 1 to 3 and Comparative Examples 1 to 2 that had been loaded and placed in quartz tube 1 were selected as test objects, and thermodynamic data were collected in real time without changing the original air intake parameters.
[0093] A high-precision K-type surface thermocouple is tightly attached to the center of the quartz tube wall corresponding to the constant temperature heating zone outside the quartz tube 1 to monitor the actual transient temperature fluctuations of the system; at the same time, a micro differential pressure sensor is connected in series in the exhaust pipe of the tail gas port 3 of the quartz tube 1 to monitor the dynamic changes in the pressure inside the furnace cavity.
[0094] The tubular quartz reactor was started strictly according to the heating program set in each embodiment and comparative example. The actual tube wall temperature and cavity gas pressure were recorded synchronously throughout the entire heating and isothermal process using a multi-channel data acquisition instrument at a sampling frequency of 1Hz.
[0095] After the experiment, the monitoring data of the entire process was exported, the maximum difference between the actual monitored temperature and the program set temperature at each stage was calculated and defined as the temperature jump amplitude, and the peak pressure change during the entire reaction cycle was extracted.
[0096] Table 1. Thermodynamic and pressure fluctuation monitoring data for each embodiment and comparative example
[0097] Test object The magnitude of the highest temperature jump in the first stage (°C) The magnitude of the highest temperature jump in the second stage (°C) Peak pressure change of the reaction system (kPa) Example 1 1.27 2.54 0.42 Example 2 0.81 1.93 0.31 Example 3 1.62 3.28 0.58 Comparative Example 1 not applicable 145.62 18.25 Comparative Example 2 not applicable 58.37 4.12
[0098] See attached document Figure 2 , Figure 2 The transient change of internal air pressure of quartz tube 1 over time during programmed heating is shown in the figure. The blue line represents Example 1, the green line represents Example 2, the cyan line represents Example 3, the red line represents Comparative Example 1, and the magenta line represents Comparative Example 2.
[0099] According to Table 1 and Figure 2 The data shows that the stepped heating combined with the block embedding process of this invention has a controlling effect on the reaction process. In Examples 1 to 3, the temperature rise in both stages of the heating process was within 3.5°C, the maximum change in the overall system pressure was 0.58 kPa, and the test curves showed gentle fluctuations. This indicates that the first-stage heat preservation process melts and infiltrates the large boron oxide blocks, forming a liquid-solid interface on the surface of the magnesium particles, which limits the ion diffusion rate and allows the magnesium thermal reduction process to release heat smoothly.
[0100] In contrast, in Comparative Example 1, which used direct powder mixing, the system temperature suddenly rose by 145.62℃ during the reaction, and the pressure change at the exhaust end reached 18.25 kPa. This rapid gas expansion and exothermic reaction easily led to material splashing. In Comparative Example 2, because the first-stage heat preservation and melting coating was not performed before direct heating, a reduction reaction occurred at local solid-phase contact points, accumulating heat and causing significant temperature and pressure fluctuations. The above test data indicate that the raw material morphology design and multi-stage programmed heating of this invention can avoid thermal runaway during the magnesian reduction process.
[0101] Test Example 2:
[0102] The final solid powders from Examples 1 to 3, Comparative Examples 2 and 3, which underwent multiple non-oxidative composite post-treatments and were completely dried, were collected as test subjects.
[0103] Using an agate mortar and pestle, grind each group of test samples until there are no obvious visible particles. Weigh about 0.5 grams of the ground powder, spread it evenly and press it onto the glass sample stage, ensuring that the sample surface is flat and flush with the edge of the sample stage.
[0104] The compacted powder sample was subjected to wide-angle qualitative scanning using an X-ray diffractometer. The X-ray source was a Cu target Kα radiation, and the working tube voltage was set to 40kV and the tube current was set to 40mA.
[0105] The 2θ angle range of the scan was set to 10° to 80°, the scan step size was set to 0.02°, the continuous scan rate was maintained at 5° / min, and the data acquisition process was carried out under ambient temperature and atmospheric conditions.
