A method for producing high-purity alumina

By using the direct gas-phase oxidation reaction of AlCl3 and O2 and the Y2O3-doped Al2O3 composite functional coating, the problems of lengthy process, water and energy consumption and pollution in the preparation of high-purity alumina have been solved, and efficient and environmentally friendly preparation of nanoscale high-purity alumina has been achieved.

CN123105693APending Publication Date: 2026-11-17CHENGDU HUARONG CHEM CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611473787.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing methods for preparing high-purity alumina are lengthy, water- and energy-intensive, and cause serious pollution, making it difficult to stably prepare high-purity alumina.

Method used

High-purity alumina was prepared by using a direct gas-phase oxidation reaction of AlCl3 and O2, combined with a high-purity inner lining for isolation and protection throughout the process and a Y2O3-doped Al2O3 composite functional coating, and by controlling the reaction temperature and cooling rate.

Benefits of technology

This method enables the efficient and environmentally friendly preparation of nano-sized high-purity alumina, resulting in high product purity, controllable particle size, reduced equipment investment and operating energy consumption, and extended reactor life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The application relates to the field of chemical materials, and provides a preparation method of high-purity aluminum oxide, which comprises the following steps: S1, fuel and oxygen are combusted in a reactor, and the reactor is subjected to lining treatment, and then an activated reactor is obtained; S2, AlCl3 is preheated to sublimate, then is delivered into the activated reactor through a carrier gas, and then is subjected to an oxidation reaction to obtain aluminum oxide primary products; S3, the activated reactor is subjected to cooling treatment to terminate the oxidation reaction in the step S2, and then is subjected to gas-solid separation, and then aluminum oxide products are obtained; the method adopts an AlCl3 and O2 direct gas phase oxidation reaction route, Y2O3 doped Al2O3 composite functional coating is constructed in situ on the lining surface of the reactor to realize lining sealing and impurity locking, combined with post-reaction temperature limiting, high-purity lining isolation protection in the whole process and bag type filtration non-contact gas-solid separation, only four links of preheating-reaction-cooling-separation are needed, no waste water is discharged, and high-purity aluminum oxide products of 4N5 level can be obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of chemical materials technology, and more specifically, to a method for preparing high-purity alumina. Background Technology

[0002] High-purity Al2O3 is currently an important industrial raw material needed by the market. Due to its high purity, high-purity alumina powder exhibits optical, electrical, magnetic, thermal and mechanical properties that are not found in conventional materials. Therefore, it is widely used as a new type of functional material in fields such as lithium-ion batteries, sapphire substrates, electronic ceramics, catalysts, electronic components, ceramics, abrasives and other high-tech fields.

[0003] Most existing methods for preparing high-purity Al2O3 involve liquid-phase or solid-phase methods to produce aluminum-related hydroxides, which are then calcined to generate oxides. The hydroxide preparation process strictly controls the purity of the final product. Furthermore, the hydroxide preparation process consumes large amounts of water, generating significant amounts of wastewater and waste gas. Additionally, the calcination of hydroxides typically employs high-temperature furnaces, which are energy-intensive and generate substantial waste gas again, placing immense environmental pressure on traditional high-purity Al2O3 preparation methods.

[0004] For example, patent CN107500324A discloses a liquid-phase method for preparing high-purity alumina. Specifically, it uses industrial aluminum hydroxide as raw material, obtains sodium aluminate solution through sodium hydroxide alkali dissolution, and then obtains aluminum hydroxide through decolorization and impurity removal, pressure desiliconization, and seed crystal decomposition. Sodium impurities are then removed through hydrothermal desodium removal and multi-stage countercurrent washing, and finally, high-temperature calcination at 1285~1450℃ for 1~3 hours yields high-purity alumina. While this method can obtain high-purity alumina with a purity of 4N5~4N6, it involves as many as seven main processes, making the process lengthy. Furthermore, the multi-stage countercurrent washing process consumes a huge amount of water and generates a large amount of difficult-to-treat alkaline wastewater. Hydrothermal desodium removal requires high-pressure conditions at 180~220℃, demanding sophisticated equipment, and the high-temperature calcination process has extremely high energy consumption and generates a large amount of combustion waste gas. Summary of the Invention

[0005] In view of the above-mentioned shortcomings in the existing technology, the core objective of this invention is to solve the technical problems of the existing liquid phase method, which is lengthy, consumes a lot of water and energy, causes serious pollution, and is difficult to stably prepare high-purity alumina.

