A method for preparing large aerogel spheres
Large aerogel spheres were prepared by heating with thermal radiation and vibration using water-soluble cellulose ethers. This solved the problem of easy breakage of silica aerogel particles during transportation and construction, improved stability and volume utilization, reduced costs, and maintained thermal insulation performance.
Patent Information
- Application Number
- CN202611410639.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-17
AI Technical Summary
Silica aerogel particles are easily broken and pulverized during transportation, mixing and construction, and have low volume utilization, resulting in high material costs and affecting their large-scale application in the field of building insulation.
Large aerogel spheres were prepared by using water-soluble cellulose ether to form a continuous adhesive network under thermal radiation heating conditions, combined with vibration and tumbling, to achieve thermal bonding and assembly of multiple aerogel particles.
It improves the overall stability and volume utilization efficiency of aerogel particles, reduces breakage and pulverization, maintains lightweight thermal insulation performance, and reduces material costs.
Smart Images

Figure CN123106076A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of building materials technology, and in particular to a method for preparing large-particle aerogel spheres. Background Technology
[0002] Silica aerogel is an ultralight inorganic material with a nanoporous network structure, characterized by low density, high porosity, low thermal conductivity, and excellent resistance to high and low temperatures. It has broad application prospects in building insulation materials, aerospace, energy, and thermal insulation protection. In recent years, to balance workability and insulation performance, silica aerogel particles have been widely used as lightweight insulating aggregates in cement-based building insulation materials, lightweight concrete, and precast insulation components.
[0003] However, due to the loose skeletal structure and low mechanical strength of silica aerogel particles, they are prone to breakage and pulverization during raw material transportation, mixing, and construction. This leads to a reduction in particle size or even powder formation, which not only weakens the lightweight insulation effect of the aerogel particles but also causes uneven dispersion of particles in cement-based materials, affecting the overall performance of the material. Furthermore, existing aerogel particles are typically small in size, requiring a large dosage to achieve a certain volumetric content when incorporated into cement-based materials, resulting in higher material costs and limiting their large-scale application in building insulation.
[0004] Currently, research on improving the mechanical stability of aerogel particles mainly focuses on methods such as particle surface coating modification, resin coating, or inorganic slurry coating. Although these methods can improve the particle's resistance to breakage to some extent, most still target individual aerogel particles for modification, failing to fully improve the volume utilization efficiency of aerogel particles in cement-based materials. Furthermore, some coating layers are quite dense, which can easily increase the material's thermal conductivity, hindering the maintenance of the aerogel material's excellent thermal insulation properties.
[0005] Therefore, developing a preparation method that can stably assemble multiple aerogel particles into large spheres while ensuring lightweight thermal insulation performance and improving particle mechanical stability and volume utilization efficiency is of great significance for promoting the engineering application of aerogel materials in cement-based building insulation materials. Summary of the Invention
[0006] To address the problems of low mechanical strength, easy breakage and pulverization during transportation, mixing and construction, low volume utilization and high application cost of existing silica aerogel particles, this invention proposes a method for preparing large aerogel spheres. This method utilizes water-soluble cellulose ether to form a continuous adhesive network under thermal radiation heating conditions, and achieves thermal bonding and assembly of multiple aerogel particles under vibration and tumbling action, thus preparing large aerogel spheres with a certain particle size and retaining the pores between particles, thereby improving the overall stability and engineering application performance of aerogel particles.
[0007] The technical solution of this invention is achieved as follows: This invention provides a method for preparing large-particle aerogel spheres, comprising the following steps: S1, place the aerogel particles in a vibratory tumbling device to keep the aerogel particles in continuous tumbling motion, preheat the tumbling aerogel particles, and spray a cellulose ether aqueous solution onto the surface of the aerogel particles after the aerogel particles reach the preset temperature. After spraying, continue to heat them by thermal radiation, so that the cellulose ether aqueous solution gradually dehydrates to form a continuous adhesive network. Under the continuous tumbling action, multiple aerogel particles collide, aggregate, and thermally bond and assemble to form spheres, forming large aerogel green spheres. The resulting large aerogel green spheres retain the interparticle pores and the nanoporous structure of the aerogel itself. S2, stop heating and keep the large aerogel pellets tumbling continuously. The cellulose ether continuously binds the network, cools and solidifies, and obtains structurally stable large aerogel pellets.
[0008] Based on the above technical solutions, preferably, the vibratory tumbling equipment is one of a vibratory polishing machine, a ball rolling machine, or a cylindrical mixer, which keeps the aerogel particles in continuous tumbling motion throughout the assembly process, and promotes particle aggregation and thermal bonding assembly into spheres through mutual collision and rolling between particles.
[0009] Specifically, during the cellulose ether aqueous solution spraying stage, the thermal bonding assembly stage, and the cooling curing stage, the aerogel particles maintain continuous tumbling motion to prevent local particle agglomeration and promote the uniform assembly of multiple aerogel particles into large aerogel spheres.
[0010] Based on the above technical solutions, preferably, the mass ratio of the aerogel particles, cellulose ether and water is 40-60:10-20:400-600.
[0011] Based on the above technical solutions, preferably, the cellulose ether aqueous solution also contains SiO2 aerogel powder.
[0012] Based on the above technical solutions, preferably, the amount of SiO2 aerogel powder added is 2%-3% of the mass of the cellulose ether, the particle size of the SiO2 aerogel powder is 10 nm-50 μm, and the specific surface area is 500-1200 m². 2 / g. The fine SiO2 aerogel powder is uniformly dispersed in the cellulose ether aqueous solution by high-speed shearing or ultrasonic dispersion.
