A cellulose ether composite additive for putty mortar and its preparation method

By using a composite additive of low-methoxyl content HPMC with starch ether, redispersible latex powder and polyacrylamide, the problem of unstable construction performance of HPMC at extreme temperatures was solved, achieving the effect of extending construction time and reducing costs at high temperatures.

CN123107439APending Publication Date: 2026-11-17CHONGQING PENGKAI FINE CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611311517.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing HPMC products have reduced water retention capacity under extreme temperature conditions, resulting in poor workability of putty and mortar. Furthermore, existing technologies require the addition of a large number of auxiliary additives, which complicates the formulation and increases costs.

Method used

A composite additive using low-methoxyl content HPMC, starch ether, redispersible latex powder, and polyacrylamide maintains good workability under high and low temperature conditions through synergistic effects, reducing dependence on retarders and large amounts of thickeners.

Benefits of technology

Extending the workable time under high temperature conditions reduces consistency loss, ensures sufficient cement hydration, improves workability, and reduces raw material costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention discloses a cellulose ether composite additive for putty mortar and its preparation method, relating to the field of building material additives. The composite additive consists of the following components by mass percentage: 88%–95% hydroxypropyl methylcellulose, 3%–6% starch ether, 1%–3% redispersible latex powder, and 1%–3% polyacrylamide, with the sum of all components being 100%. The methoxy group content of the hydroxypropyl methylcellulose is 19%–22%, and the hydroxypropoxy group content is 8%–9%. The preparation method includes weighing each component according to the specified ratio, placing them in a mixer, mixing and stirring at room temperature for 20–40 minutes at a speed of 20–30 rpm, and discharging the mixture after uniform mixing. This invention, through the synergistic compounding of low-methoxyl content HPMC with starch ether, redispersible latex powder, and polyacrylamide, significantly improves water retention and workability under extreme high and low temperature environments while reducing the total amount of additives used. This effectively extends the workability of the putty, reduces mortar consistency loss, and keeps costs under control.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of building material additives, specifically to a cellulose ether composite additive for putty mortar and its preparation method. Background Technology

[0002] Hydroxypropyl methylcellulose (HPMC), as a core functional additive in the putty and mortar industry, has become an indispensable key material in the production of building putty and premixed mortar due to its excellent thickening, water retention, bonding and film-forming properties, and plays an important role in ensuring construction quality and improving construction efficiency.

[0003] However, existing HPMC products exhibit significant limitations in performance stability under extreme temperature environments. Conventional HPMC experiences a marked decrease in water retention capacity at high temperatures, leading to excessively rapid evaporation of moisture in putty and mortar, incomplete cement hydration, accelerated consistency loss, and a substantial reduction in workable time. Simultaneously, the rapid water loss causes drying and hardening, resulting in poor troweling and coating properties. To compensate for these performance deficiencies, current technologies typically require the addition of large amounts of functional additives (such as retarders and thickeners) to maintain workability at high temperatures, but this introduces problems of increased formulation complexity and significantly higher production costs.

[0004] The existence of the above problems not only affects the quality of putty and mortar in high-temperature construction scenarios in summer, but also limits the application and promotion of HPMC products in a wider range of climatic conditions, and increases the formulation costs and quality control difficulties for building material manufacturers. Summary of the Invention

[0005] To address the shortcomings of existing technologies, this invention provides a cellulose ether composite additive for putty mortar and its preparation method, thus solving the problems mentioned in the background technology.

[0006] To achieve the above objectives, the present invention provides the following technical solution: On one hand, the present invention provides a cellulose ether composite additive for putty mortar, comprising the following raw materials in weight percentages: Hydroxypropyl methylcellulose 92%, starch ether 4%, redispersible latex powder 2%, polyacrylamide 2%; The methoxy group content in the hydroxypropyl methylcellulose is 19-22%, and the hydroxypropoxy group content in the hydroxypropyl methylcellulose is 8-9%.

[0007] Furthermore, the methoxy group content in the hydroxypropyl methylcellulose is 19.1% to 21.3%.

[0008] Furthermore, the starch ether is 301-hydroxypropyl starch ether.

[0009] Furthermore, the redispersible latex powder is Wacker 5010N.

[0010] Furthermore, the polyacrylamide is a nonionic NPAM.

[0011] On the other hand, the present invention provides a method for preparing a cellulose ether composite additive for putty mortar, comprising the following steps: S1, weigh out 92% hydroxypropyl methylcellulose, 4% starch ether, 2% redispersible latex powder, and 2% polyacrylamide by mass percentage; S2, Place the weighed raw materials into a mixer and mix them at room temperature for 20-40 minutes at a speed of 20-30 rpm. S3, after being mixed evenly, is discharged to obtain the cellulose ether composite additive for putty mortar.

