A method for preparing polypropylene foam material

By using cellulose whisker pretreatment and composite foaming agents, the problems of gas escape and cell collapse in the polypropylene foaming process were solved, enabling the preparation of high-strength, fast-foaming, and uniformly foamed polypropylene materials, thereby improving the overall performance and production stability of the materials.

CN123107162APending Publication Date: 2026-11-17WEIFANG SHUFUKANG NEW MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611277951.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2026-03-31
Filing Date
2026-08-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional polypropylene foaming processes are difficult to control gas diffusion and cell formation stably, leading to gas escape and cell collapse. Furthermore, existing modification methods suffer from high equipment modification costs, poor reaction controllability, or high foaming agent costs.

Method used

A method of cellulose whisker pretreatment and composite foaming agent is adopted to generate carboxylated cellulose whiskers through oxidation reaction, which improves their dispersibility in polypropylene. The whiskers are then combined with the foaming agent to form a continuous shell to suppress agglomeration and improve melt strength and foaming stability.

Benefits of technology

The prepared foamed polypropylene material has high strength, excellent foaming rate and stability, uniform cell structure, excellent mechanical properties, and balanced strength in all regions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention provides a method for preparing polypropylene foam material, belonging to the field of polypropylene technology. The method for preparing polypropylene foam material includes the following steps: cellulose whisker pretreatment, preparation of a composite foaming agent, and preparation of foamed polypropylene. The foamed polypropylene prepared by this invention has a tensile strength of 37.6-38.1 MPa and an impact strength of 9.5-10.3 KJ / m2. The foamed polypropylene exhibits excellent mechanical properties, reaching maximum foam volume in 126-137 s, and a foaming ratio of 9.3-10.1 times. The foaming agent also demonstrates excellent foaming rate and ratio. The carboxylated cellulose whiskers prepared by this invention have a light transmittance of 23-25% and good whisker dispersibility. The relative standard deviation of the strength of each region within the foam material prepared by this invention is 0.50-1.25%, which is small, indicating balanced strength across all regions within the foam material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing polypropylene foam material, belonging to the field of polypropylene technology. Background Technology

[0002] Polymer foam materials are composite materials with a high molecular weight resin as the matrix and a large number of microporous bubble structures inside. They can be regarded as solid / gas composite materials with gas as the filler. The bubble structure distributed in the matrix can significantly regulate the aggregation state structure, macroscopic morphology and comprehensive properties of the polymer. This makes these composite materials, which have both solid matrix properties and gas functions, have unique advantages that are difficult to achieve with conventional non-foamed polymers, such as lightweighting, heat insulation, buffering and energy absorption, and sound insulation and noise reduction.

[0003] Polypropylene, as a semi-crystalline thermoplastic polymer, possesses numerous superior properties in its foamed products: it boasts excellent thermal stability, outstanding shock absorption and energy absorption characteristics, and high deformation recovery rate, while also exhibiting excellent chemical corrosion resistance, oil resistance, and balanced tensile strength, impact strength, and toughness. Furthermore, the main component of polypropylene foamed products is thermoplastic PP resin, which is recyclable and photodegradable, making it a preferred matrix material for environmentally friendly foamed products. Simultaneously, it can be mass-produced using existing general-purpose extrusion molding and secondary processing equipment, with a simple and controllable process flow, resulting in significantly lower overall processing costs for foamed sheets compared to similar foamed materials. Based on these advantages, PP foamed materials have been widely used in food and industrial product packaging, automotive cushioning structures, and building insulation materials.

[0004] However, the traditional PP foaming process has significant shortcomings. The core reason is that its molecular structure is a highly flexible linear long chain with high crystallinity. When the system temperature rises above the crystallization melting temperature, the melt viscosity of PP drops sharply with increasing temperature, and the melt strength decreases significantly. This melting characteristic directly makes it extremely difficult to stably control the foaming process. On the one hand, the excessively low melt viscosity and melt strength cannot effectively contain the gas generated by the decomposition of the foaming agent, and the gas can easily diffuse and accumulate rapidly in the melt. On the other hand, PP resin itself has a large heat capacity, and a large amount of heat of crystallization is released during the transition from the molten state to the crystalline state, which further exacerbates the decrease in melt viscosity and strength. At the same time, the dense crystalline structure formed during the crystallization process will exert a squeezing effect on the cell, further promoting the diffusion and merging of gas. The combined effect of these two factors will lead to the easy escape of gas and excessive merging of cell during the foaming process, and even the collapse and rupture of cell walls due to the inability to withstand the internal gas pressure. Ultimately, this results in a narrow PP foaming process window and poor controllability, making it difficult to produce PP foam products with independent cell structure, fine and uniform pore size, and excellent comprehensive performance in industrial production.