[0013] Based on the above technical solutions, preferably, the aerogel particles are silicone aerogel particles with a particle size of 1-3 mm.
[0014] Based on the above technical solutions, preferably, the cellulose ether is one or more of hydroxypropyl methylcellulose ether, methylcellulose, hydroxyethyl cellulose and carboxymethyl cellulose; the viscosity of the cellulose ether is 1000-10000 mPa·s.
[0015] Based on the above technical solutions, preferably, the preheating temperature of the aerogel particles in step S1 is 30-50℃, and the temperature is further increased to 60-90℃ after the cellulose ether aqueous solution is sprayed.
[0016] The temperature of 30-50℃ is far below the "gel temperature" of cellulose ethers (usually 54-90℃, varying depending on the type). At this temperature, the sprayed solution will not gel immediately but will remain in a flowing liquid state. This allows the cellulose ether solution sufficient time to uniformly wet and adhere to the surface of each aerogel particle as the particles continue to tumble, laying the foundation for the subsequent formation of a uniform adhesive network.
[0017] When the system temperature rises to the gel point of cellulose ether (typically 54-70℃ or higher, depending on the type), the polymer chains in the solution begin to dehydrate and entangle, transforming from a free-flowing liquid into a solid gel with a certain strength and elasticity. This reversible physical gelation process is the direct driving force for achieving "thermal adhesion" between particles.
[0018] Based on the above technical solutions, preferably, the cellulose ether aqueous solution is added by multiple intermittent spraying, with 3-5 spraying times, each spraying amount being the same, a single spraying time of 5-20 seconds, and an interval of 10-120 seconds between two adjacent sprays.
[0019] If a large amount of solution is sprayed at once, it can easily lead to the concentration of binder in localized areas, forming "bridging flocculation"—that is, a single polymer chain simultaneously adsorbs multiple particles, which actually exacerbates local agglomeration. This invention, through small, multiple, and spaced sprays, allows each added cellulose ether aqueous solution sufficient time to be evenly spread and wetted during particle tumbling, avoiding agglomeration caused by excessively high local concentrations. This is consistent with the principle that aerogel dispersion in aqueous media requires "batch addition."
[0020] As mentioned earlier, the binding effect of cellulose ethers requires dehydration and gelation at 60-90℃ to be effective. Through intermittent spraying, a new batch of binder "seeds" is introduced into the system with each spray. Utilizing the 10-120 second intervals between sprays, the already wetted particles undergo initial collision, dehydration, and binding under tumbling and heating, forming small aggregate units. Subsequently, the addition of the next batch of binder promotes the reconnection of these small units, eventually growing into uniform large spheres. This essentially breaks down the complex process of "one-step spheric formation" into a multi-step controlled process of "dispersion-initial binding-reaggregation," ensuring the final spheres have a uniform structure and controllable size.
[0021] Based on the above technical solutions, preferably, the heating method in step S1 is thermal radiation heating. The thermal radiation heating method is one of near-infrared heating, mid-infrared heating, far-infrared heating, or halogen radiation heating; the wavelength range of near-infrared heating is 0.75-3 μm; the wavelength range of mid-infrared heating is 3-25 μm; the wavelength range of far-infrared heating is 25-1000 μm; and the wavelength range of halogen radiation heating is 0.76-5 μm.
[0022] Based on the above technical solutions, preferably, in step S2, the rolling is stopped when the temperature of the large aerogel pellets drops to 20-40 ℃.
[0023] The method for preparing large aerogel spheres according to the present invention has the following advantages over the prior art: (1) The present invention utilizes water-soluble cellulose ether to form a continuous bonding network under thermal radiation heating conditions, and realizes the thermal bonding assembly of multiple aerogel particles under vibration and tumbling action. This can prepare dispersed aerogel particles into structurally stable large aerogel balls, improve the overall stability of aerogel particles during transportation, stirring and construction, and reduce particle breakage and pulverization.
[0024] (2) This invention introduces fine SiO2 aerogel powder into a cellulose ether aqueous solution to form an organic-inorganic interpenetrating reinforcement structure in a continuous cellulose ether bonding network. The fine SiO2 aerogel powder, as a rigid nanonode, can effectively transfer and disperse external loads, while forming a good interfacial bond with the cellulose ether matrix, further improving the anti-breakage performance and structural stability of large aerogel spheres.
[0025] (3) The large aerogel spheres prepared by the present invention retain the interparticle pores and the nanoporous structure of the aerogel itself. While ensuring the lightweight and porous characteristics of the aerogel, large aerogel spheres with multi-level pore structure can be formed, which is beneficial to maintaining the excellent lightweight and heat insulation performance of the material.
[0026] (4) The present invention adopts a vibration thermal bonding assembly method to assemble silica aerogel particles with an original particle size of 1-3 mm into large aerogel spheres with a particle size of 4-15 mm. Under the same mass of aerogel particles, a larger filling volume can be formed, which improves the volume utilization efficiency of aerogel particles, helps to reduce the cost of aerogel materials in cement-based building materials, and improves the economic efficiency of engineering applications.
[0027] (5) The present invention adopts a preparation method that combines vibration tumbling and thermal radiation heating. The process is simple, does not require complex granulation equipment, the equipment is easy to obtain, the preparation process is continuous and stable, and it is easy to realize large-scale production and engineering application.