[0106] The raw diffraction data output by the instrument is exported, the background baseline noise caused by the instrument and the environment is deducted, and the peak position and relative intensity are compared and calculated with the standard powder diffraction card.
[0107] Table 2. Summary of X-ray diffraction characteristic peak data of the final products of each reaction system
[0108] Test object The center position of the main broadened diffraction peak (2θ) Determination of the detection status of impurity sharp peaks Relative crystallinity estimation (%) Example 1 22.34° No obvious impurity peaks were detected. 2.15 Example 2 22.18° No obvious impurity peaks were detected. 2.41 Example 3 22.56° Very faint background undulations 3.62 Comparative Example 2 22.25° <![CDATA[Significant characteristic peaks of MgO and B2O3 are detected]]> 14.28 Comparative Example 3 22.41° <![CDATA[Significant characteristic peaks of H3BO3 are detected]]> 9.57
[0109] See attached document Figure 3 , Figure 3 The diffraction intensity distribution of boron powder obtained under five different preparation parameters was recorded after wide-angle scanning. The curves in the figure were shifted equidistantly in the vertical direction for easy comparison and observation. From top to bottom, they are Example 1 (blue curve), Example 2 (green curve), Example 3 (cyan curve), Comparative Example 2 (magenta curve), and Comparative Example 3 (red curve).
[0110] Based on the data in Table 2 and Figure 3 The high-purity products prepared in the examples exhibited amorphous characteristics. In the diffraction patterns of all examples, only a broadened diffraction peak was observed near 2θ = 22°, a characteristic peak of amorphous boron. The diffraction baselines of Examples 1 and 2 were smooth, with no obvious high-frequency sharp peaks detected, and their relative crystallinity was less than 2.5%, indicating that the solid byproduct magnesium oxide in the reaction system had been effectively removed by the non-oxidizing acid leaching process. In Example 3, after isothermal holding at the upper limit of the temperature gradient, the full width at half maximum (FWHM) of the broadened peak slightly narrowed, and the relative crystallinity increased to 3.62%, indicating that the higher thermal energy caused a slight local short-range ordered rearrangement of the amorphous structure, but it still met the standards for high-purity amorphous boron powder.
[0111] Comparative Example 2, lacking the buffering and coating process of the first stage, exhibited an excessively rapid local reaction rate, leading to uneven spatial distribution of the magnesia reduction reaction. Its diffraction pattern showed, in addition to the broad peak of amorphous boron, distinct characteristic diffraction peaks of magnesium oxide appeared at 42.9° and 62.3°, and characteristic peaks of unreacted boron oxide were also detected near 27.8°. This indicates that the high-temperature melt generated by the vigorous reaction encapsulates some byproducts, forming dense agglomerates, making it impossible for subsequent mechanical crushing and acid washing processes to completely remove the internal impurities.
[0112] Comparative Example 3 confirmed the adverse effects of oxidative acid washing. At the same washing temperature and frequency as the examples, a distinct sharp peak characteristic of boric acid (H3BO3) appeared in the spectrum of Comparative Example 3. This indicates that the newly generated amorphous boron powder is highly reactive and easily oxidized by the strong oxidizing properties of nitric acid solution, resulting in surface oxidation. The hydrochloric acid combined with hydrofluoric acid washing process used in this invention is a non-oxidizing system, which can remove residual non-metallic and transition metal impurities while avoiding secondary oxidation of amorphous elemental boron.
[0113] Test Example 3:
[0114] The final amorphous boron powders from Examples 1 to 3 and Comparative Examples 1 to 2, which underwent multiple non-oxidative composite post-treatments and were in a completely dry state, were selected as the target objects for yield testing. At the same time, the actual weighing mass records of high-purity boron oxide during the initial loading stage of each reaction system were retrieved.
[0115] Based on the stoichiometric ratio of the magnesium thermal reduction of boron oxide, the theoretically limit mass of elemental boron that can be produced in each system after complete reaction is calculated, and this is used as the theoretical denominator for subsequent yield balance calculations.
[0116] The powder after deep washing and drying was weighed multiple times using an analytical balance of 0.01 g / L. When the difference between three consecutive weighing results was within 0.5 mg, the constant value was recorded as the actual boron production, and the final mass yield percentage was calculated accordingly.