[0005] To address the aforementioned industry pain points, HENaguib et al., in their research, systematically proposed four technical pathways to improve the stability of the PP extrusion foaming process and suppress gas escape and cell collapse: First, by modifying the PP matrix to enhance the PP melt strength. While methods such as matrix crosslinking and grafting modification can significantly improve melt strength, they suffer from poor reaction controllability, residual small-molecule byproducts, high equipment modification costs, and weak industrial adaptability. Second, by selecting novel foaming agents with low gas diffusion rates to slow down the migration rate of gas in the melt; however, low diffusion rates... New foaming agents are often limited by high production costs, environmental regulations, and difficulties in storage and transportation, making large-scale promotion difficult. Third, optimizing the process parameters of the entire extrusion foaming process can avoid the excessively rapid crystallization of the PP matrix. However, simply optimizing the process parameters can only slightly broaden the foaming process window and cannot fundamentally solve the defect of insufficient PP melt strength, thus limiting the potential for application improvement. Fourth, introducing nucleating agents or inorganic fillers into the PP matrix and constructing a multiphase composite system through blending and mixing can achieve the regulation and optimization of the performance of PP foam materials (Hani, E, Naguib, et al. Strategies for achieving ultra low-density polypropylene foams[J]. Polymer Engineering & Science, 2002.DOI:10.1002 / pen.11045.).

[0006] By introducing nucleating agents or inorganic fillers, this method has become the most widely used technical solution in the research and industrial application of PP foaming due to its advantages such as simple process flow, no need to modify existing production equipment, wide availability of raw materials, controllable cost, and simultaneous control of cell structure and enhancement of matrix properties. The mechanism of this method is as follows: inorganic fillers can act as heterogeneous nucleation sites in the PP matrix, reduce the cell nucleation barrier, significantly increase cell nucleation density, refine cell diameter, and improve cell uniformity. At the same time, rigid inorganic fillers can restrict the movement of PP molecular chains, increase the melt viscosity and high-temperature melt strength of the composite system, enhance the deformation resistance of cell walls, and effectively suppress gas escape and cell collapse.

[0007] Patent CN121495190A discloses a method for preparing foamed polypropylene with high compressive strength and resilience. This method introduces aluminum borate whiskers, a rigid reinforcing component, and an elastic toughening agent into the PP matrix, thereby simultaneously improving the strength and toughness of the PP matrix and suppressing gas escape during the foaming process. The resulting foamed polypropylene product has excellent compressive strength and resilience. However, this patent has the following problems: on the one hand, aluminum borate whiskers are prone to agglomeration in the PP matrix, resulting in poor dispersion uniformity. Although the overall strength of the PP matrix is ​​improved, the strength distribution within the foamed material is uneven. On the other hand, the foaming agent has poor compatibility in the matrix, leading to poor foaming stability and a decrease in the foaming rate of the product. Summary of the Invention

[0008] To address the problems existing in the prior art, this invention provides a method for preparing polypropylene foam material. The resulting polypropylene foam material possesses both high strength and high elasticity in mechanical properties and a high foaming rate, while the filler, foaming agent, and polypropylene matrix exhibit good compatibility.

[0009] To solve the above technical problems, the technical solution adopted by the present invention is as follows: A method for preparing polypropylene foam material includes the following steps: pretreatment of cellulose whiskers, preparation of a composite foaming agent, and preparation of foamed polypropylene.

