A PBS / PBAT composite material containing biodegradable bamboo fiber and its preparation method

By modifying bamboo fiber through enzymatic treatment and functional modifiers, the problems of discoloration and compatibility during bamboo fiber processing have been solved, and the mechanical properties and processing efficiency of PBS/PBAT composite materials have been improved, making them suitable for biodegradable packaging films and disposable tableware.

CN123107401APending Publication Date: 2026-11-17HEPING HELIN BAMBOO PLASTIC TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611430995.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, bamboo fiber is prone to thermal and oxidative degradation and discoloration during processing, has poor compatibility, and high shear extrusion leads to fiber breakage. Furthermore, it is difficult to balance the fluidity and melt strength of the high-filling system.

Method used

Modified bamboo fiber was treated with a compound enzyme to remove lignin, and then modified with a functional modifier at high temperature. Epoxy chain extender, melamine cyanurate, and pentaerythritol stearate were used as compound additives to improve compatibility and flowability.

Benefits of technology

It improves the tensile strength and notched impact strength of composite materials, reduces water absorption and yellow index, and is suitable for biodegradable packaging films and disposable tableware.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of polymer biodegradable materials technology, specifically disclosing a PBS / PBAT composite material containing biodegradable bamboo fiber and its preparation method. The composite material comprises the following raw materials in parts by weight: 30-40 parts polybutylene succinate, 10-20 parts polybutylene terephthalate-adipate, 40-50 parts modified bamboo fiber, 2-5 parts inorganic filler, and 0.5-2 parts composite additives. This invention removes lignin through pretreatment with a synergistic complex enzyme of ferulic acid and L-proline, effectively preventing heat-oxidative yellowing and protecting the cellulose skeleton. Further, in-situ grafting modification using epoxidized soybean oil, citric acid, and sodium hypophosphite forms a flexible buffer layer on the surface of rigid bamboo fiber, significantly improving interfacial compatibility and resisting high-shear fracture. The composite material obtained by this invention exhibits excellent tensile strength and notched impact strength, with low water absorption and yellowing index, making it suitable for wide applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer biodegradable materials technology, specifically to a PBS / PBAT composite material containing biodegradable bamboo fiber and its preparation method. Background Technology

[0002] With the advancement of global plastic bans, biodegradable polymer materials have experienced rapid development. Among them, polybutylene succinate (PBS) and polybutylene terephthalate (PBAT) have become the main alternatives to traditional general-purpose plastics due to their excellent biodegradability, processability, and good mechanical properties. However, the high production costs of PBS and PBAT severely restrict their large-scale market application.

[0003] To reduce costs and fully utilize renewable resources, adding plant fibers (such as bamboo fiber, straw fiber, and wood flour) to biodegradable polyesters has become a research hotspot. Bamboo fiber, as a natural fiber with a short growth cycle, high yield, and good rigidity, can be effectively combined with PBS / PBAT to reduce material costs and improve the material's stiffness, hardness, and heat resistance.

[0004] However, existing biodegradable composite materials containing bamboo fiber still have the following drawbacks:

[0005] First, the lignin in bamboo fiber is highly susceptible to thermal and oxidative degradation during processing, leading to discoloration and yellowing. Although there are currently methods for removing lignin using biological enzymes, conventional laccases are difficult to penetrate deep into the dense areas inside the fiber due to steric hindrance, and high-temperature, long-term enzymatic hydrolysis can easily lead to excessive hydrolysis of cellulose, damaging the fiber's inherent strength.

[0006] Secondly, bamboo fiber is highly polar and has poor compatibility with the matrix. Although conventional treatment with silane coupling agents and plasticizers has some effect, the rigid bamboo fiber is prone to mechanical fracture under the high temperature and high shear force of the twin-screw extruder, resulting in a significant decrease in the aspect ratio and a precipitous drop in the notched impact strength of the composite material.

[0007] Third, high filler content leads to poor system flowability and increased susceptibility to polyester degradation. While chain extenders and lubricants are often added, conventional additives cannot simultaneously improve melt strength and eliminate the odor associated with natural fiber degradation. Based on the above, this invention proposes a PBS / PBAT composite material containing biodegradable bamboo fiber and its preparation method. Summary of the Invention

[0008] To address the technical problems in existing technologies, such as the easy damage to the fiber matrix caused by enzymatic hydrolysis, the decrease in the aspect ratio of the fiber due to high shear extrusion, and the difficulty in balancing the fluidity and melt strength of the high-filling system, this invention proposes a PBS / PBAT composite material containing biodegradable bamboo fiber and its preparation method.

[0009] In a first aspect, the present invention provides a PBS / PBAT composite material containing biodegradable bamboo fiber, employing the following technical solution:

[0010] A PBS / PBAT composite material containing biodegradable bamboo fiber comprises the following raw materials in parts by weight: 30-40 parts of polybutylene succinate (PBS), 10-20 parts of polybutylene terephthalate-adipate (PBAT), 40-50 parts of modified bamboo fiber, 2-5 parts of inorganic filler, and 0.5-2 parts of composite additives.

[0011] The modified bamboo fiber is obtained by pretreatment with a composite enzyme agent followed by modification with a functional modifier.

[0012] Preferably, the modified bamboo fiber is prepared by the following method:

[0013] (1) Disperse bamboo fiber in buffer solution, add compound enzyme for enzymatic hydrolysis, wash and dry after treatment to obtain lignin-free bamboo fiber;

[0014] (2) After the lignin-free bamboo fiber is mixed evenly with the functional modifier, it is modified to obtain modified bamboo fiber.

[0015] Preferably, in step (1), the mesh size of the bamboo fiber is 270-325 mesh.

[0016] Preferably, in step (1), the buffer solution is an acetate-sodium acetate buffer solution with a pH of 4.5-5.5.

[0017] Preferably, in step (1), the compound enzyme agent includes laccase, xylanase, ferulic acid and L-proline in a mass ratio of 10:5-8:0.5-2:1-3.

[0018] Preferably, in step (1), the mass ratio of bamboo fiber, buffer solution and compound enzyme is 100:800-1000:3-5.

[0019] Preferably, in step (1), the enzymatic hydrolysis temperature is 45-55℃ and the treatment time is 3-5h.

