Flame-retardant polylactic acid / biomass fiber composites and their preparation methods
By coating biomass fibers with melamine-formaldehyde resin and crosslinking with epoxidized phytic acid, the flame retardant and mechanical properties of polylactic acid/biomass fiber composites have been solved, achieving simultaneous improvement in UL94 V0 flame retardancy and mechanical properties, making them suitable for applications in home furnishings, rail transportation, automotive interiors, and packaging.
Patent Information
- Application Number
- CN202611359144.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-03
- Publication Date
- 2026-11-17
AI Technical Summary
Existing polylactic acid/biomass fiber composites have poor flame retardant properties and cannot meet the UL94 V0 flame retardant requirements. Furthermore, traditional flame retardants require large amounts and easily damage the interfacial structure, leading to a decline in mechanical properties.
The biomass fiber was coated and modified with melamine-formaldehyde resin to construct a dense flame-retardant char protective layer. Then, an epoxidized phytic acid flame-retardant crosslinking agent was used to crosslink with the polylactic acid matrix to form a continuous and dense flame-retardant char layer, thereby improving interfacial compatibility.
It achieves UL94 V0 flame retardancy with low additive content, provides long-lasting and stable flame retardant effect, significantly improves mechanical properties, and is halogen-free and non-toxic, meeting green and low-carbon requirements.
Smart Images

Figure CN123107327A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer composite materials technology, and in particular to a flame-retardant polylactic acid / biomass fiber composite material and its preparation method. Background Technology
[0002] Polylactic acid (PLA) is a fully biodegradable, green polymer material with excellent mechanical properties, processing performance, and biocompatibility. It is widely used in packaging, home furnishings, automotive lightweighting, and textile structural composites. Biomass fibers, as high-quality natural plant fibers, possess advantages such as high specific strength, excellent toughness, green renewability, and low cost. They are often used as reinforcing phases to modify PLA, effectively improving the structural strength and dimensional stability of composite materials, making them a preferred raw material for preparing fully bio-based composite materials.
[0003] However, pure polylactic acid / biomass fiber composites have a fatal flaw: biomass fibers have a natural cellulose structure, are rich in flammable hydroxyl groups, have a high calorific value, and are highly flammable, producing a significant wick effect during combustion. The fibers continuously store heat and ignite the matrix resin, causing the composite material to burn continuously, accompanied by melting and dripping, making it difficult to self-extinguish. Its flame retardant properties are extremely poor, failing to meet the industrial UL94 V0 flame retardant requirements, severely restricting the large-scale application of this type of bio-based composite material in scenarios with high flame retardant and safety requirements.
[0004] Current industry solutions for flame-retardant modification of such composite materials mostly involve adding inorganic, halogenated, or phosphorus-based flame retardants, which generally suffer from several technical drawbacks: First, the large amount of flame retardant added can easily lead to agglomeration in the matrix, damaging the interfacial structure of the composite material and causing a significant decrease in mechanical properties; second, it can only achieve auxiliary flame retardancy and cannot specifically eliminate the inherent wicking effect of biomass fibers, leaving the problems of sustained combustion and dripping unresolved; third, it is difficult to balance flame retardant performance and mechanical properties, resulting in a performance trade-off. In summary, the flame-retardant performance of this type of composite material is currently poor. Summary of the Invention
[0005] The main objective of this invention is to provide a flame-retardant polylactic acid / biomass fiber composite material and its preparation method, aiming to solve the problem of poor flame-retardant performance of this type of composite material at present.
[0006] To achieve the above objectives, the present invention provides a flame-retardant polylactic acid / biomass fiber composite material, characterized in that, by weight, it comprises: 70-85 parts of polylactic acid resin, 10-20 parts of modified biomass fiber, and 3-10 parts of epoxidized phytic acid flame-retardant crosslinking agent. The modified biomass fiber is a biomass fiber with a melamine-formaldehyde resin layer on its surface, and the epoxidized phytic acid flame retardant crosslinking agent is a phytic acid derivative flame retardant crosslinking agent containing epoxy groups in its molecular structure.
[0007] In one embodiment, the biomass fiber includes any one or more of ramie fiber, flax fiber, cotton fiber, bamboo fiber, fibroin fiber, viscose fiber, and lyocell fiber.
[0008] In one embodiment, the coating thickness of the melamine-formaldehyde resin layer is 1–500 μm.
