Aerogel microparticle lightweight aggregate, its preparation method and application
By using cellulose ether coating and composite flow field technology, the problem of aerogel powder floating and agglomerating in liquid media was solved, and spherical micro-particle lightweight aggregate suitable for building materials was prepared, which improved the stability of particles and interfacial bonding ability.
Patent Information
- Application Number
- CN202611309036.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-27
- Publication Date
- 2026-11-17
AI Technical Summary
Existing aerogel particle preparation technologies suffer from high equipment and process costs, difficulties in continuous scale-up, and the tendency of hydrophobic aerogel powders to float, agglomerate, and disperse unevenly in liquid media, resulting in poor particle stability and insufficient interfacial bonding ability, which limits their engineering applications.
A cellulose ether coating layer is used to bridge hydrophobic silica aerogel powder. A composite stirring device is used to form a dual-zone composite flow field with an upper axial downward pressure flow and a lower radial shear flow, which realizes the wetting, coating, bridging and particle reconstruction of hydrophobic silica aerogel powder, forming continuous spherical microparticles.
Aerogel microparticle lightweight aggregate with adjustable particle size, high sphericity, and moderate bulk density was prepared, which solved the problem of floating and agglomeration of hydrophobic aerogel powder in liquid media, improved the stability of particles and interfacial bonding ability, and is suitable for building materials.
Smart Images

Figure CN123106050A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the fields of inorganic non-metallic materials, aerogel granulation, lightweight functional aggregates, and building additive manufacturing materials, specifically to an aerogel microparticle lightweight aggregate, its preparation method, and its application. Background Technology
[0002] Silica aerogel is an ultralight material with a three-dimensional nanoporous network structure, possessing excellent properties such as low density, high porosity, low thermal conductivity, and high specific surface area. It has broad application prospects in building energy conservation, thermal insulation, adsorption separation, catalyst carriers, and composite materials. Commercial products are mostly in the form of hydrophobic silica powder, which features low density, large specific surface area, low surface energy, and light particle weight. However, because hydrophobic aerogel powder is difficult to fully wet in aqueous systems, it tends to float on the liquid surface after being added to a liquid medium, accompanied by agglomeration, uneven dispersion, and wide particle size distribution. This leads to poor particle stability and insufficient interfacial bonding during subsequent processing, thus limiting its further engineering applications.
[0003] Existing aerogel particle preparation technologies mainly include spray or drop granulation, emulsion template granulation, sol-gel microsphere preparation, cryogranulation, mechanical spheroidization, and chemical crosslinking and curing. While these methods can improve the powder state, they often require specialized equipment, template agents, crosslinking agents, organic phases, or lengthy post-processing steps. These methods suffer from high equipment and process costs, difficulties in continuous scale-up, and potential alterations to the original pore structure and lightweight thermal insulation properties of the aerogel. Summary of the Invention
[0004] To address the problems existing in the background technology, the present invention provides an aerogel microparticle lightweight aggregate, its preparation method and application. The method is simple and efficient, and the prepared aerogel microparticle lightweight aggregate has high density.
[0005] The technical solution of the present invention to solve the above-mentioned technical problems is as follows: In a first aspect, the present invention provides an aerogel microparticle lightweight aggregate, which is formed by multiple hydrophobic silica aerogel powders bridged by a cellulose ether coating layer, retaining the porous structure of aerogel inside and having a continuous coating layer on the outside.
[0006] According to the above scheme, the particle size of the aerogel microparticle lightweight aggregate is adjustable, ranging from 100 to 4000 micrometers, the arithmetic mean of the two-dimensional apparent sphericity index of the particles is not less than 0.90, and the dry bulk density is 0.05-0.3 g / cm³.
[0007] According to the above scheme, the particle size of the aerogel microparticle lightweight aggregate is concentrated in the range of 400-500 micrometers.
[0008] The aerogel microparticle lightweight aggregate of the present invention has a spherical particle structure formed by the bridging and stacking of hydrophobic silica aerogel powder through cellulose ether.