[0020] Preferably, in step (1), washing refers to washing the enzymatic hydrolysis product with deionized water until the washing solution is neutral.

[0021] Preferably, in step (1), drying refers to drying to constant weight under vacuum conditions at 60-80℃.

[0022] Preferably, in step (2), the functional modifier includes epoxidized soybean oil, citric acid and sodium hypophosphite in a mass ratio of 10:2-4:0.8-1.2.

[0023] Preferably, in step (2), the mass ratio of deligninized bamboo fiber to functional modifier is 25:1-3.

[0024] Preferably, in step (2), the modification treatment temperature is 150-160℃, the stirring speed is 800-1000rpm, and the treatment time is 10-20min, so that in-situ esterification and ring-opening grafting reactions can occur between the components.

[0025] Preferably, the inorganic filler is food-grade talc powder with an average particle size of 800-1250 mesh.

[0026] Preferably, the composite additive comprises an epoxy chain extender, melamine cyanurate, and pentaerythritol stearate in a mass ratio of 1-2:2-4:1.

[0027] Preferably, the epoxy chain extender is BASF chain extender ADR-4368C.

[0028] Secondly, the present invention provides a method for preparing a PBS / PBAT composite material containing biodegradable bamboo fiber, using the following technical solution:

[0029] A method for preparing a PBS / PBAT composite material containing biodegradable bamboo fiber includes the following steps:

[0030] S1. Weigh each raw material according to the weight parts, and add polybutylene succinate, polybutylene terephthalate-adipate, modified bamboo fiber, inorganic filler and composite additives into the mixer for initial mixing.

[0031] S2. The pre-mixed material is added to a twin-screw extruder for melt blending, extrusion granulation, and PBS / PBAT composite material containing biodegradable bamboo fiber is obtained.

[0032] Preferably, in step S1, the initial mixing temperature is 40-60℃, the initial mixing speed is 300-500rpm, and the initial mixing time is 5-15min.

[0033] Preferably, in step S2, the set temperatures of each zone of the twin-screw extruder are: zone 1 135-145℃, zone 2 150-160℃, zone 3 160-170℃, zone 4 165-175℃, die head 160-170℃, main engine speed 200-300rpm, and length-to-diameter ratio 36-44:1.

[0034] In summary, the present invention has the following beneficial effects:

[0035] 1. This invention uses PBS and PBAT as resin base materials, and obtains PBS / PBAT composite material containing biodegradable bamboo fiber by adding modified bamboo fiber, inorganic filler and composite additives. The resulting composite material has excellent tensile strength and notched impact strength, and has low water absorption and yellow index. It can be widely used in biodegradable packaging film, disposable tableware and agricultural injection molded products.

[0036] 2. This invention introduces ferulic acid and L-proline into a composite enzyme system. Ferulic acid, as a small-molecule natural electron shuttle, plays a cyclical catalytic role in the enzymatic hydrolysis system. It can overcome the steric hindrance of laccase and penetrate deep into the lignin network of bamboo fiber for efficient oxidation, significantly amplifying the delignination efficiency of laccase and eliminating the risk of yellowing during extrusion. L-proline, as an osmotic pressure protectant, is targeted and enriched at the solid-liquid micro-interface between the enzyme and the substrate. It not only stabilizes the enzyme activity but also forms a hydrated protective layer on the surface of the cellulose crystallization region, avoiding excessive degradation and damage to the cellulose skeleton by xylanase. While deligninating and decolorizing, it maintains the mechanical strength of the material.

[0037] 3. This invention uses epoxidized soybean oil, citric acid, and sodium hypophosphite as functional modifiers. During high-speed mixing and subsequent extrusion heating, sodium hypophosphite acts as a catalyst, promoting the dehydration and esterification of one end of the tricarboxylic acid (citric acid) with the hydroxyl groups on the surface of bamboo fiber, while the other end attacks the epoxy groups of epoxidized soybean oil to initiate ring-opening crosslinking. This achieves in-situ synthesis of a macromolecular compatibilizer with long fatty chains inside the material, firmly anchoring the flexible epoxidized soybean oil to the surface of rigid bamboo fiber, forming a buffer transition layer. This greatly alleviates mechanical fracture caused by high shear, thereby achieving excellent notched impact toughness and low water absorption.

[0038] 4. This invention uses epoxy chain extender, melamine cyanurate, and pentaerythritol stearate as composite additives. The epoxy chain extender is used to repair the degradation of the matrix resin and maintain melt strength. Melamine cyanurate, as a high-temperature resistant solid lubricant and heterogeneous nucleating agent, has a graphite-like two-dimensional hydrogen bond planar structure, which generates interlayer slip under high extrusion shear, effectively reducing frictional heat generation between bamboo fibers. At the same time, melamine cyanurate crystals have excellent crystallization matching with PBS resin, which can accelerate the induction of composite material crystallization in the mold, thereby shortening the injection / extrusion molding cycle and improving industrial processing efficiency. Detailed Implementation

[0039] The present invention will be further described in detail below with reference to the embodiments.

[0040] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.

[0041] Among them, polybutylene succinate: grade FZ71, brand PTT from Thailand, purchased from Hengtai Plastic Raw Materials Business Department of Zhangmutou City, Dongguan City.

[0042] Polybutylene terephthalate (PET): Grade TH801T, brand Xinjiang Lanshan Tunhe, purchased from Shanghai Oushuo Plastics Co., Ltd.

[0043] Bamboo fiber: 300 mesh, purchased from Hubei Boshi Chemical Co., Ltd.

[0044] Laccase: Product No. FDY-2204, Brand: Xiasheng, ≥10,000 enzyme activity, purchased from Xiasheng (Beijing) Biotechnology Development Co., Ltd.

[0045] Xylanase: Product No. FDG-0001, Brand: Xiasheng, ≥5500 enzyme activity, purchased from Xiasheng (Beijing) Biotechnology Development Co., Ltd.

[0046] Ferulic acid: Product number YBB-CDF-9527, brand EBAZA, purchased from Shaanxi Yuanbeibei Biotechnology Co., Ltd.

[0047] L-proline: Product number 03261430, brand Siyang, purchased from Shandong Siyang Biotechnology Co., Ltd.

