A microporous anisotropic conductive silicone rubber and its preparation method

By employing a synergistic design of pre-wetting, hydrosilylation curing, and mechanical micro-foaming, the problems of dispersion stability and directional enrichment in conductive silicone rubber were solved, achieving a balance between the stability of the conductive network and the piezoresistive response, thereby improving the conductivity and structural integrity of the material.

CN123107380APending Publication Date: 2026-11-17PEKING UNIV +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611575691.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-12
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing microporous conductive silicone rubbers struggle to balance dispersion stability and directional enrichment, as well as structural integrity and piezoresistive response, leading to instability and cyclic drift in the conductive network.

Method used

Through the synergistic design of conductive carbon black pre-wetting, hydrosilylation curing, nitrogen mechanical micro-foaming, and calendering orientation, a continuous phase and conductive network are formed in the cell walls. The stability and piezoresistive response of the conductive network are improved by using an interface layer for fixation.

Benefits of technology

This study achieves anisotropic conductivity and piezoresistive stability in conductive silicone rubber, reduces the risk of carbon black agglomeration and cell wall defects, and improves the signal output stability of the material during compression.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107380A_ABST
    Figure CN123107380A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of conductive silicone rubber materials and provides a microporous anisotropic conductive silicone rubber and its preparation method. By pre-drying and pre-wetting conductive carbon black, an addition curing system, nitrogen mechanical micro-foaming, and calendering orientation, a continuous phase of cell walls, a conductive carbon black network, and an interface layer are constructed. This makes the porosity, cell D50, conductive anisotropy, in-plane volume resistivity, piezoresistive response, and cycling stability within a controllable range. It solves the problem of balancing dispersion stability and directional enrichment, and structural integrity and piezoresistive response. It is suitable for flexible pressure sensing, conductive buffering, and electronic interface materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of conductive silicone rubber materials, specifically to a microporous anisotropic conductive silicone rubber and its preparation method. Background Technology

[0002] Flexible electronics, pressure-sensing interfaces, wearable cushioning components, and electronic device contact materials demand conductive silicone rubbers that combine flexibility, conductive stability, compressibility, and cyclic reliability. Silicone rubber is characterized by its softness, weather resistance, heat resistance, and good moldability. Conductive carbon black can construct conductive pathways within an elastic matrix, enabling the material to generate a detectable electrical response under pressure, bending, or bonding conditions. For sheet-like conductive elastic materials, simply achieving a certain conductivity is insufficient to meet application requirements; the conductive network must also exhibit designable variations in both the in-plane and thickness directions to maintain a relatively stable signal output during contact, compression, and rebound. Simultaneously, microporous structures can reduce the compressive modulus and improve tactile response, but pore size, pore wall continuity, and conductive filler distribution collectively affect structural integrity, conductive paths, and cyclic drift. Therefore, developing silicone rubber materials that balance the dispersion stability of conductive carbon black, the directional construction of the conductive network within the pore walls, microporous compressibility, and long-term piezoresistive stability is of great significance for flexible pressure sensing and conductive cushioning materials.

[0003] Existing microporous conductive silicone rubbers typically achieve conductivity and lightweight properties by adding conductive fillers, foaming agents, or mechanical foaming. For example, Chinese patent CN115368738A discloses a microporous foamed conductive silicone rubber material and its preparation process. The raw materials include silicone rubber, conductive fillers, silica, foaming agents, vulcanizing agents, structure control agents, and coupling agents. Microporous foamed conductive silicone rubber is formed through mixing, rolling, and hot-pressing foaming. Previous studies have also reported that carbon black-filled silicone rubber can form electrical anisotropy during flow or coating, but the relationship between weak structural orientation and conductive response is still affected by the dispersion state, filler network continuity, and processing path. The above technologies indicate that microporousization, conductive fillers, and orientation processes can all improve some properties, but two types of mutually restrictive problems still easily arise: on the one hand, enhanced wetting and uniform dispersion reduce local directional enrichment, weakening anisotropic conductivity; on the other hand, relying solely on foaming and calendering orientation may cause local carbon black agglomeration, cell wall defects, or cyclic drift. Summary of the Invention

[0004] The purpose of this invention is to provide a microporous anisotropic conductive silicone rubber and its preparation method, thereby solving the technical problems of simultaneously achieving dispersion stability and directional enrichment, as well as structural integrity and piezoresistive response in current conductive silicone rubber.

[0005] This invention utilizes a synergistic design of conductive carbon black pre-wetting, hydrosilylation curing, nitrogen mechanical micro-foaming, and calendering orientation to enable conductive carbon black to maintain good dispersion stability while forming an adjustable conductive network in the continuous phase of the cell walls. Furthermore, the invention mitigates the risks of agglomeration, drift, and structural collapse through interface layer fixation and micropore compression, thereby achieving a balance between anisotropic conductivity, piezoresistive response, and cycling stability.

[0006] To achieve the above objectives, the present invention provides the following technical solution: A microporous anisotropic conductive silicone rubber is formed by hydrosilylation and curing of feed components including vinyl-terminated dimethyl polysiloxane, conductive carbon black, polymethylhydrosiloxane, 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex and 1-ethynyl-1-cyclohexanol. Of which, based on the total mass of the conductive carbon black, at least 70 wt% of the conductive carbon black is derived from a pre-wetting masterbatch, which is a masterbatch formed from conductive carbon black and vinyl-terminated dimethyl polysiloxane. The microporous anisotropic conductive silicone rubber has a continuous phase of cell walls and a conductive carbon black network distributed in the continuous phase of cell walls. The conductive carbon black surface has at least a portion of an interface layer formed by the vinyl-terminated dimethyl polysiloxane and fixed in hydrosilylation curing. The microporous anisotropic conductive silicone rubber has a porosity of 20–55 vol%, a pore D50 of 80–500 μm, an in-plane volume conductivity to thickness volume conductivity ratio of 5–40, and an in-plane volume resistivity of 10⁻⁶. 1 -10 5 Ω·cm.

[0007] Furthermore, the feed components include: Vinyl-terminated dimethyl polysiloxane 80–97 parts by weight; 3–12 parts by weight of conductive grade carbon black; 0.6–5.0 parts by weight of polymethylhydrosiloxane; 1,3-Divinyl-1,1,3,3-Tetramethyldisiloxane platinum complex, in the form of 5–200 ppm of platinum metal based on the total mass of the feed components; 0.01–0.50 parts by weight of 1-ethynyl-1-cyclohexanol; The total amount of the vinyl-terminated dimethyl polysiloxane used includes the vinyl-terminated dimethyl polysiloxane used to form the pre-wetting masterbatch.

[0008] Furthermore, the microporous anisotropic conductive silicone rubber is formed by preparing a pre-wetting masterbatch into an addition-curable conductive silicone rubber mixture, and then further preparing a precursor sheet followed by curing. The pre-wetting masterbatch, the addition-curable conductive silicone rubber mixture, and the precursor sheet are prepared through the following steps: A1. Provide pre-dried conductive grade carbon black; A2. The pre-dried conductive carbon black is added to vinyl-terminated dimethyl polysiloxane; A3. Mix under an inert atmosphere to obtain a pre-wetted mixture; A4. Disperse the pre-wetted mixture; A5. Degas the dispersed material to obtain the pre-wetting masterbatch; A6. Mix the pre-wetting masterbatch with vinyl-terminated dimethyl polysiloxane to adjust the total amount of conductive carbon black; A7. Add 1-ethynyl-1-cyclohexanol, polymethylhydrosiloxane and 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex, mix and degas to obtain the addition-curable conductive silicone rubber mixture; A8. Nitrogen gas is introduced into the addition-curable conductive silicone rubber mixture, and mechanical micro-foaming is performed to obtain a gas-containing conductive silicone rubber mixture; A9. The gas-containing conductive silicone rubber mixture is calendered into a sheet and pre-shaped to obtain the precursor sheet. The precursor sheet is cured to form the microporous anisotropic conductive silicone rubber.

[0009] Furthermore, the pre-dried conductive carbon black in step A1 is obtained by the following method: Conductive carbon black is placed in a vacuum drying container for vacuum drying, cooled under an inert atmosphere, and then transferred in a sealed manner.

[0010] Furthermore, in steps A4 and A5, the dispersion is a three-roller dispersion, and the degassing is a vacuum degassing. The pre-wetted masterbatch is used after vacuum degassing and sealed dust-proof storage.

[0011] Furthermore, in steps A7 to A9, In step A7, 1-ethynyl-1-cyclohexanol is first added and mixed, then polymethylhydrosiloxane and 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex are added, mixed and degassed to obtain the addition-curable conductive silicone rubber mixture. In step A8, the amount of nitrogen introduced is 5–35 vol% of the volume of the addition-curable conductive silicone rubber mixture. The amount of nitrogen introduced is calculated as the ratio of the difference in apparent volume of the mixture before and after mechanical microfoaming to the volume of the addition-curable conductive silicone rubber mixture before mechanical microfoaming. The amount of nitrogen introduced characterizes the apparent volume increment during the mechanical microfoaming stage. The porosity is determined by the density of the sheet after curing and post-treatment, and mechanical microfoaming is performed. In step A9, the calendering ratio is 1.2–5.0, and the sheet thickness is 0.5–8.0 mm. The calendering ratio is the ratio of the length of the calendered sheet in the calendering direction to the corresponding length of the gas-containing conductive silicone rubber mixture in the same direction before calendering.