[0009] Secondly, the present invention provides a method for preparing the above-mentioned aerogel microparticle lightweight aggregate, comprising the following steps: S1. Weigh the raw materials and mix and disperse the raw materials except for the hydrophobic silica aerogel powder evenly to obtain an aerogel polymer dispersion system. S2. The aerogel polymer dispersion system is added to a composite stirring device. The composite stirring device is equipped with an upper three-bladed propeller stirrer and a lower dispersion disc at intervals along the height direction. In the working state, a dual-zone composite flow field is formed, consisting of an upper axial downward pressure zone and a lower radial shear zone. During the stirring process, hydrophobic silica aerogel powder is added in small amounts multiple times. Under the action of the dual-zone composite flow field, the raw materials are agglomerated, sheared, and rearranged to form wet aerogel microparticles. S3. Separate and dry the wet aerogel microparticles to obtain the aerogel microparticle lightweight aggregate.
[0010] According to the above scheme, the raw materials of the aerogel microparticle lightweight aggregate include the following components in parts by weight: 40-100 parts of hydrophobic silica aerogel powder, 0.1-2 parts of cellulose ether, 0.2-3 parts of dispersant, and 100 parts of water.
[0011] Preferably, based on 100 parts by weight of water, the hydrophobic silica aerogel powder comprises 62.5-82.5 parts by weight, the cellulose ether comprises 0.4-0.8 parts by weight, and the dispersant comprises 0.8-1.5 parts by weight; more preferably, the cellulose ether comprises 0.5 parts by weight and the dispersant comprises 1 part by weight.
[0012] According to the above scheme, the cellulose ether is selected from one or more of hydroxypropyl methylcellulose (HPMC), hydroxyethyl cellulose (HEC), methylcellulose (MC), hydroxypropyl cellulose (HPC), hydroxyethyl methylcellulose (HEMC), and carboxymethyl cellulose (CMC).
[0013] According to the above scheme, the dispersant is selected from one or more of sodium dodecyl sulfate (SDS), sodium α-olefin sulfonate (AOS), sodium fatty alcohol polyoxyethylene ether sulfate (AES), sodium dodecylbenzene sulfonate (SDBS), lignin sulfonate, and hexadecyltrimethylammonium bromide (CTAB).
[0014] According to the above scheme, the average particle size of the hydrophobic silica aerogel powder is 40-120μm, preferably 40-100μm.
[0015] According to the above scheme, in step S1, cellulose ether is first added to water and stirred until dissolved or evenly dispersed to form a polymer coating solution. Then, a dispersant is added and stirring continues to obtain a polymer dispersion system capable of wetting and polymerically coating hydrophobic silica aerogel powder. This polymer dispersion system can reduce the interfacial resistance when hydrophobic silica aerogel powder enters the aqueous phase system, improve its wetting and dispersing ability, and form a continuous polymer coating layer on the particle surface, providing conditions for subsequent particle bridging, self-assembly, and spherical reconstruction.
[0016] According to the above scheme, in step S2, the hydrophobic silica aerogel powder is added in 3-5 batches. After each addition, the dual-zone composite flow field is maintained for 30 seconds to 5 minutes, so that the added silica aerogel powder undergoes wetting, coating, bridging and particle reconstruction before the next batch is added. The formation and growth process of aerogel microparticles can be controlled by adjusting the batch, the amount added per batch, the inter-batch interaction time, the axial transport action and the radial shear action.
[0017] According to the above scheme, the upper three-blade propeller mixer and the lower dispersing disc are synchronously driven by the same drive shaft.
[0018] According to the above scheme, the rotation speed of the upper three-blade propeller mixer and the lower dispersing disc is 500-2000 rpm.
[0019] According to the above scheme, the drying temperature in step S3 is 30-80℃, preferably 40-60℃, in order to maintain the original porous structure and lightweight properties of the aerogel.
[0020] The aforementioned composite mixing device includes a mixing container, a drive assembly, a three-bladed propeller mixer located in the upper part of the mixing container, and a dispersion disk located in the lower part of the mixing container; the drive assembly has an output end that synchronously drives the three-bladed propeller mixer and the dispersion disk; the three-bladed propeller mixer is configured to form an axial downward pressure circulating flow, and the dispersion disk is configured to form a radial shear flow.
[0021] Thirdly, the present invention provides the application of the above-mentioned aerogel microparticle aggregate in cement-based additive manufacturing materials, thermal insulation mortar, thermal insulation coating, lightweight thermal insulation board or polymer thermal insulation composite material.