[0028] (6) The present invention enables multiple silica aerogel particles to be assembled from their original dispersed state into large aerogel spheres with a particle size of 4-15 mm. While maintaining the porous structure of the aerogel, the particle size is increased, which is beneficial to reducing the phenomenon of particle breakage and pulverization during transportation and construction. Attached Figure Description
[0029] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0030] Figure 1 A schematic diagram of the preparation process of the method for preparing large aerogel spheres by vibration thermal bonding according to the present invention; 1-Infrared heating lamp, 2-Spraying device, 3-Cellulose ether aqueous solution, 4-Vibration and tumbling device, 5-Large aerogel particles. The dotted line with arrows in the figure indicates the vibration direction of the large aerogel particles.
[0031] Figure 2This is a macroscopic morphology image of the large aerogel spheres prepared in Example 4 of the present invention.
[0032] Figure 3 This is an internal pore diagram of the large aerogel spheres prepared in Example 4 of the present invention.
[0033] Figure 4 Image of unprocessed aerogel particles. Detailed Implementation
[0034] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0035] Example 1
[0036] like Figure 1 As shown, this embodiment provides a method for preparing large aerogel spheres using vibrational thermal bonding, including the following steps: 1. Preparation of cellulose ether aqueous solution: Weigh 500 parts (each part depends on the actual situation, in this example each part is 1g) of water and add it to a spray bottle, then add 15 parts of hydroxypropyl methylcellulose ether (HPMC) with a viscosity of 4000 mPa·s, and shake it thoroughly to make the hydroxypropyl methylcellulose ether evenly dispersed in the water to obtain cellulose ether aqueous solution.
[0037] 2. Add 50 parts of silica aerogel particles (particle size 1-3 mm) to a vibratory polisher (vibration frequency 250 Hz, vibration power 200 W), keeping the silica aerogel particles in continuous tumbling motion, while simultaneously preheating with an infrared heating device (near-infrared heating). When the temperature of the silica aerogel particles rises to 40 ℃, add the cellulose ether aqueous solution intermittently using a spray bottle. During the continuous tumbling of the silica aerogel particles, spray the cellulose ether aqueous solution in 5 applications, each spray lasting 10 s, with a 60 s interval between adjacent sprays. This allows the cellulose ether aqueous solution to gradually wet and adhere to the surface of the silica aerogel particles, entering the contact area between particles as the particles tumble. The vibratory polisher is continuously running during the spraying process, ensuring the silica aerogel particles maintain uniform movement under the impact and rolling action, promoting the uniform distribution of the cellulose ether aqueous solution on the particle surface.
[0038] After spraying, the addition of the cellulose ether aqueous solution was stopped, and the vibratory polisher was kept running continuously while near-infrared heating continued, gradually increasing the system temperature (heating rate of 5 °C / min) to 80 °C. As the temperature rose, the water in the cellulose ether aqueous solution gradually evaporated, and the hydroxypropyl methylcellulose ether gradually concentrated, forming a continuous adhesive network between the aerogel particles. Under the action of vibration and tumbling, the silica aerogel particles continuously collided, rolled, and rearranged. The contact areas between the particles gradually connected under the action of the cellulose ether adhesive network, causing multiple silica aerogel particles to gradually aggregate and assemble into large aerogel green balls. When the system temperature reached 80 °C, the infrared heating device was turned off, but the vibratory polisher continued to run, allowing the formed large aerogel green balls to gradually cool and solidify during continuous tumbling. When the particle temperature dropped to 30 °C, the vibratory polisher was turned off, resulting in structurally stable large aerogel green balls.
[0039] The macroscopic morphology of the large aerogel spheres prepared in Example 1 was observed using a digital camera. Compared with untreated silica aerogel particles, after treatment by the method of this invention, the original irregular silica aerogel particles could connect with each other through cellulose ether bonding to form large aerogel spheres with a more regular spherical structure. The original silica aerogel particles had a particle size range of 1-3 mm, while the large aerogel spheres formed after vibrational thermal bonding had a particle size range of 4-15 mm. A random sample of 100 large aerogel spheres was used for particle size analysis. The results showed that the average particle size was 8.53 ± 1.87 mm, indicating that this invention can achieve the uniform assembly of multiple small-diameter silica aerogel particles to obtain larger spherical particles. The resulting aerogel spheres had a complete overall structure, high sphericity, and no obvious cracks or breakage on the surface.
[0040] Further tests were conducted on the anti-crushing properties of the obtained large-particle aerogel spheres. 50 g samples were randomly selected from the obtained samples for testing. After compression under a 100 N load for 30 s, the samples were sieved using a standard sieve with a 1 mm aperture, and the crushing rate was calculated based on the change in sample mass before and after crushing. Each group of samples was tested in parallel three times, and the average value was taken. The results showed that the crushing rate of the original silica aerogel particles was 46.2±2.1%, while the crushing rate of the large-particle aerogel spheres prepared in this invention was 12.4±1.3%, a reduction of approximately 73.2% compared to the original silica aerogel particles. This indicates that after vibration-thermal bonding assembly, the cellulose ether forms a continuous bonding network in the contact area of multiple silica aerogel particles, connecting multiple particles to form a stable whole. Under external load, this effectively disperses stress, improves the overall mechanical stability of the particles, and thus significantly reduces particle breakage and pulverization during transportation, storage, mixing, and construction.