[0012] Furthermore, the vinyl-terminated dimethyl polysiloxane has a viscosity of 500–100000 mPa·s and a vinyl content of 0.02–1.50 mmol / g.

[0013] Furthermore, the area enrichment coefficient of the conductive carbon black in the continuous phase of the cell wall is 1.2–3.0, and the area enrichment coefficient is the ratio of the area fraction of conductive carbon black in the cell wall region to the average area fraction of conductive carbon black in the solid region of the same cross section.

[0014] Furthermore, the impedance change rate of the microporous anisotropic conductive silicone rubber under a compression pressure of 10–30 kPa is 10%–80%, and the initial impedance drift after continuous compression of 10,000–100,000 times is 2–20%.

[0015] Furthermore, the microporous anisotropic conductive silicone rubber is a sheet material with a thickness of 1.0–6.0 mm and a 10% compression modulus of 40–200 kPa.

[0016] This invention employs a pre-wetting conductive carbon black microporous hydrosilylation curing system, primarily designed to achieve a synergistic balance between dispersion stability and anisotropic conductivity. Existing technologies typically enhance wetting and uniform dispersion to improve the dispersion stability of conductive carbon black; however, excessive homogenization weakens the directional enrichment in the cell wall region, resulting in insufficient in-plane and thickness-direction conductivity differences. To improve anisotropic conductivity, microfoaming and calendering orientation intensities are usually increased, but this easily induces localized enrichment of conductive carbon black, cell wall defects, and cyclic drift. This invention, through the proportional matching and structural synergistic control of the pre-wetting masterbatch, the continuous phase in the cell wall, the conductive carbon black network, and the cured and fixed interface layer, enables the carbon black to maintain stable dispersion while forming adjustable conductive pathways in the micropore wall region, and balances structural integrity and piezoresistive response within a compressible microporous structure.

[0017] This invention also discloses a method for preparing microporous anisotropic conductive silicone rubber, comprising the following steps: S1. Provides an addition-curable conductive silicone rubber compound formulated from a pre-wetting masterbatch and vinyl-terminated dimethyl polysiloxane; S2. Nitrogen gas is introduced into the addition-curable conductive silicone rubber mixture and mechanical micro-foaming is performed to obtain a gas-containing conductive silicone rubber mixture; S3. Calendering and orienting the gas-containing conductive silicone rubber mixture; S4. The calendered sheet is cured and post-treated to obtain the microporous anisotropic conductive silicone rubber.

[0018] Further, the conductive carbon black is placed in a vacuum drying container and vacuum dried at 80–120℃ and gauge pressure of -0.10MPa to -0.08MPa for 2–6 hours. The dried conductive carbon black is cooled to 20–40℃ under nitrogen protection and transferred in a sealed manner. The weight loss during drying is calculated as the ratio of the mass difference before and after drying to the mass before drying and controlled to be 0.05–1.50wt%. The pre-dried conductive carbon black after sealed transfer enters the pre-wetting and mixing step.

[0019] Further, pre-dried conductive carbon black and vinyl-terminated dimethyl polysiloxane are added to a closed mixing device at a mass ratio of 1:0.8–3.0 and mixed for 20–90 min under a nitrogen atmosphere and at 30–80°C to obtain a pre-wetting mixture. The pre-wetting mixture is dispersed 3–8 times by a three-roller with a roller gap of 5–50 μm, and the discharge temperature is controlled at 30–90°C. Then, it is vacuum degassed for 10–40 min under a gauge pressure of -0.10 MPa to -0.08 MPa to obtain a pre-wetting masterbatch. The pre-wetting masterbatch is stored in a sealed dust-proof environment and then proceeds to the preparation step of the addition-curing conductive silicone rubber mixture.

[0020] Furthermore, image analysis of agglomerate size was performed on the pre-wetted masterbatch after vacuum degassing. The equivalent circle diameter of each agglomerate was converted according to the image scale, and the cumulative distribution of agglomerate particle size was recorded. The particle size corresponding to the cumulative distribution reaching 90% was recorded as agglomerate D90. The agglomerate D90 was controlled to be 5–50 μm. Pre-wetted masterbatch that met this range entered the mixing step with vinyl-terminated dimethyl polysiloxane. Five fields of view were taken from each sample for statistical analysis.

[0021] Further, the pre-wetting masterbatch is mixed with vinyl-terminated dimethyl polysiloxane to make the total amount of conductive carbon black 3–12 parts by mass; 0.01–0.50 parts by mass of 1-ethynyl-1-cyclohexanol is added at 20–45°C and mixed for 5–30 min, followed by 0.6–5.0 parts by mass of polymethylhydrosiloxane and 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex, with a platinum content of 5–200 ppm based on the total mass of all added components of the addition-curable conductive silicone rubber mixture; all components are mixed at 20–45°C for 10–60 min and degassed at a gauge pressure of -0.10 MPa to -0.08 MPa for 5–30 min to obtain the addition-curable conductive silicone rubber mixture.

[0022] Further, nitrogen gas, with a volume of 5–35 vol% of the volume of the addition-curable conductive silicone rubber mixture, is introduced into the addition-curable conductive silicone rubber mixture at 20–50°C, and mechanical micro-foaming is performed for 1–15 min to obtain a gas-containing conductive silicone rubber mixture; the gas-containing conductive silicone rubber mixture is calendered into a sheet with a thickness of 0.5–8.0 mm at a calendering ratio of 1.2–5.0, and pre-shaped at 60–100°C for 0.5–5.0 min to obtain a precursor sheet; the precursor sheet is cured at 90–160°C for 3–20 min, and post-treated at 150–200°C for 0.5–2 h to obtain a microporous anisotropic conductive silicone rubber, wherein the vinyl-terminated dimethyl polysiloxane covering the surface of conductive carbon black in the pre-wetting masterbatch is fixed in the silicone rubber matrix during the curing stage.

[0023] Furthermore, cross-sectional image analysis is performed on the cured and post-treated sheet along the thickness direction. The equivalent circle diameter of each cell in the cross-section is recorded as the cumulative distribution of cell size, and the equivalent circle diameter corresponding to the cumulative distribution reaching 50% is recorded as cell D50, where cell D50 is 80–500 μm. In the same cross-sectional image along the thickness direction, the continuous phase region around the cell is divided into cell wall region, and the matrix region without cells is divided into solid region. The area fraction of conductive carbon black in the cell wall region and the solid region are calculated respectively, and the ratio of the area fraction of conductive carbon black in the cell wall region to the average area fraction of conductive carbon black in the solid region is used as the area enrichment coefficient, where the area enrichment coefficient is 1.2–3.0.

[0024] This invention employs a coupled process of nitrogen mechanical micro-foaming, calendering orientation, curing, and post-treatment to achieve, fix, or amplify the aforementioned synergistic effects. Existing preparation methods, if solely focused on achieving uniform carbon black mixing, easily obtain dispersion but struggle to form a stable in-plane oriented conductive network. Simply increasing the foaming or calendering orientation intensity may result in unstable bubbles, localized carbon black aggregation, and insufficient continuity of the cell walls. This invention first reduces the tendency of carbon black agglomeration by pre-wetting the masterbatch, then provides compressible space through nitrogen mechanical micro-foaming, adjusts the spatial distribution of cells and the conductive network through calendering orientation, and uses addition curing and post-treatment to fix the interface layer and continuous phase structure. This allows the microporous structure, conductive pathways, and elastic recovery to synergistically form within the same process chain, thereby improving the preparation process's ability to balance dispersion stability, anisotropic conductivity, and cyclic piezoresistive stability.

[0025] Pre-wetting masterbatch and calendering orientation constitute the core synergistic technical features of this invention. Pre-wetting masterbatch primarily alleviates the agglomeration and interfacial instability of conductive carbon black in vinyl-terminated dimethyl polysiloxane. While enhancing this treatment alone is beneficial for dispersion, it may lead to an overly uniform carbon black distribution, weakening the conductive network differences in the cell wall regions. Calendering orientation primarily promotes the formation of a continuous cell wall phase with directional differences and a conductive carbon black network in the gas-containing conductive silicone rubber mixture. While improving this effect alone is beneficial for anisotropic conductivity, it may cause local enrichment, cell wall thinning, and cyclic drift. This invention, through matching the pre-wetting mass ratio, agglomerate D90, nitrogen introduction amount, calendering ratio, and hydrosilylation curing sequence, allows these two technical features to mutually correct each other, balancing dispersion stability and directional enrichment, structural integrity and piezoresistive response within the same microporous elastic matrix.

[0026] Beneficial technical effects 1. The present invention pre-wets a masterbatch by pre-forming at least 70 wt% conductive carbon black with vinyl-terminated dimethyl polysiloxane, thereby forming an interface layer on the carbon black surface that is compatible with the silicone rubber matrix, and then curing and fixing it by hydrosilylation. This helps to reduce the risk of agglomeration and migration when dry powder is directly mixed in, and improves the stability of the conductive network.

