An organic-inorganic composite modified high-plasticity clay material and its preparation method
The organic-inorganic composite modification method of sodium-based bentonite and carboxymethyl cellulose has solved the problem that low-plasticity clay is difficult to meet the standards of high-plasticity clay, and has achieved improvements in liquid limit, plasticity index and clay content, making it suitable for erosion resistance and crack resistance in water conservancy projects.
Patent Information
- Application Number
- CN202611477085.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-22
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies cannot effectively transform low-plasticity clay into high-plasticity clay that meets the requirements of liquid limit ≥50% and plasticity index >20 through conventional bentonite modification, and the clay content index is not fully considered, resulting in limited modification effects.
An organic-inorganic composite modification method using sodium-based bentonite and carboxymethyl cellulose was adopted to improve the liquid limit and plasticity index of clay through synergistic effect. This method involves mixing sodium-based bentonite and carboxymethyl cellulose with natural low-plasticity clay to form an organic-inorganic composite structure.
The modified clay achieved the liquid limit and plasticity index standards of high-plasticity clay, with a clay content of more than 30%, good impermeability and workability, and reduced project costs.
Smart Images

Figure CN123106090A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of high plasticity clay materials, specifically relating to an organic-inorganic composite modified high plasticity clay material and its preparation method. Background Technology
[0002] High-plasticity clay refers to highly plastic and expansive clay rich in montmorillonite. In engineering classifications, GB / T50123-2019 and GB / T 50145-2007 do not yet define high-plasticity clay. The international standard ASTM D2487-17 defines high-plasticity clay (Fat clay) as follows: the liquid limit of the sample after oven drying is higher than 75% of the original liquid limit determined before oven drying; more than 50% of the dry mass of the sample passes through a 200-mesh sieve; and the point on the relationship between the plasticity index (PI) and the liquid limit (LL) of the sample should fall on or above the "A" line of the plasticity chart (CH region). Figure 1 Based on extensive literature and engineering research, this invention defines the engineering criteria for high-plasticity clay as follows: liquid limit ≥ 50% and plasticity index > 20. Simultaneously, high-plasticity clay also possesses advantages such as high clay content, high expansibility, low permeability, and sufficient mechanical strength. It is widely used in contact areas such as earth-core dams and galleries, core walls and secondary walls, and core walls and concrete slabs on both banks, to improve the erosion resistance and crack resistance of the contact areas between the core wall and the dam foundation slope.
[0003] In practical engineering projects, the natural soil at some project sites cannot meet the requirements for high-plasticity clay, necessitating external procurement and leading to increased project costs and supply difficulties. Existing technologies typically modify low-plasticity clay by incorporating bentonite. Bentonite, with montmorillonite as its main mineral, has strong water absorption; upon absorbing water, it swells to form a gel, filling pores and reducing free water. Its high specific surface area promotes cation exchange and flocculation, generating colloids such as calcium silicate, forming a three-dimensional network structure. This significantly enhances particle bonding and cohesion, increases compressive strength and plasticity index, and reduces permeability.
[0004] However, simply adding bentonite has limited effect on modifying low-plasticity clay. When the natural low-plasticity clay itself has low plasticity, even with a large proportion of bentonite, it is still difficult to make the modified clay simultaneously meet the dual requirements of liquid limit ≥50% and plasticity index >20, as well as other requirements. Therefore, it is necessary to develop a modified material and its preparation method that can effectively modify low-plasticity clay into high-plasticity clay, making it simultaneously meet the requirements of liquid limit and plasticity index.
[0005] In existing studies on bentonite modification of low-plasticity clay, simply increasing the bentonite content to improve the plasticity index often results in insufficient liquid limit of the modified soil. For example, research shows that modified soil prepared by blending natural soil with 15% sodium-based bentonite has not yet met the standards for high-plasticity clay, and even when the blending content is increased to 20%, some samples still do not fall into the category of high-plasticity clay. Simple inorganic modification is insufficient to simultaneously meet the dual requirements of liquid limit and plasticity index.
[0006] While some modification methods can achieve the required plasticity index, the liquid limit value still falls below the 50% threshold. For example, after adding 20% sodium-based bentonite to natural soil, some modified soils have a plasticity index greater than 20, but a liquid limit of only 47.92%-48.61%, close to but not reaching the 50% threshold. Current technologies lack effective solutions to improve the liquid limit to the required level.