[0048] Epoxidized soybean oil: Model JYS1541, brand Jiyesheng, purchased from Wuhan Jiyesheng Chemical Co., Ltd.

[0049] Food-grade talc powder: 800 mesh and 1250 mesh, brand name Zhanteng, purchased from Lingshou County Zhanteng Mineral Products Processing Plant.

[0050] BASF chain extender ADR-4368C: purchased from Guangzhou Huiwangcheng Chemical Co., Ltd.

[0051] Melamine cyanurate: CAS No. 37640-57-6, model FR-MCA10, purchased from Guangzhou Yinyuan New Materials Co., Ltd.

[0052] Pentaerythritol stearate: CAS No. 115-83-3, Product No. JH-213, purchased from Jining Tangyi Chemical Co., Ltd.

[0053] Examples 1-3 provide a PBS / PBAT composite material containing biodegradable bamboo fiber and its preparation method.

[0054] Example 1

[0055] A PBS / PBAT composite material containing biodegradable bamboo fiber comprises the following raw materials in parts by weight: 35 parts polybutylene succinate, 15 parts polybutylene terephthalate-adipate, 45 parts modified bamboo fiber, 3.5 parts inorganic filler, and 1.2 parts composite additives.

[0056] The modified bamboo fiber is obtained by the following method:

[0057] (1) Control the mass ratio of bamboo fiber, buffer solution and compound enzyme to 100:900:4. Disperse 300 mesh bamboo fiber in an acetate-sodium acetate buffer solution with a pH of 5. Add compound enzyme (compound enzyme includes laccase, xylanase, ferulic acid and L-proline in a mass ratio of 10:6.5:1.2:2). Perform enzymatic hydrolysis at 50°C for 4 hours. After the treatment, wash the enzymatic hydrolysis product with deionized water until the washing liquid is neutral. Then dry it under vacuum at 70°C to constant weight to obtain lignin-free bamboo fiber.

[0058] (2) Control the mass ratio of deligninized bamboo fiber and functional modifier to 25:2. After the deligninized bamboo fiber and functional modifier (functional modifier includes epoxidized soybean oil, citric acid and sodium hypophosphite in a mass ratio of 10:3:1) are mixed evenly, the modified bamboo fiber is subjected to modification treatment for 15 minutes at a temperature of 155℃ and a stirring speed of 900rpm to obtain modified bamboo fiber.

[0059] The inorganic filler is food-grade talc powder with an average particle size of 1250 mesh;

[0060] The composite additives include BASF chain extender ADR-4368C, melamine cyanurate, and pentaerythritol stearate in a mass ratio of 1.5:3:1.

[0061] A method for preparing a PBS / PBAT composite material containing biodegradable bamboo fiber includes the following steps:

[0062] S1. Weigh each raw material according to the weight parts, add polybutylene succinate, polybutylene terephthalate-adipate, modified bamboo fiber, inorganic filler and composite additives into the mixer for initial mixing, control the initial mixing temperature to be 50℃, the initial mixing speed to be 400rpm, and the initial mixing time to be 10min, to obtain the material after initial mixing.

[0063] S2. The pre-mixed material is added to a twin-screw extruder for melt blending, extrusion granulation, and the set temperature of each zone of the twin-screw extruder is controlled as follows: Zone 1 140℃, Zone 2 155℃, Zone 3 165℃, Zone 4 170℃, Die head 165℃, main machine speed 250rpm, and length-to-diameter ratio 40:1 to obtain PBS / PBAT composite material containing biodegradable bamboo fiber.

[0064] Example 2

[0065] A PBS / PBAT composite material containing biodegradable bamboo fiber comprises the following raw materials in parts by weight: 30 parts polybutylene succinate, 10 parts polybutylene terephthalate-adipate, 40 parts modified bamboo fiber, 2 parts inorganic filler, and 0.5 parts composite additive.

[0066] The modified bamboo fiber is obtained by the following method:

[0067] (1) Control the mass ratio of bamboo fiber, buffer solution and compound enzyme to 100:800:3. Disperse 300 mesh bamboo fiber in an acetate-sodium acetate buffer solution with pH 4.5. Add compound enzyme (compound enzyme includes laccase, xylanase, ferulic acid and L-proline in a mass ratio of 10:5:0.5:1). Perform enzymatic hydrolysis at 45℃ for 5 hours. After the treatment, wash the enzymatic hydrolysis product with deionized water until the washing liquid is neutral. Then dry it under vacuum at 60℃ to constant weight to obtain lignin-free bamboo fiber.

[0068] (2) Control the mass ratio of deligninized bamboo fiber and functional modifier to 25:1. After the deligninized bamboo fiber and functional modifier (functional modifier includes epoxidized soybean oil, citric acid and sodium hypophosphite in a mass ratio of 10:2:0.8) are mixed evenly, the modified bamboo fiber is subjected to modification treatment for 20 minutes at a temperature of 150℃ and a stirring speed of 800rpm to obtain modified bamboo fiber.

[0069] The inorganic filler is food-grade talc powder with an average particle size of 800 mesh;

[0070] The composite additives include BASF chain extender ADR-4368C, melamine cyanurate, and pentaerythritol stearate in a mass ratio of 1:2:1.

[0071] A method for preparing a PBS / PBAT composite material containing biodegradable bamboo fiber includes the following steps:

[0072] S1. Weigh each raw material according to the weight parts, add polybutylene succinate, polybutylene terephthalate-adipate, modified bamboo fiber, inorganic filler and composite additives into the mixer for initial mixing, control the initial mixing temperature to 40℃, the initial mixing speed to 300rpm, and the initial mixing time to 15min to obtain the initial mixed material.

[0073] S2. The pre-mixed material is added to a twin-screw extruder for melt blending, extrusion granulation, and the set temperature of each zone of the twin-screw extruder is controlled as follows: Zone 1 135℃, Zone 2 150℃, Zone 3 160℃, Zone 4 165℃, Die head 160℃, main machine speed 200rpm, and length-to-diameter ratio 36:1 to obtain PBS / PBAT composite material containing biodegradable bamboo fiber.