[0027] 2. This invention combines nitrogen mechanical micro-foaming with calendering orientation to create directional differences between the continuous phase of the cell wall and the conductive carbon black network in the sheet. This avoids insufficient anisotropy caused by simple uniform dispersion and reduces the risk of local enrichment and cell wall defects caused by simple reinforcement orientation, thereby obtaining tunable conductive anisotropy.

[0028] 3. By controlling porosity, cell D50 and 10% compressive modulus, this invention enables the material to exhibit detectable impedance changes at lower compressive pressures. At the same time, the continuous cell walls and solidified interface layer maintain structural integrity, which helps to reduce initial impedance drift after cyclic compression.

[0029] 4. This invention forms a continuous process chain of pre-drying, pre-wetting, three-roll dispersion, vacuum degassing, micro-foaming, pre-shaping, curing and post-treatment. The parameters of each step are clearly defined, which can reduce the impact of moisture, bubble runaway and carbon black agglomeration on product consistency and facilitate sheet production and quality control.

[0030] 5. The preparation method of the present invention does not depend on a specific brand or special supplier. The main raw materials can be obtained commercially or through commercial purchase. The key structure and performance can be evaluated through image analysis, resistivity testing and compression cycle testing, which is conducive to its application in flexible pressure sensing, conductive buffer and electronic interface materials. Attached Figure Description

[0031] Figure 1 The graph shows the relative change in internal resistivity after cyclic compression in Example 1 and Comparative Example 8.

[0032] Figure 2 The graph shows the relationship between compression pressure and resistance change rate for Examples 1, 5, and 10.

[0033] Figure 3 The graphs show the initial impedance drift curves of continuous compression for Examples 1, 5, and 10.

[0034] Figure 4 The diagram shows the influence of conductivity anisotropy ratio and initial impedance drift on samples with different amounts of conductive carbon black.

[0035] Figure 5 This is a comparison of macroscopic optical photographs of the final product of Example 1 and the final product of Comparative Example 5; wherein, Figure 5 Figure a in the image is a macroscopic optical photograph of the final product of Example 1; Figure 5 Figure b in the figure is a macroscopic optical photograph of the final product of Comparative Example 5.

[0036] Figure 6 The images show the SEM morphology and SEM-EDS surface scan comparison of the final product of Example 1 and the final product of Comparative Example 5; wherein, Figure 6 Figure a in the image is a medium-magnification SEM image of the final product of Example 1; Figure 6 Figure b in the figure is a medium-magnification SEM image of the final product of Comparative Example 5; Figure 6 Figure c in the image is a high-magnification SEM image of the final product of Example 1; Figure 6 Image d in the figure is a high-magnification SEM image of the final product of Comparative Example 5. Detailed Implementation

[0037] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings.

[0038] Example 1 In this embodiment, the preparation scale and product form are as follows: 1 part by mass corresponds to 10.0 g for sheet-level preparation, resulting in microporous anisotropic conductive silicone rubber sheets. The feed components are 80 parts by mass of vinyl-terminated dimethyl polysiloxane, 3 parts by mass of conductive carbon black, 0.6 parts by mass of polymethylhydrosiloxane, 0.01 parts by mass of 1-ethynyl-1-cyclohexanol, and a 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex, with the platinum complex having a content of 5 ppm based on metallic platinum. Vinyl-terminated dimethyl polysiloxane is a commercially available addition-curing silicone rubber base polymer with a viscosity of 500 mPa·s and a vinyl content of 0.02 mmol / g; conductive carbon black is a commercially available conductive powder with a moisture content ≤0.5 wt% and an ash content ≤1.0 wt%; polymethylhydrosiloxane is a commercially available addition-curing crosslinking component; 1-ethynyl-1-cyclohexanol is analytical grade; and the platinum complex is a commercially available addition-curing catalyst. Based on the total mass of conductive carbon black, 70 wt% of the conductive carbon black comes from pre-wetted masterbatch.

[0039] Step E1-1: Pre-dry conductive carbon black. Place 3 parts by mass of conductive carbon black in a vacuum drying container and vacuum dry at 80℃ and a gauge pressure of -0.10MPa for 2 hours. Then, purge with nitrogen gas of ≥99.9% purity and cool to 20℃. Transfer to a mixing container in a sealed manner. Weigh before and after drying and calculate the drying loss. The drying loss is 0.05wt%.

[0040] Step E1-2: Prepare pre-wetting masterbatch. Add 2.1 parts by mass of pre-dried conductive carbon black to 1.68 parts by mass of vinyl-terminated dimethyl polysiloxane, with a mass ratio of pre-dried conductive carbon black to vinyl-terminated dimethyl polysiloxane of 1:0.8. The materials are mechanically mixed for 20 min at 300 rpm under a nitrogen atmosphere and at 30°C to obtain a pre-wetting mixture. The pre-wetting mixture is then dispersed three times using a three-roller system with a roller gap of 50 μm, at a discharge temperature of 30°C. Subsequently, it is degassed under vacuum at a gauge pressure of -0.10 MPa for 10 min to obtain the pre-wetting masterbatch. Image analysis of the pre-wetting masterbatch shows an agglomerate D90 of 5.2 ± 0.4 μm.

[0041] Step E1-3: Prepare an addition-curable conductive silicone rubber mixture. Mix the pre-wetted masterbatch, the remaining 0.9 parts by mass of conductive carbon black, and the remaining vinyl-terminated dimethyl polysiloxane to make the total amount of vinyl-terminated dimethyl polysiloxane 80 parts by mass and the total amount of conductive carbon black 3 parts by mass. Add 0.01 parts by mass of 1-ethynyl-1-cyclohexanol at 20°C and mix for 5 min. Then add 0.6 parts by mass of polymethylhydrosiloxane and a platinum complex to make the platinum content 5 ppm. Mix all components at 20°C for 10 min with a stirring speed of 300 rpm, and degas for 5 min under a gauge pressure of -0.10 MPa to obtain the addition-curable conductive silicone rubber mixture.

[0042] Steps E1-4: Microfoaming, calendering, and curing. Nitrogen gas is introduced into the addition-curable conductive silicone rubber mixture at 20°C. The nitrogen volume is 5 vol% of the volume of the addition-curable conductive silicone rubber mixture. Mechanical microfoaming is performed for 1 min at a stirring speed of 500 rpm to obtain a gas-containing conductive silicone rubber mixture. The gas-containing conductive silicone rubber mixture is calendered into sheets at a calendering ratio of 1.2, with a sheet thickness of 1.0 mm. The sheets are pre-shaped at 60°C for 0.5 min, then cured at 90°C for 3 min, and post-treated at 150°C for 0.5 h to obtain a microporous anisotropic conductive silicone rubber.

[0043] Quality inspection methods and results: Three sheet samples from this embodiment were taken and cut into 30mm × 30mm specimens. Porosity was calculated using the density method, and the cell D50 was statistically analyzed using cross-sectional images. In-plane and thickness volume resistivity were measured using the conductive rubber resistivity test method, and the ratio of in-plane to thickness volume conductivity was calculated. The 10% compressive modulus was obtained through compressive stress-strain testing. The test results were: 20 vol% porosity, cell D50 of 82 ± 6 μm, area enrichment factor of 1.2, ratio of in-plane to thickness volume conductivity of 5.4 ± 0.3, and in-plane volume resistivity of (9.8 ± 0.6) × 10⁻⁶. 4 The impedance change rate under 10 kPa compression pressure is 10.8 ± 0.9%, the initial impedance drift after 10,000 compression cycles is 18.6 ± 1.4%, and the 10% compression modulus is 42 ± 3 kPa.

[0044] The features and application scenarios of this embodiment are as follows: This embodiment adopts a relatively conservative low ratio scheme and mild process conditions, with a low amount of conductive carbon black, small microporous structure size, and good sheet flexibility, making it suitable for flexible contact materials that require low pressure tactile response, low compressive modulus and thin conductive buffer.

[0045] Example 2 Raw materials and proportions: 1 part by mass corresponds to 10.0 g of raw materials to prepare microporous anisotropic conductive silicone rubber sheets. The raw materials consist of 97 parts by mass of vinyl-terminated dimethyl polysiloxane (100,000 mPa·s, vinyl content 1.50 mmol / g); 12 parts by mass of conductive carbon black; 5.0 parts by mass of polymethylhydrosiloxane; 0.50 parts by mass of 1-ethynyl-1-cyclohexanol; and 200 ppm of 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex (calculated as platinum metal). All conductive carbon black was introduced from pre-wetted masterbatch. Vinyl-terminated dimethyl polysiloxane, conductive carbon black, polymethylhydrosiloxane, and 1-ethynyl-1-cyclohexanol were all commercially available or purchased raw materials. Batch records were kept based on moisture content, volatile matter, and appearance before use.

