A phase change coating for rails and its preparation method

By combining double-layer wall material phase change microcapsule coating with reflective-radiative cooling, the problems of single temperature control and complicated construction of rails are solved, achieving multiple temperature control effects and improved weather resistance, and simplifying the construction process.

CN123107500APending Publication Date: 2026-11-17ZHENGZHOU UOBOC NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611589290.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing rail cooling coatings have a single temperature control mode, poor weather resistance, and require rust removal and primer application during on-site construction, which is complicated and results in low efficiency during skylight operations.

Method used

The coating uses a double-layer wall material phase change microcapsule coating, which combines rutile titanium dioxide to reflect sunlight and nano-modified sodium lanthanum molybdate to provide infrared radiation cooling. It also incorporates phytic acid-imidazolium compound to achieve in-situ rust prevention and mechanical anchoring, eliminating the need for primer application.

Benefits of technology

It achieves multiple coordinated temperature control, reduces rail temperature by 10~15℃, improves weather resistance, simplifies construction procedures, and is suitable for rail service conditions with strong ultraviolet radiation and large temperature differences between day and night.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of rail coating technology, specifically to a rail phase change coating and its preparation method. The coating of this invention is a two-component polyurethane-organosilicon-fluorine modified phenol-oxygen hybrid system. Component A contains resin, phytic acid-imidazolium metal passivation complexing agent, and organosilicon modified wetting and anchoring agent; component B is a curing and crosslinking component. The core is a double-layer wall material phase change microcapsule, combined with rutile titanium dioxide solar reflection and nano-modified sodium lanthanum molybdate infrared radiation cooling to achieve triple synergistic temperature control. This invention's coating can be applied directly after degreasing and derusting, without the need for a primer; the microcapsule's double-layer wall is covalently bonded, resistant to thermal cycling, and exhibits excellent UV aging performance; it can lower the rail web temperature by 10-15°C, reducing rail temperature compressive stress, suppressing the risk of rail buckling and runaway, suitable for rapid operation during railway nighttime maintenance windows, and suitable for long-term outdoor use of rails.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of rail coating technology, specifically to a rail phase change coating and its preparation method. Background Technology

[0002] Steel rails are exposed to the open environment for extended periods, and due to solar radiation and the alternating day and night cycles, the temperature of the rail web can rise rapidly to 60-70°C. This heat generates enormous thermal stress in the rails, easily leading to major track safety hazards such as rail buckling and runaway. Currently, railways mainly rely on manual inspections and temperature monitoring to control defects, which is a passive approach and insufficient to curb rail temperature rise at its source. Using cooling coatings to passively control the temperature of the rail web is an important technological direction for reducing peak rail temperatures and alleviating thermal stress.

[0003] Most existing rail cooling coatings rely on a single solar radiation reflection mechanism for cooling, resulting in a relatively simple functional mode. They only reduce heat input through reflected radiation and lack multiple coordinated control methods for heat absorption buffering and outward radiation heat dissipation, thus limiting the overall cooling effect. At the same time, the outdoor environment where rails are located has strong ultraviolet radiation and drastic temperature differences between day and night. After long-term service, ordinary cooling coatings are prone to aging, chalking, and cracking, and their protective and temperature control performance deteriorates rapidly, making it difficult to meet the requirements for long-term stable use of railway lines.

[0004] In addition, the surface of the rails on site generally has floating rust and micro-rust layers. Most existing coating systems require rust removal and primer application. However, railway lines only have a short window of opportunity for track maintenance at night. The degreasing, rust removal, and multi-coating process is cumbersome and inefficient. Therefore, developing a rail-specific coating with multiple temperature control effects, excellent weather resistance, and the ability to be applied directly after degreasing and rust removal is a practical engineering requirement for ensuring the safety of track operation. Summary of the Invention

[0005] The purpose of this invention is to provide a rail phase change coating and its preparation method, so as to solve the problems of existing rail cooling coatings having a single temperature control mode, poor weather resistance, and requiring rust removal and primer application for on-site construction, which are complicated and have low efficiency during skylight operations.