[0117] During the disassembly and cleaning of the reaction tube, the mass of reaction splashes and slag scattered on the outside of the pyrolytic boron nitride crucible 5 and the inner wall of the quartz tube 1 is carefully collected and weighed to macroscopically assess the degree of material mechanical loss during the reaction process.
[0118] Table 3. Summary of Test Results of Target Product Yield and Splash Loss for Each Reaction System
[0119] Test object Initial boron oxide input (g) Theoretical boron yield (g) Actual constant-weight boron yield (g) Final target yield (%) Total mass of splash collected (g) Example 1 35.1425 10.9168 10.2882 94.24 0.1251 Example 2 34.8912 10.8387 9.6627 89.15 0.0814 Example 3 35.2106 10.9380 10.0278 91.68 0.2106 Comparative Example 1 35.0874 10.8997 4.7762 43.82 14.3625 Comparative Example 2 35.1158 10.9085 7.3676 67.54 1.8547
[0120] See attached document Figure 4 , Figure 4The figure shows the product conversion efficiency distribution of the final preparation system under different charging strategies and temperature control curves. The solid line marked with a black square corresponds to the final target yield represented by the left main coordinate axis, and the dashed line marked with a hollow triangle corresponds to the total mass of splash collected represented by the right secondary coordinate axis. The experimental batch distribution of Examples 1 to 3 and Comparative Examples 1 and 2 is shown in parallel on the horizontal axis.
[0121] Based on the data in Table 3, combined with Figure 4 The spatial distribution of reactants and the gradient of the thermal field directly determine the final conversion efficiency of the target product. Mechanical losses of materials and dead zones at the solid-liquid interface during the preparation of industrial-grade high-purity materials are core engineering barriers limiting large-scale production. Examples 1 to 3 achieved actual boron powder yields close to or exceeding 90% under the process background of ensuring a high impurity removal rate. In Example 1, by using the most suitable stepped isothermal platform and block size combination, the total mass of splashes detached from the reaction zone was successfully suppressed to a low level of 0.1251g, and the system yield reached 94.24%. The temperature buffer zone constructed by the stepped heating process allows boron oxide reaching its melting point to slowly penetrate into the pore network of the underlying solid magnesium particles by gravity. This not only effectively inhibits the diffusion and escape of gaseous magnesium vapor but also anchors the core reactants at the microscopic scale, physically avoiding material loss caused by hot gas entrainment. The fully wetted reaction interface maximizes the local thermodynamic equilibrium of the system towards the formation of elemental boron.
[0122] Powdered precursors exhibit drastically different engineering behaviors when faced with violently exothermic reactions. In Comparative Example 1, the yield of the powder raw material mixture system dropped to 43.82%. The huge specific surface area of the powder system instantly released an extremely large latent heat of reaction when the temperature was raised to the critical point of the reaction activation energy, causing the temperature of local micro-regions to rise sharply and exceed the upper limit of the system's capacity, triggering a material boiling phenomenon. Up to 14.3625g of material forcibly broke through the physical constraints of the pyrolysis boron nitride crucible 5, and a large amount of unreacted or semi-molten intermediate products condensed on the inner wall of the quartz tube 1, which was far from the heating center. This uncontrollable eruption would inevitably lead to serious equipment contamination and material waste in an actual production line. After canceling the first-stage stepped heat preservation operation, the total yield of the system dropped to 67.54%. Solid materials directly undergo local contact reactions in a high-temperature environment. The widespread existence of interface contact dead zones not only prevents the reaction front from reaching the core of the material, but the contraction effect caused by local overheating also leads to premature agglomeration and decoupling of the reactants. The experimental data above, through the dimension of macroscopic mass balance, verify that macroscopic bulk embedding combined with stepped thermal field control is not only a necessary and safe means to control the exothermic reaction, but also the underlying process foundation for achieving high-conversion mass production of high-purity amorphous boron powder.