[0007] Existing polymer-modified bentonite technologies mostly focus on modifying bentonite itself, without systematically studying ternary composite systems of low-plasticity clay, bentonite, and polymers. The synergistic effects of polymer type and dosage with bentonite type and dosage have not yet been fully revealed.
[0008] Current technologies do not adequately consider the clay content index of modified high-plasticity clay. Studies have shown that soil permeability coefficient is positively correlated with clay content, and low permeability performance is difficult to guarantee when the clay content is below 30%. Existing modification schemes often neglect this key indicator of clay content.
[0009] Existing research on the mechanism of bentonite-modified clay mainly focuses on single modification methods, lacking a systematic explanation of the synergistic effect mechanism of "inorganic modification (bentonite) + organic modification (polymer)". In particular, the synergistic mechanism of polymer intercalation and bentonite pore-blocking effect has not been fully revealed. Summary of the Invention
[0010] The purpose of this invention is to address the technical challenge of achieving high-plasticity clay standards (liquid limit ≥50%, plasticity index >20) and high clay particle content (>30%) through conventional bentonite modification of natural low-plasticity clay in existing technologies. This invention provides an organic-inorganic composite modified high-plasticity clay material and its preparation method. By synergistically applying sodium-based bentonite and carboxymethyl cellulose (CMC) to natural low-plasticity clay, this invention achieves a synergistic effect of inorganic and organic modification, ensuring that the modified clay meets the requirements for high-plasticity clay standards in both liquid limit and plasticity index.
[0011] The technical solution adopted in this invention is: an organic-inorganic composite modified high-plasticity clay material, comprising the following components by mass parts: 79-81 parts of natural low-plasticity clay; 19-21 parts of sodium-based bentonite; 0-1 part carboxymethyl cellulose; The rest is water; The amount of carboxymethyl cellulose added is based on the total dry mass of natural low-plasticity clay and sodium-based bentonite, plus a percentage by mass.
[0012] Preferably, the natural low-plasticity clay has a mass fraction of 80 parts.
[0013] Preferably, the natural low-plasticity clay is taken from a soil yard in the project area, with sampling depths of 1, 3, and 5 meters. The liquid limit of the natural low-plasticity clay is 24%-36%, and the plasticity index is 9-21, both lower than the engineering standards for high-plasticity clay (liquid limit ≥50%, plasticity index >20). The main mineral components of the natural low-plasticity clay are quartz, calcite, dolomite, chlorite, montmorillonite, and anorthite, and the main oxides are SiO2, Al2O3, and CaO, with small amounts of Fe2O3, K2O, MgO, and Na2O. The specific gravity of the natural low-plasticity clay is 2.5-2.7, and the clay content is 13%-34%.
[0014] The functions of natural low-plasticity clay are: ① As a modified matrix material, its plasticity index and liquid limit can be improved by incorporating bentonite and polymers; ② The active sites on the surface of clay particles can undergo physicochemical reactions with bentonite and polymers to form a stable composite structure; ③ The cost of natural clay is much lower than that of high-plasticity clay transported over long distances, which can significantly reduce engineering costs.
[0015] Preferably, the sodium-based bentonite is in the form of 20 parts by weight.
[0016] Preferably, the sodium-based bentonite (B) is prepared by artificial sodium modification of natural calcium-based bentonite; the main oxides of sodium-based bentonite are SiO2, Al2O3, Fe2O3, and CaO, and contain small amounts of TiO2, MgO, Na2O, and Cl; the Na2O content is 2.56%, and the (Na2O+K2O) / (CaO+MgO) ratio is 0.25; the main mineral components of sodium-based bentonite are montmorillonite, kaolinite, quartz, and calcite, and the interlayer spacing of the characteristic diffraction peaks of montmorillonite d(001) is 12.72 Å; the liquid limit of sodium-based bentonite is 138.23%, the plastic limit is 29.83%, and the plasticity index is 108.4; the particle size of sodium-based bentonite is unimodal, and the median particle size D50 is 541 nm.
[0017] The functions of sodium-based bentonite are: ① As an inorganic modifier, its high montmorillonite content and strong expansibility can significantly improve the plasticity index of low-plasticity clay; ② Bentonite particles fill the pores between natural soil particles, forming a dense structure and reducing the permeability coefficient; ③ The hydration and expansion of bentonite can enhance the water retention performance of modified soil.
[0018] Preferably, the carboxymethyl cellulose is 1 part by weight.