[0041] Example 2
[0042] The difference between Example 2 and Example 1 is that the viscosity of hydroxypropyl methylcellulose ether is 10000 mPa·s. The specific steps are as follows: 1. Preparation of cellulose ether aqueous solution: Weigh 500 parts (the amount of each part depends on the actual situation, and each part in this example is 1g) of water and add it to a spray bottle. Then add 15 parts of hydroxypropyl methylcellulose ether (HPMC) with a viscosity of 10000 mPa·s. Shake thoroughly to make the hydroxypropyl methylcellulose ether evenly dispersed in the water to obtain cellulose ether aqueous solution.
[0043] 2. Add 50 parts of silica aerogel particles (particle size 1-3 mm) to a vibratory polisher (vibration frequency 250 Hz, vibration power 200 W) to keep the silica aerogel particles in continuous rolling motion, while simultaneously turning on the infrared heating device for preheating (near-infrared heating). When the temperature of the silica aerogel particles rises to 50 ℃ (in this example, HPMC has a high viscosity, so a preheating temperature of 50 ℃ is selected), add the cellulose ether aqueous solution prepared above through a spray bottle using an intermittent spraying method (same as in Example 1). Subsequent steps are the same as in Example 1.
[0044] The large aerogel spheres obtained in this embodiment all have a particle size range of 4-15 mm, indicating that cellulose ethers of different viscosities can achieve thermal bonding and assembly of multiple aerogel particles.
[0045] The macroscopic morphology of the large aerogel spheres prepared in Example 2 was observed using a digital camera. The results showed that when hydroxypropyl methylcellulose ether with a viscosity of 10000 mPa·s was used as the binder, multiple silica aerogel particles could still connect with each other through the cellulose ether bonding effect, forming large aerogel spheres with intact structure and high sphericity. A random sample of 100 large aerogel spheres was selected for particle size analysis. The results showed that the particle size range of the obtained large aerogel spheres was 4-15 mm, with an average particle size of 8.91 ± 1.74 mm, indicating that increasing the viscosity of hydroxypropyl methylcellulose ether does not affect the thermal bonding and assembly process of the aerogel particles.
[0046] The crushing resistance of the obtained large aerogel particles was further tested using the same method as in Example 1. The results showed that the crushing rate of the large aerogel particles prepared in Example 2 was 10.8 ± 1.2%, which was approximately 76.6% lower than the crushing rate of the original silica aerogel particles (46.2 ± 2.1%). This indicates that using a higher viscosity hydroxypropyl methylcellulose ether can form a more stable continuous bonding network between aerogel particles, thereby further improving the overall mechanical stability and crushing resistance of the large aerogel particles.
[0047] Further cross-sectional observation of the large aerogel spheres revealed that the interior of the obtained large aerogel spheres was still composed of multiple silica aerogel particles, with obvious pore structures between the particles. At the same time, the nanoporous structure of the silica aerogel particles themselves was also preserved. This indicates that increasing the viscosity of hydroxypropyl methylcellulose ether does not destroy the original hierarchical pore structure of the aerogel particles. Hydroxypropyl methylcellulose ethers of different viscosity ranges can achieve thermal bonding and assembly of multiple aerogel particles, and large aerogel spheres with good mechanical stability can be prepared.
[0048] Example 3
[0049] This embodiment provides a method for preparing large aerogel spheres using vibrational thermal bonding, including the following steps: 1. Preparation of cellulose ether aqueous solution: Weigh 500 parts (the amount of each part depends on the actual situation, and each part in this example is 1g) of water and add it to a spray bottle. Then add 15 parts of hydroxyethyl cellulose (HEC) with a viscosity of 5000 mPa·s. Shake thoroughly to disperse the hydroxyethyl cellulose evenly in the water to obtain cellulose ether aqueous solution.
[0050] 2. Add 50 parts of silica aerogel particles (particle size 1-3 mm) to a cylindrical mixer, keeping the particles in continuous tumbling motion while simultaneously preheating with an infrared heating device (far-infrared heating). When the silica aerogel particle temperature reaches 40 ℃, add the above-mentioned cellulose ether aqueous solution intermittently using a spray bottle. During the continuous tumbling of the silica aerogel particles, spray the cellulose ether aqueous solution evenly in 5 applications, each spray lasting 10 seconds, with a 60-second interval between adjacent sprays, allowing the cellulose ether aqueous solution to gradually adhere to the surface of the silica aerogel particles. Continue running the cylindrical mixer and continue infrared heating during the spraying process, raising the system temperature to 70 ℃. As the moisture gradually evaporates, the hydroxyethyl cellulose gradually concentrates, forming an adhesive structure in the contact area of the aerogel particles. Under the tumbling action, the silica aerogel particles collide and rearrange, gradually assembling into large aerogel green balls under the action of the cellulose ether. After reaching 70 ℃, the infrared heating device was turned off, while the cylindrical mixer continued to run, allowing the resulting large aerogel pellets to cool and solidify. When the particle temperature dropped to 30 ℃, the equipment was shut off. The resulting large aerogel pellets had a particle size range of 4-15 mm, indicating that cellulose ethers of different types and viscosities can achieve thermal bonding and assembly of multiple aerogel particles.
[0051] The macroscopic morphology of the large aerogel spheres prepared in Example 3 was observed using a digital camera. The results showed that when hydroxyethyl cellulose (HEC) was used as the binding material, multiple silica aerogel particles could still effectively connect during vibration and tumbling, forming large aerogel spheres with a relatively regular spherical structure. A random sample of 100 large aerogel spheres was selected for particle size analysis. The results showed that the particle size range of the obtained large aerogel spheres was 4-15 mm, with an average particle size of 8.18 ± 1.65 mm, indicating that hydroxyethyl cellulose can also promote the stable assembly of multiple silica aerogel particles to form large aerogel spheres.