[0074] Example 3

[0075] A PBS / PBAT composite material containing biodegradable bamboo fiber comprises the following raw materials in parts by weight: 40 parts polybutylene succinate, 20 parts polybutylene terephthalate-adipate, 50 parts modified bamboo fiber, 5 parts inorganic filler, and 2 parts composite additives.

[0076] The modified bamboo fiber is obtained by the following method:

[0077] (1) Control the mass ratio of bamboo fiber, buffer solution and compound enzyme to 100:1000:5. Disperse 300 mesh bamboo fiber in an acetate-sodium acetate buffer solution with a pH of 5.5. Add compound enzyme (compound enzyme includes laccase, xylanase, ferulic acid and L-proline in a mass ratio of 10:8:2:3). Perform enzymatic hydrolysis at 55°C for 3 hours. After the treatment, wash the enzymatic hydrolysis product with deionized water until the washing liquid is neutral. Then dry it under vacuum at 80°C to constant weight to obtain lignin-free bamboo fiber.

[0078] (2) Control the mass ratio of deligninized bamboo fiber and functional modifier to 25:3. After the deligninized bamboo fiber and functional modifier (functional modifier includes epoxidized soybean oil, citric acid and sodium hypophosphite in a mass ratio of 10:4:1.2) are mixed evenly, the modified bamboo fiber is subjected to modification treatment for 10 minutes at a temperature of 160℃ and a stirring speed of 1000rpm to obtain modified bamboo fiber.

[0079] The inorganic filler is food-grade talc powder with an average particle size of 800 mesh;

[0080] The composite additives include BASF chain extender ADR-4368C, melamine cyanurate, and pentaerythritol stearate in a mass ratio of 2:4:1.

[0081] A method for preparing a PBS / PBAT composite material containing biodegradable bamboo fiber includes the following steps:

[0082] S1. Weigh each raw material according to the weight parts, add polybutylene succinate, polybutylene terephthalate-adipate, modified bamboo fiber, inorganic filler and composite additives into the mixer for initial mixing, control the initial mixing temperature at 60℃, the initial mixing speed at 500rpm, and the initial mixing time at 5min to obtain the initial mixed material.

[0083] S2. The pre-mixed material is added to a twin-screw extruder for melt blending, extrusion granulation, and the set temperature of each zone of the twin-screw extruder is controlled as follows: Zone 1 145℃, Zone 2 160℃, Zone 3 170℃, Zone 4 175℃, Die head 170℃, main engine speed 300rpm, and length-to-diameter ratio 44:1 to obtain PBS / PBAT composite material containing biodegradable bamboo fiber.

[0084] To verify the comprehensive performance of the PBS / PBAT composite material containing biodegradable bamboo fiber provided by this invention, comparative examples 1-8 were set up, wherein:

[0085] Comparative Example 1

[0086] Comparative Example 1 is the same as Example 1, except that the ferulic acid in the compound enzyme was replaced with L-proline by mass. Details are as follows:

[0087] A PBS / PBAT composite material containing biodegradable bamboo fiber comprises the following raw materials in parts by weight: 35 parts polybutylene succinate, 15 parts polybutylene terephthalate-adipate, 45 parts modified bamboo fiber, 3.5 parts inorganic filler, and 1.2 parts composite additives.

[0088] The modified bamboo fiber is obtained by the following method:

[0089] (1) Control the mass ratio of bamboo fiber, buffer solution and compound enzyme to 100:900:4. Disperse 300 mesh bamboo fiber in an acetate-sodium acetate buffer solution with a pH of 5. Add compound enzyme (compound enzyme includes laccase, xylanase and L-proline in a mass ratio of 10:6.5:3.2). Perform enzymatic hydrolysis at 50°C for 4 hours. After the treatment, wash the enzymatic hydrolysis product with deionized water until the washing liquid is neutral. Then dry it under vacuum at 70°C to constant weight to obtain lignin-free bamboo fiber.

[0090] (2) Control the mass ratio of deligninized bamboo fiber and functional modifier to 25:2. After the deligninized bamboo fiber and functional modifier (functional modifier includes epoxidized soybean oil, citric acid and sodium hypophosphite in a mass ratio of 10:3:1) are mixed evenly, the modified bamboo fiber is subjected to modification treatment for 15 minutes at a temperature of 155℃ and a stirring speed of 900rpm to obtain modified bamboo fiber.

[0091] The inorganic filler is food-grade talc powder with an average particle size of 1250 mesh;

[0092] The composite additives include BASF chain extender ADR-4368C, melamine cyanurate, and pentaerythritol stearate in a mass ratio of 1.5:3:1.

[0093] A method for preparing a PBS / PBAT composite material containing biodegradable bamboo fiber includes the following steps:

[0094] S1. Weigh each raw material according to the weight parts, add polybutylene succinate, polybutylene terephthalate-adipate, modified bamboo fiber, inorganic filler and composite additives into the mixer for initial mixing, control the initial mixing temperature to be 50℃, the initial mixing speed to be 400rpm, and the initial mixing time to be 10min, to obtain the material after initial mixing.

[0095] S2. The pre-mixed material is added to a twin-screw extruder for melt blending, extrusion granulation, and the set temperature of each zone of the twin-screw extruder is controlled as follows: Zone 1 140℃, Zone 2 155℃, Zone 3 165℃, Zone 4 170℃, Die head 165℃, main machine speed 250rpm, and length-to-diameter ratio 40:1 to obtain PBS / PBAT composite material containing biodegradable bamboo fiber.

[0096] Comparative Example 2

[0097] Comparative Example 2 is the same as Example 1, except that L-proline and other components in the complex enzyme were replaced with ferulic acid. Details are as follows:

[0098] A PBS / PBAT composite material containing biodegradable bamboo fiber comprises the following raw materials in parts by weight: 35 parts polybutylene succinate, 15 parts polybutylene terephthalate-adipate, 45 parts modified bamboo fiber, 3.5 parts inorganic filler, and 1.2 parts composite additives.