[0012] Furthermore, in step S2, the mixing time is 30 minutes and the mixer speed is 24 rpm.

[0013] Furthermore, the mixer is a V-type mixer.

[0014] This invention provides a cellulose ether composite additive for putty mortar and its preparation method, which has the following beneficial effects: This invention utilizes HPMC with a methoxyl content of 19%~22%, which has fewer hydrophobic groups and a relatively increased proportion of hydrophilic groups on its molecular chain, enhancing the interaction with water molecules and giving HPMC a higher gel temperature. Under high-temperature construction conditions, the composite additive can still effectively lock in free water in mortar and putty, slowing down the water evaporation rate during cement hydration, thereby significantly extending the workable time and reducing the loss of mortar consistency over time. Simultaneously, the improved water retention ensures sufficient cement hydration, avoiding poor strength development caused by excessive water loss.

[0015] This invention utilizes a synergistic blend of low-methoxyl content HPMC with starch ether, redispersible latex powder, and polyacrylamide to maintain excellent workability under extreme high and low temperature conditions. Specifically, the starch ether's thickening and anti-sagging effects improve the smoothness of the putty application, the redispersible latex powder enhances the internal adhesion and stability of the paste, and the polyacrylamide further improves the system's cohesiveness and water retention uniformity. The synergistic effect of these four components ensures that the putty does not dry too quickly at high temperatures and maintains good workability at low temperatures, effectively overcoming the shortcomings of traditional HPMC whose workability deteriorates due to temperature fluctuations.

[0016] This invention eliminates the need for conventional additives such as retarders and large amounts of thickeners. It utilizes only low-methoxyl content HPMC as the main component, supplemented with a small amount of functional additives, to achieve the required water retention and workability under high-temperature conditions. The total amount of additives used is small, and the formulation is simplified, effectively reducing raw material and compounding costs while ensuring stable quality, thus demonstrating excellent economic practicality. Detailed Implementation

[0017] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0018] This invention provides a cellulose ether composite additive for putty mortar, comprising the following raw materials by weight percentage: HPMC 92%, starch ether 4%, redispersible latex powder 2%, and polyacrylamide 2%; wherein the HPMC has a methoxy content of 19-22% and a hydroxypropoxy content of 8-9%.

[0019] The cellulose ether composite additive for putty mortar described in this invention comprises 92% HPMC. The HPMC has a methoxyl content of 19-22%, which can be any value between 19.1%, 19.8%, 21.3%, or 19-22%. The HPMC has a hydroxypropoxyl content of 8-9%, which can be any value between 8.3%, 8.7%, 8.4%, or 8-9%.

[0020] The cellulose ether composite additive for putty mortar described in this invention also includes 4% starch ether. In this invention, the starch ether is 301-hydroxypropyl starch ether, which has thickening, water-retaining, and anti-sagging properties.

[0021] The cellulose ether composite additive for putty mortar described in this invention also includes 2% redispersible latex powder. In this invention, the redispersible latex powder is Wacker 5010N redispersible latex powder, which is a white powder copolymerized from vinyl acetate and ethylene. It can be redispersed in water and can improve the bonding strength, flexural strength, and workability of the mortar.

[0022] The cellulose ether composite additive for putty mortar described in this invention also includes 2% polyacrylamide. In this invention, the polyacrylamide is a nonionic NPAM, which is a water-soluble polymer and can act as a thickener, water retainer, and flocculator.

[0023] This invention also provides a method for preparing the above-mentioned cellulose ether composite additive for putty mortar, comprising the following steps: S1, weigh out 92% hydroxypropyl methylcellulose, 4% starch ether, 2% redispersible latex powder, and 2% polyacrylamide by mass percentage; S2, Place the weighed raw materials into a mixer and mix them at room temperature for 20-40 minutes at a speed of 20-30 rpm. S3, after mixing evenly until the appearance and color are consistent and there are no lumps, is discharged to obtain the cellulose ether composite additive for putty mortar.

[0024] Preferably, the mixing time is 30 min and the mixing speed is 24 rpm.

[0025] Preferably, the mixer is an SFM-11 type laboratory small V-type mixer, the mixing cylinder is made of stainless steel, the rotation speed is 20~90 rpm (adjustable), and the mixing time can be set to 1~999 minutes.

[0026] The present invention also provides an application of the above-mentioned cellulose ether composite additive for putty mortar in putty or premixed mortar.