[0009] In one embodiment, the epoxy group content in the epoxidized phytic acid flame retardant crosslinking agent is 1%–30% by mass.
[0010] The present invention also provides a method for preparing the flame-retardant polylactic acid / biomass fiber composite material as described above, comprising the following steps: The biomass fiber was ultrasonically cleaned using a mixed solution of acetone and ethanol, and then dried to obtain pretreated biomass fiber. The pretreated biomass fiber was immersed in a melamine-formaldehyde resin solution. The pH value, reaction temperature and soaking time of the system were adjusted to form a resin coating layer on the surface of the pretreated biomass fiber. After the reaction was completed, the fiber was taken out, dried and cured to obtain modified biomass fiber. Amination-modified phytic acid intermediates are prepared by reacting phytic acid with polyamine compounds, and then the amination-modified phytic acid intermediates are subjected to a ring-opening addition reaction with epichlorohydrin to prepare an epoxidized phytic acid flame retardant crosslinking agent. Polylactic acid resin, the modified biomass fiber, and the epoxidized phytic acid flame retardant crosslinking agent are mixed uniformly according to the specified ratio, and then subjected to molding treatment to obtain a flame retardant polylactic acid / biomass fiber composite material.
[0011] In one embodiment, the volume ratio of acetone to ethanol in the acetone-ethanol mixture is 1:1, and the ultrasonic cleaning time is 20–40 min.
[0012] In one embodiment, the melamine-formaldehyde resin solution has a pH of 8.0–9.0, a reaction temperature of 55–70°C, a soaking time of 1–10 h, and a drying and curing temperature of 70–90°C.
[0013] In one embodiment, the polyamine compound includes any one or more of ethylenediamine, butanediamine, pentanediamine, hexanediamine, phenylenediamine, 4,4'-diaminodiphenylmethane, 3,5-dimethylthiotoluenediamine, diethylaminoethylamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, and polyetheramine.
[0014] In one embodiment, in the step of preparing the amino-modified phytic acid intermediate by reacting phytic acid with a polyamine compound, the molar ratio of phytic acid to the polyamine compound is 1:1–1:12, and the amino-modified phytic acid intermediate is prepared by stirring at room temperature for 1–10 h.
[0015] In one embodiment, in the step of preparing an epoxidized phytic acid flame retardant crosslinking agent by performing a ring-opening addition reaction between the amino-modified phytic acid intermediate and epichlorohydrin under the action of a catalyst, the molar ratio of amino-modified phytic acid to epichlorohydrin is 1:1–1:12, and the epoxidized phytic acid flame retardant crosslinking agent is prepared by reacting under weakly alkaline catalytic conditions at 30–90°C for 1–20 h.
[0016] This invention provides a flame-retardant polylactic acid / biomass fiber composite material. It employs melamine-formaldehyde resin to integrally coat and modify the biomass fiber, constructing a dense, high-temperature resistant flame-retardant char protective layer on the fiber surface. This effectively isolates the combustible cellulose inside the fiber from contact with oxygen and high-temperature heat sources, inhibiting the fiber's heat storage and ignition. This fundamentally eliminates the problems of wick ignition, continuous burning, and melting dripping inherent in traditional composite materials, resulting in a long-lasting and stable flame-retardant effect. Furthermore, epoxidized phytic acid possesses both flame-retardant and cross-linking functions. The epoxy groups on its molecular chain can undergo cross-linking reactions with the hydroxyl groups on the melamine resin surface, the terminal carboxyl groups and terminal hydroxyl groups of the polylactic acid matrix, respectively. On one hand, this promotes the formation of a continuous and dense flame-retardant char layer during combustion, achieving synergistic flame retardancy. On the other hand, it significantly improves the interfacial compatibility between the biomass fiber and the polylactic acid matrix, reduces interfacial defects, and significantly enhances the tensile, flexural, and other mechanical properties of the composite material, breaking through the performance bottleneck of traditional modification technologies. The overall flame-retardant system of this invention, with an addition amount not exceeding 10%, enables the composite material to stably achieve UL94. With a V0 flame retardant rating, it boasts high flame retardant efficiency. The low filler addition effectively avoids problems such as filler agglomeration and poor matrix plasticization, maximizing the preservation of the excellent processing performance and basic mechanical properties of polylactic acid composites. The flame retardant raw material, phytic acid, is a natural plant extract that is halogen-free, non-toxic, and pollution-free. The modification process is simple, mild, and highly controllable, with no harmful byproducts generated throughout the process. It meets the development requirements of green, low-carbon, and bio-based materials and can be widely used in flame retardant fields such as home furnishings, rail transportation, automotive interiors, and packaging, with broad prospects for industrial application. Attached Figure Description
[0017] Figure 1 This is a flowchart of the epoxidized phytic acid preparation reaction provided by the embodiment of the present invention (taking triethylenetetramine as an example). Figure 2 These are the infrared spectra of amino-modified phytic acid and epoxidized phytic acid provided in the embodiments of the present invention.