[0052] The crushing resistance of the obtained large aerogel particles was further tested using the same method as in Example 1. The results showed that the crushing rate of the large aerogel particles prepared in Example 3 was 13.6 ± 1.5%, which was approximately 70.6% lower than the crushing rate of the original silica aerogel particles (46.2 ± 2.1%). This indicates that hydroxyethyl cellulose can form a stable bonded structure between aerogel particles, significantly improving the overall mechanical stability and crushing resistance of the large aerogel particles.
[0053] Further cross-sectional observation of the large aerogel spheres revealed that their internal structure is composed of multiple silica aerogel particles assembled together, with a distinct porous structure between the particles. This also preserves the nanoporous structure of the silica aerogel particles themselves, indicating that using hydroxyethyl cellulose as a binder does not disrupt the original hierarchical porous structure and lightweight properties of the aerogel material. Although its breakage resistance is slightly lower than that of the hydroxypropyl methylcellulose system, it still meets the requirements for preparing large aerogel spheres, further demonstrating the good applicability of this invention to different types of cellulose ethers.
[0054] Example 4
[0055] The difference between this embodiment and Example 1 is that fine SiO2 aerogel powder was added to the cellulose ether aqueous solution. The specific steps are as follows: 1. Preparation of an aqueous solution of cellulose ether containing fine SiO2 aerogel powder: Weigh 500 parts (each part depends on the actual situation; in this example, each part is 1 g) of water and add it to a container. Then add 15 parts of hydroxypropyl methylcellulose ether (HPMC) with a viscosity of 4000 mPa·s, and add 2.5% by mass of fine SiO2 aerogel powder (particle size of 10 nm-50 μm, specific surface area of 800 m²). 2 / g). The fine SiO2 aerogel powder was uniformly dispersed in the cellulose ether aqueous solution by stirring at 3000 rpm for 30 min using a high-speed shear dispersion method, resulting in a cellulose ether aqueous solution containing a nano-reinforcing phase.
[0056] 2. Add 50 parts of silica aerogel particles (particle size 1-3 mm) to a vibratory polisher, keeping the particles in continuous tumbling motion while preheating with an infrared heating device. When the temperature of the silica aerogel particles reaches 40 ℃, add the cellulose ether aqueous solution containing fine SiO2 aerogel powder intermittently using a spray bottle. During the continuous tumbling of the silica aerogel particles, spray the cellulose ether aqueous solution in 5 applications, each spray lasting 10 seconds, with a 60-second interval between adjacent sprays, ensuring the cellulose ether aqueous solution adheres evenly to the surface of the silica aerogel particles. Keep the vibratory polisher running continuously during spraying to maintain uniform movement of the silica aerogel particles due to collision and rolling.
[0057] After spraying, the addition of the cellulose ether aqueous solution was stopped, and the vibratory polisher was kept running continuously while infrared heating continued, gradually raising the system temperature to 80 ℃. As the temperature increased, the water in the cellulose ether aqueous solution gradually evaporated, and the hydroxypropyl methylcellulose ether gradually concentrated, forming a continuous adhesive network between the aerogel particles. Simultaneously, fine SiO2 aerogel powder was uniformly dispersed within the adhesive network, forming an organic-inorganic interpenetrating reinforced structure. Under the vibration and tumbling action, the silica aerogel particles continuously collided, rolled, and rearranged. The contact areas between the particles gradually connected under the action of the reinforced adhesive network, causing multiple silica aerogel particles to gradually aggregate and assemble into large aerogel green balls.
[0058] When the system temperature rises to 80 ℃, the infrared heating device is turned off, while the vibratory polishing machine continues to run, allowing the formed large aerogel spheres to gradually cool and solidify during continuous tumbling. When the particle temperature drops to 30 ℃, the vibratory polishing machine is turned off, resulting in structurally stable large aerogel spheres.
[0059] The macroscopic morphology of the large aerogel spheres prepared in Example 4 was observed using a digital camera. Specific images are shown below. Figure 2 As shown in the figure. The results indicate that the original irregular silica aerogel particles can be interconnected through the bonding effect of cellulose ether containing nano-reinforcing phase to form large aerogel spheres with a more regular spherical structure. The particle size range of the original silica aerogel particles is 1-3 mm, and the particle size range of the large aerogel spheres formed after vibrational thermal bonding assembly is 4-15 mm. A random sample of 100 large aerogel spheres was used for particle size analysis, and the results showed that the average particle size was 8.72 ± 1.65 mm, indicating that the addition of fine SiO2 aerogel powder does not affect the uniform assembly process of multiple small-diameter silica aerogel particles.
[0060] The crushing resistance of the obtained large aerogel spheres was further tested using the same method as in Example 1. The results showed that the crushing rate of the large aerogel spheres prepared in Example 4 was 9.2 ± 0.9%, which was approximately 25.8% lower than that of Example 1 (12.4 ± 1.3%) without the addition of fine SiO2 aerogel powder, and approximately 80.1% lower than that of the original silica aerogel particles (46.2 ± 2.1%). This indicates that the organic-inorganic interpenetrating reinforcement structure formed by the fine SiO2 aerogel powder in the cellulose ether bonding network can effectively transfer and disperse external loads, further improving the overall mechanical stability and crushing resistance of the large aerogel spheres.