[0010] The method for pretreating cellulose whiskers is as follows: cellulose whiskers are added to deionized water and stirred evenly. Then, tetramethylpiperidine oxide and sodium bromide are added to the solution, and sodium hypochlorite solution is added dropwise. After the addition is completed, the mixture is stirred at 180-200 rpm for 3-4 hours at room temperature in the dark. After the reaction is completed, the mixture is washed, filtered and dried to obtain carboxylated cellulose whiskers, which are the pretreated cellulose whiskers. The cellulose whiskers are of type C-CNC99; The sodium hypochlorite solution has a mass concentration of 8-12%; The dripping rate is 0.2-0.5 g / s; The mass ratio of the cellulose whiskers, deionized water, tetramethylpiperidine oxide, sodium bromide, and sodium hypochlorite solution is 1:95-100:0.1-0.3:1:8-13.

[0011] The method for preparing the composite foaming agent is as follows: foaming agent AC and zinc oxide ZnO are mixed evenly and then added to a ball mill. The ball-to-material ratio is controlled at 5:1. The mixture is ball-milled at 180-200 rpm at room temperature for 20-30 minutes. After ball milling, the mixture is sieved to obtain the ball-milled powder. The ball-milled powder is then added to anhydrous ethanol, and ethylenediamine is added. The solution temperature is controlled at 39-41℃, and the mixture is stirred at 40-50 rpm for 30-40 minutes. After stirring, the mixture is filtered and dried to obtain the activated powder. The pretreated cellulose is then... Whiskers were added to deionized water and stirred until homogeneous. The mixture was then subjected to ultrasonic treatment at room temperature, with the ultrasonic power controlled at 280-300W for 20-30 minutes. After ultrasonication, silica was added, and ultrasonication continued for 10-15 minutes. A composite dispersion was obtained after ultrasonication. The activated powder was added to the composite dispersion, the solution temperature was raised to 40-45℃, and the pH of the system was adjusted to 4.5-5.0. The mixture was stirred at 280-310 rpm for 3-4 hours. After the reaction was complete, the mixture was filtered, washed, and dried to obtain the composite foaming agent. The mass ratio of the foaming agent AC to zinc oxide ZnO is 10-15:1; The mass ratio of the ball-milled powder, anhydrous ethanol, and ethylenediamine is 1-1.3:10-15:5-7; The mass ratio of the pretreated cellulose whiskers, deionized water, and silica is 1-2:60-80:0.2-0.4. The mass ratio of the activated powder to the composite dispersion is 1-1.5:16-21.

[0012] The method for preparing foamed polypropylene is as follows: polypropylene chips, composite foaming agent, antioxidant 1010 and zinc stearate are added to a high-speed mixer and mixed at room temperature for 20-30 minutes to obtain a premix; the premix is ​​added to a twin-screw extruder, the processing temperature is controlled at 160-190℃ and the screw speed is 180-220rpm, and the foamed polypropylene is obtained by melt extrusion and granulation. The mass ratio of the polypropylene chips, composite foaming agent, antioxidant 1010, and zinc stearate is 100:3-5:0.2-0.5:0.1-0.3.

[0013] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. By oxidizing cellulose whiskers with sodium hypochlorite, the primary hydroxyl groups of the cellulose whiskers are oxidized to carboxyl groups, resulting in carboxylated cellulose whiskers. The carboxylated cellulose whiskers repel each other due to electrostatic attraction, which improves the dispersibility of the cellulose whiskers, avoids the agglomeration of cellulose whiskers, and improves the strength uniformity of the polypropylene product. The cellulose whiskers are also attracted by electrostatic attraction and adsorbed onto the surface of the rough AC foaming agent particles to form a continuous shell. The steric hindrance between the continuous shells inhibits the agglomeration of the foaming agent particles, thereby improving the dispersibility of the foaming agent particles in the polypropylene matrix and increasing the foaming rate and foaming stability.

[0014] 2. The foamed polypropylene prepared by this invention has a tensile strength of 37.6-38.1 MPa and an impact strength of 9.5-10.3 KJ / m. 2 The foamed polypropylene exhibits excellent mechanical properties, reaching maximum foam volume in 126-137 seconds with a foaming ratio of 9.3-10.1 times. The foaming agent demonstrates excellent foaming rate and ratio. The carboxylated cellulose whiskers prepared by this invention have a light transmittance of 23-25% and good whisker dispersibility. The relative standard deviation of the strength of each region within the foamed material prepared by this invention is 0.50-1.25%, which is small, indicating balanced strength across all regions within the foamed material. Detailed Implementation

[0015] To provide a clearer understanding of the technical features, objectives, and effects of the present invention, specific embodiments of the present invention are now described.