[0006] To achieve the above objectives, the present invention adopts the following technical solution: a rail phase change coating, comprising component A and component B; Component A comprises resin, pigments, fillers, and functional additives; component B is a curing and crosslinking component. By weight: Component A: 24-34 parts of fluorinated modified phenolic resin, 7-13 parts of methyl phenyl siloxane oligomer, 3-7 parts of monoepoxy isobutyl glycidyl ether reactive diluent, 0.1-0.3 parts of epoxy ring-opening catalyst, 1.2-2.2 parts of phytic acid-imidazolium compound, 0.8-1.6 parts of organosilicon modified polymer wetting and anchoring agent, 0.4-0.8 parts of polyolefin wax powder, 1.0-2.0 parts of dispersant, 0.3-0.9 parts of defoamer, 0.4-1.1 parts of leveling agent, and 0.3-0.5 parts of activated 4Å molecular sieve powder; Component B: 19-27 parts of isocyanate-terminated aminosilane composite curing agent, 6-10 parts of phenylsiloxane crosslinking prepolymer; The total amount of functional fillers added is 38-56 parts; of which, 23-33 parts are double-wall material phase change microcapsules, 11-19 parts are radiation-reflective refrigeration composite pigments and fillers, and 4-6 parts are auxiliary fillers. The pH of component A is controlled at 6.0~7.2 using an organic amine regulator, and the total hydroxyl content of component A to the equivalent of -NCO in component B is 1:0.95~1.15.

[0007] Furthermore, the preparation method of the phytic acid-imidazolium complex is as follows: 50-70 wt% phytic acid was slowly added dropwise to a 2-methylimidazolium ethanol solution and stirred to complex; the molar ratio of phytic acid to 2-methylimidazolium was 1:6-8; ethanol and free water were removed by vacuum distillation, and the mixture was dried under vacuum and pulverized through a 300-400 mesh sieve.

[0008] Furthermore, the double-walled phase change microcapsule comprises, from the inside out, a phase change energy storage core sphere, an inner high-elastic polyurethane-hybrid siloxane buffer wall layer, and an outer fluorine-modified phenoloxy-phenyl siloxane dense weather-resistant protective wall layer; the inner and outer wall layers are bonded by siloxane condensation to form Si-O-Si covalent bonds. By weight, the raw materials for the double-wall phase change microcapsules include: 63-73 parts of core material, 2.5-5.0 parts of core material modifying agent, 1.8-3.6 parts of spherical alumina nanoparticles, 8-14 parts of inner wall material, and 12-18 parts of outer wall material.

[0009] Furthermore, the core material is a compound of heptadecane, octadecane, and eicosane; the mass ratio of heptadecane:octadecane:eicosane is (26~36):(41~51):(14~24); the phase change temperature range is 44~64℃, and the latent heat of phase change is 165~186J / g.

[0010] Furthermore, the core material modifying agent includes 1.8 to 3.0 parts of methylphenyl silicone oil, 0.6 to 1.1 parts of γ-mercaptopropyltrimethoxysilane, and 0.9 to 2.0 parts of organically modified nano-montmorillonite.

[0011] Furthermore, the inner high-elastic polyurethane-hybrid siloxane buffer wall layer raw material includes 5-8 parts of toluene diisocyanate modified polyether polyol, 2-4 parts of aminopropyltriethoxysilane, and 0.9-1.9 parts of fumed silica. The outer fluorine-modified phenolic-phenylsiloxane dense weather-resistant protective wall layer raw materials include 7-11 parts of fluorine-modified phenolic resin, 3-5 parts of phenylsiloxane crosslinked prepolymer, 1.0-2.6 parts of nano-kaolin, and 0.9-1.9 parts of cerium-doped nano-titanium dioxide.

[0012] Furthermore, the radiation-reflective cooling composite pigment and filler comprises, by weight, 5-10 parts of rutile titanium dioxide, 2-4 parts of nano-modified sodium lanthanum molybdate, and 3-5 parts of flaky barite powder.

[0013] Furthermore, the auxiliary filler comprises, by weight, 1-2 parts of fumed silica and 3-4 parts of precipitated barium sulfate.

[0014] The preparation method of the above-mentioned bilayer wall material phase change microcapsules includes the following steps: S11. Heptadecane, octadecane, and eicosane are heated and melted, core material modifiers are added and stirred, and then spherical alumina nanoparticles are added and sheared at high speed to obtain the modified phase change core material oil phase. S12. Prepare an aqueous phase containing styrene-maleic anhydride copolymer emulsifier, and adjust the pH to 4.5~5.5; add the oil phase to the aqueous phase, homogenize and emulsify at high speed to obtain an O / W emulsion; S13, emulsion insulation, toluene diisocyanate modified polyether polyol and aminopropyltriethoxysilane are added dropwise, the reaction is heated and then fumed silica is added and stirred to complete the polymerization of the inner wall material and obtain the microcapsule intermediate; S14. Filter and wash the S13 microcapsule intermediate to separate the aqueous phase; then transfer it to an anhydrous low-polarity organic solvent dispersion system, heat the system and add a mixture of fluorine-modified phenolic resin and phenylsiloxane crosslinked prepolymer dropwise, then add nano-kaolin and cerium-doped nano-titanium dioxide; adjust the system to be weakly acidic, keep the reaction at the temperature, and the inner and outer wall layers undergo siloxane condensation to form Si-O-Si covalent bonds; S15. Cooling, filtering, washing, vacuum drying, and sieving to obtain the finished product of double-walled phase change microcapsules.