[0006] This invention is specifically achieved through the following technical solutions: The purpose of this invention is to provide a method for preparing high-purity alumina, comprising the following steps: S1. Combust fuel and oxygen in a reactor, and then line the reactor to obtain an activated reactor. S2. AlCl3 is preheated to sublimation and then transported to the activation reactor via a carrier gas. After oxidation, alumina primary product is obtained. S3. The activated reactor is cooled to terminate the oxidation reaction in step S2, and then gas-solid separation is performed to obtain the alumina product.

[0007] Furthermore, in step S1, the oxygen content of the combustion is 30% to 50% in excess, and the combustion raises the temperature of the reaction zone to 1300 to 1400°C.

[0008] More preferably, the fuel is toluene with a purity of ≥99.5%, and the oxygen has a purity of ≥99.999%. Oxygen-enriched combustion ensures that toluene is completely converted into CO2 and H2O, avoiding the generation of free carbon, such as carbon black, which pollutes the product due to local oxygen deficiency. At the same time, the high-temperature flame performs thermal etching cleaning on the inner lining surface, removing organic pollutants and low-melting-point impurities adsorbed during installation or shutdown, providing a clean and highly active substrate surface for subsequent coatings.

[0009] Further, in step S2, the AlCl3 is preheated to 200~250℃. By controlling the ratio of the heat transfer medium and oxygen, and simultaneously adjusting the carrier gas flow rate, the starting temperature of the oxidation reaction is controlled to ensure that the temperature after the oxidation reaction ends does not exceed 1850℃.

[0010] More preferably, the AlCl3 raw material has a purity ≥99.999%, and is preheated to 200~250℃ to completely sublimate it; the carrier gas is high-purity nitrogen, high-purity argon, or a mixture of nitrogen and chlorine in a mass ratio of 0~1:1, all with a purity ≥99.999%. The oxidation reaction is a direct gas-phase oxidation reaction of AlCl3 and O2, and the reaction formula is as follows: 4AlCl3(g)+3O2(g) → 2α-Al2O3(s)+6Cl2(g); The enthalpy change of the reaction ΔH= The reaction temperature is 1013.5 kJ, indicating a strongly exothermic reaction. Specifically, the initial temperature of the oxidation reaction is controlled by adjusting at least one parameter among the carrier gas flow rate, oxygen flow rate, and AlCl3 feed rate, ensuring that the temperature does not exceed 1850°C after the oxidation reaction, thus preventing rapid grain growth.

[0011] Further, in step S3, the cooling treatment is as follows: a cooling gas is introduced into the reaction product to reduce the temperature of the reaction zone to below the reaction termination temperature within 3.5 to 20 ms to quench the oxidation reaction, and then the temperature is further reduced to ≤220℃ with a cooling duration of 4 to 6 s; the cooling gas is either nitrogen or argon.

[0012] In this invention, after the oxidation reaction is completed, a cooling gas (high-purity nitrogen or high-purity argon, purity ≥99.999%) is introduced into the reaction product to rapidly reduce the temperature of the reaction zone to below 1000℃ within 3.5~20ms, thereby quenching and terminating the oxidation reaction. This millisecond-level quenching effectively inhibits the continued growth of Al2O3 grains through the ripening mechanism, locking the grain size at the nanometer / submicron level. Then, with a cooling duration of 4~6s, the temperature is further gradient-reduced to ≤220℃ to meet the operating temperature requirements of the bag filter, while preventing Cl2 and residual water vapor from condensing into corrosive acid due to overcooling. The gas-solid separation is performed using a bag filter. Before use, the bag filter undergoes a pre-coating process: pure alumina powder is introduced and run for 30~60 minutes to form a dense alumina powder layer on the filter bag surface. This prevents subsequent products from directly contacting the filter bag fibers and metal skeleton, thus eliminating external contamination during the collection process.

[0013] Furthermore, the lining process includes the following steps: S11. During the combustion and heating process of the reactor, a composite slurry is sprayed onto the inner lining surface of the reactor to form a sealing coating on the inner lining surface of the reactor. S12. The sealing coating is subjected to oxidative activation treatment to obtain the activated reactor.