[0016] Example 1 A method for preparing polypropylene foam material includes the following steps: pretreatment of cellulose whiskers, preparation of a composite foaming agent, and preparation of foamed polypropylene.

[0017] (1) Pretreatment of cellulose whiskers Cellulose whiskers were added to deionized water and stirred until homogeneous. Then, tetramethylpiperidine oxide and sodium bromide were added to the solution, followed by the dropwise addition of sodium hypochlorite solution. After the addition was complete, the mixture was stirred at 190 rpm for 3.5 h at room temperature in the dark. After the reaction was completed, the mixture was washed, filtered, and dried to obtain carboxylated cellulose whiskers, i.e., pretreated cellulose whiskers. The cellulose whiskers are of type C-CNC99; The sodium hypochlorite solution has a mass concentration of 11%. The dropping rate is 0.3 g / s; The mass ratio of the cellulose whiskers, deionized water, tetramethylpiperidine oxide, sodium bromide, and sodium hypochlorite solution is 1:97:0.2:1:10.

[0018] (2) Preparation of composite foaming agent AC and ZnO were mixed evenly and then added to a ball mill. The ball-to-powder ratio was controlled at 5:1. The mixture was ball-milled at 190 rpm for 25 min at room temperature. After ball milling, the mixture was sieved to obtain the ball-milled powder. The ball-milled powder was added to anhydrous ethanol, and ethylenediamine was added. The solution temperature was controlled at 40℃, and the mixture was stirred at 45 rpm for 35 min. After stirring, the mixture was filtered and dried to obtain the activated powder. The pretreated cellulose whiskers were added to deionized water and stirred evenly. The mixture was then ultrasonically treated at room temperature. The ultrasonic power was controlled at 290 W for 25 min. After ultrasonic treatment, silica was added, and ultrasonic treatment was continued for 13 min. After ultrasonic treatment, a composite dispersion was obtained. The activated powder was added to the composite dispersion, the solution temperature was raised to 43℃, the pH of the system was adjusted to 4.7, and the mixture was stirred at 290 rpm for 3.5 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain the composite foaming agent. The mass ratio of the foaming agent AC to zinc oxide ZnO is 13:1; The mass ratio of the ball-milled powder, anhydrous ethanol, and ethylenediamine is 1.2:13:6; The mass ratio of the pretreated cellulose whiskers, deionized water, and silica is 1.5:70:0.3. The mass ratio of the activated powder to the composite dispersion is 1.3:18.

[0019] (3) Preparation of foamed polypropylene 1000g of polypropylene chips, 40g of composite foaming agent, 3g of antioxidant 1010 and 2g of zinc stearate were added to a high-speed mixer and mixed at room temperature for 25 minutes to obtain a premix. The premix was then added to a twin-screw extruder, and the processing temperature was controlled at 175℃ and the screw speed was 195rpm. After melt extrusion and granulation, foamed polypropylene was obtained.

[0020] Example 2 A method for preparing polypropylene foam material includes the following steps: pretreatment of cellulose whiskers, preparation of a composite foaming agent, and preparation of foamed polypropylene.

[0021] (1) Pretreatment of cellulose whiskers Cellulose whiskers were added to deionized water and stirred until homogeneous. Tetramethylpiperidine oxide and sodium bromide were then added to the solution, followed by the dropwise addition of sodium hypochlorite solution. After the addition was complete, the mixture was stirred at 180 rpm for 3 hours at room temperature in the dark. After the reaction was completed, the mixture was washed, filtered, and dried to obtain carboxylated cellulose whiskers, i.e., pretreated cellulose whiskers. The cellulose whiskers are of type C-CNC99; The sodium hypochlorite solution has a mass concentration of 8%; The dropping rate is 0.2 g / s; The mass ratio of the cellulose whiskers, deionized water, tetramethylpiperidine oxide, sodium bromide, and sodium hypochlorite solution is 1:95:0.1:1:8.