[0018] The realization of the objective, functional features and advantages of the present invention will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation
[0019] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0020] It should be noted that if the embodiments of the present invention involve directional indicators (such as up, down, left, right, front, back, etc.), the directional indicators are only used to explain the relative positional relationship and movement of the components in a certain specific posture (as shown in the figure). If the specific posture changes, the directional indicators will also change accordingly.
[0021] Furthermore, if the embodiments of this invention involve descriptions such as "first" or "second," these descriptions are for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined with "first" or "second" may explicitly or implicitly include at least one of those features. Additionally, the meaning of "and / or" throughout the text includes three parallel solutions; for example, "A and / or B" includes solution A, solution B, or a solution where both A and B are satisfied simultaneously. Furthermore, the technical solutions of the various embodiments can be combined with each other, but this must be based on the ability of those skilled in the art to implement them. When the combination of technical solutions is contradictory or impossible to implement, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection claimed by this invention.
[0022] This invention provides a flame-retardant polylactic acid / biomass fiber composite material, comprising, by weight: 70-85 parts polylactic acid resin, 10-20 parts modified biomass fiber, and 3-10 parts epoxidized phytic acid flame-retardant crosslinking agent; wherein the modified biomass fiber is a biomass fiber with a melamine-formaldehyde resin layer on its surface, and the epoxidized phytic acid flame-retardant crosslinking agent is a phytic acid derivative flame-retardant crosslinking agent containing epoxy groups in its molecular structure.
[0023] This invention provides a flame-retardant polylactic acid / biomass fiber composite material. It employs melamine-formaldehyde resin to integrally coat and modify the biomass fiber, constructing a dense, high-temperature resistant flame-retardant char protective layer on the fiber surface. This effectively isolates the combustible cellulose inside the fiber from contact with oxygen and high-temperature heat sources, inhibiting the fiber's heat storage and ignition. This fundamentally eliminates the problems of wick ignition, continuous burning, and melting dripping inherent in traditional composite materials, resulting in a long-lasting and stable flame-retardant effect. Furthermore, epoxidized phytic acid possesses both flame-retardant and cross-linking functions. The epoxy groups on its molecular chain can undergo cross-linking reactions with the hydroxyl groups on the melamine resin surface, the terminal carboxyl groups and terminal hydroxyl groups of the polylactic acid matrix, respectively. On one hand, this promotes the formation of a continuous and dense flame-retardant char layer during combustion, achieving synergistic flame retardancy. On the other hand, it significantly improves the interfacial compatibility between the biomass fiber and the polylactic acid matrix, reduces interfacial defects, and significantly enhances the tensile, flexural, and other mechanical properties of the composite material, breaking through the performance bottleneck of traditional modification technologies. The overall flame-retardant system of this invention, with an addition amount not exceeding 10%, enables the composite material to stably achieve UL94. With a V0 flame retardant rating, it boasts high flame retardant efficiency. The low filler addition effectively avoids problems such as filler agglomeration and poor matrix plasticization, maximizing the preservation of the excellent processing performance and basic mechanical properties of polylactic acid composites. The flame retardant raw material, phytic acid, is a natural plant extract that is halogen-free, non-toxic, and pollution-free. The modification process is simple, mild, and highly controllable, with no harmful byproducts generated throughout the process. It meets the development requirements of green, low-carbon, and bio-based materials and can be widely used in flame retardant fields such as home furnishings, rail transportation, automotive interiors, and packaging, with broad prospects for industrial application.