[0046] In the preparation process, 12 parts by mass of conductive carbon black were placed in a vacuum drying container and vacuum dried at 120℃ and -0.08 MPa for 6 hours. The mixture was then cooled to 40℃ by purging with nitrogen gas of ≥99.9% purity and transferred in a sealed environment. The drying weight loss was 1.50 wt%. Subsequently, 12 parts by mass of the pre-dried conductive carbon black and 36 parts by mass of vinyl-terminated dimethyl polysiloxane were added to a closed mixing device at a mass ratio of 1:3.0 and mixed for 90 minutes at 80℃ under a nitrogen atmosphere at a mixing speed of 600 rpm. The resulting pre-wetted mixture was dispersed through a three-roller system with a roller gap of 5 μm eight times at a discharge temperature of 90℃. It was then degassed under vacuum at -0.08 MPa for 40 minutes to obtain the pre-wetted masterbatch. Image analysis showed that the agglomerate D90 was 49.0 ± 2.6 μm.

[0047] In the post-processing step, the pre-wetted masterbatch is mixed with the remaining vinyl-terminated dimethyl polysiloxane, resulting in a total vinyl-terminated dimethyl polysiloxane content of 97 parts by mass and a total conductive carbon black content of 12 parts by mass. 0.50 parts by mass of 1-ethynyl-1-cyclohexanol are added at 45°C and mixed for 30 min. Then, 5.0 parts by mass of polymethylhydrosiloxane and a platinum complex are added, controlling the platinum content to 200 ppm. All components are mixed at 45°C for 60 min with a stirring speed of 800 rpm, and degassed for 30 min under a gauge pressure of -0.08 MPa to obtain an addition-curable conductive silicone rubber compound.

[0048] For molding and curing, nitrogen gas was introduced into the addition-curable conductive silicone rubber mixture at 50°C, with the nitrogen volume being 35 vol% of the mixture's volume. Mechanical micro-foaming was performed for 15 min to obtain a gas-containing conductive silicone rubber mixture. This mixture was then calendered at a calendering ratio of 5.0 to a sheet thickness of 6.0 mm. The sheet was pre-shaped at 100°C for 5.0 min, cured at 160°C for 20 min, and post-treated at 200°C for 2 h to obtain a microporous anisotropic conductive silicone rubber.

[0049] Quality inspection methods and results: The sample was cut along the thickness direction and cross-sectional image analysis was performed. The equivalent circle diameters of at least 300 cells were statistically analyzed, yielding a cell D50 of 496±21 μm. The porosity was calculated to be 55 vol% using the density method. The ratio of the conductive carbon black area fraction in the cell wall region to the average conductive carbon black area fraction in the solid region was 3.0. The in-plane volume resistivity was (1.4±0.2)×10⁻⁶. 1 The in-plane volume conductivity to thickness volume conductivity ratio is 38.8±1.8 Ω·cm. The impedance change rate of the sheet under 30 kPa compression pressure is 78.5±3.2%, the initial impedance drift after 100,000 continuous compressions is 2.4±0.5%, and the 10% compression modulus is 198±8 kPa.

[0050] The features of this embodiment are that it adopts a high load and strong structural orientation scheme, and the amount of conductive carbon black, micro-foaming amount, rolling ratio and post-treatment strength are in a high range. The resulting sheet is suitable for electronic interface materials that require in-plane conductivity continuity, high conductivity anisotropy and high structural retention capability.

[0051] Example 3 In this embodiment, samples were prepared under certain process conditions with medium-conductivity carbon black content and a bias towards the low-value range. The target product was a microporous anisotropic conductive silicone rubber sheet. The formulation consisted of 90 parts by weight of vinyl-terminated dimethyl polysiloxane, 7.5 parts by weight of conductive carbon black, 2.8 parts by weight of polymethylhydrosiloxane, 0.25 parts by weight of 1-ethynyl-1-cyclohexanol, and a platinum complex, with a platinum content of 100 ppm. The vinyl-terminated dimethyl polysiloxane had a viscosity of 30000 mPa·s and a vinyl content of 0.70 mmol / g; the 90 wt% conductive carbon black was derived from a pre-wetted masterbatch.

[0052] Pretreatment stage: 7.5 parts by weight of conductive carbon black were vacuum dried at 100℃ and gauge pressure -0.10MPa for 4 hours, cooled to 30℃ under nitrogen protection and transferred in a sealed manner, with a drying weight loss of 0.60wt%. 6.75 parts by weight of pre-dried conductive carbon black were mixed with 12.15 parts by weight of vinyl-terminated dimethyl polysiloxane, with a mass ratio of pre-dried conductive carbon black to vinyl-terminated dimethyl polysiloxane of 1:1.8. The mixture was mixed at 50℃ for 60 minutes under a nitrogen atmosphere at a mixing speed of 500 rpm to obtain a pre-wetting mixture.

[0053] Dispersion and degassing stage: The pre-wetted mixture was fed into a three-roll disperser with a roller gap of 5 μm, dispersed 5 times, and the discharge temperature was 60℃. After dispersion, the material was vacuum degassed for 25 min under a gauge pressure of -0.10 MPa to obtain pre-wetted masterbatch. Image analysis showed that the D90 of the pre-wetted masterbatch agglomerates was 18.6 ± 1.2 μm. The pre-wetted masterbatch was mixed with the remaining vinyl-terminated dimethyl polysiloxane and the remaining conductive carbon black, and the total amount of conductive carbon black was adjusted to 7.5 parts by mass.

[0054] Preparation of the curing mixture: 0.25 parts by mass of 1-ethynyl-1-cyclohexanol were added at 30°C and mixed for 15 min. Subsequently, 2.8 parts by mass of polymethylhydrosiloxane and platinum complex were added. All components were mixed at 30°C for 35 min with a stirring speed of 600 rpm, and degassed for 18 min under a gauge pressure of -0.10 MPa to obtain an addition-curable conductive silicone rubber mixture.

[0055] Microporous sheet formation stage: Nitrogen gas is introduced at 30℃, with a nitrogen volume of 18 vol% of the volume of the addition-curable conductive silicone rubber mixture. Mechanical micro-foaming is performed for 8 minutes to obtain a gas-containing conductive silicone rubber mixture. The gas-containing conductive silicone rubber mixture is calendered at a calendering ratio of 3.0 to form a sheet with a thickness of 0.5 mm. The calendered sheet is pre-shaped at 80℃ for 2.5 minutes, cured at 125℃ for 10 minutes, and post-treated at 175℃ for 1.0 h to obtain microporous anisotropic conductive silicone rubber.

[0056] Quality testing methods and results: Density, cross-sectional image, resistivity, compression response, and cyclic compression tests were performed on the samples, with a sample quantity of 3 pieces. The results showed a porosity of 38 vol%, a pore D50 of 212 ± 12 μm, an area enrichment factor of 2.1, an in-plane volume conductivity to thickness volume conductivity ratio of 22.4 ± 1.1, and an in-plane volume resistivity of (8.6 ± 0.5) × 10⁻⁶. 2 The impedance change rate is 48.2±2.1% under a compression pressure of 20 kPa, the initial impedance drift after 50,000 consecutive compressions is 7.9±0.8%, and the 10% compression modulus is 121±5 kPa.

[0057] The applicable scenarios for this embodiment are: the conductive carbon black content, micro-foaming degree and calendering strength of this embodiment are in the medium range, and the dispersion state of the pre-wetted masterbatch is improved by the finer roller gap, making it suitable for flexible pressure-response materials that need to take into account soft compression, stable electrical output and sheet forming.

[0058] Example 4 I. Preparation Object and Raw Material State: Microporous anisotropic conductive silicone rubber was prepared in sheet form, with 1 part by mass corresponding to 10.0 g. The feed composition consisted of 88 parts by mass of vinyl-terminated dimethyl polysiloxane, 10 parts by mass of conductive carbon black, 4.0 parts by mass of polymethylhydrosiloxane, 0.35 parts by mass of 1-ethynyl-1-cyclohexanol, and a platinum complex, with the platinum complex having a content of 150 ppm based on metallic platinum. The vinyl-terminated dimethyl polysiloxane had a viscosity of 1000 mPa·s and a vinyl content of 1.00 mmol / g. The conductive carbon black was a commercially available conductive powder; its flowability and dryness were checked before use.

[0059] II. Preparation of Pre-wetting Masterbatch: 10 parts by weight of conductive carbon black were vacuum dried at 120℃ and -0.08 MPa for 2 hours, then cooled to 40℃ under nitrogen and transferred in a sealed environment. The drying loss was 1.50 wt%. 8 parts by weight of the pre-dried conductive carbon black were mixed with 24 parts by weight of vinyl-terminated dimethyl polysiloxane, with a mass ratio of 1:3.0. The materials were mixed under nitrogen atmosphere at 80℃ for 20 minutes, then dispersed using a three-roll mill with a roller gap of 50 μm for 8 passes. The discharge temperature was 90℃. Subsequently, the mixture was degassed under vacuum at -0.08 MPa for 40 minutes to obtain the pre-wetting masterbatch. The agglomerate D90 was 42.0 ± 2.0 μm, meeting the requirements for subsequent mixing steps.