[0019] Preferably, the carboxymethyl cellulose (CMC) is an anionic polymer, a white to pale yellow powder, readily soluble in water, and its aqueous solution is neutral or slightly alkaline; the degree of substitution (DS) of carboxymethyl cellulose is 0.7-1.2, and the viscosity is 300-800 mPa·s (2% aqueous solution, 25℃); the carboxymethyl cellulose molecular chain contains a large number of strongly hydrophilic functional groups such as carboxymethyl (-CH2COOH) and hydroxyl (-OH).
[0020] The functions of carboxymethyl cellulose (CMC) are: ① As an organic modifier, it enters the interlayer domain of bentonite and montmorillonite through intercalation, increasing the interlayer spacing; ② The polymer hydrogel has a blocking effect on the large pores between bentonite particles; ③ The long-chain polymer constructs an "organic-inorganic" interpenetrating network with bentonite and other clays through intermolecular forces, giving the modified clay anti-agglomeration and environmental responsiveness; ④ The strong hydrophilic functional groups of CMC can significantly improve the water retention capacity and liquid limit of the modified clay.
[0021] Preferably, the water is tap water or deionized water, used to adjust the moisture content of the modified soil.
[0022] The method for preparing organic-inorganic composite modified high-plasticity clay provided by the present invention includes the following steps: (1) Pretreatment of natural low plasticity clay: Dry the natural low plasticity clay at 105℃ for 8 hours, crush the dried soil sample with a wooden mallet, pass it through a 0.5 mm standard sieve, and seal it for later use. (2) Pretreatment of sodium-based bentonite: Dry sodium-based bentonite at 105°C to constant weight, grind it through a 200-mesh sieve, and seal it for later use; (3) Preparation of carboxymethyl cellulose solution: Weigh carboxymethyl cellulose according to the proportion, add deionized water, and stir at room temperature until completely dissolved to obtain carboxymethyl cellulose solution; (4) Dry material mixing: Weigh the pretreated natural low-plasticity clay and sodium-based bentonite according to the ratio, place them in a mixing container, and dry mix at room temperature for 5-10 minutes to ensure that the two powders are fully mixed and uniform, thus obtaining the mixed dry material; (5) Add water and mix: Slowly add carboxymethyl cellulose solution and the remaining deionized water to the mixed dry material while stirring; mix thoroughly for 10-15 minutes until the soil sample is uniform and free of particles and exhibits good plasticity; (6) Aging and curing: Cover the mixed modified soil with plastic film and seal it at room temperature for 24 hours to allow the bentonite to fully hydrate and expand and the carboxymethyl cellulose to fully penetrate and intercalate; (7) Performance testing: Take the aged modified soil sample and test the liquid limit, plastic limit and plasticity index using a liquid limit and plastic limit combined tester according to the standard GB / T 50123-2019 for geotechnical testing methods; test the clay content using the densitometer method.
[0023] Preferably, in step (3), the mass ratio of carboxymethyl cellulose to water is 1:15; in step (5), the mixture is brought to a moisture content of 18-22%.
[0024] The synergistic modification mechanism of the organic-inorganic composite modified high-plasticity clay of this invention can be mainly divided into three aspects: (1) Double layer theory: Montmorillonite particles in bentonite are flaky, often with positively charged edges and permanently negatively charged surfaces. This negative charge attracts cations (Na+) from the surrounding medium. + Ca 2+ ) forms a diffused electric double layer, such as Figure 2 As shown, the hydrated cations within the electric double layer attract water molecules to form a viscous bound water film that surrounds the low-plasticity clay particles. This water film acts as a lubricant and adsorbent, such as... Figure 3 As shown, the addition of CMC makes it easier for particles to slide relative to each other without breaking when subjected to force. The addition of CMC enhances the attraction between particles and the thickness of the hydration layer. The thicker the double electric layer, the more water is needed to separate the particles, which leads to a slight increase in plasticity and a significant increase in liquid limit, in order to achieve the purpose of increasing the plasticity index.
[0025] (2) Function of plugging holes: Figure 4 This study demonstrates the changes in pore channels between natural soil particles under the synergistic effect of bentonite and polymers. Sodium-based bentonite, with montmorillonite as its main mineral, exhibits strong water absorption and swelling properties. Upon absorbing water, bentonite particles undergo crystalline layer expansion (nanoscale) and double-layer expansion (hundred-nanometer scale). The expanded bentonite gel fills the large and medium pores between the natural soil particles, effectively dividing the original large and medium pores into numerous tiny seepage channels. Furthermore, carboxymethyl cellulose forms a polymer hydrogel network in water, interpenetrating within these channels, further blocking the tiny pores between both bentonite and natural soil particles. The synergistic effect of bentonite and polymers fills the originally developed pore channels between natural soil particles, forming a dense microstructure.