[0099] The modified bamboo fiber is obtained by the following method:

[0100] (1) Control the mass ratio of bamboo fiber, buffer solution and compound enzyme to 100:900:4. Disperse 300 mesh bamboo fiber in an acetate-sodium acetate buffer solution with a pH of 5. Add compound enzyme (compound enzyme includes laccase, xylanase and ferulic acid in a mass ratio of 10:6.5:3.2). Perform enzymatic hydrolysis at 50°C for 4 hours. After the treatment, wash the enzymatic hydrolysis product with deionized water until the washing liquid is neutral. Then dry it under vacuum at 70°C to constant weight to obtain lignin-free bamboo fiber.

[0101] (2) Control the mass ratio of deligninized bamboo fiber and functional modifier to 25:2. After the deligninized bamboo fiber and functional modifier (functional modifier includes epoxidized soybean oil, citric acid and sodium hypophosphite in a mass ratio of 10:3:1) are mixed evenly, the modified bamboo fiber is subjected to modification treatment for 15 minutes at a temperature of 155℃ and a stirring speed of 900rpm to obtain modified bamboo fiber.

[0102] The inorganic filler is food-grade talc powder with an average particle size of 1250 mesh;

[0103] The composite additives include BASF chain extender ADR-4368C, melamine cyanurate, and pentaerythritol stearate in a mass ratio of 1.5:3:1.

[0104] A method for preparing a PBS / PBAT composite material containing biodegradable bamboo fiber includes the following steps:

[0105] S1. Weigh each raw material according to the weight parts, add polybutylene succinate, polybutylene terephthalate-adipate, modified bamboo fiber, inorganic filler and composite additives into the mixer for initial mixing, control the initial mixing temperature to be 50℃, the initial mixing speed to be 400rpm, and the initial mixing time to be 10min, to obtain the material after initial mixing.

[0106] S2. The pre-mixed material is added to a twin-screw extruder for melt blending, extrusion granulation, and the set temperature of each zone of the twin-screw extruder is controlled as follows: Zone 1 140℃, Zone 2 155℃, Zone 3 165℃, Zone 4 170℃, Die head 165℃, main machine speed 250rpm, and length-to-diameter ratio 40:1 to obtain PBS / PBAT composite material containing biodegradable bamboo fiber.

[0107] Comparative Example 3

[0108] Comparative Example 3 is the same as Example 1, except that the citric acid in the functional modifier is replaced by sodium hypophosphite. Details are as follows:

[0109] A PBS / PBAT composite material containing biodegradable bamboo fiber comprises the following raw materials in parts by weight: 35 parts polybutylene succinate, 15 parts polybutylene terephthalate-adipate, 45 parts modified bamboo fiber, 3.5 parts inorganic filler, and 1.2 parts composite additives.

[0110] The modified bamboo fiber is obtained by the following method:

[0111] (1) Control the mass ratio of bamboo fiber, buffer solution and compound enzyme to 100:900:4. Disperse 300 mesh bamboo fiber in an acetate-sodium acetate buffer solution with a pH of 5. Add compound enzyme (compound enzyme includes laccase, xylanase, ferulic acid and L-proline in a mass ratio of 10:6.5:1.2:2). Perform enzymatic hydrolysis at 50°C for 4 hours. After the treatment, wash the enzymatic hydrolysis product with deionized water until the washing liquid is neutral. Then dry it under vacuum at 70°C to constant weight to obtain lignin-free bamboo fiber.

[0112] (2) Control the mass ratio of deligninized bamboo fiber and functional modifier to 25:2. After the deligninized bamboo fiber and functional modifier (functional modifier includes epoxidized soybean oil and sodium hypophosphite in a mass ratio of 10:4) are mixed evenly, the modified bamboo fiber is subjected to modification treatment for 15 minutes at a temperature of 155℃ and a stirring speed of 900rpm to obtain modified bamboo fiber.

[0113] The inorganic filler is food-grade talc powder with an average particle size of 1250 mesh;

[0114] The composite additives include BASF chain extender ADR-4368C, melamine cyanurate, and pentaerythritol stearate in a mass ratio of 1.5:3:1.

[0115] A method for preparing a PBS / PBAT composite material containing biodegradable bamboo fiber includes the following steps:

[0116] S1. Weigh each raw material according to the weight parts, add polybutylene succinate, polybutylene terephthalate-adipate, modified bamboo fiber, inorganic filler and composite additives into the mixer for initial mixing, control the initial mixing temperature to be 50℃, the initial mixing speed to be 400rpm, and the initial mixing time to be 10min, to obtain the material after initial mixing.

[0117] S2. The pre-mixed material is added to a twin-screw extruder for melt blending, extrusion granulation, and the set temperature of each zone of the twin-screw extruder is controlled as follows: Zone 1 140℃, Zone 2 155℃, Zone 3 165℃, Zone 4 170℃, Die head 165℃, main machine speed 250rpm, and length-to-diameter ratio 40:1 to obtain PBS / PBAT composite material containing biodegradable bamboo fiber.

[0118] Comparative Example 4

[0119] Comparative Example 4 is the same as Example 1, except that the sodium hypophosphite in the functional modifier is replaced by citric acid. Details are as follows:

[0120] A PBS / PBAT composite material containing biodegradable bamboo fiber comprises the following raw materials in parts by weight: 35 parts polybutylene succinate, 15 parts polybutylene terephthalate-adipate, 45 parts modified bamboo fiber, 3.5 parts inorganic filler, and 1.2 parts composite additives.

[0121] The modified bamboo fiber is obtained by the following method:

[0122] (1) Control the mass ratio of bamboo fiber, buffer solution and compound enzyme to 100:900:4. Disperse 300 mesh bamboo fiber in an acetate-sodium acetate buffer solution with a pH of 5. Add compound enzyme (compound enzyme includes laccase, xylanase, ferulic acid and L-proline in a mass ratio of 10:6.5:1.2:2). Perform enzymatic hydrolysis at 50°C for 4 hours. After the treatment, wash the enzymatic hydrolysis product with deionized water until the washing liquid is neutral. Then dry it under vacuum at 70°C to constant weight to obtain lignin-free bamboo fiber.

[0123] (2) Control the mass ratio of deligninized bamboo fiber and functional modifier to 25:2. After the deligninized bamboo fiber and functional modifier (functional modifier includes epoxidized soybean oil and citric acid with a mass ratio of 10:4) are mixed evenly, the modified bamboo fiber is subjected to modification treatment for 15 minutes at a temperature of 155℃ and a stirring speed of 900rpm to obtain modified bamboo fiber.