[0022] The beneficial effects of this invention are as follows: This invention adopts a small-batch, multiple-feeding method, which allows the hydrophobic silica aerogel powder to gradually complete wetting, coating, and interparticle bridging. After forming a continuous agglomerate that can be transported as a whole, the continuous agglomerate is transported to the radial shear region formed by the lower dispersion disc by the axial downward pressure flow generated by the upper three-bladed propeller agitator, so that it undergoes shearing splitting, rolling rearrangement, and spheroidization. The subsequently added aerogel powder is further adsorbed onto the surface of the formed microparticles and continues to grow. This makes the dispersion, critical agglomeration, overall transport, shear reconstruction, and particle growth a continuous granulation process, reducing the powder floating and local disordered agglomeration that are easy to occur during one-time feeding. Moreover, the critical agglomeration state that can be transported as a whole is used as the process node for composite flow field control, so that the dispersion, agglomeration, and particle reconstruction steps form a continuous and observable process chain. It is convenient to adjust the feeding and stirring process according to the overall downward movement of particles and the reconstruction phenomenon after shearing. The process is simple and does not require precision equipment.
[0023] Furthermore, the cellulose ether and the dispersant work together to improve the wetting and bridging conditions of the hydrophobic silica aerogel powder in the aqueous phase, so that the sheared microparticles still maintain the bridging structure and provide a surface for the subsequent adsorption and growth of particles. Attached Figure Description
[0024] Figure 1 A three-dimensional dual-zone composite flow field simulation diagram showing the combined effect of the upper axial downward pressure flow field and the lower radial shear flow field. Figure 2 This is a diagram showing the velocity distribution in the XY direction across the horizontal cross section of the composite flow field. Figure 3 This is a schematic diagram of the velocity distribution of the composite flow field in the YZ plane. Figure 4 A schematic diagram illustrating the mechanism of aerogel particle wetting and coating, critical aggregation, overall compression transport, shear splitting and reconstruction, and re-adsorption growth; Figure 5 The diagram shows the structure of the composite flow field stirring device and the top view of the dispersion disk. A is the structural diagram of the composite flow field stirring device, and B is the top view of the dispersion disk. Figure 6 Macroscopic stage photographs of the aerogel microparticle preparation process; Figure 7 The microstructure of aerogel as it grows from initial powder, initial mixing, and primary microspheres to its final formed state; Figure 8 The two-dimensional roundness, two-dimensional sphericity, and two-dimensional apparent sphericity index of the final formed microspheres; Figure 9 These are photographs of wet and dry aerogel microparticles obtained in groups G1 and G2 of Example 1 using different dispersants; Figure 10These are the products obtained from groups G2 and G3 in Example 1 using different rotation speeds.
[0025] Among them, 1. stirring container, 2. drive assembly, 3. three-blade propeller mixer, 4. dispersion disc, 5. axial downward pressure circulation flow, and 6. radial shear flow. Detailed Implementation
[0026] The principles and features of the present invention are described below with reference to the accompanying drawings and specific embodiments. The examples given are only for explaining the present invention and are not intended to limit the scope of the present invention.
[0027] This invention provides an aerogel microparticle lightweight aggregate, which is formed by multiple hydrophobic silica aerogel powders bridged by a cellulose ether coating layer. The aerogel retains its porous structure inside and has a continuous coating layer on the outside.
[0028] In some specific embodiments, the particle size of the aerogel microparticle lightweight aggregate is adjustable, ranging from 100 to 4000 micrometers, with an arithmetic mean of the two-dimensional apparent sphericity index of the particles not less than 0.90, and a dry bulk density of 0.05-0.3 g / cm³.
[0029] Preferably, the particle size of the aerogel microparticle lightweight aggregate is concentrated in the range of 400-500 micrometers.
[0030] Aerogel microparticle lightweight aggregate has a spherical particle structure formed by the bridging and stacking of hydrophobic silica aerogel powder through cellulose ether.
[0031] The present invention also provides a method for preparing the above-mentioned aerogel microparticle lightweight aggregate, comprising the following steps: S1. Weigh the raw materials and mix and disperse the raw materials except for the hydrophobic silica aerogel powder evenly to obtain an aerogel polymer dispersion system. S2. The aerogel polymer dispersion system is added to the composite stirring device. The composite stirring device is equipped with an upper three-blade propeller stirrer and a lower dispersion disc at intervals along the height direction. In the working state, a dual-zone composite flow field is formed, consisting of an upper axial downward pressure zone and a lower radial shear zone. During the stirring process, hydrophobic silica aerogel powder is added to the composite stirring device in small amounts and multiple times. Under the action of the dual-zone composite flow field, the raw materials are agglomerated, sheared, and rearranged to form wet aerogel microparticles. S3. Separate and dry the wet aerogel microparticles to obtain the aerogel microparticle lightweight aggregate.