[0026] (3) Intercalation: Carboxymethyl cellulose molecules enter the interlayer domains of bentonite-montmorillonite through cation exchange, hydrogen bonding, and cation bridging, altering the microstructure of the bentonite layers. XRD analysis shows that the interlayer spacing of the d(001) characteristic diffraction peaks of sodium-based bentonite is 12.72 Å (approximately 1.272 nm). After carboxymethyl cellulose intercalation modification, the interlayer spacing of the d(001) characteristic diffraction peaks of the high-plasticity clay increases to 1.434-1.453 nm. According to the Bragg equation, the shift of XRD peaks to lower diffraction angles leads to an increase in interlayer spacing, proving that the long-chain polymer of carboxymethyl cellulose has successfully intercalated into the interlayer of montmorillonite. Figure 5 As shown, long-chain polymers insert into the interlayer through intermolecular forces, constructing an "organic-inorganic" interpenetrating network with clays such as bentonite. This endows the modified clay with anti-agglomeration properties and enhances its environmental responsiveness and water retention performance.
[0027] The pore-blocking and intercalation effects work together to enhance the water retention, plasticity index, and liquid limit of modified high-plasticity clay, enabling it to meet the engineering standards for high-plasticity clay.
[0028] The differences between this patent and existing published patents are as follows: (1) A compound polymer modified bentonite seepage barrier material and its preparation method and application (Application No.: 202111333703.2) Synopsis: This patent discloses a polymer-modified bentonite seepage barrier material, comprising the following components by mass fraction: 80-95% sodium-modified bentonite, 0.5%-15% polyanionic cellulose, and 0.7%-2.5% hydroxypropyl methylcellulose. This material, through polymer-modified bentonite, is applied to seepage barrier barriers in contaminated sites.
[0029] Differences from this patent: ① Different raw materials: This patent directly modifies bentonite with polymers, without involving the modification and utilization of low-plasticity clay. ② Different application scenarios: This patent is used for seepage prevention barriers in contaminated sites, while this patent is used for erosion and crack resistance in contact parts of hydraulic engineering projects such as earth-core dams. ③ Different technical approaches: This patent only improves the seepage prevention performance of bentonite through polymer modification, while this patent systematically improves the plasticity index, liquid limit, and clay content through organic-inorganic composite modification of "low-plasticity clay + sodium-based bentonite + carboxymethyl cellulose". ④ No systematic optimization of the plasticity index and liquid limit of the modified material, while this patent uses precise proportioning design for engineering standards of high-plasticity clay with a liquid limit ≥50% and a plasticity index >20.
[0030] (2) A block polyurethane polymer, its polymer-modified bentonite admixture and its preparation and application (Application No.: 201911281296.8) Synopsis: This patent discloses a block polyurethane polymer, its polymer-modified bentonite admixture, its preparation method, and its applications. The block polyurethane polymer is a cationic amphiphilic block polymer, obtained by condensing a polyionic liquid with a specific structure obtained from the condensation of amines and dihaloalkanes with an isocyanate-terminated polyurethane prepolymer. Through intercalation modification, this admixture achieves enhanced activity and controlled adsorption of the clay component and controlled release of the polymer component, effectively improving the mechanical properties and chloride ion penetration resistance of concrete.
[0031] Differences from this patent: ① Different polymer types: This patent uses block polyurethane polymers (synthetic polymers), while this patent uses carboxymethyl cellulose (a natural cellulose derivative, biodegradable and environmentally friendly). ② Different modification targets: This patent uses bentonite as the modification target to prepare concrete admixtures, while this patent uses natural low-plasticity clay as the modification target to prepare high-plasticity clay materials. ③ Different application fields: This patent is used in the field of concrete to improve mechanical properties and chloride ion penetration resistance, while this patent is used in the field of water conservancy engineering seepage prevention to improve the plasticity and seepage resistance of clay. ④ Different focuses on the intercalation mechanism: This patent focuses on the influence of polymer intercalation on the workability and mechanical properties of concrete, while this patent focuses on the effect of polymer intercalation on increasing the interlayer spacing of montmorillonite and its effect on improving water retention and liquid limit.