[0124] The inorganic filler is food-grade talc powder with an average particle size of 1250 mesh;

[0125] The composite additives include BASF chain extender ADR-4368C, melamine cyanurate, and pentaerythritol stearate in a mass ratio of 1.5:3:1.

[0126] A method for preparing a PBS / PBAT composite material containing biodegradable bamboo fiber includes the following steps:

[0127] S1. Weigh each raw material according to the weight parts, add polybutylene succinate, polybutylene terephthalate-adipate, modified bamboo fiber, inorganic filler and composite additives into the mixer for initial mixing, control the initial mixing temperature to be 50℃, the initial mixing speed to be 400rpm, and the initial mixing time to be 10min, to obtain the material after initial mixing.

[0128] S2. The pre-mixed material is added to a twin-screw extruder for melt blending, extrusion granulation, and the set temperature of each zone of the twin-screw extruder is controlled as follows: Zone 1 140℃, Zone 2 155℃, Zone 3 165℃, Zone 4 170℃, Die head 165℃, main machine speed 250rpm, and length-to-diameter ratio 40:1 to obtain PBS / PBAT composite material containing biodegradable bamboo fiber.

[0129] Comparative Example 5

[0130] Comparative Example 5 is the same as Example 1, except that the independent modification treatment in step (2) is omitted, and the functional modifier is added to the mixer along with other raw materials in step S1 for initial mixing. Specifically:

[0131] A PBS / PBAT composite material containing biodegradable bamboo fiber comprises the following raw materials in parts by weight: 35 parts polybutylene succinate, 15 parts polybutylene terephthalate-adipate, 45 parts delignified bamboo fiber, 3.6 parts functional modifier, 3.5 parts inorganic filler, and 1.2 parts composite additive;

[0132] The delignin-treated bamboo fiber is obtained by the following method:

[0133] The mass ratio of bamboo fiber, buffer solution, and compound enzyme was controlled at 100:900:4. Bamboo fiber with a mesh size of 300 was dispersed in an acetate-sodium acetate buffer solution with a pH of 5. The compound enzyme (containing laccase, xylanase, ferulic acid, and L-proline in a mass ratio of 10:6.5:1.2:2) was added, and enzymatic hydrolysis was carried out at 50°C for 4 hours. After the treatment, the enzymatic hydrolysis product was washed with deionized water until the washing liquid was neutral. Then, it was dried to constant weight under vacuum at 70°C to obtain lignin-free bamboo fiber.

[0134] The functional modifiers include epoxidized soybean oil, citric acid, and sodium hypophosphite in a mass ratio of 10:3:1;

[0135] The inorganic filler is food-grade talc powder with an average particle size of 1250 mesh;

[0136] The composite additives include BASF chain extender ADR-4368C, melamine cyanurate, and pentaerythritol stearate in a mass ratio of 1.5:3:1.

[0137] A method for preparing a PBS / PBAT composite material containing biodegradable bamboo fiber includes the following steps:

[0138] S1. Weigh each raw material according to the weight parts, add polybutylene succinate, polybutylene terephthalate-adipate, lignin-free bamboo fiber, functional modifier, inorganic filler and composite additive to the mixer for initial mixing, control the initial mixing temperature to 50℃, the initial mixing speed to 400rpm, and the initial mixing time to 10min to obtain the initial mixed material.

[0139] S2. The pre-mixed material is added to a twin-screw extruder for melt blending, extrusion granulation, and the set temperature of each zone of the twin-screw extruder is controlled as follows: Zone 1 140℃, Zone 2 155℃, Zone 3 165℃, Zone 4 170℃, Die head 165℃, main machine speed 250rpm, and length-to-diameter ratio 40:1 to obtain PBS / PBAT composite material containing biodegradable bamboo fiber.

[0140] Comparative Example 6

[0141] Comparative Example 6 is the same as Example 1, except that the modified bamboo fiber was replaced with raw bamboo fiber that had not undergone any pretreatment or modification. Specifically:

[0142] A PBS / PBAT composite material containing biodegradable bamboo fiber comprises the following raw materials in parts by weight: 35 parts polybutylene succinate, 15 parts polybutylene terephthalate-adipate, 45 parts bamboo fiber, 3.5 parts inorganic filler, and 1.2 parts composite additives.

[0143] The inorganic filler is food-grade talc powder with an average particle size of 1250 mesh.

[0144] The composite additives include BASF chain extender ADR-4368C, melamine cyanurate, and pentaerythritol stearate in a mass ratio of 1.5:3:1.

[0145] A method for preparing a PBS / PBAT composite material containing biodegradable bamboo fiber includes the following steps:

[0146] S1. Weigh each raw material according to the weight parts, add polybutylene succinate, polybutylene terephthalate-adipate, bamboo fiber, inorganic filler and composite additives into the mixer for initial mixing, control the initial mixing temperature at 50℃, the initial mixing speed at 400rpm, and the initial mixing time at 10min to obtain the initial mixed material.

[0147] S2. The pre-mixed material is added to a twin-screw extruder for melt blending, extrusion granulation, and the set temperature of each zone of the twin-screw extruder is controlled as follows: Zone 1 140℃, Zone 2 155℃, Zone 3 165℃, Zone 4 170℃, Die head 165℃, main machine speed 250rpm, and length-to-diameter ratio 40:1 to obtain PBS / PBAT composite material containing biodegradable bamboo fiber.

[0148] Comparative Example 7

[0149] Comparative Example 7 is the same as Example 1, except that the melamine cyanurate in the composite additive is replaced by pentaerythritol stearate. Details are as follows:

[0150] A PBS / PBAT composite material containing biodegradable bamboo fiber comprises the following raw materials in parts by weight: 35 parts polybutylene succinate, 15 parts polybutylene terephthalate-adipate, 45 parts modified bamboo fiber, 3.5 parts inorganic filler, and 1.2 parts composite additives.