[0015] The method for preparing rail phase change coatings using the above-mentioned double-walled phase change microcapsules includes the preparation of component A and component B. Preparation steps for component A: S21, activated 4Å molecular sieve powder is pre-dispersed in methylphenylsiloxane oligomer to prepare a dispersion mother liquor; S22. Fluorine-modified phenolic resin, S11 dispersion mother liquor, and monoepoxy isobutyl glycidyl ether reactive diluent are mixed and stirred at low speed to obtain the resin matrix. S23. Add phytic acid-imidazolium complex, epoxy ring-opening catalyst, organosilicon modified polymer wetting and anchoring agent, dispersant, defoamer, and leveling agent to the S12 resin matrix, stir and disperse, and adjust the pH to 6.0~7.2 with organic amine. S24. Add radiation-reflective cooling composite pigments and fillers, and auxiliary fillers, and disperse at high speed; add double-layer wall material phase change microcapsules under low-speed stirring, and filter and package to obtain component A; Preparation steps for component B: S31. Under dry nitrogen protection conditions, add isocyanate-terminated aminosilane composite curing agent, add phenylsiloxane crosslinking prepolymer, stir and mix evenly, detect the -NCO content, seal and package to obtain component B.

[0016] The beneficial effects of this invention are: 1. The microcapsule wall material of this invention adopts a polyurethane-hybrid siloxane high-elasticity buffer wall layer, which absorbs the volume expansion and contraction of phase change by relying on the high elongation of polyurethane segments; a fluorine-modified phenoloxy-phenylsiloxane dense weather-resistant protective wall layer is adopted; covalent bonds are formed between the inner and outer layers by siloxane condensation, which reduces the risk of interlayer delamination under thermal cycling conditions; fluorine segments and cerium-doped titanium oxide ultraviolet shielding components are introduced into the outer layer, which is suitable for the service conditions of steel rails exposed to strong ultraviolet rays and large temperature difference between day and night.

[0017] 2. Component A of this invention introduces a phytic acid-imidazolium metal passivation complexing agent and an organosilicon-modified polymer wetting and anchoring agent; on the one hand, it generates an iron phytic acid passivation film in situ on the rail surface to achieve in-situ rust prevention; on the other hand, it reduces interfacial tension, and the resin wets the micro-unevenness of the rail, forming mechanical anchoring after curing; after degreasing and rust removal, it can be painted directly, eliminating the need for the primer application window, reducing on-site construction procedures, and avoiding the disadvantages of short nighttime window periods for railways.

[0018] 3. This invention employs a triple synergistic temperature control system: rutile titanium dioxide reflects sunlight, reducing heat input; double-layer wall material phase change microcapsules absorb peak heat in the rail's 44-64℃ temperature range by relying on the latent heat of solid-liquid phase change, smoothing out temperature peaks; and nano-modified sodium lanthanum molybdate utilizes an 8-13μm atmospheric window to achieve infrared radiation cooling, dissipating heat into outer space. The three elements work synergistically to lower the rail temperature by 10-15℃, reducing thermal stress on the rail and mitigating the risk of track bulging. Detailed Implementation

[0019] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments of the present invention.

[0020] The coating of this invention is a two-component polyurethane-organosilicon-fluorine modified phenol-oxygen hybrid system; A is a resin + pigment, filler + functional additive component, and B is a curing and crosslinking component; the core functional unit is a double-layer wall material phase change microcapsule, which realizes phase change heat storage and peak reduction; combined with solar light reflection + 8~13μm atmospheric window infrared radiation filler, it achieves triple temperature control; the matching passivation-anchoring additive can be directly applied to the surface of the rail web substrate after degreasing and removing oil and rust.