[0022] (2) Preparation of composite foaming agent AC and ZnO were mixed evenly and then added to a ball mill. The ball-to-powder ratio was controlled at 5:1. The mixture was ball-milled at 180 rpm for 20 min at room temperature. After ball milling, the mixture was sieved to obtain the ball-milled powder. The ball-milled powder was added to anhydrous ethanol, and ethylenediamine was added. The solution temperature was controlled at 39℃, and the mixture was stirred at 40 rpm for 30 min. After stirring, the mixture was filtered and dried to obtain the activated powder. The pretreated cellulose whiskers were added to deionized water and stirred evenly. The mixture was then ultrasonically treated at room temperature. The ultrasonic power was controlled at 280W for 20 min. After ultrasonic treatment, silica was added, and ultrasonic treatment was continued for 10 min. After ultrasonic treatment, a composite dispersion was obtained. The activated powder was added to the composite dispersion, the solution temperature was raised to 40℃, the pH of the system was adjusted to 4.5, and the mixture was stirred at 280 rpm for 3 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain the composite foaming agent. The mass ratio of the foaming agent AC to zinc oxide ZnO is 10:1; The mass ratio of the ball-milled powder, anhydrous ethanol, and ethylenediamine is 1:10:5; The mass ratio of the pretreated cellulose whiskers, deionized water, and silica is 1:60:0.2. The mass ratio of the activated powder to the composite dispersion is 1:16.

[0023] (3) Preparation of foamed polypropylene 1000g of polypropylene chips, 30g of composite foaming agent, 2g of antioxidant 1010 and 1g of zinc stearate were added to a high-speed mixer and mixed at room temperature for 20 minutes to obtain a premix. The premix was then added to a twin-screw extruder, and the processing temperature was controlled at 160℃ and the screw speed was 180rpm. After melt extrusion and granulation, foamed polypropylene was obtained.

[0024] Example 3 A method for preparing polypropylene foam material includes the following steps: pretreatment of cellulose whiskers, preparation of a composite foaming agent, and preparation of foamed polypropylene.

[0025] (1) Pretreatment of cellulose whiskers Cellulose whiskers were added to deionized water and stirred until homogeneous. Tetramethylpiperidine oxide and sodium bromide were then added to the solution, followed by the dropwise addition of sodium hypochlorite solution. After the addition was complete, the mixture was stirred at 200 rpm for 4 hours at room temperature in the dark. After the reaction was completed, the mixture was washed, filtered, and dried to obtain carboxylated cellulose whiskers, i.e., pretreated cellulose whiskers. The cellulose whiskers are of type C-CNC99; The sodium hypochlorite solution has a mass concentration of 12%. The dropping rate is 0.5 g / s; The mass ratio of the cellulose whiskers, deionized water, tetramethylpiperidine oxide, sodium bromide, and sodium hypochlorite solution is 1:100:0.3:1:13.

[0026] (2) Preparation of composite foaming agent AC and ZnO were mixed evenly and then added to a ball mill. The ball-to-powder ratio was controlled at 5:1. The mixture was ball-milled at 200 rpm for 30 min at room temperature. After ball milling, the mixture was sieved to obtain the ball-milled powder. The ball-milled powder was added to anhydrous ethanol, and ethylenediamine was added. The solution temperature was controlled at 41℃, and the mixture was stirred at 50 rpm for 40 min. After stirring, the mixture was filtered and dried to obtain the activated powder. The pretreated cellulose whiskers were added to deionized water and stirred evenly. The mixture was then ultrasonically treated at room temperature. The ultrasonic power was controlled at 300W for 30 min. After ultrasonic treatment, silica was added, and ultrasonic treatment was continued for 15 min. After ultrasonic treatment, a composite dispersion was obtained. The activated powder was added to the composite dispersion, the solution temperature was raised to 45℃, the pH of the system was adjusted to 5.0, and the mixture was stirred at 310 rpm for 4 h. After the reaction was completed, the mixture was filtered, washed, and dried to obtain the composite foaming agent. The mass ratio of the foaming agent AC to zinc oxide ZnO is 15:1; The mass ratio of the ball-milled powder, anhydrous ethanol, and ethylenediamine is 1.3:15:7; The mass ratio of the pretreated cellulose whiskers, deionized water, and silica is 2:80:0.4. The mass ratio of the activated powder to the composite dispersion is 1.5:21.