[0027] Compared with existing technologies, this invention provides a cellulose ether composite additive for putty mortar, comprising 92% hydroxypropyl methylcellulose (HPMC), 4% starch ether, 2% redispersible latex powder, and 2% polyacrylamide; wherein the HPMC has a methoxy group content of 19-22% and a hydroxypropoxy group content of 8-9%. Under fixed raw material ratios and low dosage conditions, this invention, by selecting HPMC with a methoxy group content of 19%-22% and a hydroxypropoxy group content of 8%-9%, and combining it with a small amount of functional additives, prepares a cellulose ether composite additive for putty mortar that possesses excellent water retention, good workability, and qualified bonding strength. The methoxy group content of HPMC is the main control variable, playing a decisive role in the gel temperature and water retention performance of HPMC; the hydroxypropoxy group content fluctuates normally with the production process, and in this invention, it is maintained within the conventional range of 8%-9%. By controlling the methoxy group content within this specific range, HPMC can have a higher gel temperature, thereby maintaining a stable water-retaining network under high-temperature environments.

[0028] To further understand the present invention, the following embodiments illustrate the cellulose ether composite additive for putty mortar and its preparation method provided by the present invention. The scope of protection of the present invention is not limited by the following embodiments.

[0029] Examples and Comparative Examples Example 1 HPMC with a methoxy group content of 19.1% and a hydroxypropoxy group content of 8.3% was selected. The following raw materials were weighed by mass percentage: HPMC 92%, 301 hydroxypropyl starch ether 4%, Wacker 5010N redispersible latex powder 2%, and nonionic NPAM polyacrylamide 2%. The above raw materials were placed in an SFM-11V mixer and mixed at room temperature for 30 minutes at a mixing speed of 24 rpm to obtain the cellulose ether composite additive for putty mortar.

[0030] Example 2 The only difference from Example 1 is that the selected HPMC has a methoxy content of 19.8% and a hydroxypropoxy content of 8.7%. The other raw material types, ratios, and mixing conditions are the same as in Example 1.

[0031] Example 3 The only difference from Example 1 is that the selected HPMC has a methoxy content of 21.3% and a hydroxypropoxy content of 8.4%. All other raw material types, ratios, and mixing conditions are the same as in Example 1.

[0032] Comparative Example 1 The difference from Example 1 is that the selected HPMC has a methoxy content of 22.7% and a hydroxypropoxy content of 7.9%; the compounding ratio is 88% HPMC, 4% starch ether, 2% redispersible latex powder, 4% polyacrylamide, and an additional 2% retarder. The mixing conditions are the same as in Example 1.

[0033] Performance testing The composite additives prepared in Examples 1-3 and Comparative Example 1 were added to putty and mortar matrices in the same dosage, and their performance was tested according to the following method.

[0034] (1) Water retention performance test The water retention of putty was tested according to JG / T 298-2010 "Putty for Interior Building Use"; the water retention of mortar was tested according to Appendix C of GB / T 25181-2019 "Premixed Mortar", using the filter paper method to test the water retention rate at the corresponding temperatures. The test results of water retention performance at room temperature (25℃) and extreme environments (-5℃, 40℃) are shown in Table 1 and Table 2, respectively.

[0035] Table 1. Water retention capacity (%) at room temperature Table 2 Water retention capacity under extreme environments (%) As shown in Tables 1 and 2, the HPMC used in Examples 1-3 had a methoxyl content ranging from 19% to 22% (19.1%, 19.8%, and 21.3%, respectively) and a hydroxypropoxyl content ranging from 8% to 9% (8.3%, 8.7%, and 8.4%, respectively). Under the same raw material ratio and mixing conditions, Examples 1-3 exhibited excellent water retention performance under both room temperature and extreme high and low temperature environments. Compared with Comparative Example 1, the water retention rate of mortar in Examples 1-3 increased by 2.7 to 9.1 percentage points, and the water retention rate of putty increased by 4.8 to 9.0 percentage points. Especially under the high temperature condition of 40 ℃, the water retention performance of Comparative Example 1, due to the use of HPMC with a high methoxyl content (22.7%) and the addition of a retarder, decreased significantly, while Examples 1-3 still maintained a high water retention rate. This indicates that HPMC with a low methoxyl content has a higher gelation temperature, which can effectively delay thermal gelation and maintain the stability of the water-retaining network under high temperature conditions.

[0036] (2) Putty workability test The workability time of the putty under standard and extreme temperature conditions was tested according to JG / T 298-2010 "Putty for Interior Building Use". The test results are shown in Table 3.

[0037] Table 3. Putty workability time (h) As shown in Table 3, under the condition of a fixed formula ratio, the HPMC selected in Examples 1-3 all had methoxyl content within a specific range of 19%-22% (19.1%, 19.8%, and 21.3%, respectively). Their workability under each temperature condition was significantly better than that of Comparative Example 1, which had a methoxyl content of 22.7%. At a high temperature of 40℃, the workability of Example 2 reached 3.4 hours, a 36.0% extension compared to Comparative Example 1. This indicates that HPMC with a methoxyl content within the range of 19%-22% synergistically works with a small amount of functional additives under a fixed ratio, exhibiting a good retarding effect at high temperatures and effectively extending the working window.