[0024] Furthermore, the biomass fiber includes any one or more of ramie fiber, flax fiber, cotton fiber, bamboo fiber, fibroin fiber, viscose fiber, and lyocell fiber. It is applicable to the vast majority of biomass waste fibers or virgin fibers, with a wide range of raw material sources, low cost, and strong compatibility with coating processes.
[0025] On the other hand, the coating thickness of the melamine-formaldehyde resin layer is 1–500 μm. 1 μm can effectively form a complete, continuous, and dense single-layer or multi-layer resin film. When it is less than 1 μm, the coating layer may not be able to completely cover the active sites on the fiber surface, resulting in the cellulose still being ignitable at high temperatures, and the wick effect cannot be eliminated. The thickness of 500 μm is the upper limit threshold for the processability and flexibility of the composite material, which can avoid breakage and pulverization during extrusion, thus losing the reinforcing effect. By precisely controlling the soaking time and resin concentration, the coating thickness can be customized arbitrarily within this wide range to meet the emphasis on flexibility or flame retardancy in different application scenarios.
[0026] In this embodiment, the epoxy group content in the epoxidized phytic acid flame retardant crosslinking agent is 1%–30% by mass. By controlling the ratio of phytic acid to polyamine and the reaction time with ECH, the epoxy value can be precisely tailored, thereby balancing the crosslinking density, flame retardant efficiency, and processing fluidity of the composite material.
[0027] Based on the above-mentioned flame-retardant polylactic acid / biomass fiber composite material, the present invention provides a method for preparing a flame-retardant polylactic acid / biomass fiber composite material, which is used to prepare the above-mentioned flame-retardant polylactic acid / biomass fiber composite material, that is, it has all the technical features of the above-mentioned flame-retardant polylactic acid / biomass fiber composite material, and therefore also has the technical effects brought about by all the above-mentioned technical features.
[0028] The preparation method of the flame-retardant polylactic acid / biomass fiber composite material includes the following steps: S10. The biomass fiber is ultrasonically cleaned using a mixed solution of acetone and ethanol, and then dried to obtain pretreated biomass fiber. The acetone + ethanol mixture has the ability to dissolve both non-polar waxes and polar pectins. Ultrasonic assistance can peel off physically adsorbed impurities from the fiber surface. It removes impurities such as wax, dust, and pectin from the fiber surface. After cleaning, it is placed in a constant temperature oven at 60–80℃ to dry to constant weight, removes free moisture, and is sealed for later use, thus eliminating the influence of surface impurities on coating modification and interfacial bonding.
[0029] S20. The pretreated biomass fiber is immersed in a melamine-formaldehyde resin solution. The pH value, reaction temperature and soaking time of the system are adjusted to form a resin coating layer on the surface of the pretreated biomass fiber. After the reaction is completed, the fiber is taken out, dried and cured to obtain modified biomass fiber. An impregnation-drying-curing process is employed, utilizing the condensation reaction of methoxy / hydroxymethyl groups in melamine-formaldehyde resin under heating conditions to form an in-situ crosslinked film on the fiber surface. Compared to grafting modification, this method is simpler to operate, more controllable, and suitable for continuous industrial production.
[0030] S30. Phytic acid is reacted with polyamine compounds to prepare an amino-modified phytic acid intermediate, and then the amino-modified phytic acid intermediate is subjected to a ring-opening addition reaction with epichlorohydrin to prepare an epoxidized phytic acid flame retardant crosslinking agent. A two-step method was employed—first amination (introducing an active hydrogen), followed by addition with epichlorohydrin. This route avoids the strong exothermic reaction and side reactions of the direct reaction of phytic acid with ECH, and improves the grafting efficiency and safety of the epoxy groups.
[0031] S40. Polylactic acid resin, the modified biomass fiber, and the epoxidized phytic acid flame retardant crosslinking agent are mixed uniformly according to the specified ratio, and then subjected to molding treatment to obtain flame retardant polylactic acid / biomass fiber composite material.
[0032] The method for preparing flame-retardant polylactic acid / biomass fiber composite material provided by this invention has a clear process, mild conditions, uses conventional plastic processing equipment throughout the process, is highly compatible with existing polylactic acid modification production lines, and is easy to industrialize.