[0014] Further, the composite slurry comprises: the composite slurry includes (1) and / or (2): (1) By weight, 85-92 parts of α-Al2O3 micro powder, 3-8 parts of Y2O3 nano powder, and 5-10 parts of boehmite sol on a dry basis; (2) Boehmite sol with a solid content of 20 wt% by weight.

[0015] Furthermore, the composite slurry also contains ammonium polyacrylate dispersant, and the amount of ammonium polyacrylate dispersant added is 0.5~1.5wt% of the total solids of the composite slurry.

[0016] More specifically, in this invention, the ammonium polyacrylate dispersant has a purity ≥99.9% and an ash content <50ppm; the slurry is ball-milled in a high-purity alumina ball mill for 4-6 hours to ensure uniform dispersion of all components. The ammonium polyacrylate prevents the agglomeration of nano-Y2O3 particles through a dual mechanism of electrostatic repulsion and steric hindrance, ensuring the slurry's flowability and atomization uniformity during spraying; its molecular chains undergo complete thermal decomposition at 200-400℃, producing CO2, H2O, and NH3, leaving no ash residue and not affecting product purity.

[0017] Further, in step S11, when the reactor furnace temperature is raised to 1300~1350℃, the composite slurry is sprayed onto the inner lining surface of the reactor. After spraying, the temperature is further raised to 1350~1400℃ and held for 20~40 minutes. The sealing coating is obtained by sintering. The thickness of the sealing coating is 0.2~0.8mm.

[0018] In this invention, during the process of boehmite sol transforming into alumina, many hydroxyl groups are formed on the surface. These hydroxyl groups react chemically with aluminum atoms on the surface of the liner substrate to form chemical bonds, namely Al-O-Al. As a result, the resulting sealing coating is more firmly bonded than the existing process of directly splicing the liner and is less likely to fall off in subsequent reactions.

[0019] Further, in step S12, the sealing coating is subjected to an oxidative activation treatment at 1350~1400℃ for 30~60 minutes under conditions where only oxygen is introduced, and then the activated reactor is obtained.

[0020] In this invention, after sintering in step S11, fuel supply is stopped, and only oxygen is introduced. The sealing coating is then subjected to oxidative activation treatment at 1350~1400℃ for 30~60 minutes to obtain the activated reactor. During this process, Y 3+ Replace part of Al 3+ Entering the Al2O3 lattice, due to Y 3+ With Al 3+ Size mismatch generates a strong lattice strain field, inducing the formation of a large number of charge-compensated oxygen vacancies in the vicinity of the Al2O3 lattice via oxygen desorption. The concentration of these vacancies is 1-2 orders of magnitude higher than that generated by thermal desorption from the pure Al2O3 surface. These oxygen vacancies are strong Lewis acid adsorption sites for AlCl3 molecules. When AlCl3 molecules approach the coating surface, they are captured and activated by these oxygen vacancies, significantly reducing the apparent activation energy of the direct oxidation reaction of AlCl3, allowing the reaction to proceed faster and more completely at the same temperature. Simultaneously, Y... 3+ Segregation at α-Al2O3 grain boundaries forms pinning, effectively suppressing abnormal grain growth in the coating at subsequent service temperatures of 1850℃, ensuring the long-term stability of the coating's microstructure.

[0021] The technical solutions of the embodiments of the present invention have at least the following advantages and beneficial effects: (1) The present invention adopts the direct gas phase oxidation reaction route of AlCl3 and O2, combined with the high-purity inner lining isolation protection throughout the process and the impurity locking effect of Y2O3 doped Al2O3 composite functional coating, effectively blocking the volatilization-migration-deposition pollution cycle of metal chlorides under high temperature Cl2 atmosphere.

[0022] (2) The present invention effectively inhibits the ripening growth of Al2O3 grains by combining the reaction temperature not exceeding 1850℃ with the 3.5~20ms millisecond-level quenching. The average particle size of the product can be controlled within the range of 42~67nm.

[0023] (3) The present invention forms a dense sealing coating through lining treatment, which effectively prevents the product from scaling and clogging on the inner wall of the reactor. The yield of the example can reach 92.5%~94.8%.

[0024] (4) Y in the composite coating of the present invention 3+ The grain boundary pinning effect effectively inhibits the abnormal growth of coating grains. Combined with repeatable online repair for each batch, it effectively extends the service life of the reactor and has low operating costs.