[0032] (3) A modified bentonite and its modification method and application (Application No.: 201910379685.8) Synopsis: This patent discloses a modified bentonite, its modification method, and its application. The modified bentonite comprises an inorganic phosphorus-based polymer, citric acid, and bentonite parent material, wherein the inorganic phosphorus-based polymer is sodium hexametaphosphate. The bentonite is modified by a composite process using the inorganic phosphorus-based polymer and citric acid.
[0033] Differences from this patent: ① Different modifiers: This patent uses inorganic phosphorus-based polymers (sodium hexametaphosphate) and citric acid as modifiers, while this patent uses medium-viscosity sodium-based bentonite and carboxymethyl cellulose to modify low-plasticity clay. ② Different modification targets: This patent directly modifies the bentonite parent material, while this patent modifies the natural low-plasticity clay-bentonite composite system. ③ Different modification purposes: This patent aims to improve the dispersibility and application performance of bentonite itself, while this patent aims to transform low-plasticity clay into high-plasticity clay that meets engineering standards. ④ It does not involve the control of plasticity index and liquid limit, while the core of this patent lies in simultaneously improving the liquid limit and plasticity index through organic-inorganic composite modification.
[0034] The present invention has the following beneficial effects: (1) Dual achievement of liquid limit and plasticity index: This invention achieves a liquid limit of 58.15%-58.87% and a plasticity index of 37.36-39.05 in the modified soil through an organic-inorganic composite modification scheme of "natural low-plasticity clay + 20% sodium-based bentonite + 1% carboxymethyl cellulose", while meeting the engineering standard of liquid limit ≥50% and plasticity index >20 for high-plasticity clay. Compared with the case where the liquid limit of some formulations is only 47.92%-48.61% when using simple inorganic modification (natural soil + 20% sodium-based bentonite), this invention increases the liquid limit by about 10 percentage points by adding 1% CMC, effectively solving the technical bottleneck of insufficient liquid limit.
[0035] (2) Clay content meets the standard: The organic-inorganic composite modified high plasticity clay prepared by this invention has a clay content of more than 30% (reaching 33.51%-37.38%). According to a large number of studies at home and abroad, the soil permeability coefficient is positively correlated with the clay content, and a clay content of more than 30% can ensure that the modified soil has low permeability performance.
[0036] (3) Low permeability: This invention achieves low hydraulic conductivity of modified high plasticity clay to calcium chloride solution and seawater during long-term permeation through the synergistic effect of pore-blocking (bentonite and polymer fill the pores between natural soil particles to form a dense structure) and intercalation (polymer is inserted between bentonite layers to construct an "organic-inorganic" interpenetrating network).
[0037] (4) Strong applicability: This invention has been verified by systematic experiments on natural soil samples collected from multiple soil yards, sampling points at different locations, and at different depths (1 m, 3 m, 5 m), proving that the modification scheme has good applicability to low plasticity clay from different sources.
[0038] (5) Significant cost advantage: This invention utilizes the low-plasticity clay resources in the project location and modifies them by adding sodium-based bentonite and a small amount of carboxymethyl cellulose, replacing the high-cost high-plasticity clay that is transported over long distances, which can significantly reduce the cost of engineering materials.
[0039] (6) Excellent construction performance: The modified high plasticity clay prepared by the present invention has good workability, is easy to compact and construct, and can meet the filling requirements of the contact parts of water conservancy projects such as soil core wall dams. Attached Figure Description
[0040] Figure 1 Plastic diagram; Figure 2 A detailed structural diagram of the diffused double layer; Figure 3 Diagram showing the formation of a bound water film; Figure 4 This is a schematic diagram illustrating the synergistic pore-blocking effect of bentonite and polymer. Figure 5 This is a schematic diagram of the carboxymethyl cellulose intercalation process. Detailed Implementation
[0041] The present invention will be further described below with reference to the accompanying drawings and specific embodiments. Example 1
[0042] In Example 1, an organic-inorganic composite modified high-plasticity clay was prepared. The components, by mass parts, are as follows: 80 parts of natural low-plasticity clay (1 m depth), 20 parts of sodium bentonite, 1 part of carboxymethyl cellulose, and appropriate amount of water (the moisture content is controlled to be ±2% of the optimum moisture content).