[0033] Furthermore, in the acetone and ethanol mixed solution, the volume ratio of acetone to ethanol is 1:1, and the ultrasonic cleaning time is 20–40 min. The volume ratio of acetone to ethanol combines azeotropic properties with the solubility parameters of waxes and pectins on the fiber surface; the ultrasonic time avoids incomplete removal of impurities and damage to the fibrillary structure on the fiber surface, and the pretreated fiber surface significantly improves the wetting and spreading properties of the subsequent resin solution.
[0034] On the other hand, the melamine-formaldehyde resin solution has a pH of 8.0–9.0, a reaction temperature of 55–70℃, a soaking time of 1–10 h, and a drying and curing temperature of 70–90℃. The weakly alkaline conditions effectively inhibit the self-aggregation (gelation) of melamine-formaldehyde resin in aqueous solution, promoting slow and uniform deposition and condensation of the resin on the fiber surface. By precisely controlling the pH, reaction temperature, and soaking time, the thickness of the resin coating layer can be controlled. After the reaction, the fiber is removed, dried, and cured, forming a dense and uniform flame-retardant coating layer on the surface of the biomass fiber, resulting in modified biomass fiber, thus blocking the fiber wicking effect at its source.
[0035] In this embodiment, the polyamine compound includes any one or more of ethylenediamine, butanediamine, pentanediamine, hexanediamine, phenylenediamine, 4,4'-diaminodiphenylmethane, 3,5-dimethylthiotoluenediamine, diethylaminoethylamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, and polyetheramine. Using natural, non-toxic phytic acid as the core raw material, an amination reaction is carried out with the polyamine compound to prepare an amino-modified phytic acid intermediate. The amino-modified phytic acid intermediate is then subjected to a ring-opening addition reaction with epichlorohydrin under the action of a catalyst to prepare an epoxidized phytic acid flame retardant crosslinking agent.
[0036] On the other hand, in the step of preparing the amination-modified phytic acid intermediate by reacting phytic acid with polyamine compounds, the molar ratio of phytic acid to polyamine compounds is 1:1–1:12, and the amination-modified phytic acid intermediate is prepared by stirring at room temperature for 1–10 hours. By controlling the molar ratio, the nitrogen and phosphorus content in the final epoxidized phytic acid can be adjusted to achieve an optimized match of the "phosphorus-nitrogen" synergistic flame retardant effect. This amination reaction is essentially an exothermic acid-base neutralization reaction, which can proceed spontaneously without external heating. By controlling the stirring time, problems such as uneven reaction or oxidation and discoloration due to prolonged exposure to air can be avoided.
[0037] Similarly, please see Figures 1 to 2In the step of preparing an epoxidized phytic acid flame retardant crosslinking agent by reacting the amino-modified phytic acid intermediate with epichlorohydrin under the action of a catalyst, the molar ratio of amino-modified phytic acid to epichlorohydrin is 1:1–1:12, and the reaction is carried out under weakly alkaline catalytic conditions at 30–90°C for 1–20 h. This ensures that the epoxy group content of the final product is stable at 1%–30%, and that the product is a viscous liquid or a low-melting-point solid at room temperature, facilitating uniform dispersion with PLA and participation in the in-situ crosslinking reaction during subsequent melt blending.
[0038] It should be noted that in step S40, the molding process includes melt blending and extrusion granulation using a twin-screw extruder, followed by injection molding after drying.
[0039] Furthermore, the twin-screw extrusion temperature is set to 180–200℃, the screw speed is 200–300 r / min, and the composite material is obtained by melt blending, extrusion granulation and drying, followed by injection molding.
[0040] Based on the above-mentioned flame-retardant polylactic acid / biomass fiber composite material and its preparation method, the present invention provides the following specific embodiments.
[0041] Example 1: A flame-retardant polylactic acid / biomass fiber composite material with wick-free properties, wherein the raw material mass ratio is: 82 parts polylactic acid resin, 12 parts melamine resin modified biomass fiber, and 6 parts epoxidized phytic acid.