[0025] (5) The present invention adopts the direct gas phase oxidation reaction of AlCl3. From raw materials to products, only four main steps are required: preheating, reaction, cooling and separation. Equipment investment and operating energy consumption are significantly reduced, and it is environmentally friendly with no wastewater and waste residue discharge. Detailed Implementation

[0026] Example 1 This embodiment provides a method for preparing high-purity alumina, including the following steps: S1. Reactor preheating, combustion, and lining treatment: Toluene with a purity of 99.5% and oxygen with a purity of 99.999% were introduced into the reactor using an oxygen-enriched combustion method, with an oxygen excess of 30%. The mixture was ignited, raising the temperature of the reaction zone to 1350℃. During the combustion and heating process, the following lining treatment was performed simultaneously: S11. When the reactor furnace temperature reaches 1320℃, the composite slurry is atomized and sprayed onto the reactor lining surface using a specially designed high-purity alumina water-cooled spray gun. The spraying pressure is 0.4MPa, the spraying distance is 150mm, and the spray gun moving speed is 10cm / s. After spraying, the temperature is further increased to 1380℃ and held for 30 minutes. A sealing coating is then obtained through in-situ sintering, with a coating thickness of 0.5mm and a porosity of less than 1%.

[0027] The composite slurry is prepared as follows: 90 parts of α-Al2O3 micro powder with a purity of 99.999% and a D50 of 1.0 μm, 5 parts of Y2O3 nanopowder with a purity of 99.999% and a D50 of 50 nm, and 5 parts of boehmite sol with a solid content of 20 wt% (on a dry basis) are added to ultrapure water with a resistivity ≥18 MΩ·cm, and 1.0 wt% of ammonium polyacrylate dispersant with a purity of 99.9% and an ash content of less than 50 ppm is added; a composite slurry with a solid content of 50 wt% and a viscosity of 200 cP at 25℃ is prepared; the slurry is ball-milled in a high-purity alumina ball mill for 5 hours to ensure uniform dispersion of each component.

[0028] After the sintering of steps S12 and S11 is completed, the supply of toluene is stopped and the system is switched to supplying only oxygen. The oxygen flow rate is 1.5 times the normal combustion flow rate. The sealing coating is then subjected to oxidation activation treatment at 1380°C for 45 minutes to obtain an activated reactor.

[0029] S2 and AlCl3 preheating and oxidation reaction: AlCl3 powder with a purity of 99.999% (purity range ≥99.999%) was preheated to 220°C in a sublimation apparatus (pressurized to 0.25-0.5 MPaG and heated) to completely sublimate it into gas. A mixture of nitrogen and chlorine was used as the carrier gas, with a mass ratio of nitrogen to chlorine of 1:1. The carrier gas flow rate was 2.0 times the AlCl3 gas flow rate. The AlCl3 gas was then fed into the activation reactor prepared in step S1. AlCl3 underwent a direct gas-phase oxidation reaction with oxygen at high temperature. The AlCl3 gas flow rate and the oxygen flow rate were both controlled at 50 L / min, i.e., the molar ratio of oxygen to AlCl3 was approximately 1:1. By adjusting the carrier gas flow rate to 2.0 times the AlCl3 gas flow rate, i.e., 100 L / min, the carrier gas was used as a diluent and heat sink to absorb part of the reaction heat and prevent a rapid increase in system temperature. By controlling the material ratio and carrier gas flow rate as described above, the initial temperature of the oxidation reaction can be established stably, and the temperature after the reaction ends does not exceed 1830℃, thus avoiding rapid grain growth.

[0030] S3, Cooling quenching and gas-solid separation: After the oxidation reaction is complete, high-purity nitrogen gas (99.999% purity) is immediately introduced into the reaction products as a cooling gas to rapidly reduce the temperature of the reaction zone to below 1000℃ within 8ms, thereby quenching and terminating the oxidation reaction. Then, with a cooling duration of 5s, the temperature is further reduced in a gradient to no higher than 220℃ to meet the operating temperature requirements of the bag filter.

[0031] The cooled gas-solid mixture is passed through a bag filter for gas-solid separation to obtain high-purity alumina powder. The bag filter is pre-treated with a powder cake layer before use: pure alumina powder is passed through and the filter runs for 45 minutes, forming a dense alumina powder cake layer on the surface of the filter bag.