[0061] Further cross-sectional observation of the large aerogel spheres is shown in the following image. Figure 3 As shown, the results indicate that the obtained large aerogel spheres are assembled from multiple silica aerogel particles, with a distinct pore structure between the particles, while also retaining the nanoporous structure of the silica aerogel particles themselves. The fine SiO2 aerogel powder is mainly distributed within the cellulose ether bonding network, without disrupting the original hierarchical pore structure of the aerogel particles. This demonstrates that the present invention can further improve the mechanical stability of the material through nano-reinforcement while maintaining its lightweight and porous properties.
[0062] Example 5
[0063] The difference between this embodiment and embodiment 4 is that 2% of the mass of HPMC fine SiO2 aerogel powder is added; the rest is the same as in embodiment 4.
[0064] One hundred large aerogel spheres were randomly selected for particle size analysis. The results showed that the average particle size was 8.65 ± 1.71 mm. The crushing resistance of the obtained large aerogel spheres was further tested using the same method as in Example 1. The results showed that the crushing rate of the large aerogel spheres was 9.8 ± 1.1%, which was approximately 21.0% lower than that of Example 1 (12.4 ± 1.3%) without the addition of fine SiO2 aerogel powder, and approximately 78.8% lower than that of the original silica aerogel particles (46.2 ± 2.1%).
[0065] Example 6
[0066] The difference between this embodiment and embodiment 4 is that 3% of the mass of HPMC fine SiO2 aerogel powder is added; the rest is the same as in embodiment 4.
[0067] One hundred large aerogel spheres were randomly selected for particle size analysis. The results showed that the average particle size was 8.79 ± 1.68 mm. The crushing resistance of the obtained large aerogel spheres was further tested using the same method as in Example 1. The results showed that the crushing rate of the large aerogel spheres was 9.0 ± 1.0%, which was approximately 27.4% lower than that of Example 1 (12.4 ± 1.3%) without the addition of fine SiO2 aerogel powder, and approximately 80.5% lower than that of the original silica aerogel particles (46.2 ± 2.1%).
[0068] Examples 4-6 show that as the amount of fine SiO2 aerogel powder added increases, the average particle size of the resulting large aerogel spheres changes relatively little, while the crushing rate gradually decreases. This indicates that the addition of fine SiO2 aerogel powder can enhance the bonding network between aerogel particles and improve the anti-breakage performance of large aerogel spheres.
[0069] Example 7
[0070] The difference between this embodiment and Embodiment 4 is that the cellulose ether is methylcellulose, and the mass ratio of aerogel particles, cellulose ether and water is 40:10:400.
[0071] When the temperature of the silica aerogel particles reaches 30 °C, a cellulose ether aqueous solution containing fine SiO2 aerogel powder is sprayed three times using a sprayer, each spray lasting 20 seconds, with a 120-second interval between each spray. This ensures the cellulose ether aqueous solution adheres evenly to the surface of the silica aerogel particles. During spraying, a vibratory polisher is continuously running to maintain uniform movement of the silica aerogel particles through collision and rolling. After spraying, the vibratory polisher continues to run while infrared heating is applied, gradually raising the system temperature to 60 °C. The infrared heating device is then turned off, but the vibratory polisher continues running, allowing the formed large aerogel spheres to gradually cool and solidify during continuous tumbling. When the particle temperature drops to 20 °C, the vibratory polisher is turned off, resulting in structurally stable large aerogel spheres.
[0072] One hundred large aerogel spheres were randomly selected for particle size analysis. The results showed that the average particle size was 8.26 ± 1.73 mm. Further tests were conducted on the crushing resistance of the obtained large aerogel spheres, using the same method as in Example 1. The results showed that the crushing rate of the large aerogel spheres was 11.3 ± 1.2%.
[0073] Example 8
[0074] The difference between this embodiment and Embodiment 4 is that the cellulose ether is carboxymethyl cellulose, and the mass ratio of aerogel particles, cellulose ether and water is 60:20:600.
[0075] When the temperature of the silica aerogel particles reaches 40 °C, a cellulose ether aqueous solution containing fine SiO2 aerogel powder is sprayed four times using a sprayer, with each spray lasting 5 seconds and an interval of 10 seconds between adjacent sprays, ensuring that the cellulose ether aqueous solution adheres evenly to the surface of the silica aerogel particles. During the spraying process, a vibratory polisher is continuously running, maintaining uniform movement of the silica aerogel particles through collision and rolling. After spraying, the vibratory polisher continues to run while infrared heating is applied, gradually raising the system temperature to 90 °C. The infrared heating device is then turned off, but the vibratory polisher continues running, allowing the formed large aerogel spheres to gradually cool and solidify during continuous tumbling. When the particle temperature drops to 40 °C, the vibratory polisher is turned off, resulting in structurally stable large aerogel spheres.
[0076] One hundred large aerogel spheres were randomly selected for particle size analysis. The results showed that the average particle size was 8.47 ± 1.69 mm. The crushing resistance of the obtained large aerogel spheres was further tested using the same method as in Example 1. The results showed that the crushing rate of the large aerogel spheres was 10.5 ± 1.1%.
[0077] Comparative Example 1 The difference between this comparative example and Example 1 is that no cellulose ether aqueous solution was added; instead, the silica aerogel particles were treated solely by heat treatment. The specific method is as follows: Fifty parts of silica aerogel particles (1-3 mm in diameter) were added to a vibratory polisher, and the particles were kept in continuous tumbling motion while the infrared heating device was turned on for preheating. Once the temperature of the silica aerogel particles reached 40 °C, the cellulose ether aqueous solution was not added, and infrared heating continued until the system temperature reached 80 °C. After reaching 80 °C, the infrared heating device was turned off, but the vibratory polisher continued to run, allowing the silica aerogel particles to cool naturally to 30 °C. The vibratory polisher was then turned off, yielding the treated aerogel particles.