[0123] Test Example 4:
[0124] Amorphous boron powders from Examples 1 to 3, as well as Comparative Examples 3 and 4, which underwent multi-step compounding and purification and were vacuum dried to constant weight, were selected as the test objects for elemental quantitative analysis.
[0125] Accurately weigh 0.15 g of each boron powder sample and place it in a polytetrafluoroethylene microwave digestion vessel. Add a mixed digestion solution of high-purity nitric acid and trace amounts of hydrofluoric acid. Perform high-temperature and high-pressure digestion in a closed microwave digester until the solid sample is completely dissolved to form a clear solution. Then, remove excess fluoride ions by acid removal treatment.
[0126] After digestion and acid removal, the solution was transferred to a 50 mL polytetrafluoroethylene volumetric flask and diluted to the mark with ultrapure water. At the same time, a blank control solution and a series of concentration gradient standard solutions containing mixed standard solutions of multiple elements such as silicon, magnesium, aluminum, and iron were prepared.
[0127] Full-spectrum trace element analysis of each sample solution was performed using inductively coupled plasma mass spectrometry in helium collision cell mode. The absolute mass concentration of each impurity element was calculated based on the standard curve, and the purity of the boron main component of the sample was calculated by reverse calculation using the difference method.
[0128] Table 4. Test results of main component purity and trace impurity element content of the final products of each system
[0129] Test object Boron (B) main component purity (%) Silicon (Si) content (ppm) Magnesium (Mg) content (ppm) Aluminum (Al) content (ppm) Iron (Fe) content (ppm) Example 1 99.9992 0.85 1.12 0.35 0.16 Example 2 99.9988 1.25 1.84 0.62 0.45 Example 3 99.9990 0.98 1.35 0.41 0.28 Comparative Example 3 98.42 187.36 314.52 25.41 48.65 Comparative Example 4 97.15 1845.27 56.83 142.74 12.59
[0130] See attached document Figure 5 , Figure 5 The figure shows the absolute concentration trends of four key trace impurities in the product under different preparation processes and consumable conditions. The vertical axis uses a logarithmic scale to encompass the distribution differences between extremely low and extremely high content ranges. In the figure, the solid line with a solid circle represents Example 1, the dashed line with a hollow square represents Example 2, the dotted line with a hollow triangle represents Example 3, the thick dotted line with a hollow rhombus represents Comparative Example 3, and the thin solid line marked with an asterisk represents Comparative Example 4.
[0131] Based on the data in Table 4, combined with Figure 5Ultimately, the purity limit of high-purity amorphous materials is often not constrained by the conversion rate of the main reaction itself, but rather directly controlled by the corrosion resistance of the high-temperature reaction vessel material and the coordination and exfoliation capabilities of the post-treatment cleaning solution. In the early powder preparation stage in the laboratory, the microscopic interfacial reaction between the reactants and the inner wall of the vessel under high-temperature conditions has always been a hidden source of interference leading to an upper limit on batch purity. Examples 1 to 3, through systematic material isolation and chemically targeted purification, achieved a stable purity of the main boron component at the 5N (99.999%) level, with Example 1 reaching 99.9992%. This data was obtained based on the extremely strong chemical inertness exhibited by the pyrolytic boron nitride crucible 5 under a reducing atmosphere at 1000 degrees Celsius. During long-term heat preservation, no matrix peeling or ion migration occurred, physically blocking the intrusion paths of exogenous silicon and aluminum impurities. During the deep non-oxidizing pickling stage, the system of trace hydrofluoric acid combined with electronic-grade hydrochloric acid precisely erodes and dissolves the trace silicate impurities and deep transition metals that are inherently present in the raw materials. This reduces the absolute residual amount of silicon, magnesium and iron in the product to a low level of less than 2 ppm, which fully meets the stringent control requirements of high-end semiconductor vapor deposition sources for trace contaminants.