[0043] Preparation process: (1) Dry the natural low-plasticity clay at 105℃ for 8 hours. Crush the dried soil sample with a wooden mallet, pass it through a 0.5mm standard sieve, and seal it for later use. Dry the sodium-based bentonite at 105℃ to constant weight, grind it through a 200-mesh sieve, and seal it for later use. (2) Weigh 1 part of carboxymethyl cellulose and add 15 parts of deionized water (the mass ratio of carboxymethyl cellulose to water is 1:15). Stir at 200 r / min for 30 minutes at room temperature until completely dissolved to obtain a carboxymethyl cellulose solution. (3) Weigh 80 parts of pretreated natural low-plasticity clay and 20 parts of pretreated sodium-based bentonite, place them in a mixing container, and dry mix at room temperature for 8 minutes to ensure that the two powders are fully mixed and uniform, thus obtaining a mixed dry material; (4) Slowly add the carboxymethyl cellulose solution and the remaining deionized water to the mixed dry material while stirring, so that the mixture reaches the optimal moisture content (approximately 18-22%). Mix thoroughly for 12 minutes until the soil sample is uniform, free of particles, and exhibits good plasticity; (5) Cover the mixed modified soil with plastic film and seal it at room temperature for 24 hours; (6) Take the aged modified soil sample and test the liquid limit, plastic limit and plasticity index using the liquid limit and plastic limit combined tester according to the "Standard for Geotechnical Test Methods" (GB / T 50123-2019); test the clay content using the densitometer method.
[0044] Performance test results: liquid limit 58.15%, plastic limit 19.10%, plasticity index 39.05, and clay content 33.51%. All indicators meet the engineering standards for high plasticity clay (liquid limit ≥50%, plasticity index >20, clay content >30%).
[0045] Example 2 In Example 2, an organic-inorganic composite modified high-plasticity clay was prepared. The components, by mass parts, are as follows: 80 parts of natural low-plasticity clay (3 m depth), 20 parts of sodium bentonite, 1 part of carboxymethyl cellulose, and appropriate amount of water.
[0046] The preparation process is the same as in Example 1.
[0047] Performance test results: liquid limit 58.87%, plastic limit 20.37%, plasticity index 38.50, and clay content 37.38%. All indicators meet the engineering standards for high plasticity clay. Example 3
[0048] In Example 3, an organic-inorganic composite modified high-plasticity clay was prepared. The components, by mass parts, are as follows: 80 parts of natural low-plasticity clay (5 m depth), 20 parts of sodium bentonite, 1 part of carboxymethyl cellulose, and appropriate amount of water.
[0049] The preparation process is the same as in Example 1.
[0050] Performance test results: liquid limit 58.58%, plastic limit 21.22%, plasticity index 37.36, and clay content 37.36%. All indicators meet the engineering standards for high plasticity clay.
[0051] Comparative Example 1 In Example 1, an inorganic modified high-plasticity clay was prepared. Its components, by mass parts, are as follows: 80 parts of natural low-plasticity clay (1 m depth), 20 parts of sodium bentonite, and appropriate amount of water (without carboxymethyl cellulose added, used as an inorganic modification control sample).
[0052] Preparation process: (1) Dry the natural low-plasticity clay at 105℃ for 8 hours, crush the dried soil sample with a wooden mallet, pass it through a 0.5 mm standard sieve, and seal it for later use. Dry the sodium-based bentonite at 105℃ to constant weight, grind it through a 200-mesh sieve, and seal it for later use. (2) Weigh 80 parts of pretreated natural low-plasticity clay and 20 parts of pretreated sodium-based bentonite, place them in a mixing container, and dry mix at room temperature for 8 minutes to ensure that the two powders are fully mixed and uniform, thus obtaining a mixed dry material; (3) Slowly add deionized water to the dry mixture while stirring, until the mixture reaches the optimal moisture content. Mix thoroughly for 12 minutes; (4) Cover the mixed modified soil with plastic film and seal it at room temperature for 24 hours; (5) Take aged modified soil samples for liquid limit and plastic limit and clay content tests.
[0053] Performance test results: liquid limit 47.92%, plastic limit 16.42%, plasticity index 31.50. Although the plasticity index is greater than 20, the liquid limit is less than 50%, which does not meet the liquid limit requirement for high plasticity clay.
[0054] Comparative Example 2 In Comparative Example 2, a simple inorganic modified clay was prepared. Its components, by mass parts, are as follows: 80 parts of natural low-plasticity clay (3 m depth), 20 parts of sodium bentonite, and appropriate amount of water (without carboxymethyl cellulose).
[0055] The preparation process is the same as in Example 4 (without adding CMC).
[0056] Performance test results: liquid limit 48.61%, plastic limit 15.88%, plasticity index 32.73. Although the plasticity index is greater than 20, the liquid limit is less than 50%, which does not meet the liquid limit requirement for high plasticity clay.