[0078] The macroscopic morphology of the aerogel particles obtained in Comparative Example 1 was observed using a digital camera. The results showed that, due to the absence of cellulose ether binder, under conditions of vibration tumbling and heat treatment alone, there was no effective bonding between the silica aerogel particles. The particles maintained their original irregular morphology, and no interparticle connection or aggregation occurred, thus failing to form structurally stable large aerogel spheres. A random sample of 100 particles was used for particle size analysis. The results showed that the particle size range after treatment remained 1-3 mm, with an average particle size of 1.95 ± 0.36 mm, essentially consistent with the original silica aerogel particles.
[0079] Further tests were conducted on the anti-crushing properties of the treated particles, using the same methods as in Example 1. The results showed that the crushing rate of the treated particles was 47.1±2.4%, which was basically consistent with the original silica aerogel particles (46.2±2.1%). This indicates that simply using heat treatment and vibration tumbling cannot improve the overall mechanical stability of the particles, nor can it achieve stable bonding between multiple aerogel particles. This demonstrates that cellulose ether, as the key binding component of this invention, can form a continuous bonding network between aerogel particles, which is a necessary condition for achieving the thermal bonding and assembly of multiple aerogel particles to form large aerogel spheres.
[0080] Comparative Example 2 The difference between this comparative example and Example 1 is that the vibration and tumbling method is not used; instead, static heating is employed to dehydrate and solidify the cellulose ether aqueous solution. The specific method is as follows: First, a cellulose ether aqueous solution was prepared according to the method in Example 1. Fifty parts of silica aerogel particles were evenly spread in a container. When the particle temperature reached 40 °C, the prepared cellulose ether aqueous solution was uniformly sprayed onto the surface of the silica aerogel particles. Then, an infrared heating device was turned on to raise the system temperature to 80 °C, promoting the evaporation of water in the cellulose ether aqueous solution and the formation of an adhesive structure. After reaching the set temperature, the infrared heating device was turned off, and the system was allowed to cool naturally to 30 °C to obtain the treated aerogel particles.
[0081] The macroscopic morphology of the aerogel particles obtained in Comparative Example 2 was observed using a digital camera. The results showed that, in the absence of vibration and tumbling, the cellulose ether aqueous solution mainly concentrated in localized areas, leading to the adhesion of some silica aerogel particles. In other areas, particles lacked effective connections, forming only a small number of irregularly shaped aggregates, making it difficult to form large aerogel spheres with uniform structure and high sphericity. A random sample of 100 aggregated particles was used for particle size analysis. The results showed that the particle size was mainly distributed between 3 and 8 mm, with an average particle size of 5.21 ± 1.64 mm, indicating a large dispersion in particle size distribution.
[0082] The resulting agglomerated particles were further tested for their anti-crushing properties using the same method as in Example 1. The results showed that the crushing rate of the treated particles was 30.8±1.8%, which, although lower than the original silica aerogel particles (46.2±2.1%), was still significantly higher than the large aerogel spheres prepared in Example 1 (12.4±1.3%). This indicates that without vibration and tumbling, cellulose ether is difficult to distribute uniformly in the contact area of the aerogel particles, failing to form a continuous and stable adhesive network, resulting in uneven particle connection and low overall mechanical stability. Therefore, the vibration and tumbling process can promote collision, rolling, and rearrangement between aerogel particles, enabling the cellulose ether adhesive network to form uniformly in the particle contact area, thereby promoting the stable assembly of multiple aerogel particles into large aerogel spheres with complete structure and excellent mechanical properties.
[0083] Comparative Example 3 The difference between this comparative example and Example 4 is that the amount of fine SiO2 aerogel powder added is too small, specifically 0.5% of the mass of cellulose ether, to illustrate that the expected reinforcing effect cannot be achieved when the amount added is insufficient.
[0084] The crushing resistance of the obtained large aerogel spheres was tested using the same method as in Example 1. The results showed that the crushing rate of the large aerogel spheres prepared in Comparative Example 3 was 11.8 ± 1.1%, which was not significantly different from that of Example 1 (12.4 ± 1.3%) without the addition of fine SiO2 aerogel powder. This indicates that when the amount of fine SiO2 aerogel powder added is too low, the nanoparticles cannot form a continuous reinforcing structure in the cellulose ether bonding network and cannot effectively exert a physical reinforcing effect, thus contributing little to improving the crushing resistance of the large aerogel spheres.
[0085] Comparative Example 4 The difference between this comparative example and Example 4 is that the amount of fine SiO2 aerogel powder added is excessive, specifically 8% of the mass of cellulose ether, to illustrate that adding more than the preferred amount will have a negative impact.
[0086] During the spraying process, it was observed that due to the excessive addition of fine SiO2 aerogel powder, the viscosity of the cellulose ether aqueous solution increased significantly, the atomization effect deteriorated, the spraying was uneven, and powder agglomeration occurred in some areas.