[0027] (3) Preparation of foamed polypropylene 1000g of polypropylene chips, 50g of composite foaming agent, 5g of antioxidant 1010 and 3g of zinc stearate were added to a high-speed mixer and mixed at room temperature for 30 minutes to obtain a premix. The premix was then added to a twin-screw extruder, and the processing temperature was controlled at 190℃ and the screw speed was 220rpm. After melt extrusion and granulation, foamed polypropylene was obtained.

[0028] Comparative Example 1 Based on Example 1, the change is that the cellulose whiskers are not pretreated. In the step of preparing the composite foaming agent, untreated cellulose whiskers are used. All other operations are the same.

[0029] Comparative Example 2 Based on Example 1, the change is that the preparation step of the composite foaming agent is omitted. The method for preparing foamed polypropylene is as follows: 1000g of polypropylene chips, 25g of AC foaming agent, 4g of ZnO, 8g of pretreated cellulose whiskers, 7g of silica, 3g of antioxidant 1010 and 2g of zinc stearate are added to a high-speed mixer and mixed at room temperature for 30 minutes to obtain a premix; the premix is ​​added to a twin-screw extruder, the processing temperature is controlled at 190℃ and the screw speed is 220rpm, and the foamed polypropylene is obtained by melt extrusion and granulation.

[0030] Experimental Example 1: Performance Testing of Polypropylene Foamed Material The performance of the foamed polypropylene prepared in Examples 1-3 and Comparative Examples 1-2 was tested. Tensile strength was tested according to ASTM D638-2003, "Standard Test Method for Tensile Properties of Plastics"; impact strength was tested according to ASTM D256-1997, "Standard Test Method for Cantilever Impact Properties of Plastics"; foaming rate was calculated using a gas metering foaming rate tester based on the water displacement method, according to GB / T22048-2022; and foaming ratio was measured using the water displacement method to determine the apparent density of the foamed material and the apparent density of the material before foaming, according to ISO 1183-1987. The test results are shown in Table 1. Table 1. Polypropylene performance test results

[0031] Experimental Example 2: Cellulose Whisker Dispersibility Test The surface-treated cellulose whiskers of Examples 1-3 and the untreated cellulose whiskers of Comparative Example 1 were tested using a UV-Vis spectrophotometer. The transmittance at 600 nm was measured to quantitatively characterize the dispersibility and agglomeration degree of carboxylated cellulose whiskers in water. The better the whisker dispersion, the lower the transmittance of its aqueous solution at 600 nm. The test results are shown in Table 2. Table 2 Results of Cellulose Whiskers Dispersibility Test

[0032] Experimental Example 3: Strength Uniformity Test of Polypropylene Foam Material in Different Regions The strength properties of foamed polypropylene prepared in Examples 1-3 and Comparative Examples 1-2 were tested at different locations. Each sample was a standard specimen (150mm × 10mm × 4mm) formed after extrusion granulation from the same batch. Referring to the standard ASTM D638-2003, "Standard Test Method for Tensile Properties of Plastics," each standard specimen was divided into five test regions along its length, labeled Region 1, Region 2, Region 3, Region 4, and Region 5. Three parallel tensile specimens were cut from each region, with the specimen dimensions conforming to the specifications. A total of 15 test specimens were prepared for each sample. The pretreated specimens were sequentially clamped onto an electronic universal testing machine, and the tensile rate was set to 50mm / min. The tensile strength of each specimen was tested according to the ASTM D638-2003 standard. The test data for each specimen were recorded, and the average tensile strength and relative standard deviation (RSD) (standard deviation / average value × 100%) of the three parallel specimens in each region were calculated. A smaller relative standard deviation indicates a more uniform strength within the polypropylene foam. The test results are shown in Table 3. Table 3. Test results of strength uniformity performance in different regions inside polypropylene foam material.

[0033] As shown in Table 1, the tensile strength of the foamed polypropylene prepared in Examples 1-3 is 37.6-38.1 MPa, and the impact strength is 9.5-10.3 KJ / m. 2 The foamed polypropylene exhibits excellent mechanical properties, reaching its maximum foam volume in 126-137 seconds with a foaming ratio of 9.3-10.1 times. The foaming agent demonstrates excellent foaming rate and ratio. In Comparative Example 1, no cellulose whiskers were pretreated. In the preparation of the composite foaming agent, cellulose whiskers with relatively poor dispersibility were used, resulting in slightly lower tensile strength and impact strength of the prepared polypropylene product. In Comparative Example 2, no composite foaming agent was used, and the foamed product took a long time to reach its maximum foam volume.