[0060] III. Preparation of Addition-Cured Conductive Silicone Rubber Mixture: Add the pre-wetted masterbatch, the remaining 2 parts by weight of conductive carbon black, and the remaining vinyl-terminated dimethyl polysiloxane to a mixing device and mix at 25°C for 15 min. Add 0.35 parts by weight of 1-ethynyl-1-cyclohexanol and mix for 30 min. Then add 4.0 parts by weight of polymethylhydrosiloxane and platinum complex, mix at 45°C for 60 min with a stirring speed of 650 rpm, and degas for 30 min under a gauge pressure of -0.08 MPa.

[0061] IV. Molding, Curing, and Post-treatment: Nitrogen gas was introduced into the addition-curable conductive silicone rubber mixture at 50℃, with the nitrogen volume being 35 vol% of the mixture volume. Mechanical micro-foaming was performed for 15 min to obtain a gas-containing conductive silicone rubber mixture. The gas-containing conductive silicone rubber mixture was calendered at a calendering ratio of 5.0 to form a sheet with a thickness of 8.0 mm. The sheet was pre-shaped at 100℃ for 5.0 min, cured at 160℃ for 20 min, and post-treated at 200℃ for 2 h to obtain a microporous anisotropic conductive silicone rubber.

[0062] V. Quality Inspection Methods and Results: The samples underwent cross-sectional image analysis, resistivity testing, compression response testing, and cyclic compression testing. The equivalent circle diameter of at least 300 cells was statistically analyzed, and the cell D50 was 348±18 μm. The porosity calculated by the density method was 45 vol%; the area enrichment coefficient was 2.8; the ratio of in-plane volumetric conductivity to thickness volumetric conductivity was 31.6±1.4; and the in-plane volumetric resistivity was (1.9±0.3)×10⁻⁶. 2 Ω·cm; the rate of change of impedance under a compression pressure of 30 kPa is 64.8 ± 2.7%; the initial impedance drift after 100,000 consecutive compressions is 5.3 ± 0.7%; the 10% compression modulus is 162 ± 6 kPa.

[0063] VI. Process characteristics and application directions of this embodiment: This embodiment adopts a higher micro-foaming amount, a higher rolling ratio and more sufficient post-processing conditions. The sheet thickness and cell structure are suitable for withstanding large compression displacement, and are applicable to conductive buffer pads, pressure-sensitive interface layers and flexible electronic components that require thicker elastic support.

[0064] Comparative Example 1: Basically the same as Example 1, except that the conductive carbon black was added in dry powder form during the preparation of the addition-curable conductive silicone rubber mixture, and no pre-wetting masterbatch was prepared. The amount of vinyl-terminated dimethyl polysiloxane was 80 parts by weight, the amount of conductive carbon black was 3 parts by weight, the amount of polymethylhydrosiloxane was 0.6 parts by weight, the amount of 1-ethynyl-1-cyclohexanol was 0.01 parts by weight, the amount of platinum was 5 ppm, the amount of nitrogen introduced was 5 vol%, the calendering ratio was 1.2, the sheet thickness was 1.0 mm, the pre-setting conditions were 60°C and 0.5 min, the curing conditions were 90°C and 3 min, and the post-treatment conditions were 150°C and 0.5 h.

[0065] Comparative Example 2: Basically the same as Example 1, except that the mass ratio of pre-dried conductive carbon black to vinyl-terminated dimethyl polysiloxane was adjusted to 1:0.4 when preparing the pre-wetting masterbatch. The total amount of vinyl-terminated dimethyl polysiloxane was still 80 parts by mass, the total amount of conductive carbon black was still 3 parts by mass, polymethylhydrosiloxane was 0.6 parts by mass, 1-ethynyl-1-cyclohexanol was 0.01 parts by mass, the platinum content was 5 ppm, the nitrogen introduction amount was 5 vol%, the calendering ratio was 1.2, the sheet thickness was 1.0 mm, and the curing and post-treatment conditions were maintained as curing at 90°C for 3 min and post-treatment at 150°C for 0.5 h.

[0066] Comparative Example 3: Basically the same as Example 1, except that the gap between the three-roll disperser was adjusted to 100 μm when preparing the pre-wetted masterbatch, the number of dispersion passes was still 3, the mass ratio of pre-dried conductive carbon black to vinyl-terminated dimethyl polysiloxane was 1:0.8, the total amount of conductive carbon black was 3 parts by mass, the total amount of vinyl-terminated dimethyl polysiloxane was 80 parts by mass, polymethylhydrosiloxane was 0.6 parts by mass, 1-ethynyl-1-cyclohexanol was 0.01 parts by mass, the platinum content was 5 ppm, the nitrogen introduction amount was 5 vol%, the rolling ratio was 1.2, and the sheet thickness was 1.0 mm.

[0067] Comparative Example 4: Basically the same as Example 1, except that the amount of nitrogen introduced in the micro-foaming step was adjusted to 2 vol%, the mechanical micro-foaming time was 1 min, the amount of vinyl-terminated dimethyl polysiloxane was 80 parts by mass, the amount of conductive carbon black was 3 parts by mass, the amount of polymethylhydrosiloxane was 0.6 parts by mass, the amount of 1-ethynyl-1-cyclohexanol was 0.01 parts by mass, the amount of platinum was 5 ppm, the rolling ratio was 1.2, the sheet thickness was 1.0 mm, and the pre-setting, curing and post-treatment conditions were 60°C and 0.5 min, 90°C and 3 min, and 150°C and 0.5 h, respectively.

[0068] Comparative Example 5: Basically the same as Example 1, except that the amount of nitrogen introduced in the micro-foaming step was adjusted to 45 vol%, the mechanical micro-foaming time was 1 min, the amount of vinyl-terminated dimethyl polysiloxane was 80 parts by mass, the amount of conductive carbon black was 3 parts by mass, the amount of polymethylhydrosiloxane was 0.6 parts by mass, the amount of 1-ethynyl-1-cyclohexanol was 0.01 parts by mass, the amount of platinum was 5 ppm, the rolling ratio was 1.2, the sheet thickness was 1.0 mm, and the pre-setting, curing and post-treatment conditions were 60°C and 0.5 min, 90°C and 3 min, and 150°C and 0.5 h, respectively.

[0069] Comparative Example 6: Basically the same as Example 1, except that the calendering ratio was adjusted to 1.0, the nitrogen introduction amount was 5 vol%, the mechanical micro-foaming time was 1 min, the vinyl-terminated dimethyl polysiloxane was 80 parts by mass, the conductive carbon black was 3 parts by mass, the polymethylhydrosiloxane was 0.6 parts by mass, the 1-ethynyl-1-cyclohexanol was 0.01 parts by mass, the platinum content was 5 ppm, the sheet thickness was 1.0 mm, and the pre-setting, curing and post-treatment conditions were 60°C and 0.5 min, 90°C and 3 min, and 150°C and 0.5 h, respectively.

[0070] Comparative Example 7: Basically the same as Example 1, except that 1-ethynyl-1-cyclohexanol was not added when preparing the addition-curable conductive silicone rubber mixture, the amount of vinyl-terminated dimethyl polysiloxane was 80 parts by weight, the amount of conductive carbon black was 3 parts by weight, the amount of polymethylhydrosiloxane was 0.6 parts by weight, the content of platinum metal was 5 ppm, the proportion of conductive carbon black in the pre-wetting masterbatch was 70 wt%, the amount of nitrogen introduced was 5 vol%, the calendering ratio was 1.2, the sheet thickness was 1.0 mm, and the pre-setting, curing and post-treatment conditions were 60℃ and 0.5 min, 90℃ and 3 min, and 150℃ and 0.5 h, respectively.

[0071] Comparative Example 8: Basically the same as Example 1, except that the 0.5h post-treatment at 150℃ was omitted, the sheet was directly cooled to 25℃ after curing at 90℃ for 3min, the content of vinyl-terminated dimethyl polysiloxane was 80 parts by weight, the content of conductive carbon black was 3 parts by weight, the content of polymethylhydrosiloxane was 0.6 parts by weight, the content of 1-ethynyl-1-cyclohexanol was 0.01 parts by weight, the content of platinum was 5ppm, the amount of nitrogen introduced was 5vol%, the rolling ratio was 1.2, and the sheet thickness was 1.0mm.

[0072] Comparative Example 9: Essentially the same as Example 1, except that the pre-wetting masterbatch preparation step was retained, but calendering and orientation were not performed after microfoaming. The gas-containing conductive silicone rubber mixture was directly placed into a 1.0 mm thick flat mold for shaping. The composition included 80 parts by weight of vinyl-terminated dimethyl polysiloxane, 3 parts by weight of conductive carbon black, 0.6 parts by weight of polymethylhydrosiloxane, 0.01 parts by weight of 1-ethynyl-1-cyclohexanol, 5 ppm of platinum, and 5 vol% nitrogen introduction. The pre-shaping, curing, and post-treatment conditions were 60°C and 0.5 min, 90°C and 3 min, and 150°C and 0.5 h, respectively. This comparative example was used to investigate the synergistic relationship between the pre-wetting masterbatch and calendering and orientation.