[0151] The modified bamboo fiber is obtained by the following method:

[0152] (1) Control the mass ratio of bamboo fiber, buffer solution and compound enzyme to 100:900:4. Disperse 300 mesh bamboo fiber in an acetate-sodium acetate buffer solution with a pH of 5. Add compound enzyme (compound enzyme includes laccase, xylanase, ferulic acid and L-proline in a mass ratio of 10:6.5:1.2:2). Perform enzymatic hydrolysis at 50°C for 4 hours. After the treatment, wash the enzymatic hydrolysis product with deionized water until the washing liquid is neutral. Then dry it under vacuum at 70°C to constant weight to obtain lignin-free bamboo fiber.

[0153] (2) Control the mass ratio of deligninized bamboo fiber and functional modifier to 25:2. After the deligninized bamboo fiber and functional modifier (functional modifier includes epoxidized soybean oil, citric acid and sodium hypophosphite in a mass ratio of 10:3:1) are mixed evenly, the modified bamboo fiber is subjected to modification treatment for 15 minutes at a temperature of 155℃ and a stirring speed of 900rpm to obtain modified bamboo fiber.

[0154] The inorganic filler is food-grade talc powder with an average particle size of 1250 mesh;

[0155] The compound additives include BASF chain extender ADR-4368C and pentaerythritol stearate in a mass ratio of 1.5:4.

[0156] A method for preparing a PBS / PBAT composite material containing biodegradable bamboo fiber includes the following steps:

[0157] S1. Weigh each raw material according to the weight parts, add polybutylene succinate, polybutylene terephthalate-adipate, modified bamboo fiber, inorganic filler and composite additives into the mixer for initial mixing, control the initial mixing temperature to be 50℃, the initial mixing speed to be 400rpm, and the initial mixing time to be 10min, to obtain the material after initial mixing.

[0158] S2. The pre-mixed material is added to a twin-screw extruder for melt blending, extrusion granulation, and the set temperature of each zone of the twin-screw extruder is controlled as follows: Zone 1 140℃, Zone 2 155℃, Zone 3 165℃, Zone 4 170℃, Die head 165℃, main machine speed 250rpm, and length-to-diameter ratio 40:1 to obtain PBS / PBAT composite material containing biodegradable bamboo fiber.

[0159] Comparative Example 8

[0160] Comparative Example 8 is the same as Example 1, except that the pentaerythritol stearate in the composite additive is replaced by melamine cyanurate. Details are as follows:

[0161] A PBS / PBAT composite material containing biodegradable bamboo fiber comprises the following raw materials in parts by weight: 35 parts polybutylene succinate, 15 parts polybutylene terephthalate-adipate, 45 parts modified bamboo fiber, 3.5 parts inorganic filler, and 1.2 parts composite additives.

[0162] The modified bamboo fiber is obtained by the following method:

[0163] (1) Control the mass ratio of bamboo fiber, buffer solution and compound enzyme to 100:900:4. Disperse 300 mesh bamboo fiber in an acetate-sodium acetate buffer solution with a pH of 5. Add compound enzyme (compound enzyme includes laccase, xylanase, ferulic acid and L-proline in a mass ratio of 10:6.5:1.2:2). Perform enzymatic hydrolysis at 50°C for 4 hours. After the treatment, wash the enzymatic hydrolysis product with deionized water until the washing liquid is neutral. Then dry it under vacuum at 70°C to constant weight to obtain lignin-free bamboo fiber.

[0164] (2) Control the mass ratio of deligninized bamboo fiber and functional modifier to 25:2. After the deligninized bamboo fiber and functional modifier (functional modifier includes epoxidized soybean oil, citric acid and sodium hypophosphite in a mass ratio of 10:3:1) are mixed evenly, the modified bamboo fiber is subjected to modification treatment for 15 minutes at a temperature of 155℃ and a stirring speed of 900rpm to obtain modified bamboo fiber.

[0165] The inorganic filler is food-grade talc powder with an average particle size of 1250 mesh;

[0166] The composite additives include BASF chain extender ADR-4368C and melamine cyanurate in a mass ratio of 1.5:4.

[0167] A method for preparing a PBS / PBAT composite material containing biodegradable bamboo fiber includes the following steps:

[0168] S1. Weigh each raw material according to the weight parts, add polybutylene succinate, polybutylene terephthalate-adipate, modified bamboo fiber, inorganic filler and composite additives into the mixer for initial mixing, control the initial mixing temperature to be 50℃, the initial mixing speed to be 400rpm, and the initial mixing time to be 10min, to obtain the material after initial mixing.

[0169] S2. The pre-mixed material is added to a twin-screw extruder for melt blending, extrusion granulation, and the set temperature of each zone of the twin-screw extruder is controlled as follows: Zone 1 140℃, Zone 2 155℃, Zone 3 165℃, Zone 4 170℃, Die head 165℃, main machine speed 250rpm, and length-to-diameter ratio 40:1 to obtain PBS / PBAT composite material containing biodegradable bamboo fiber.

[0170] Performance testing

[0171] The comprehensive properties of the PBS / PBAT composite materials containing biodegradable bamboo fiber prepared in Examples 1-3 and Comparative Examples 1-8 were tested respectively.

[0172] 1. Tensile strength and elongation at break: The test was conducted in accordance with the national standard GB / T 1040.2-2022 "Determination of tensile properties of plastics - Part 2: Test conditions for molded and extruded plastics", with a tensile speed of 50 mm / min.

[0173] 2. Notched impact strength: The notched impact test of the cantilever beam was carried out in accordance with the national standard GB / T 1043.1-2008 "Determination of impact properties of simply supported plastic beams - Part 1: Non-instrumental impact test".

[0174] 3.24h water absorption rate: Referring to the national standard GB / T 1034-2008 "Determination of water absorption of plastics", the mass increase rate was tested after the sample was immersed in distilled water at 23℃ for 24 hours.

[0175] 4. Yellow Index (YI): Tested using a spectrophotometer according to the standard ASTM E 313 Yellow Index (plastics, coatings), the degree of yellowing of the material surface is measured. The higher the value, the more severe the heat discoloration.

[0176] The test results are shown in Table 1:

[0177] Table 1:

[0178]

[0179] As shown in Table 1, the PBS / PBAT composite materials containing biodegradable bamboo fiber prepared in Examples 1-3 of this invention have excellent mechanical properties, low water absorption and yellow index, and their overall performance is significantly better than that of Comparative Examples 1-8.