[0042] Preparation steps: 1. Fiber pretreatment: Ramie short-cut fibers are ultrasonically cleaned with acetone and ethanol sequentially for 30 minutes, and then dried at 70℃ to constant weight; 2. Coating modification: Prepare a uniform melamine resin solution, adjust the pH value of the system to 8.5, immerse the pretreated ramie short-cut fiber in the resin solution and keep it warm for 2 hours under a constant temperature of 65℃, and dry and cure at 80℃ to obtain uniformly coated modified ramie fiber. 3. Preparation of epoxidized phytic acid: Phytic acid and triethylenetetramine were reacted at room temperature for 2 hours at a molar ratio of 1:6. The pH of the system was adjusted to 8.0 and mixed with epichlorohydrin, which was 6 times the molar amount of phytic acid. The mixture was reacted at 75°C for 3 hours. After purification and drying, epoxidized phytic acid with high epoxy group content was prepared. 4. Melt blending: All raw materials are uniformly mixed, and the mixture is extruded at a twin-screw extrusion temperature of 180–200℃, extruded into granules, and then injection molded to obtain a composite material.
[0043] The composite material prepared in this embodiment has a total flame retardant system addition of only 6%. After UL94 flame retardant testing, it stably meets the V0 flame retardant standard. During the combustion process, there is no continuous combustion, no melting dripping, and no secondary ignition. The wick effect is completely eliminated. Compared with the unmodified polylactic acid / biomass fiber composite material, the tensile and flexural mechanical strengths are improved by 18%. The flame retardant performance and mechanical properties are optimized simultaneously. The tensile and flexural mechanical strengths of the unmodified polylactic acid / biomass fiber composite material are 42.3 MPa and 74.3 MPa, respectively.
[0044] Example 2, Raw material ratio: 78 parts polylactic acid resin, 15 parts melamine resin-coated flax fiber, 7 parts epoxidized phytic acid, preparation process is the same as in Example 1.
[0045] Test results show that the composite material has a stable flame retardant rating of V0, tight interfacial bonding, further optimized mechanical properties, and improved tensile and flexural mechanical strength by 20% and 18% respectively, demonstrating excellent flame retardancy and long-lasting performance.
[0046] Example 3, Raw material ratio: 70 parts polylactic acid resin, 20 parts melamine resin-coated cotton fiber, and 10 parts epoxidized phytic acid.
[0047] Preparation steps: 1. Fiber pretreatment: Cotton short-cut fibers are ultrasonically cleaned with acetone and ethanol sequentially for 30 minutes, and then dried at 70℃ to constant weight; 2. Coating modification: Prepare a uniform melamine resin solution, adjust the pH to 8.5, immerse the pretreated cotton fibers in the resin solution at 65℃ and keep them warm for 2 hours, then dry and cure at 80℃ to obtain modified cotton fibers; 3. Preparation of epoxidized phytic acid: Same as in Example 1; 4. Melt blending: All raw materials are uniformly mixed, and the twin-screw extrusion temperature is 180–200℃. The mixture is then extruded, granulated, and injection molded.
[0048] Test results: With a total addition of 10% flame retardant system, the UL94 test achieved a V0 rating, exhibiting no dripping or wick effect during combustion. Compared to unmodified polylactic acid / cotton fiber composites, tensile strength increased by 22%, flexural strength increased by 19%, and interfacial bonding was tighter.
[0049] Example 4, Raw material ratio: 85 parts polylactic acid resin, 10 parts melamine resin-coated bamboo fiber, and 5 parts epoxidized phytic acid.
[0050] Preparation steps: 1. Fiber pretreatment: Bamboo short-cut fibers are ultrasonically cleaned with acetone and ethanol for 30 minutes in sequence, and then dried at 70℃ to constant weight; 2. Coating modification: Same as Example 1, coating time 1.5h, curing temperature 80℃; 3. Preparation of epoxidized phytic acid: Same as in Example 1; 4. Melt blending: Same as in Example 1.
[0051] Test results: With a total addition of 5% flame retardant system, the UL94 test achieved a V0 rating, with a self-extinguishing time of ≤2s and no wick effect. The mechanical properties were improved by 18% (tensile) and 16% (flexural) compared to the unmodified composite material, and the fibers were evenly dispersed.
[0052] Example 5, Raw material ratio: 80 parts polylactic acid resin, 13 parts melamine resin-coated lyocell fiber, and 7 parts epoxidized phytic acid.
[0053] Preparation steps: 1. Fiber pretreatment: Lyocell short-cut fibers are cleaned and dried using the same method; 2. Coating modification: Adjust the pH of the melamine resin solution to 8.5, coat at 65℃ for 2.5h, and dry and cure at 80℃; 3. Preparation of epoxidized phytic acid: Same as in Example 1; 4. Melt blending: Twin-screw extrusion temperature 185–195℃, the rest is the same as in Example 1.