[0032] Example 2 The difference between this embodiment and Embodiment 1 is that the amount of Y2O3 nanopowder added to the composite slurry is changed to 8 parts, while the rest is the same as in Embodiment 1.

[0033] Example 3 The difference between this embodiment and Embodiment 1 is that the boehmite sol with a solid content of 20wt% in the composite slurry is replaced with 7 parts on a dry basis, while the rest remains the same as in Embodiment 1.

[0034] Example 4 The difference between this embodiment and Embodiment 1 is that the temperature of the oxidation activation treatment in step S12 is 1350℃, while the rest is the same as in Embodiment 1.

[0035] Example 5 The difference between this embodiment and embodiment 1 is that the quenching time in step S3 is 15ms, while the rest is the same as in embodiment 1.

[0036] Comparative Example 1 The difference between this comparative example and Example 1 is that Y2O3 nanopowder is not added to the composite slurry, while the rest of the contents are the same as in Example 1.

[0037] Comparative Example 2 The difference between this comparative example and Example 1 is that boehmite sol is not added to the composite slurry, while the rest of the contents are the same as in Example 1.

[0038] Comparative Example 3 The difference between this comparative example and Example 1 is that the temperature exceeds 1850°C after the reaction in step S2, reaching 1900°C. The rest of the contents are the same as in Example 1.

[0039] Experimental Example 1 This experimental example uses the method provided in Example 1 to prepare high-purity Al2O3 powder, and compares and analyzes the impurity content of different batches and qualities of AlCl3 raw materials and the resulting products, as detailed below: Inductively coupled plasma mass spectrometry (ICP-MS) was used to quantitatively analyze 12 key impurity elements in AlCl3 raw materials and Al2O3 products, including calcium, copper, iron, potassium, magnesium, manganese, sodium, nickel, silicon, zinc, zirconium, and silver. The testing standard followed the national standard 4N5 (total impurity content ≤ 50 ppm) for impurity content in high-purity alumina. Impurity detection data from multiple batches of AlCl3 raw materials and corresponding Al2O3 products are shown in Table 1 below. Table 1. Detection data of impurity content in AlCl3 raw materials and Al2O3 products (unit: ppm)

[0040] According to the data analysis in Table 1, compared with the total impurities requirement of ≤50ppm corresponding to the 4N5 standard: the total impurities of product E1 are about 6.7ppm, product E2 are about 19.7ppm, and product E3 are about 14.0ppm. The total impurities of all three batches are less than 50ppm, and all meet the total impurities requirement of the 4N5 standard.

[0041] Experimental Example 2 This experimental example uses the methods described in Examples 1-6 and Comparative Examples 1-4 to prepare high-purity Al2O3 powder, and the average particle size, purity, and yield of the obtained products are detected and compared to investigate the influence of key parameters of the present invention on product performance, as detailed below: The average particle size of the product was determined using a laser particle size analyzer.

[0042] The purity of the product was determined by inductively coupled plasma mass spectrometry (based on the mass fraction of the main element Al2O3).

[0043] The yield was calculated as follows: Yield = (actual mass of collected Al2O3 powder ÷ theoretical mass of generated Al2O3) × 100%, where the theoretical mass of generated Al2O3 was calculated based on the amount of AlCl3 added in step S2 according to the stoichiometric ratio of the reaction formula 4AlCl3(g) + 3O2(g) → 2α-Al2O3(s) + 6Cl2(g). The product performance test results of each embodiment and comparative example are shown in Table 2 below. Table 2 Results of Product Performance Tests

[0044] Analysis of the data in Table 2 shows that the alumina powders prepared in Examples 1-6 have an average particle size of 42-67 nm, a purity of 99.995%-99.998% (corresponding to 4N5-4N8 level), and a yield of 89.6%-92.1%. Among them, in Example 2, the particle size was the smallest (42 nm), the purity was the highest (99.997%), and the yield was the highest (92.1%) when the amount of Y2O3 added was increased to 8 parts, indicating that an appropriate increase in Y2O3 can increase the oxygen vacancy concentration, enhance the catalytic effect, and refine the grain size. In Example 4, when the activation temperature was reduced to 1350℃, the particle size increased to 50 nm and the yield decreased to 89.6%, indicating that the reduction in activation temperature affects the yield of Y2O3. 3+ Diffusion efficiency; furthermore, in Example 5, when the quenching time was extended to 15ms, the particle size increased to 65nm, verifying that the present invention can still obtain nanoscale high-purity alumina products within this quenching time, and the data consistency is good.