[0032] The upper three-bladed propeller agitator and lower dispersing disc within the composite mixing device form a dual-zone composite flow field consisting of an upper axial downward compression zone and a lower radial shear zone. This composite flow field triggers critical aggregation and remodeling. A three-dimensional simulation diagram of the synergistic effect of the upper axial downward compression flow field and the lower radial shear flow field is shown below. Figure 1 As shown, the velocity distribution diagram in the XY direction of the horizontal cross section of the composite flow field is as follows: Figure 2 As shown, the velocity distribution diagram in the YZ direction of the vertical section is as follows: Figure 3 As shown. Specifically, the added hydrophobic silica aerogel powder undergoes wetting, coating, and bridging. When the system transitions from a predominantly discrete state to a state where it forms a continuous aggregate that can be transported as a whole under the action of an axially downward pressure flow field, this state is defined as the critical aggregation state. After reaching the critical aggregation state, the continuous aggregate is transported downward under the action of the axially downward pressure flow field and enters the lower radial shear zone. Through shearing, splitting, rolling rearrangement, and spheroidization, it forms multiple spherical aerogel microparticles. The added hydrophobic silica aerogel powder is adsorbed onto the surface of the spherical aerogel microparticles formed above, causing them to grow and densify.
[0033] As hydrophobic silica aerogel powder is continuously added, the particles in the system undergo wetting, dispersion, collision, and gradual enrichment processes. In the initial stage, due to the low particle concentration, the system is mainly in a dispersed state and cannot yet form stable spherical particles. As the amount added increases, a continuous contact network gradually forms between the particles. When the system reaches a critical aggregation state, the particle aggregates, under the action of an axial downward pressure flow field, enter the high-shear region formed by the lower dispersion disk. Under radial shear, they undergo redispersion, rolling, collision, and bridging reconstruction, and the large-size aggregates gradually transform into multiple spherical microparticles. In subsequent continuous feeding processes, newly added particles are continuously adsorbed onto the surface of the spherical microparticles and undergo continuous adsorption, growth, and densification processes, ultimately forming aerogel microparticles with uniform particle size, stable structure, and high sphericity. A schematic diagram of the mechanism of aerogel particle wetting and coating, critical aggregation, overall downward pressure transport, shear splitting and reconstruction, and re-adsorption and growth is shown below. Figure 4 As shown.
[0034] In step S2, the hydrophobic silica aerogel powder is added in 3-5 batches. After each addition, the dual-zone composite flow field is maintained for 30 seconds to 5 minutes before the next addition. The particle size and particle size distribution of the resulting aerogel microparticles are adjusted by regulating the batch size, the amount added per batch, the inter-batch interaction time, and the radial shear strength. The inter-batch interaction time is used to allow the previously added hydrophobic silica aerogel powder to complete wetting, cellulose ether coating, inter-particle bridging, and shear reconstruction. If the inter-batch interaction time is too short, the previously added powder has not yet formed a relatively stable coating and bridging structure, and continued addition can easily lead to localized enrichment of the powder. As the inter-batch interaction time increases, the added particles gradually complete agglomeration and reconstruction, and can serve as an adsorption and growth matrix for subsequently added particles. Radial shear strength is affected by factors such as the rotational speed of the dispersion disc, the size of the dispersion disc, the tooth structure, the relative position of the dispersion disc and the stirring vessel, and the rheological properties of the system; axial transport is affected by factors such as the rotational speed of the three-bladed propeller agitator, the blade size, the blade inclination angle, the installation height, and the rheological properties of the system; axial transport and radial shear together determine the transport, splitting, rearrangement, and re-adsorption process of continuous agglomerates.
[0035] Hydrophobic silica aerogel powder, with its surface modified for hydrophobicity, exhibits low surface free energy and high hydrophobicity, making it prone to floating, difficult to wet, and easily agglomerate in aqueous systems. This invention utilizes the synergistic effect of a polymer coating system and a composite flow field to achieve a controllable transformation of hydrophobic silica aerogel powder from a dispersed state to spherical microparticles, without the need for traditional granulation processes such as chemical crosslinking agents, template agents, or spray granulation.