[0132] At high temperatures, the quartz crucible inevitably underwent an interfacial displacement reaction with magnesium vapor, generating complex magnesium silicate and free elemental silicon. This side reaction directly resulted in up to 1845.27 ppm of free silicon penetrating and anchoring in the interstitial spaces of the product matrix, causing the boron purity of the system to drop to 97.15%. Because the silicon impurities deep within the powder had formed a strong interfacial contact with the boron matrix, conventional acid leaching was completely ineffective in removing them. The intervention of a strong oxidizing nitric acid solution instantly dissolved the surface free metal while simultaneously triggering a rapid secondary oxidation reaction on the surface of the amorphous boron powder. The resulting dense oxide film acted as a mass transfer barrier layer at the microscale, tightly sealing the magnesium salts and transition metals that had not yet diffused out of the particles within the core structure of the powder, blocking the mass exchange channels, and causing the residual magnesium and iron content to deviate from the acceptable standard for high-purity materials. These transverse trace analysis results indicate that the preparation of high-purity powders requires a tight process loop between contamination interception at the front end of the reaction and non-oxidative stripping at the back end.
[0133] Test Example 5;
[0134] Amorphous boron powder prepared and completely vacuum dried in Examples 1 to 3, as well as Comparative Examples 1 and 3, was selected as the test object for total oxygen content.
[0135] Inside a glove box filled with high-purity argon, approximately 15 milligrams of powder sample were accurately weighed, wrapped in a high-purity tin bag, clamped with tweezers, and the trapped gas inside was squeezed out. The sample was then placed in a matching deoxidized nickel basket for testing.
[0136] Turn on the inert gas melting infrared absorption oxygen, nitrogen, and hydrogen analyzer, and continuously introduce helium as a carrier gas into the built-in graphite crucible. Start the pulse heating program, apply a large current to the graphite crucible, and cause the temperature inside the test chamber to jump to 2200℃ in a very short time.
[0137] The sample undergoes complete melting at high temperature, during which the oxygen element reacts with the graphite crucible in a carbothermal reduction reaction, converting into carbon monoxide and carbon dioxide gases. This mixed gas is then carried by a helium gas stream into an infrared detection cell. The total oxygen content of the sample is calculated by analyzing the area of the integrated infrared characteristic absorption peak. During this process, the system utilizes a segmented programmed temperature desorption technique, quantifying and recording the specific values of adsorbed oxygen on the powder surface and bound oxygen within the crystal lattice according to the temperature range of oxygen gas release.
[0138] Table 5. Analysis data of total oxygen content in the final products of each reaction system
[0139] Test object Oxygen content on powder surface (ppm) Oxygen content inside the powder (ppm) Total oxygen content (ppm) Total oxygen mass fraction (%) Example 1 3.25 1.83 5.08 0.0005 Example 2 4.12 2.15 6.27 0.0006 Example 3 3.86 1.98 5.84 0.0006 Comparative Example 1 3845.22 875.46 4720.68 0.4720 Comparative Example 3 4216.85 652.13 4868.98 0.4869
[0140] See attached document Figure 6 , Figure 6 This figure illustrates the specific sources, distribution, and total variation of oxygen impurities in the products under different preparation processes. The horizontal axis corresponds to different experimental examples and comparative batches, while the vertical axis represents the oxygen content in parts per million. Solid lines with black squares represent the total oxygen content of the powder, dashed lines with hollow circles represent the adsorbed oxygen content desorbed from the powder surface, and dotted lines with hollow triangles represent the bound oxygen content within the powder lattice.
[0141] Based on the data in Table 5, combined with Figure 6The total oxygen content reflects the powder's actual ability to resist environmental oxidation throughout the entire preparation cycle. In semiconductor thin film deposition or high-energy fuel applications, micron-sized powders are highly susceptible to deep oxidation due to their high specific surface area, resulting in the final product being covered by an insulating oxide layer, thus losing the material's intrinsic physicochemical activity. Test data shows that the total oxygen mass fraction of the products in Examples 1 to 3 was effectively reduced to below 0.0007% (7 ppm), with the test value of Example 1 being only 5.08 ppm. This core indicator is far lower than the conventional oxygen content level of several thousand ppm in traditional powder processes. The physical morphology of the bulk boron oxide precursor reduces the gas-solid contact surface at the reaction front. In the initial material weighing and filling environment of the experiment, the capillary path for moisture to penetrate into the precursor matrix was effectively blocked, allowing the reaction system to enter the closed high-temperature reduction stage without carrying excess water and oxygen impurities. After entering the wet purification stage, based on the non-oxidizing composite acid washing process, the residual soluble byproducts were smoothly stripped off. Because acidic reagents with strong oxidation potential are eliminated, the newly generated amorphous boron maintains extremely high chemical inertness in the entire aqueous washing environment, thus eliminating secondary oxidation during the post-treatment process.