[0057] Comparative Example 3 In Comparative Example 3, a simple inorganic modified clay was prepared. Its components, by mass parts, are as follows: 80 parts of natural low-plasticity clay (taken from sampling point W10-3 in the western area, at a depth of 3 m), 20 parts of medium-viscosity sodium-based bentonite, and appropriate amount of water (without added carboxymethyl cellulose).
[0058] The preparation process is the same as in Example 4 (without adding CMC).
[0059] Performance test results: liquid limit 48.55%, plastic limit 16.96%, plasticity index 31.59. Although the plasticity index is greater than 20, the liquid limit is less than 50%, which does not meet the liquid limit requirement for high plasticity clay.
[0060] Performance comparison between the examples and comparative examples: As shown in Table 1, although the modified soils of Comparative Examples 1-3 (with the addition of 20% sodium bentonite alone) met the plasticity index requirement (>20), their liquid limits were all below 50%, failing to meet the liquid limit requirements for high-plasticity clays. In contrast, Examples 1-3, with the addition of 1% CMC to the same bentonite content, all showed a liquid limit increase to over 58%, an increase of approximately 10 percentage points. Simultaneously, the plasticity index further increased to over 37, and the clay content was all greater than 30%. This fully demonstrates the crucial role of organic modification of carboxymethyl cellulose in improving the liquid limit, as well as the synergistic effect of "organic-inorganic" composite modification.
[0061] Table 1 Test parameters for different formulation schemes
[0062] In summary, the innovation of this invention lies in: (1) Organic-inorganic composite modified formulation: a specific ratio of natural low-plasticity clay + 20% sodium-based bentonite + 1% carboxymethyl cellulose. This formulation has been verified through extensive experiments to stably achieve the triple requirements of liquid limit ≥50%, plasticity index >20, and clay content >30%. The selection of sodium-based bentonite content (20%) and carboxymethyl cellulose content (1%) are key parameters. Below this content, the liquid limit is insufficient, while above this content, the cost may increase and the performance improvement is limited.
[0063] (2) Application of carboxymethyl cellulose intercalation modification: Carboxymethyl cellulose was used as an organic intercalating agent to modify the low-plasticity clay-bentonite composite system. Carboxymethyl cellulose enters the interlayer domain of bentonite-montmorillonite through cation exchange, hydrogen bonding and cation bridging, increasing the interlayer spacing and constructing an "organic-inorganic" interpenetrating network.
[0064] (3) Synergistic effect mechanism of pore plugging and intercalation: The physical pore plugging effect of bentonite and the chemical intercalation effect of carboxymethyl cellulose work synergistically to enhance the water retention, plasticity index and liquid limit of modified soil, so that the modified soil can reach the standard of high plasticity clay with low bentonite content.
[0065] (4) Wide applicability of raw materials: This invention has been systematically verified by collecting natural soil samples from multiple soil yards at different depths, proving that the modification scheme has good applicability to low plastic clays from different sources and with different initial plasticity indices.
[0066] (5) Application scenarios: The modified high plasticity clay of this invention is used in seepage prevention engineering of soil core wall dams, especially for erosion and crack resistance at the contact parts of the core wall and dam foundation, corridor, and concrete cover plates on both banks.
[0067] Those skilled in the art should understand that the above embodiments do not limit the scope of protection of the present invention in any way. All technical solutions obtained by equivalent substitution or other means fall within the scope of protection of the present invention. Parts not covered in this invention are the same as or can be implemented using existing technology.
Claims
1. An organic-inorganic composite modified high-plasticity clay material, characterized in that: By mass, the components are as follows: 79-81 parts of natural low-plasticity clay; 19-21 parts of sodium-based bentonite; 0-1 part carboxymethyl cellulose; The rest is water; The amount of carboxymethyl cellulose added is based on the total dry mass of natural low-plasticity clay and sodium-based bentonite, plus a percentage by mass.
2. The organic-inorganic composite modified high-plasticity clay material according to claim 1, characterized in that: The natural low-plasticity clay has a mass fraction of 80 parts.