[0180] As can be seen from Example 1 and Comparative Examples 1 and 2, when ferulic acid is lacking in the composite enzyme (Comparative Example 1), the yellow index of the composite material increases significantly. This is because without ferulic acid as an electron shuttle, laccase cannot overcome steric hindrance to penetrate the fiber network and oxidize lignin, resulting in residual lignin turning yellow due to heat and oxygen during subsequent hot extrusion. When L-proline is lacking (Comparative Example 2), the tensile strength and impact strength of the composite material decrease significantly, proving that L-proline, as an osmotic pressure protectant, plays a role in shielding the excessive hydrolysis and degradation of cellulose. Its absence causes the cellulose skeleton to be destroyed by enzymes, resulting in the loss of its reinforcing load-bearing capacity.

[0181] As shown in Examples 1 and Comparative Examples 3 and 4, when the functional modifier lacks citric acid (Comparative Example 3) or sodium hypophosphite (Comparative Example 4), the notched impact strength of the composite material decreases significantly, and the water absorption rate increases significantly. This indicates that sodium hypophosphite and citric acid are indispensable and must coexist to dehydrate and esterify in the heated system and attack the ring-opening of epoxidized soybean oil, forming a hydrophobic and flexible buffer transition layer in situ on the polar surface of bamboo fiber.

[0182] As shown in Example 1 and Comparative Example 5, directly adding the functional modifier to the extrusion blend (Comparative Example 5) significantly degrades the mechanical strength and water resistance of the resulting composite material. The mechanism is that the resin matrix melts rapidly in the extruder, encapsulating the bamboo fiber and cutting off the contact channel between the functional modifier and the fiber hydroxyl groups. This hinders the in-situ grafting reaction, leaving severe defects at the two-phase interface, which then lead to stress concentration and fracture under high shear.

[0183] As can be seen from Example 1 and Comparative Example 6, compared with the unmodified raw bamboo fiber (Comparative Example 6), Example 1 shows substantial improvement in toughness, strength and yellowing resistance.

[0184] As shown in Examples 1 and Comparative Examples 7 and 8, replacing melamine cyanurate with pentaerythritol stearate (Comparative Example 7) by an equal mass resulted in a significant decrease in tensile strength and color. This confirms that the unique two-dimensional planar slip structure of melamine cyanurate effectively reduces the high shear frictional heat generated between rigid bamboo fibers, preventing the resulting localized thermal degradation. The absence of pentaerythritol stearate (Comparative Example 8) leads to a decrease in the external lubricity of the system, and the flow shear variation of the melt during processing results in a slight decrease in the overall mechanical properties of the material. Both components synergistically exert a lubricating and crystallization-inducing effect within the composite additive system, addressing both internal and external needs.

[0185] This specific embodiment is merely an explanation of the present invention and is not intended to limit the invention. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they are within the scope of the claims of the present invention.

Claims

1. A PBS / PBAT composite material containing biodegradable bamboo fiber, characterized in that, The raw materials include the following parts by weight: 30-40 parts of polybutylene succinate, 10-20 parts of polybutylene terephthalate-adipate, 40-50 parts of modified bamboo fiber, 2-5 parts of inorganic filler, and 0.5-2 parts of composite additives. The modified bamboo fiber is obtained by pretreatment with a composite enzyme agent followed by modification with a functional modifier.

2. The PBS / PBAT composite material containing biodegradable bamboo fiber according to claim 1, characterized in that, The modified bamboo fiber is prepared by the following method: (1) Disperse bamboo fiber in buffer solution, add compound enzyme for enzymatic hydrolysis, wash and dry after treatment to obtain lignin-free bamboo fiber; (2) After the lignin-free bamboo fiber is mixed evenly with the functional modifier, it is modified to obtain modified bamboo fiber.

3. The PBS / PBAT composite material containing biodegradable bamboo fiber according to claim 2, characterized in that, In step (1), the compound enzyme includes laccase, xylanase, ferulic acid and L-proline in a mass ratio of 10:5-8:0.5-2:1-3.

4. The PBS / PBAT composite material containing biodegradable bamboo fiber according to claim 2, characterized in that, In step (1), the mass ratio of bamboo fiber, buffer solution and compound enzyme is 100:800-1000:3-5.

5. The PBS / PBAT composite material containing biodegradable bamboo fiber according to claim 2, characterized in that, In step (2), the functional modifiers include epoxidized soybean oil, citric acid and sodium hypophosphite in a mass ratio of 10:2-4:0.8-1.

2.

6. The PBS / PBAT composite material containing biodegradable bamboo fiber according to claim 2, characterized in that, In step (2), the mass ratio of deligninized bamboo fiber to functional modifier is 25:1-3.

7. The PBS / PBAT composite material containing biodegradable bamboo fiber according to claim 1, characterized in that, The composite additives include an epoxy chain extender, melamine cyanurate, and pentaerythritol stearate in a mass ratio of 1-2:2-4:

1.

8. A method for preparing a PBS / PBAT composite material containing biodegradable bamboo fiber as described in any one of claims 1-7, characterized in that, Includes the following steps: S1. Weigh each raw material according to the weight parts, and add polybutylene succinate, polybutylene terephthalate-adipate, modified bamboo fiber, inorganic filler and composite additives into the mixer for initial mixing. S2. The pre-mixed material is added to a twin-screw extruder for melt blending, extrusion granulation, and PBS / PBAT composite material containing biodegradable bamboo fiber is obtained.

9. The method for preparing the PBS / PBAT composite material containing biodegradable bamboo fiber according to claim 8, characterized in that, In step S1, the initial mixing temperature is 40-60℃, the initial mixing speed is 300-500 rpm, and the initial mixing time is 5-15 min.

10. The method for preparing the PBS / PBAT composite material containing biodegradable bamboo fiber according to claim 8, characterized in that, In step S2, the set temperatures for each zone of the twin-screw extruder are: Zone 1 135-145℃, Zone 2 150-160℃, Zone 3 160-170℃, Zone 4 165-175℃, and the die head 160-170℃. The main extruder speed is 200-300 rpm, and the length-to-diameter ratio is 36-44:1.