[0036] In one specific embodiment of the present invention, a schematic diagram of the composite stirring device is shown below. Figure 5 As shown, the above-mentioned composite stirring device includes a stirring container 1, a driving assembly 2, a three-bladed propeller agitator 3 located at the upper part of the stirring container, and a dispersing disk 4 located at the lower part of the stirring container; the driving assembly has an output end that synchronously drives the three-bladed propeller agitator and the dispersing disk; the three-bladed propeller agitator is configured to form an axial downward pressure circulating flow 5, and the dispersing disk is configured to form a radial shear flow 6.
[0037] The aforementioned aerogel microparticle aggregates can be used to prepare cement-based additive manufacturing materials, thermal insulation mortars, thermal insulation coatings, lightweight thermal insulation boards, or polymer thermal insulation composite materials.
[0038] Example 1: Preparation of Aerogel Microparticle Lightweight Aggregate In this embodiment, the raw materials for preparing aerogel microparticle lightweight aggregate are: 33 g of hydrophobic silica aerogel powder, 0.2 g of hydroxypropyl methylcellulose (HPMC, nominal viscosity of 60000-200000 mPa·s, the nominal viscosity being the viscosity of a 2wt% aqueous solution at 20 degrees Celsius as stated in the supplier's product manual), 0.4 g of sodium dodecyl sulfate (SDS), and 40 g of deionized water, wherein the particle size of the hydrophobic silica aerogel powder is 40 micrometers.
[0039] The specific preparation method is as follows: HPMC was added to water and stirred until homogeneous to obtain a polymer coating solution. SDS was then added to the polymer coating solution to obtain a polymer dispersion system.
[0040] The composite stirring device was adjusted to a working state capable of forming an axial downward pressure flow field and a radial shear flow field. The polymer dispersion system was added to the composite stirring device, and hydrophobic silica aerogel powder with an average particle size of approximately 40 micrometers was added in 5 batches, with 6.6 g added in each batch. The rotation speed of the composite flow field was 2000 r / min. After the first batch was added, the composite flow field was maintained for 60 s before adding the second batch. Subsequent batches were added at 60 s intervals. After the fifth batch was added, stirring was continued for 10 min until the particle size and morphology of the microparticles were basically stable.
[0041] As aerogel powder is continuously added, the system gradually transitions from a floating and dispersed state to a continuous agglomeration state. When the critical agglomeration state is reached, the powder exhibits a significant overall downward pressure, and the hydrophobic aerogel transforms from a powder state to a microparticle state, accompanied by the particles bulging and circulating from the cup wall. After stirring for another 5 to 15 minutes, the microparticle size tends to stabilize. To characterize the evolution of the particles over time, the moment when the aerogel powder is first added is denoted as t0, and the moment when the overall downward movement of the continuous agglomerates is first observed is denoted as t1: Before t0 to t1, the particles successively exhibit floating on the liquid surface, gradual wetting, and dispersion and coating; at t1, the coated particles form a continuously transportable agglomerate and undergo overall downward pressure; after t1, the continuous agglomerate enters the radial shear zone, splitting and rolling rearrange to form multiple primary spherical microparticles, denoted as t2; after stirring for another 10 minutes, the primary microparticles reach a relatively stable size state through re-adsorption growth and densification, denoted as t3. Samples have been taken at each stage and recorded using microscopic imaging.
[0042] The aerogel powder was added in small amounts multiple times. The preparation process was recorded sequentially, including the aqueous polymer phase, the polymer dispersion containing the dispersant, the initial feeding stage, the continued growth of the primary microspheres, and the final saturation state. Macroscopic stage photographs are shown below. Figure 6 As shown; the corresponding microstructure is as follows Figure 7 As shown. By Figure 7It can be seen that after the initial mixing, the initial powder comes into contact with the polymer agglomerate, and then forms primary microspheres, which continue to grow in subsequent feeding, eventually resulting in a microsphere body with relatively complete boundaries.
[0043] The obtained wet microparticles were separated and dried at a low temperature of 40 to 60 degrees Celsius to obtain spherical aerogel microparticle lightweight aggregate. This lightweight aggregate is formed by multiple hydrophobic silica aerogel powders connected by a cellulose ether bridging layer, maintaining a porous internal structure and having a continuous coating layer on the outside.