[0038] (3) Mortar consistency loss test According to Appendix A of GB / T 25181-2019 "Premixed Mortar", the initial consistency (cone depth in mm) was first measured using a cone penetration tester (standard cone), and then the cone depth was measured after standing for 1 h and 2 h respectively. The loss rate was calculated according to the formula. The test results are shown in Table 4.

[0039] Table 4 Mortar Consistency Loss (%) As shown in Table 4, under a fixed formulation system, the HPMC used in Examples 1-3 had a methoxyl content ranging from 19% to 22%. Comparative Example 1, with a methoxyl content exceeding this range (22.7%), exhibited significantly higher mortar consistency loss rates under various temperature conditions compared to the examples. At a high temperature of 40℃, Example 2 showed a consistency loss rate of only 2.68% over 2 hours, while Comparative Example 1 reached 5.24%. This demonstrates that by selecting HPMC with a methoxyl content ranging from 19% to 22%, the present invention, under fixed proportions and low dosage conditions, can effectively suppress mortar consistency loss under high-temperature conditions and improve workability.

[0040] (4) Bond strength test The bonding strength of the putty was determined according to the bonding strength test method in JG / T 298-2010 "Putty for Interior Use in Buildings"; the bonding strength of the mortar was determined according to the tensile bond strength test method in JGJ / T 70-2009 "Standard for Test Methods of Basic Performance of Building Mortar". The test results are shown in Table 5.

[0041] Table 5 Bond strength (MPa): As shown in Table 5, the bonding strength of putty and mortar slightly decreased with the reduction of HPMC methoxyl content. However, the putty bonding strength of Examples 1-3 all met the requirement of not less than 0.5 MPa in JG / T 298-2010, and the mortar strength also approached or reached the engineering application standard. Combining the test results of water retention, workability, and consistency loss, it can be seen that with a fixed ratio of 92% HPMC, 4% starch ether, 2% redispersible latex powder, and 2% polyacrylamide, by selecting HPMC with a methoxyl content of 19-22%, the strength can be maintained at the industry standard qualification level while significantly improving the water retention performance and workability of the composite additive under extreme temperatures, and effectively reducing raw material costs.

[0042] In summary, this invention, under conditions of fixed raw material ratios and low admixture, utilizes HPMC with a methoxyl content of 19%–22% and a hydroxypropoxyl content of 8%–9%, ​​combined with a small amount of functional additives, to prepare a cellulose ether composite additive for putty mortar that possesses excellent water retention, good workability, and satisfactory bond strength. The methoxyl content is the main control variable, while the hydroxypropoxyl content fluctuates normally with the production process, remaining within the conventional range of 8%–9%. By controlling the methoxyl content within this specific range, the water retention and workability of the composite additive can be significantly improved under extreme temperatures while maintaining bond strength that meets industry standards. This allows for wide application in building putty and premixed mortar fields.

[0043] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A cellulose ether composite additive for putty mortars, characterized by: Including the following percentages by weight of raw materials: Hydroxypropyl methylcellulose 92%, starch ether 4%, redispersible latex powder 2%, polyacrylamide 2%; The methoxy group content in the hydroxypropyl methylcellulose is 19-22%, and the hydroxypropoxy group content in the hydroxypropyl methylcellulose is 8-9%.

2. The cellulose ether composite additive for putty mortar according to claim 1, characterized in that: The methoxy group content in the hydroxypropyl methylcellulose is 19.1% to 21.3%.

3. The cellulose ether composite additive for putty mortar according to claim 1, characterized in that: The starch ether is 301-hydroxypropyl starch ether.

4. The cellulose ether composite additive for putty mortar according to claim 1, characterized in that: The redispersible latex powder is Wacker 5010N.

5. The cellulose ether composite additive for putty mortar according to claim 1, characterized in that: The polyacrylamide is a nonionic NPAM.

6. A method for preparing a cellulose ether composite additive for spackling mortar according to any one of claims 1 to 5, characterized in that: Includes the following steps: S1, weigh out 92% hydroxypropyl methylcellulose, 4% starch ether, 2% redispersible latex powder, and 2% polyacrylamide by mass percentage; S2, Place the weighed raw materials into a mixer and mix them at room temperature for 20-40 minutes at a speed of 20-30 rpm. S3, after being mixed evenly, is discharged to obtain the cellulose ether composite additive for putty mortar.

7. The method for preparing a cellulose ether composite additive for putty mortar according to claim 6, characterized in that: In step S2, the mixing time is 30 minutes and the mixer speed is 24 rpm.

8. The preparation method of the cellulose ether composite additive for putty mortar according to claim 6, characterized in that: The mixer is a V-type mixer.