[0073] Comparative Example 10: Essentially the same as Example 1, except that after preparing the pre-wetting masterbatch, polymethylhydrosiloxane and a platinum complex were added first and mixed for 10 min during the preparation of the addition-curable conductive silicone rubber mixture, followed by the addition of 1-ethynyl-1-cyclohexanol and mixing for 5 min. The composition was 80 parts by weight of vinyl-terminated dimethylpolysiloxane, 3 parts by weight of conductive carbon black, 0.6 parts by weight of polymethylhydrosiloxane, 0.01 parts by weight of 1-ethynyl-1-cyclohexanol, 5 ppm of platinum, 5 vol% nitrogen introduction, a calendering ratio of 1.2, and a sheet thickness of 1.0 mm. The pre-setting, curing, and post-treatment conditions were 60°C and 0.5 min, 90°C and 3 min, and 150°C and 0.5 h, respectively. This comparative example was used to investigate the synergistic relationship between the interface layer fixation and curing sequence.

[0074] Characterization and performance testing: The test subjects were the sheets from Examples 1–4 and all comparative examples. The purpose was to determine the in-plane volume resistivity, the thickness-direction volume resistivity, and the conductivity anisotropy ratio calculated from the two. The principle was to measure the resistance under specified electrode contact and sample dimensions, convert the volume resistivity according to the geometric dimensions, and then calculate the volume conductivity from the reciprocal of the resistivity. The resistivity of conductive silicone rubber was tested according to GB / T 2439-2001. The samples were equilibrated at 25±2℃ and 50±5% relative humidity for 24 hours, with n=3. The mean and standard deviation of the in-plane volume resistivity, the mean and standard deviation of the thickness-direction volume resistivity, and the mean and standard deviation of the conductivity anisotropy ratio were recorded. The in-plane test direction was the direction within the sheet surface, and the thickness test direction was the sheet thickness direction. The ratio of the in-plane volume conductivity to the thickness-direction volume conductivity is called the conductivity anisotropy ratio, and it is calculated according to the ratio of the reciprocals of the corresponding volume resistivity.

[0075] The test subjects were the cross-sections of the sheets from Examples 1–4 and all comparative examples, with the aim of determining porosity and cell D50. The principle was to calculate porosity by the difference between the solid density and the apparent density of the foamed sheet, and to statistically analyze the distribution of the equivalent circle diameter of the cells using cross-sectional microscopic images. Density determination was performed according to GB / T 533-2008. Cell size was analyzed using optical microscopy or scanning electron microscopy, with at least 300 cells counted. The mean and standard deviation of porosity, and the mean and standard deviation of cell D50 were recorded. Porosity was calculated as the difference between the apparent density of the foamed sheet and the density of unfoamed solid silicone rubber with the same formulation.

[0076] The test objects were pre-wetted masterbatch and cured sheet cross-sections, with the aim of determining the D90 of agglomerates and the area enrichment coefficient of conductive carbon black. The principle was to convert the microscopic images to a scale to calculate the equivalent circle diameter of the agglomerates and the carbon black area fraction in the cell wall region. The D90 of the agglomerates was taken as the particle size at which the cumulative distribution reached 90%. The area enrichment coefficient was the ratio of the area fraction of conductive carbon black in the cell wall region to the average area fraction of conductive carbon black in the solid region. Five fields of view were taken for each sample, and the mean and standard deviation of the agglomerate D90, and the mean and standard deviation of the area enrichment coefficient were recorded.

[0077] The test subjects were the sheets from Examples 1–4 and all comparative examples, with the aim of evaluating the 10% compressive modulus and low-pressure piezoresistive response. The principle involved recording the stress-strain curve and real-time impedance within a compression fixture. The 10% compressive modulus was characterized by the compressive stress corresponding to 10% strain, and the impedance change rate was calculated as the percentage of the absolute value of the impedance difference before and after compression to the initial impedance. The compressive stress-strain test followed GB / T 7757-2009, and the synchronous impedance test employed a two-electrode clamping method. The pressure points were 10 kPa, 20 kPa, and 30 kPa, with n=3. The mean and standard deviation of the 10% compressive modulus and the mean and standard deviation of the impedance change rate were recorded.

[0078] The test subjects were the sheets from Examples 1–4 and all comparative examples, with the aim of evaluating the electrical stability after continuous compression. The principle involved cyclic compression at a fixed compression frequency and pressure range, recording the initial impedance before each cycle and the initial impedance after a specified number of cycles in the recovery state, and calculating the initial impedance drift. Test conditions were 25±2℃, relative humidity 50±5%, compression pressure 10–30 kPa, frequency 1 Hz, and the number of cycles set to 10,000, 50,000, and 100,000 cycles, n=3. The mean and standard deviation of the initial impedance drift and the appearance integrity record field after each cycle were recorded. The initial impedance drift was calculated as a percentage of the absolute value of the difference between the initial impedance in the recovery state after each cycle and the initial impedance before each cycle, relative to the initial impedance before each cycle. In Table 1, the initial impedance drift of Examples 1, 2, 3, and 4 corresponds to 10,000, 100,000, 50,000, and 100,000 continuous compressions, respectively; the initial impedance drift of Comparative Examples 1–10 corresponds to 10,000 continuous compressions. Figure 3 The initial impedance drift of the sample shown is a continuous record of 0–100,000 cycles of compression under the same test conditions.

[0079] The test objects were conductive carbon black, pre-wetting masterbatch, and addition-curable conductive silicone rubber mixtures used in the preparation process, with the aim of evaluating the stability of the process. The principle was to calculate the loss on drying by the mass difference before and after drying, record the degassing state by images of residual bubbles before and after vacuum degassing, and estimate the amount of nitrogen introduced by the volume change before and after micro-foaming, comparing this to the set value. Test conditions included weighing at 25±2℃, an electronic balance accuracy of 0.1mg, at least five fields of view for image analysis, and recording of the loss on drying, residual bubble level, nitrogen introduction deviation, and apparent uniformity of the mixture.

[0080] Figure 1 The diagram shows the relative change in internal resistivity after cyclic compression according to the present invention. Example 1 and Comparative Example 8 were used as test samples to compare the relative changes in internal resistivity under different numbers of compression cycles. The results show that the resistivity change in Example 1 was relatively slow after continuous compression, while the change was greater in the sample without post-treatment. This indicates that appropriate post-treatment after curing helps stabilize the silicone rubber network and conductive pathways.

[0081] Figure 2 The graph shows the relationship between compression pressure and impedance change rate of this invention. Examples 1, 5, and 10 were used as test samples, and the impedance change rate was compared under compression pressures of 10–30 kPa. The results show that Example 1 exhibits a stable response with increasing compression pressure, while samples with excessive nitrogen introduction or altered feeding order show greater response fluctuations, indicating that the microporous structure and curing sequence jointly affect the stability of the piezoresistive response.

[0082] Figure 3This is a graph showing the initial impedance drift after continuous compression according to the present invention. Examples 1, 5, and 10 were used as test samples to compare the initial impedance drift after 0–100,000 compression cycles. The results show that the drift in Example 1 increases relatively gradually with the number of cycles, while the drift increases significantly in samples with excessive nitrogen introduction or altered feeding order. This indicates that a suitable microporous structure and a reasonable curing sequence help maintain the stability of the conductive network.

[0083] Figure 4 This diagram illustrates the effect of the amount of conductive carbon black used in this invention on the conductivity anisotropy ratio and initial impedance drift. Based on the conditions of Example 1 (80 parts by weight of vinyl-terminated dimethyl polysiloxane, 0.6 parts by weight of polymethylhydrosiloxane, 0.01 parts by weight of 1-ethynyl-1-cyclohexanol, 5 ppm platinum content, 5 vol% nitrogen introduction, a rolling ratio of 1.2, and a sheet thickness of 1.0 mm), the amount of conductive carbon black was varied from 2.0 to 14.0 parts by weight. The range of 3–12 parts by weight corresponds to the range of conductive carbon black used in this invention, while 2.0 and 14.0 parts by weight serve as out-of-range controls to examine the trend of the conductive carbon black usage. The results show that a medium-to-high proportion of conductive carbon black can form a more continuous conductive network and avoid excessive filling that leads to increased cycle drift, indicating that a moderate amount of conductive carbon black can simultaneously achieve anisotropic conductivity and cycle stability.

[0084] Figure 5 The image shows a macroscopic optical photograph comparison between the final product of Example 1 and the final product of Comparative Example 5, used to compare the effect of moderate microfoaming conditions on the macroscopic integrity and molding uniformity of the microporous anisotropic conductive silicone rubber sheet. Figure 5 a is a macroscopic optical photograph of the final product of Example 1. The sample is a microporous anisotropic conductive silicone rubber sheet with a thickness of 1.0 mm. The cut sample size is 30 mm × 30 mm. The nitrogen introduction amount is 5 vol%, the porosity is 20 vol%, and the cell D50 is 82 ± 6 μm. Figure 5 b is a macroscopic optical photograph of the final product of Comparative Example 5. The sample is also a conductive silicone rubber sheet with a thickness of 1.0 mm, but the nitrogen introduction amount is increased to 45 vol%, which is used to compare the risk of sheet surface roughness, increased pores or local collapse under high gas introduction amount.