[0044] For both the initial powder and the final formed microspheres, ImageJ / Fiji was used for two-dimensional image characterization: spatial calibration, grayscale conversion, and background subtraction were performed first, followed by thresholding and watershed segmentation to separate adherent particles; only particles with closed contours, continuous white bodies, areas exceeding a preset minimum threshold, and not truncated by image boundaries were retained. Particle size was characterized by the maximum two-dimensional Feret particle size or the two-dimensional equivalent circle diameter; two-dimensional roundness was calculated using 4πA / P². The average values of the two-dimensional roundness, two-dimensional sphericity, and two-dimensional apparent sphericity index of the final formed microspheres were 0.984, 0.864, and 0.920, respectively. The sample size was 54, and the error bar was the standard deviation. Figure 8 As shown.
[0045] Example 2: Effects of different dispersant systems, stirring intensity, and aerogel powder particle size on particle structure Following the method in Example 1, SDS and CTAB were used as dispersants for comparison, and the effect of stirring intensity on particle structure was determined by adjusting the shear strength of the lower dispersion disc. The specific raw material ratios, aerogel powder particle sizes, and stirring speeds for different groups are shown in Table 1 below.
[0046] Table 1
[0047] Photographs of dry and wet aerogel microparticles from groups G1 and G2 are shown below. Figure 9 As shown, the test results showed that in group G1, the bulk density of wet aerogel microparticles obtained using CTAB as a dispersant was approximately 0.132 g / cm³, and the bulk density of dry aerogel microparticles obtained after drying was approximately 0.080 g / cm³. In group G2, the wet bulk density obtained using SDS as a dispersant was approximately 0.166 g / cm³, and the dry bulk density was approximately 0.098 g / cm³. Aerogel granulation was observed in both systems. The particles obtained from the SDS system were more dense and uniform under the experimental conditions; therefore, SDS was chosen as the preferred dispersant.
[0048] Groups G2, G3, and G6 were stirred at different speeds, with G2 and G3 yielding products as follows: Figure 10As shown, group G2 forms stable particles with relatively dense and uniform structure, while group G3 cannot form stable particles, resulting in finer / loose materials. Group G6 can also form stable particles (not shown in the figure). This is because as the radial shear in the lower part increases, local large agglomerates are broken up in time, and the rolling rearrangement and sphericity of microparticles are improved. However, the shear in G3 is too strong, causing excessive destruction of the already formed bridging structure. If the shear is insufficient, the system is prone to retaining irregular flocs. Therefore, the lower dispersion disc should provide sufficient but not excessive radial shear, and match it with the upper axial downward pressure transport.
[0049] Groups G2, G4, and G5 use aerogel powder particles with different particle sizes (40μm, 25μm, and 80μm). Among them, group G4 cannot form complete and stable spherical microparticles, while groups G2 and G5 can complete critical aggregation and shear reconstruction and form microparticles.
[0050] Experimental results show that, under the same process conditions, hydrophobic aerogel powders with an average particle size of about 25 μm and below are prone to forming stable flocs during the process of composite flow field due to their larger particle specific surface area and enhanced interparticle interaction. They are difficult to complete the rearrangement process from particle aggregates to spherical dense microparticles, and ultimately fail to obtain spherical microparticles with complete morphology and stable structure.
[0051] Under the conditions of the composite flow field, continuous batch feeding and polymer dispersion system described in this invention, hydrophobic silica aerogel powders with average particle sizes of about 40 micrometers and 80 micrometers can complete the processes of wetting, dispersion, critical aggregation, shear reconstruction and microparticle growth.
[0052] Examples using hydrophobic silica aerogel powders with average particle sizes of approximately 40 micrometers and 80 micrometers demonstrate that microparticles can be formed within the process window of this invention. The feeding rate, critical agglomeration state, and final particle size distribution may differ for different raw material particle sizes and should be selected in conjunction with actual process parameters.
[0053] The above experimental results show that, under the process conditions described in this invention, the initial particle size of the aerogel powder is an important factor affecting wetting, critical agglomeration, and microparticle growth behavior. Preferably, hydrophobic silica aerogel powder with an average particle size of 40–120 micrometers is used; more preferably, hydrophobic silica aerogel powder with a particle size of 40–100 micrometers is used.