[0142] Altering the physical form of materials and the washing reagents can rapidly transform potential oxidation risks into substantial microstructural defects. Comparative Example 1 used a direct mixing reaction of powdered precursors. The high porosity of the micron-sized powder caused it to adsorb a large amount of ambient moisture during the brief material transfer process. This free water instantly vaporized upon contact with a high-temperature thermal field, triggering a complex localized hydrolysis reaction. The resulting nascent oxides were deeply embedded in the reaction matrix, leading to a sharp increase in bound oxygen within the product, with the total oxygen content rising to 4720.68 ppm. Incorrect selection of wet washing reagents can also lead to irreversible material degradation. Comparative Example 3 introduced nitric acid as a washing agent, and the test data revealed oxygen contamination. The strong oxidizing acid, while dissolving free metal impurities, also initiated a severe oxidative erosion of the highly reactive elemental boron surface. The large amount of surface-adsorbed oxygen desorbed at low temperatures during infrared detection, reaching a surface oxygen value as high as 4216.85 ppm, confirmed the formation of a large amount of boric acid and boron oxide passivation layer around the powder. This secondary oxidation at the chemical level compromised the purity limits of the powder. Therefore, constructing a physical barrier at the front end of the charging process to inhibit water and oxygen adsorption and adopting a non-oxidative chemical stripping strategy at the back end of purification are the fundamental process boundaries to ensure the high-purity, low-oxygen preparation of highly active boron powder.
Claims
1. A method for preparing high-purity boron, characterized in that, Includes the following steps: According to the ratio, high-purity magnesium particles and blocky high-purity boron oxide are sequentially loaded into the pretreated pyrolytic boron nitride crucible (5) so that the blocky high-purity boron oxide is completely embedded by the high-purity magnesium particles. The pyrolytic boron nitride crucible (5) is then sealed to obtain the reaction system. The reaction system was placed under an inert atmosphere for a step-by-step temperature-programmed reduction reaction, and the temperature was kept constant after the first stage of heating. In the second stage, the temperature was increased and held constant, and then cooled to room temperature to obtain the reaction product. The cooled reaction product was mechanically crushed, and then subjected to initial acid leaching with hydrochloric acid solution, followed by deep acid leaching with a mixture of electronic-grade high-purity hydrochloric acid solution containing hydrofluoric acid or electronic-grade high-purity hydrochloric acid solution. After being ultrasonically washed with hot water until neutral, it was vacuum dried to obtain high-purity amorphous boron powder.
2. The method for preparing high-purity boron according to claim 1, characterized in that, The theoretical stoichiometric molar ratio of 1:3, which allows the blocky high-purity boron oxide to undergo a reduction reaction with the high-purity magnesium particles, is used as the basis for weighing and batching. The actual molar amount of the high-purity magnesium particles added is 3% to 15% in excess of the theoretical requirement. The characteristic size of the blocky high-purity boron oxide is 5-50 mm; The high-purity magnesium particles are irregular particles, and the particle size of the high-purity magnesium particles is 0.5 to 5 mm.
3. The method for preparing high-purity boron according to claim 1, characterized in that, Before loading the pyrolytic boron nitride crucible (5), the pyrolytic boron nitride crucible (5) and the blocky high-purity boron oxide and the high-purity magnesium particles used as reaction raw materials are pretreated as follows: The pyrolytic boron nitride crucible (5) was completely immersed in aqua regia for 1-2 hours, then rinsed with deionized water 3-5 times, and dried in a drying oven at 100°C for later use. The blocky high-purity boron oxide was placed in a vacuum drying oven and dried at 110–130°C for 1.5–3 hours before being removed and sealed. The high-purity magnesium particles were placed in a vacuum drying oven and dried at 70–90°C for 0.5–2 hours before being removed and sealed.