[0045] Furthermore, Comparative Example 1 showed a product purity of 99.99%, a particle size of 120 nm, and a yield of 85.3%, verifying that the absence of Y2O3 led to a slower reaction rate and an increased particle size; Comparative Example 2 showed a product purity of 99.98%, a particle size of 95 nm, and a yield of 82.7%, verifying that the absence of boehmite sol led to an incomplete coating and Cl2 leakage contamination; Comparative Example 3 showed a product purity of 99.99%, a particle size of 180 nm, and a yield of 83.9%, verifying that temperatures exceeding 1850℃ after the reaction caused abnormal grain growth and other key issues.

[0046] In summary, the key features of this invention, such as the synergistic addition of Y2O3 and boehmite sol, the reaction temperature not exceeding 1850℃, and the quenching time controlled within 3.5~20ms, are indispensable and work together to achieve the stable preparation of nanoscale high-purity alumina powder. The product purity can reach the level of 4N5 or higher, and the particle size can be controlled at the nanoscale.

Claims

1. A method for producing high-purity alumina, characterized by, Includes the following steps: S1. Combust fuel and oxygen in a reactor, and then line the reactor to obtain an activated reactor. S2. AlCl3 is preheated to sublimation, then transported to the activation reactor via carrier gas, and subsequently oxidized to obtain primary alumina. S3. The activated reactor is cooled to terminate the oxidation reaction in step S2, and then subjected to gas-solid separation to obtain a high-purity alumina product.

2. The method of producing high-purity alumina according to claim 1, characterized by, In step S1, the oxygen content of the combustion is 30% to 50% in excess, and the combustion raises the temperature of the reaction zone to 1300 to 1400°C.

3. The method for preparing high-purity alumina according to claim 1, characterized in that, In step S2, the AlCl3 is preheated to 200~250℃.

4. The method for preparing high-purity alumina according to claim 1, characterized in that, In step S2, the starting temperature of the oxidation reaction is controlled to ensure that the temperature after the oxidation reaction ends does not exceed 1850°C.

5. The method for preparing high-purity alumina according to claim 1, characterized in that, In step S3, the cooling process is as follows: cooling gas is introduced into the reaction product to reduce the temperature of the reaction zone to below the reaction termination temperature within 3.5~20ms to quench the oxidation reaction, and then the temperature is further reduced to ≤220℃ with a cooling duration of 4~6s. And / or, the cooling gas is either nitrogen or argon.

6. The method for preparing high-purity alumina according to any one of claims 1 to 5, characterized in that, The lining process includes the following steps: S11. During the combustion and heating process of the reactor, a composite slurry is sprayed onto the inner lining surface of the reactor to form a sealing coating on the inner lining surface of the reactor. S12. The sealing coating is subjected to oxidative activation treatment to obtain the activated reactor.

7. The method for preparing high-purity alumina according to claim 6, characterized in that, The composite slurry includes (1) and / or (2): (1) By weight, 85-92 parts of α-Al2O3 micro powder, 3-8 parts of Y2O3 nano powder, and 5-10 parts of boehmite sol on a dry basis; (2) Boehmite sol with a solid content of 20 wt% by weight.

8. The method for preparing high-purity alumina according to claim 7, characterized in that, The composite slurry also contains ammonium polyacrylate dispersant, and the amount of ammonium polyacrylate dispersant added is 0.5~1.5wt% of the total solids of the composite slurry.

9. The method for preparing high-purity alumina according to claim 6, characterized in that, In step S11, when the furnace temperature of the reactor is raised to 1300~1350℃, the composite slurry is sprayed onto the inner lining surface of the reactor. After spraying, the temperature is raised to 1350~1400℃ and held for 20~40 minutes. The sealing coating is obtained by sintering. The thickness of the sealing coating is 0.2~0.8mm.

10. The method for preparing high-purity alumina according to claim 6, characterized in that, In step S12, the sealing coating is oxidized and activated at 1350~1400℃ for 30~60 minutes under oxygen-only conditions to obtain the activated reactor.

Citation Information

Patent Citations

  • Method for preparing high-purity aluminium oxide

    CN107500324A