3. The organic-inorganic composite modified high-plasticity clay material according to claim 2, characterized in that: The natural low-plasticity clay was taken from a soil yard in the project area, with sampling depths of 1, 3, and 5 meters. The liquid limit of the natural low-plasticity clay was 24%-36%, and the plasticity index was 9-21, both lower than the engineering standards for high-plasticity clay. The main mineral components of the natural low-plasticity clay were quartz, calcite, dolomite, chlorite, montmorillonite, and anorthite, and the main oxides were SiO2, Al2O3, and CaO, with small amounts of Fe2O3, K2O, MgO, and Na2O. The specific gravity of the natural low-plasticity clay was 2.5-2.7, and the clay content was 13%-34%.
4. The organic-inorganic composite modified high-plasticity clay material according to claim 3, characterized in that: The sodium-based bentonite is present in 20 parts by weight.
5. The organic-inorganic composite modified high-plasticity clay material according to claim 4, characterized in that: The sodium-based bentonite is prepared by artificial sodium modification of natural calcium-based bentonite. The main oxides of sodium-based bentonite are SiO2, Al2O3, Fe2O3, and CaO, with small amounts of TiO2, MgO, Na2O, and Cl. The Na2O content is 2.56%, and the (Na2O+K2O) / (CaO+MgO) ratio is 0.
25. The main mineral components of sodium-based bentonite are montmorillonite, kaolinite, quartz, and calcite. The interlayer spacing of the characteristic diffraction peaks of montmorillonite d001 is 12.72 Å. The liquid limit of sodium-based bentonite is 138.23%, the plastic limit is 29.83%, and the plasticity index is 108.
4. The particle size of sodium-based bentonite exhibits a unimodal distribution, with a median particle size D50 of 541 nm.
6. The organic-inorganic composite modified high-plasticity clay material according to claim 5, characterized in that: The carboxymethyl cellulose is 1 part by weight.
7. The organic-inorganic composite modified high-plasticity clay material according to claim 6, characterized in that: The carboxymethyl cellulose is an anionic polymer, a white to pale yellow powder, easily soluble in water, and its aqueous solution is neutral or slightly alkaline; the degree of substitution of carboxymethyl cellulose is 0.7-1.2, and its viscosity is 300-800 mPa·s; the carboxymethyl cellulose molecular chain contains hydrophilic functional groups such as carboxymethyl and hydroxyl groups.
8. The organic-inorganic composite modified high-plasticity clay material according to claim 7, characterized in that: The water is tap water or deionized water.
9. A method for preparing an organic-inorganic composite modified high-plasticity clay material as described in claims 1, 2, 3, 4, 5, 6, 7, or 8, characterized in that: Includes the following steps: (1) Pretreatment of natural low plasticity clay: Dry the natural low plasticity clay at 105℃ for 8 hours, crush the dried soil sample with a wooden mallet, pass it through a 0.5 mm standard sieve, and seal it for later use. (2) Pretreatment of sodium-based bentonite: Dry sodium-based bentonite at 105°C to constant weight, grind it through a 200-mesh sieve, and seal it for later use; (3) Preparation of carboxymethyl cellulose solution: Weigh carboxymethyl cellulose according to the proportion, add deionized water, and stir at room temperature until completely dissolved to obtain carboxymethyl cellulose solution; (4) Dry material mixing: Weigh the pretreated natural low-plasticity clay and sodium-based bentonite according to the ratio, place them in a mixing container, and dry mix at room temperature for 5-10 minutes to ensure that the two powders are fully mixed and uniform, thus obtaining the mixed dry material; (5) Add water and mix: Slowly add carboxymethyl cellulose solution and the remaining deionized water to the mixed dry material while stirring; mix thoroughly for 10-15 minutes until the soil sample is uniform and free of particles and exhibits good plasticity; (6) Aging and curing: Cover the mixed modified soil with plastic film and seal it at room temperature for 24 hours to allow the bentonite to fully hydrate and expand and the carboxymethyl cellulose to fully penetrate and intercalate. (7) Performance testing: Take the aged modified soil sample and test the liquid limit, plastic limit and plasticity index using a liquid limit and plastic limit combined tester according to the standard GB / T 50123-2019 for geotechnical testing methods; test the clay content using the densitometer method.
10. The method for preparing an organic-inorganic composite modified high-plasticity clay material according to claim 1, characterized in that: In step (3), the mass ratio of carboxymethyl cellulose to water is 1:15; in step (5), the mixture is brought to a moisture content of 18-22%.
Citation Information
Patent Citations
A modified bentonite, its modification method and application
CN110182819B
A block polyurethane polymer, its polymer-modified bentonite admixture, and its preparation and application.
CN112979905B
Compound polymer modified bentonite anti-seepage barrier material as well as preparation method and application thereof
CN114149203A