4. The method for preparing high-purity boron according to claim 1, characterized in that, The step of sequentially loading high-purity magnesium particles and blocky high-purity boron oxide into the pretreated pyrolytic boron nitride crucible (5) is as follows: A layer of high-purity magnesium particles is laid flat at the bottom of the pyrolysis boron nitride crucible (5), with a thickness of 2-5 mm; The blocky high-purity boron oxide is placed at the center of the bottom layer of high-purity magnesium particles; The remaining high-purity magnesium particles are poured into the pyrolytic boron nitride crucible (5), completely filling the gap between the blocky high-purity boron oxide and the inner wall of the pyrolytic boron nitride crucible (5) and covering the top of the blocky high-purity boron oxide.
5. The method for preparing high-purity boron according to claim 1, characterized in that, Before placing the reaction system under an inert atmosphere for a step-by-step temperature-programmed reduction reaction, the following steps are also included: Connect the inlet (2) of the quartz tube (1) to an argon gas source, open the tail gas port (3), and introduce argon gas into the quartz tube (1) at a gas flow rate of 400-600 mL / min for 10-15 min. Place the sealed pyrolytic boron nitride crucible (5) into the quartz boat (4) and push it into the quartz tube (1). After sealing the system, continue to introduce argon gas at a flow rate of 400-600 mL / min for 20-30 min.
6. The method for preparing high-purity boron according to claim 5, characterized in that, The process parameters for the stepped temperature-programmed reduction reaction are as follows: The argon flow rate in the quartz tube (1) is reduced to 50-100 mL / min to maintain a slightly positive pressure state in the quartz tube (1); Start the heating program. In the first stage, the system temperature is raised from room temperature to 450-550℃ at a heating rate of 10-15℃ / min, and then kept at 450-550℃ for 30-60 minutes. In the second stage, the system temperature was increased to 800-1000℃ at a heating rate of 10-15℃ / min, and then maintained at 800-1000℃ for 1.5-3 hours.
7. The method for preparing high-purity boron according to claim 1, characterized in that, The specific operation of the initial acid leaching is as follows: The mechanically crushed reaction product was added to an excess of hydrochloric acid solution with a concentration of 2-4 mol / L, and the reaction was mechanically stirred at room temperature for 2-4 hours. After the reaction was stopped, the primary filter residue of the solid phase was separated by vacuum filtration.
8. The method for preparing high-purity boron according to claim 7, characterized in that, The specific steps of the deep acid leaching are as follows: The initial filter residue is transferred to a polytetrafluoroethylene beaker, and an electronic-grade high-purity hydrochloric acid solution or a mixed solution of electronic-grade high-purity hydrochloric acid containing no more than 5% hydrofluoric acid by mass is added. The mixture is soaked in a water bath at 30-50°C and slowly stirred for 1-2 hours. After the process is completed, it is filtered again to obtain a solid powder after deep acid leaching.
9. The method for preparing high-purity boron according to claim 8, characterized in that, The specific steps of the hot water ultrasonic washing and vacuum drying are as follows: The solid powder after deep acid leaching is added to deionized water at 60-80°C, placed in an ultrasonic cleaner for ultrasonic oscillation for 10-20 minutes, filtered, and the hot water ultrasonic washing step is repeated 3-5 times until the pH value of the filtrate is neutral. Place the washed powder in a vacuum drying oven and dry it at 80-100℃ for 2-6 hours until the powder quality is constant.
10. An apparatus for implementing the method for preparing high-purity boron according to any one of claims 1-9, characterized in that, include: Quartz tube (1), wherein the quartz tube (1) is provided with an air inlet (2) and an exhaust outlet (3); Quartz boat (4) is disposed inside the quartz tube (1); A pyrolytic boron nitride crucible (5) is placed inside the quartz boat (4). The pyrolytic boron nitride crucible (5) has a sealed structure. The interior of the pyrolytic boron nitride crucible (5) is used to contain the blocky high-purity boron oxide and the high-purity magnesium particles.