[0054] Test results: Flame retardant rating V0, with no sustained combustion, no dripping, and no secondary ignition. Mechanical properties are improved by more than 20% compared to the unmodified composite material, with a significant increase in interfacial shear strength and no migration of flame retardant.
[0055] The present invention also provides the following comparative examples.
[0056] Comparative Example 1 (without epoxidized phytic acid, only modified fiber was used).
[0057] Raw material ratio: 82 parts polylactic acid resin and 12 parts melamine resin-coated ramie fiber (excluding epoxidized phytic acid).
[0058] Preparation steps: Same as in Example 1, but the preparation and addition of epoxidized phytic acid are omitted.
[0059] Test results: No UL94 rating was given. A noticeable wick effect was still observed during combustion. Although the coating partially suppressed dripping, the burning was persistent and it could not self-extinguish. Tensile strength decreased by 12%, flexural strength decreased by 15%, and interfacial bonding was weak.
[0060] Comparative Example 2 (without melamine resin coating, using only epoxidized phytic acid).
[0061] Raw material ratio: 82 parts polylactic acid resin, 12 parts unmodified ramie fiber, and 6 parts epoxidized phytic acid.
[0062] Preparation steps: Same as in Example 1, but the fibers are not coated with melamine resin, but are directly blended with polylactic acid and epoxidized phytic acid after washing and drying.
[0063] Test Results: The UL94 test showed no rating. During combustion, exposed fibers resulted in a significant wick effect, with the flame spreading along the fibers, severe melting and dripping, and no self-extinguishing capability. Mechanical properties were improved by 3% in tensile strength and 2% in flexural strength due to the partially improved interface caused by epoxidized phytic acid. Comparative Example 3 (epoxidized phytic acid was replaced with ordinary phosphate ester flame retardant).
[0064] Raw material ratio: 82 parts polylactic acid resin, 12 parts melamine resin-coated ramie fiber, and 6 parts triphenyl phosphate.
[0065] Preparation steps: Same as in Example 1, but epoxidized phytic acid is replaced with triphenyl phosphate, which has no epoxy crosslinking function.
[0066] Test results: The UL94 test only achieved level V2. It produced molten droplets during combustion and ignited absorbent cotton. The wick effect was partially suppressed but not completely eliminated. Tensile strength decreased by 7%, flexural strength decreased by 6%, and there were obvious defects at the interface. The flame retardant showed a tendency to migrate.
[0067] Comparative Example 4 (the biomass fiber content is too high, exceeding the scope of the claims).
[0068] Raw material ratio: 60 parts polylactic acid resin, 30 parts ramie fiber coated with melamine resin, and 10 parts epoxidized phytic acid (the fiber ratio exceeds the upper limit of the claims by 20 parts).
[0069] Preparation steps: Same as in Example 1.
[0070] Test results: UL94 test, V1 rating, with a relatively long burning time. Due to excessive fibers, the coating layer was incomplete, resulting in localized wicking effects. Mechanical properties actually decreased due to fiber agglomeration, with tensile strength decreasing by 2% and flexural strength by 3%.
[0071] Comparative Example 5 (the amount of epoxidized phytic acid added was too low).
[0072] Raw material ratio: 84 parts polylactic acid resin, 15 parts melamine resin-coated ramie fiber, 1 part epoxidized phytic acid (3 parts for lower claims).
[0073] Preparation steps: Same as in Example 1.
[0074] Test results: UL94 test showed no rating; insufficient epoxidized phytic acid resulted in a lack of cross-linking and flame retardant effects; during combustion, a noticeable wick effect was observed, with melting and dripping, and no self-extinguishing properties. Interfacial bonding was poor, and mechanical properties were similar to those of the unmodified composite material.
[0075] Performance test conclusions: This invention, through melamine resin fiber coating modification combined with epoxidized phytic acid synergistic crosslinking technology, constructs an integrated modification system of "interfacial oxygen barrier flame retardancy + matrix crosslinking enhancement," completely solving the candle wick effect problem of polylactic acid / biomass fiber composites. Under low load conditions with a total flame retardant system addition of ≤10%, the product stably achieves UL94 V0 flame retardancy, while significantly optimizing the composite material interface structure and improving mechanical properties, fully meeting the project assessment indicators and industrial application standards.