[0085] Figure 6 The images show the SEM morphology and SEM-EDS surface scan comparison of the final product of Example 1 and the final product of Comparative Example 5, used to compare the effect of moderate micro-foaming on the control of cell size, pore wall continuity and element spatial distribution. Figure 6 Image a is a medium-magnification SEM image of the final product of Example 1, showing multiple pores and a continuous pore wall structure. Figure 6 b is a medium-magnification SEM image of the final product of Comparative Example 5, showing coarsening of the pores, widening of the pore size distribution, or thinning of the pore walls in some areas. Figure 6 c is a high-magnification SEM image of the final product of Example 1, showing the local morphology of the pore walls and the dispersion state of conductive carbon black in the silicone rubber pore walls. Figure 6 d is a high-magnification SEM image of the final product of Comparative Example 5, showing thin pore walls, local microcracks, or areas of filler enrichment.

[0086]

[0087] To verify the electrical stability of the microporous anisotropic conductive silicone rubber and its preparation method described in this invention during cyclic use, the relative change in in-plane resistivity after cyclic compression was first tested on Examples 1 and 8. The results are as follows: Figure 1 As shown. Example 1 employs a process route combining conductive carbon black pre-wetting, hydrosilylation curing, nitrogen mechanical micro-bubbling, calendering orientation, and post-treatment; Comparative Example 8 omits the post-treatment step. Figure 1 It can be seen that as the number of cyclic compressions increases, the relative change in in-plane resistivity of Example 1 is relatively small, and the trend is relatively gentle, indicating that its conductive network can maintain good continuity and recovery stability during repeated compression and release. In contrast, the relative change in resistivity of Comparative Example 8 increased significantly after the post-treatment was removed, indicating that the silicone rubber network and filler interface were not sufficiently fixed without proper post-treatment, and the conductive pathways were more prone to migration, relaxation, or local reconstruction during cyclic compression. The above results show that proper post-treatment after curing can further stabilize the conductive pathways composed of the silicone rubber crosslinking network and conductive carbon black, thereby reducing the electrical drift caused by cyclic compression.

[0088] Based on the preliminary verification of cycle stability, the effects of microporous structure and curing sequence on low-pressure piezoresistive response behavior were further investigated, and the results are as follows: Figure 2 As shown. Figure 2Using Example 1, Comparative Example 5, and Comparative Example 10 as test samples, the impedance change rate was compared within a compression pressure range of 10–30 kPa. In Example 1, the nitrogen introduction amount was 5 vol%, the sheet thickness was 1.0 mm, and the rolling ratio was 1.2, which enabled the formation of a moderately porous structure. In Comparative Example 5, the nitrogen introduction amount was increased to 45 vol% to evaluate the effect of excessive foaming on the piezoresistive response. In Comparative Example 10, the order of addition of 1-ethynyl-1-cyclohexanol, polymethylhydrosiloxane, and the platinum complex was changed to evaluate the effect of the curing process on the construction of the conductive network. The test results show that the impedance change rate of Example 1 exhibits a relatively stable and identifiable trend with increasing compression pressure, indicating that its microporous compression space can effectively amplify the changes in the pore wall contact state and the spacing of conductive pathways under low pressure, thereby forming a controllable piezoresistive response. In contrast, Comparative Example 5, due to excessive nitrogen introduction, increased the risk of pore coarsening and pore wall thinning, making the local structure prone to non-uniform deformation under pressure, leading to aggravated impedance response fluctuations. Comparative Example 10, due to a change in the feeding sequence, experienced a decrease in the matching between conductive carbon black dispersion, interface fixation, and the formation of the cured network, resulting in reduced consistency in the conductive network response during compression. Therefore, a suitable microporous structure and a reasonable curing sequence jointly affect the stability of the piezoresistive response.

[0089] Furthermore, to evaluate the reliability of the aforementioned low-voltage response structure under long-term use conditions, initial impedance drift tests were conducted on Examples 1, 5, and 10 after 0–100,000 cycles of compression. The results are as follows: Figure 3 As shown. By Figure 3 It can be seen that in Example 1, the initial impedance drift increase is relatively small after high-cycle compression, and the drift curve is relatively flat, indicating that its conductive path has good structural retention ability during repeated compression and recovery. This result is consistent with... Figure 2 The stable piezoresistive response of Example 1 is consistent with that of the present invention, indicating that the present invention can maintain the synergistic stability of the conductive network and the microporous framework during long-term compression cycling. In contrast, Comparative Example 5, due to the introduction of excessive nitrogen, suffers from decreased microporous structure stability, making it more prone to local pore wall collapse, irreversible changes in pore size, or rearrangement of conductive pathways during cycling; Comparative Example 10, due to an unreasonable curing sequence, has insufficient interface fixation between the conductive carbon black and the silicone rubber matrix, resulting in a more significant initial impedance drift after cyclic compression. The above results indicate that the combination of appropriate microfoaming and a reasonable curing sequence helps to maintain the stability of the conductive network while providing space for compression deformation.

[0090] After determining that the process structure has a significant impact on piezoresistive response and cycle stability, the effect of conductive carbon black dosage on anisotropic conductivity and cycle drift was further investigated. The results are as follows: Figure 4 As shown. Figure 4Based on the formulation and process conditions of Example 1, namely 80 parts by mass of vinyl-terminated dimethyl polysiloxane, 0.6 parts by mass of polymethylhydrosiloxane, 0.01 parts by mass of 1-ethynyl-1-cyclohexanol, 5 ppm of platinum, 5 vol% nitrogen introduction, a calendering ratio of 1.2, and a sheet thickness of 1.0 mm, the amount of conductive carbon black was adjusted to 2.0–14.0 parts by mass. Test results showed that when the amount of conductive carbon black was too low, the conductive particles in the continuous phase of the pore walls had insufficient contact, making it difficult to form a stable and continuous conductive network, resulting in limited anisotropic conductivity. As the amount of conductive carbon black increased to a medium-high ratio range, the conductive particles gradually formed more continuous in-plane conductive pathways under the influence of calendering orientation and enrichment on the pore walls, improving the conductivity anisotropy ratio. However, when the amount of conductive carbon black was too high, the interaction between fillers increased, the system viscosity increased, the risk of local agglomeration and stress concentration increased, and the initial impedance drift after cyclic compression might actually increase. Therefore, it is clear that more conductive carbon black is not necessarily better; it needs to be matched with pre-wetting dispersion, microporous structure, and calendering orientation. This invention controls the amount of conductive carbon black within a moderate range, ensuring that it forms an effective conductive network in the continuous phase of the cell walls while avoiding overfilling that could lead to agglomeration, drift, and structural embrittlement.

[0091] To further verify the necessity of moderate micro-foaming conditions from the perspective of macroscopic molding quality, macroscopic optical photographs of the final product of Example 1 and the final product of Comparative Example 5 were compared. The results are as follows: Figure 5 As shown. Figure 5 a is the final product of Example 1, which is a microporous anisotropic conductive silicone rubber sheet with a thickness of 1.0 mm and a cut size of 30 mm × 30 mm. The nitrogen introduction amount is 5 vol%, the porosity is 20 vol%, and the cell D50 is 82 ± 6 μm. Figure 5 As can be seen, the sheet of Example 1 is continuous, soft, and uniform in appearance, with good edge and surface integrity. This indicates that under low nitrogen introduction and moderate calendering conditions, the conductive carbon black pre-wetting dispersion system can form a stable molding structure together with the silicone rubber matrix. Figure 5 b is the final product of Comparative Example 5, which is also a conductive silicone rubber sheet with a thickness of 1.0 mm, but the amount of nitrogen introduced is increased to 45 vol%. Compared with Example 1, Comparative Example 5 is more likely to show phenomena such as surface roughness, increased pore marks, or localized bubble collapse, indicating that excessive gas introduction will weaken the overall structural integrity of the sheet and reduce the micropore distribution and macroscopic molding uniformity.

[0092] Based on the macroscopic molding effect, the microstructure of Example 1 and Comparative Example 5 was further compared and analyzed using SEM morphology and SEM-EDS surface scanning. The results are as follows: Figure 6 As shown. Figure 6Image a is a medium-magnification SEM image of the final product of Example 1, which shows multiple bubbles and continuous pore wall structure. This indicates that under the conditions of 5 vol% nitrogen introduction and a rolling ratio of 1.2, a relatively stable microporous structure can be formed inside the silicone rubber matrix, and the pore walls still maintain continuous load-bearing and conductive connection. Figure 6 b is a medium-magnification SEM image of the final product of Comparative Example 5. The bubbles exhibit coarsening, wider pore size distribution, or localized thinning of the pore walls, indicating that excessive nitrogen introduction makes bubble growth difficult to control, thereby reducing the uniformity of the pore wall structure and compression recovery stability. The above morphological results are consistent with... Figure 5 The macroscopic photographs corroborate each other, indicating that moderate micro-foaming helps to balance sheet integrity and piezoresistive response stability.