[0054] Example 3: Application of Aerogel Microparticle Lightweight Aggregate The hydrophobic aerogel microparticle lightweight aggregate obtained in Example 1 can be added to cement-based additive manufacturing materials to replace part of the fine aggregate or used as a lightweight functional aggregate. Compared with the direct addition of easily floating hydrophobic aerogel powder, spherical microparticles exhibit better operability in terms of metering, feeding, and slurry dispersion. The specific improvement in rheology, extrudability, mechanical properties, and thermal conductivity should be determined through comparative experiments based on the actual formulation.
[0055] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. An aerogel microparticle lightweight aggregate, characterized in that, It is formed by bridging multiple hydrophobic silica aerogel powders with a cellulose ether coating layer, retaining the porous structure of the aerogel inside and having a continuous coating layer on the outside.
2. The aerogel microparticle lightweight aggregate according to claim 1, characterized in that, The aerogel microparticle lightweight aggregate has an adjustable particle size, ranging from 100 to 4000 micrometers, with an arithmetic mean of the two-dimensional apparent sphericity index of the particles not less than 0.90, and a dry bulk density of 0.05-0.3 g / cm³.
3. The method for preparing aerogel microparticle lightweight aggregate as described in claim 1 or 2, characterized in that, Includes the following steps: S1. Weigh the raw materials and mix and disperse the raw materials except for the hydrophobic silica aerogel powder evenly to obtain an aerogel polymer dispersion system. S2. The aerogel polymer dispersion system is added to a composite stirring device. The composite stirring device is equipped with an upper three-bladed propeller stirrer and a lower dispersion disc at intervals along the height direction. In the working state, a dual-zone composite flow field is formed, consisting of an upper axial downward pressure zone and a lower radial shear zone. During the stirring process, hydrophobic silica aerogel powder is added in small amounts multiple times. Under the action of the dual-zone composite flow field, the raw materials are agglomerated, sheared, and rearranged to form wet aerogel microparticles. S3. Separate and dry the wet aerogel microparticles to obtain the aerogel microparticle lightweight aggregate.
4. The method for preparing aerogel microparticle lightweight aggregate according to claim 3, characterized in that, The raw materials of the aerogel microparticle lightweight aggregate include the following components in parts by weight: 40-100 parts of hydrophobic silica aerogel powder, 0.1-2 parts of cellulose ether, 0.2-3 parts of dispersant, and 100 parts of water.
5. The method for preparing aerogel microparticle lightweight aggregate according to claim 4, characterized in that, The cellulose ether is selected from one or more of hydroxypropyl methylcellulose, hydroxyethyl cellulose, methylcellulose, hydroxypropyl cellulose, hydroxyethyl methylcellulose, and carboxymethyl cellulose.
6. The method for preparing aerogel microparticle lightweight aggregate according to claim 4, characterized in that, The dispersant is selected from one or more of sodium dodecyl sulfate, sodium α-olefin sulfonate, sodium fatty alcohol polyoxyethylene ether sulfate, sodium dodecylbenzene sulfonate, lignin sulfonate, and hexadecyltrimethylammonium bromide.
7. The method for preparing aerogel microparticle lightweight aggregate according to claim 4, characterized in that, The average particle size of the hydrophobic silica aerogel powder is 40-120 μm.
8. The method for preparing aerogel microparticle lightweight aggregate according to claim 3, characterized in that, In step S2, the hydrophobic silica aerogel powder is added in 3-5 batches. After each addition, the dual-zone composite flow field is maintained for 30 seconds to 5 minutes, allowing the added silica aerogel powder to undergo wetting, coating, bridging, and particle reconstruction before the next batch is added. The formation and growth process of aerogel microparticles are controlled by adjusting the batch size, the amount added per batch, the inter-batch interaction time, the axial transport action, and the radial shear action.
9. The method for preparing aerogel microparticle lightweight aggregate according to claim 3, characterized in that, The upper three-blade propeller mixer and the lower dispersing disc rotate at 500-2000 rpm.
10. The application of the aerogel microparticle lightweight aggregate according to claim 1 or 2 in cement-based additive manufacturing materials, thermal insulation mortar, thermal insulation coating, lightweight thermal insulation board or polymer thermal insulation composite material.