[0034] As shown in Table 2, the light transmittance of the carboxylated cellulose whiskers prepared in Examples 1-3 is 23-25%, and the whiskers have good dispersibility. In contrast, Comparative Example 1 did not perform surface treatment on the cellulose whiskers, and the whiskers had poor dispersibility.

[0035] As shown in Table 3, the relative standard deviation of the strength of each region inside the foamed material prepared in Examples 1-3 is 0.50-1.25%, which is small and the strength of each region inside the foamed material is uniform. In contrast, the polypropylene foamed material prepared by Comparative Example 1 using cellulose whiskers with relatively poor dispersibility has lower strength uniformity in each region than that of Example 1.

[0036] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for producing a polypropylene foamed material, characterized by, The preparation method includes the following steps: pretreatment of cellulose whiskers, preparation of composite foaming agent, and preparation of foamed polypropylene; The method for preparing the composite foaming agent is as follows: foaming agent AC and zinc oxide ZnO are mixed evenly and then added to a ball mill and ball-milled for 20-30 minutes. After ball milling, the mixture is sieved to obtain the ball-milled powder. The ball-milled powder is added to anhydrous ethanol, ethylenediamine is added, and after stirring and mixing, the mixture is filtered and dried to obtain the activated powder. Pretreated cellulose whiskers are added to deionized water, stirred evenly, and then ultrasonically treated at room temperature. After ultrasonic treatment, silica is added, and ultrasonic treatment is continued. After ultrasonic treatment, a composite dispersion is obtained. The activated powder is added to the composite dispersion, the solution temperature is raised to 40-45℃, the pH of the system is adjusted to 4.5-5.0, and the mixture is stirred at 280-310 rpm for 3-4 hours. After the reaction is completed, the mixture is filtered, washed, and dried to obtain the composite foaming agent.

2. The method for preparing a polypropylene foam material according to claim 1, characterized in that, The mass ratio of the foaming agent AC to zinc oxide ZnO is 10-15:1; The mass ratio of the ball-milled powder, anhydrous ethanol, and ethylenediamine is 1-1.3:10-15:5-7; The mass ratio of the pretreated cellulose whiskers, deionized water, and silica is 1-2:60-80:0.2-0.

4. The mass ratio of the activated powder to the composite dispersion is 1-1.5:16-21.

3. The method for preparing a polypropylene foam material according to claim 1, characterized in that, The method for pretreating cellulose whiskers is as follows: cellulose whiskers are added to deionized water and stirred evenly. Then, tetramethylpiperidine oxide and sodium bromide are added to the solution, and sodium hypochlorite solution is added dropwise. After the addition is completed, the mixture is stirred at 180-200 rpm for 3-4 hours at room temperature in the dark. After the reaction is completed, the mixture is washed, filtered and dried to obtain carboxylated cellulose whiskers, which are the pretreated cellulose whiskers.

4. The method for preparing a polypropylene foam material according to claim 1, characterized in that, The cellulose whiskers are of type C-CNC99; The sodium hypochlorite solution has a mass concentration of 8-12%; The dripping rate is 0.2-0.5 g / s; The mass ratio of the cellulose whiskers, deionized water, tetramethylpiperidine oxide, sodium bromide, and sodium hypochlorite solution is 1:95-100:0.1-0.3:1:8-13.

5. The method for preparing a polypropylene foam material according to claim 1, characterized in that, The method for preparing foamed polypropylene is as follows: polypropylene chips, composite foaming agent, antioxidant 1010 and zinc stearate are added to a high-speed mixer and mixed at room temperature for 20-30 minutes to obtain a premix; the premix is ​​added to a twin-screw extruder, the processing temperature is controlled at 160-190℃ and the screw speed is 180-220rpm, and the foamed polypropylene is obtained by melt extrusion and granulation.

6. The method for preparing a polypropylene foam material according to claim 1, characterized in that, The mass ratio of the polypropylene chips, composite foaming agent, antioxidant 1010, and zinc stearate is 100:3-5:0.2-0.5:0.1-0.3.