[0093] Further observation of high-magnification SEM images, Figure 6 c shows that the local morphology of the pore walls in Example 1 is relatively continuous, and the conductive carbon black can be distributed relatively uniformly in the pore walls of the silicone rubber. Combined with the dispersion result that the D90 of the pre-wetting masterbatch agglomerates is 5.2±0.4μm, it can be seen that pre-wetting and three-roll dispersion can reduce the coarse agglomeration of conductive carbon black in the silicone rubber system, making it easier for conductive particles to build stable conductive pathways along the continuous phase of the pore walls during subsequent micro-foaming and calendering processes. Figure 6 d shows that Comparative Example 5 has thin pore walls, local microcracks, or filler-rich areas, indicating that excessive foaming may disrupt the uniformity of the microporous structure and cause local interruptions or uneven enrichment of the conductive network, ultimately leading to increased piezoresistive response fluctuations and cyclic impedance drift. SEM-EDS surface scan results were used to compare the elemental distribution uniformity in the pore wall region between Example 1 and Comparative Example 5.

[0094] In conclusion, Figures 1 to 6 The performance characteristics of this invention are reflected from multiple aspects, including resistivity cyclic change, low-voltage impedance response, long-period initial impedance drift, optimized conductive filler dosage, macroscopic sheet integrity, and microscopic pore and filler distribution. Example 1, under the synergistic effect of parameters such as conductive carbon black dosage, 5 vol% nitrogen introduction, 20 vol% porosity, 82 ± 6 μm pore D50, 1.2 rolling ratio, and 1.0 mm sheet thickness, can form a microporous conductive silicone rubber with a complete structure, continuous pore walls, stable conductive network, and anisotropic characteristics. Compared with comparative examples that omit post-treatment, over-foam, or change the feeding sequence, this invention can reduce conductive filler agglomeration and drift, microporous structure collapse, and piezoresistive response fluctuations, effectively solving the technical problems of balancing dispersion stability and directional enrichment, and structural integrity and piezoresistive response in existing conductive silicone rubbers.

[0095] As can be seen from the performance of the examples and comparative examples in Table 1, Examples 1–4 exhibit a relatively coordinated trend in terms of agglomerate D90, conductivity anisotropy ratio, cell size D50, piezoresistive response, and cyclic impedance drift. In the conventional comparative examples, after eliminating pre-wetting, reducing the pre-wetting ratio, or widening the three-roll gap, the agglomerate D90 increased, accompanied by an increase in resistivity and drift; when the nitrogen introduction amount was too low or too high, the cell size and compression response deviated significantly; eliminating post-treatment or changing the order of inhibitor addition affected cyclic stability. In the synergistic comparative examples, when the pre-wetting masterbatch was retained without calendering orientation, or when calendering orientation was retained without preparing the pre-wetting masterbatch, the conductivity anisotropy and drift performance were weaker than in Example 1, indicating that the pre-wetting masterbatch, calendering orientation, and curing order jointly participate in the regulation of dispersion stability, directional conductivity enrichment, and cyclic stability.

[0096] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that any equivalent structural transformations made under the concept of the present invention and using the contents of the specification and drawings of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A microporous anisotropic conductive silicone rubber, characterized in that, It is formed by hydrosilylation and curing of feed components including vinyl-terminated dimethyl polysiloxane, conductive carbon black, polymethylhydrosiloxane, 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex and 1-ethynyl-1-cyclohexanol. Of which, based on the total mass of the conductive carbon black, at least 70 wt% of the conductive carbon black is derived from a pre-wetting masterbatch, which is a masterbatch formed from conductive carbon black and vinyl-terminated dimethyl polysiloxane. The microporous anisotropic conductive silicone rubber has a continuous phase of cell walls and a conductive carbon black network distributed in the continuous phase of cell walls. The conductive carbon black surface has at least a portion of an interface layer formed by the vinyl-terminated dimethyl polysiloxane and fixed in hydrosilylation curing. The microporous anisotropic conductive silicone rubber has a porosity of 20–55 vol%, a pore D50 of 80–500 μm, an in-plane volume conductivity to thickness volume conductivity ratio of 5–40, and an in-plane volume resistivity of 10⁻⁶. 1 -10 5 Ω·cm.

2. The microporous anisotropic conductive silicone rubber according to claim 1, characterized in that, The feed components include: Vinyl-terminated dimethyl polysiloxane 80–97 parts by weight; 3–12 parts by weight of conductive grade carbon black; 0.6–5.0 parts by weight of polymethylhydrosiloxane; 1,3-Divinyl-1,1,3,3-Tetramethyldisiloxane platinum complex, in the form of 5–200 ppm of platinum metal based on the total mass of the feed components; 0.01–0.50 parts by weight of 1-ethynyl-1-cyclohexanol.

3. The microporous anisotropic conductive silicone rubber according to claim 1, characterized in that, The microporous anisotropic conductive silicone rubber is formed by preparing an addition-curable conductive silicone rubber mixture from a pre-wetting masterbatch, and then further preparing a precursor sheet followed by curing. The pre-wetting masterbatch, the addition-curable conductive silicone rubber mixture, and the precursor sheet are prepared through the following steps: A1. Provide pre-dried conductive grade carbon black; A2. The pre-dried conductive carbon black is added to vinyl-terminated dimethyl polysiloxane; A3. Mix under an inert atmosphere to obtain a pre-wetted mixture; A4. Disperse the pre-wetted mixture; A5. Degas the dispersed material to obtain the pre-wetting masterbatch; A6. Mix the pre-wetting masterbatch with vinyl-terminated dimethyl polysiloxane to adjust the total amount of conductive carbon black; A7. Add 1-ethynyl-1-cyclohexanol, polymethylhydrosiloxane and 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex, mix and degas to obtain the addition-curable conductive silicone rubber mixture; A8. Nitrogen gas is introduced into the addition-curable conductive silicone rubber mixture, and mechanical micro-foaming is performed to obtain a gas-containing conductive silicone rubber mixture; A9. The gas-containing conductive silicone rubber mixture is calendered into a sheet and pre-shaped to obtain the precursor sheet. The precursor sheet is cured to form the microporous anisotropic conductive silicone rubber.

4. The microporous anisotropic conductive silicone rubber according to claim 3, characterized in that, The pre-dried conductive carbon black in step A1 is obtained by the following method: Conductive carbon black is placed in a vacuum drying container for vacuum drying, cooled under an inert atmosphere, and then transferred in a sealed manner.

5. The microporous anisotropic conductive silicone rubber according to claim 3, characterized in that, In steps A4 and A5, the dispersion is performed by three-roller dispersion, and the degassing is performed by vacuum degassing. The pre-wetted masterbatch is used after vacuum degassing and sealed dust-proof storage.

6. The microporous anisotropic conductive silicone rubber according to claim 3, characterized in that, In steps A7 to A9, In step A7, 1-ethynyl-1-cyclohexanol is first added and mixed, then polymethylhydrosiloxane and 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex are added, mixed and degassed to obtain the addition-curable conductive silicone rubber mixture. In step A8, the amount of nitrogen introduced is 5–35 vol% of the volume of the addition-curable conductive silicone rubber mixture, and mechanical micro-foaming is performed. In step A9, the rolling ratio is 1.2–5.0 and the sheet thickness is 0.5–8.0 mm.

7. The microporous anisotropic conductive silicone rubber according to claim 1, characterized in that, The impedance change rate of the microporous anisotropic conductive silicone rubber under a compression pressure of 10–30 kPa is 10%–80%, and the initial impedance drift after continuous compression of 10,000–100,000 times is 2–20%.

8. The microporous anisotropic conductive silicone rubber according to claim 1, characterized in that, The microporous anisotropic conductive silicone rubber is a sheet material with a thickness of 1.0–6.0 mm and a 10% compression modulus of 40–200 kPa.

9. A method for preparing microporous anisotropic conductive silicone rubber as described in any one of claims 1-8, characterized in that, Includes the following steps: S1. Provides an addition-curable conductive silicone rubber compound formulated from a pre-wetting masterbatch and vinyl-terminated dimethyl polysiloxane, wherein at least 70 wt% of the conductive carbon black is derived from the pre-wetting masterbatch based on the total mass of the conductive carbon black; S2. Nitrogen gas is introduced into the addition-curable conductive silicone rubber mixture and mechanical micro-foaming is performed to obtain a gas-containing conductive silicone rubber mixture; S3. Calendering and orienting the gas-containing conductive silicone rubber mixture; S4. The calendered sheet is cured and post-treated to obtain the microporous anisotropic conductive silicone rubber.

10. The preparation method according to claim 9, characterized in that, The calendering orientation in step S3 causes the conductive carbon black in the microporous anisotropic conductive silicone rubber obtained after curing the gas-containing conductive silicone rubber mixture obtained in step S2 to reach an area enrichment coefficient of 1.2–3.0 in the cell wall region. The area enrichment coefficient is the ratio of the area fraction of conductive carbon black in the cell wall region to the average area fraction of conductive carbon black in the solid region of the same cross section.

Citation Information

Patent Citations

  • Microcellular foaming conductive silicone rubber material and preparation process thereof