[0076] The above are merely preferred embodiments of the present invention and do not limit the scope of the patent. Any equivalent structural or procedural transformations made based on the description and drawings of the present invention, or direct or indirect applications in other related technical fields, are similarly included within the scope of patent protection of the present invention.
Claims
1. A flame-retardant polylactic acid / biomass fiber composite material, characterized in that, By weight, it includes: 70–85 parts polylactic acid resin, 10–20 parts modified biomass fiber, and 3–10 parts epoxidized phytic acid flame retardant crosslinking agent. The modified biomass fiber is a biomass fiber with a melamine-formaldehyde resin layer on its surface, and the epoxidized phytic acid flame retardant crosslinking agent is a phytic acid derivative flame retardant crosslinking agent containing epoxy groups in its molecular structure.
2. The flame-retardant polylactic acid / biomass fiber composite material according to claim 1, characterized in that, The biomass fiber includes any one or more of ramie fiber, flax fiber, cotton fiber, bamboo fiber, fibroin fiber, viscose fiber, and lyocell fiber.
3. The flame-retardant polylactic acid / biomass fiber composite material according to claim 1, characterized in that, The thickness of the melamine-formaldehyde resin coating layer is 1–500 μm.
4. The flame-retardant polylactic acid / biomass fiber composite material according to claim 1, characterized in that, The epoxy group content in the epoxidized phytic acid flame retardant crosslinking agent is 1%–30% by mass.
5. A method for preparing a flame-retardant polylactic acid / biomass fiber composite material as described in any one of claims 1-4, characterized in that, Includes the following steps: The biomass fiber was ultrasonically cleaned using a mixed solution of acetone and ethanol, and then dried to obtain pretreated biomass fiber. The pretreated biomass fiber was immersed in a melamine-formaldehyde resin solution. The pH value, reaction temperature and soaking time of the system were adjusted to form a resin coating layer on the surface of the pretreated biomass fiber. After the reaction was completed, the fiber was taken out, dried and cured to obtain modified biomass fiber. Amination-modified phytic acid intermediates are prepared by reacting phytic acid with polyamine compounds, and then the amination-modified phytic acid intermediates are subjected to a ring-opening addition reaction with epichlorohydrin to prepare an epoxidized phytic acid flame retardant crosslinking agent. Polylactic acid resin, the modified biomass fiber, and the epoxidized phytic acid flame retardant crosslinking agent are mixed uniformly according to the specified ratio, and then subjected to molding treatment to obtain a flame retardant polylactic acid / biomass fiber composite material.
6. The method for preparing the flame-retardant polylactic acid / biomass fiber composite material according to claim 5, characterized in that, In the acetone and ethanol mixture, the volume ratio of acetone to ethanol is 1:1, and the ultrasonic cleaning time is 20–40 min.
7. The method for preparing the flame-retardant polylactic acid / biomass fiber composite material according to claim 5, characterized in that, The melamine-formaldehyde resin solution has a pH of 8.0–9.0, a reaction temperature of 55–70℃, a soaking time of 1–10 h, and a drying and curing temperature of 70–90℃.
8. The method for preparing the flame-retardant polylactic acid / biomass fiber composite material according to claim 5, characterized in that, The polyamine compounds include any one or more of ethylenediamine, butanediamine, pentanediamine, hexanediamine, phenylenediamine, 4,4'-diaminodiphenylmethane, 3,5-dimethylthiotoluenediamine, diethylaminoethylamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, and polyetheramine.
9. The method for preparing the flame-retardant polylactic acid / biomass fiber composite material according to claim 5, characterized in that, In the step of preparing the amino-modified phytic acid intermediate by reacting phytic acid with a polyamine compound, the molar ratio of phytic acid to the polyamine compound is 1:1–1:12, and the amino-modified phytic acid intermediate is prepared by stirring at room temperature for 1–10 h.
10. The method for preparing the flame-retardant polylactic acid / biomass fiber composite material according to claim 5, characterized in that, In the step of preparing the epoxidized phytic acid flame retardant crosslinking agent by performing a ring-opening addition reaction between the amino-modified phytic acid intermediate and epichlorohydrin under the action of a catalyst, the molar ratio of amino-modified phytic acid to epichlorohydrin is 1:1–1:12, and the reaction is carried out under weakly alkaline catalytic conditions at 30–90℃ for 1–20 h.