[0087] The crushing resistance of the obtained product was tested using the same method as in Example 1. The results showed that the crushing rate of the product obtained in Comparative Example 4 was 16.5±1.8%, which was not only higher than that of Example 4 (9.2±0.9%), but also higher than that of Example 1 without the addition of fine SiO2 aerogel powder (12.4±1.3%). The reason for this is that excessive fine SiO2 aerogel powder is difficult to disperse uniformly in the cellulose ether aqueous solution. After drying, it easily forms agglomerates within the bonding network. These agglomerates become stress concentration points, which, under external force, induce crack propagation, leading to a decrease in the crushing resistance of the large aerogel particles. Furthermore, excessive fine SiO2 aerogel powder accumulates on the surface of the aerogel particles and in the pores between particles, blocking part of the pore structure and hindering the maintenance of good thermal insulation properties of the material.
[0088] Based on the results of Example 4 and Comparative Examples 3-4, it can be seen that the present invention controls the addition amount of fine SiO2 aerogel powder within the range of 2%-3% of the cellulose ether mass. This not only fully utilizes the physical reinforcing effect of nanoparticles and significantly improves the anti-breakage performance of large aerogel spheres, but also avoids problems such as insignificant reinforcing effect due to insufficient addition amount, and uneven dispersion, increased viscosity, pore blockage and deterioration of mechanical properties due to excessive addition amount. It has reasonable technical and economic advantages.
[0089] Comparative Example 5 The difference between this comparative example and Example 1 is that the amount of hydroxypropyl methylcellulose ether (HPMC) added is excessive (the mass ratio of aerogel particles, cellulose ether and water is 50:30:500), to illustrate that adding more than the preferred range will have a negative impact.
[0090] Results Analysis: When excessive HPMC was added, the viscosity of the cellulose ether aqueous solution increased significantly, resulting in decreased atomization and spreading performance during spraying. This led to localized enrichment on the surface of some aerogel particles, causing excessive adhesion and uneven agglomeration between particles. Simultaneously, excessive cellulose ether tended to accumulate in the pores between particles, reducing the thickness and uniformity of the resulting adhesive layer. This resulted in a wider particle size distribution and reduced structural uniformity in the large aerogel spheres, which negatively impacted their overall breakage resistance and the maintenance of their hierarchical porous structure.
[0091] Comparative Example 6 The difference between this comparative example and Example 1 is that the amount of hydroxypropyl methylcellulose ether (HPMC) added is too small (the mass ratio of aerogel particles, cellulose ether, and water is 50:5:500), to illustrate that adding more than the preferred range will have a negative impact. The specific method is as follows: Results Analysis: When the amount of HPMC added is too small, the cellulose ether adhesive layer that can be formed on the surface of the aerogel particles and in the contact area between particles is insufficient, making it difficult to construct a continuous and stable adhesive network. During the vibration and tumbling process, although some particles can initially aggregate, the bonding strength between particles is low, and the structure of the large aerogel spheres formed is relatively loose. They are prone to detachment and breakage during subsequent collisions and stress. Therefore, the average particle size of the obtained particles is small, and the crushing rate is significantly increased.
[0092] In summary, both excessive and insufficient HPMC addition are detrimental to the stable preparation of large aerogel spheres. Controlling the mass ratio of aerogel particles, cellulose ether, and water within the range defined in this invention is beneficial for balancing the spray dispersion performance of the cellulose ether aqueous solution, the interparticle adhesion effect, and the structural stability of the resulting large aerogel spheres.
[0093] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method of making macro-particle aerogel spheres, characterized by, Includes the following steps: S1, preheat the tumbling aerogel particles, then spray an aqueous solution of cellulose ether onto their surface. After spraying, large aerogel pellets are formed under continued heating and tumbling. S2, stop heating and keep the large aerogel pellets tumbling, while the cellulose ether cools and solidifies to obtain large aerogel pellets.
2. A process for the preparation of macro-particle aerogel spheres as claimed in claim 1, wherein, The mass ratio of the aerogel particles, cellulose ether, and water is 40-60:10-20:400-600.
3. The method for preparing large aerogel spheres as described in claim 1, characterized in that, The cellulose ether aqueous solution also contains SiO2 aerogel powder.
4. The method for preparing large aerogel spheres as described in claim 3, characterized in that, The SiO2 aerogel powder is added at 2%-3% of the mass of the cellulose ether, and the particle size of the SiO2 aerogel powder is 10 nm-50 μm, with a specific surface area of 500-1200 m². 2 / g.
5. The method of claim 1, wherein the aerogel spheres have a diameter of 1 mm to 10 mm. The aerogel particles are silica aerogel particles.
6. The method for preparing large aerogel spheres as described in claim 1, characterized in that, The cellulose ether is one or more of hydroxypropyl methylcellulose ether, methylcellulose, hydroxyethyl cellulose, and carboxymethyl cellulose; the viscosity of the cellulose ether is 1000-10000 mPa·s.
7. The method of claim 1, wherein the aerogel spheres have a diameter of about 1 mm to about 10 mm. The preheating temperature of the aerogel particles in step S1 is 30-50 ℃, and after the cellulose ether aqueous solution is sprayed, it is heated to 60-90 ℃.
8. The method for preparing large aerogel spheres as described in claim 1, characterized in that, The cellulose ether aqueous solution is added by multiple intermittent spraying, with 3-5 sprayings, each spraying lasting 5-20 seconds, and the interval between two adjacent sprays being 10-120 seconds.
9. The method for preparing large aerogel spheres as described in claim 1, characterized in that, The heating method in step S1 is thermal radiation heating.
10. The method for preparing large-particle aerogel spheres as described in claim 1, characterized in that, In step S2, the rolling is stopped when the temperature of the large aerogel pellets drops to 20-40 ℃.