[0021] The raw materials of this invention, by mass parts: Component A: 24-34 parts of fluorinated modified phenolic resin, 7-13 parts of methylphenylsiloxane oligomer, 3-7 parts of monoepoxy isobutyl glycidyl ether reactive diluent; 0.1-0.3 parts of epoxy ring-opening catalyst; 1.2-2.2 parts of metal passivation complexing agent (phytic acid-imidazolium compound); 0.8-1.6 parts of substrate wetting and anchoring agent (organosilicon modified polymer wetting agent); 0.4-0.8 parts of polyolefin wax powder; 1.0-2.0 parts of dispersant; 0.3-0.9 parts of defoamer; 0.4-1.1 parts of leveling agent; 0.3-0.5 parts of activated 4Å molecular sieve powder; Component B: 19-27 parts of isocyanate-terminated aminosilane composite curing agent; 6-10 parts of phenylsiloxane crosslinked prepolymer; The total amount of functional fillers added is 38-56 parts; of which, 23-33 parts are double-wall material phase change microcapsules; 11-19 parts are radiation-reflective refrigeration composite pigments and fillers; and 4-6 parts are auxiliary fillers.

[0022] Fluorine-modified phenolic resin: The phenolic resin main link is branched with fluorine segments, which combines the adhesion and toughness of phenolic resin with the UV and weather resistance of CF bonds. As the main body for film formation, it undergoes urethane cross-linking with the isocyanate component B to construct a continuous phase of the paint film. At the same time, the fluorine segments endow the paint film with UV resistance and water vapor corrosion resistance, making it suitable for outdoor service of steel rails. The phenoxy polar groups enhance the intrinsic adhesion to metal steel rails.

[0023] Methylphenylsiloxane oligomers: Low molecular weight prepolymers of siloxanes containing methyl and phenyl side groups, with reactive silanol groups, introducing Si-O inorganic segments to improve the temperature resistance, hydrolysis resistance, and weather resistance of the paint film; the phenyl groups improve compatibility with organic resins and prevent siloxane precipitation and delamination; the silanol groups can participate in the cross-linking of the system to improve the density of the paint film.

[0024] Mono-epoxy isobutyl glycidyl ether reactive diluent: A mono-epoxy functional group reactive diluent, a non-inert solvent, participates in the cross-linking reaction, reduces the viscosity of component A system, improves the rheological properties of spraying / brushing during construction, and does not introduce volatile organic solvents; the epoxy groups of this component undergo a ring-opening reaction within the system to generate hydroxyl groups, which then undergo a cross-linking reaction with isocyanate of component B and are integrated into the paint film network, avoiding the residual seepage of small molecule diluents and ensuring the water and salt spray resistance of the paint film.

[0025] Epoxy ring-opening catalyst: Tris(dimethylaminomethyl)phenol is used to catalyze the ring-opening of the epoxy group of monoepoxy isobutyl glycidyl ether to generate hydroxyl groups under room temperature conditions. The hydroxyl groups generated by ring opening further undergo cross-linking reaction with component B isocyanate, avoiding the residue of unreacted small molecule diluent.

[0026] Metal passivation complexing agent: Phytic acid molecules contain polyhydroxy phosphate groups, which react with iron atoms on the surface of the rail to form a dense, insoluble phytic acid iron passivation film on the surface of slightly rusted and oxidized rails; imidazole synergistically accelerates the complexation film formation, providing in-situ passivation and rust prevention for the rail substrate and inhibiting further corrosion of the substrate.

[0027] Phytic acid (50-70 wt.%) was slowly added dropwise to a 2-methylimidazole ethanol solution, and the mixture was stirred to neutralize and complex. The molar ratio of phytic acid to 2-methylimidazole was 1:6-8. All ethanol and free water in the reaction system were removed by vacuum distillation to obtain a viscous phytic acid-imidazole complex salt product. After vacuum drying, pulverizing and grinding, the product was passed through a 300-400 mesh sieve to obtain the phytic acid-imidazole complex.

[0028] Organosilicon-modified polymer substrate wetting and anchoring agent: a polymer wetting agent with organosilicon side chains linked to a polymer main link, which is different from ordinary small molecule organosilicon leveling agents; its function is to reduce the interfacial tension between the coating and the rail metal, promote the resin to fully wet the micro-uneven and rough surface of the rail, and enable the resin to penetrate into the micro-pores on the rail surface. After the resin cures, it forms a mechanical anchoring structure, thereby improving the adhesion of the coating film to the surface of the rail substrate.

[0029] Polyolefin wax powder: improves the anti-dust properties of the paint film and further inhibits the migration and precipitation of small molecules of the phase change core material to the paint film surface.

[0030] Dispersant: Polymer pigment dispersant (polyacrylate) coats the surface of inorganic fillers and microcapsules to prevent filler agglomeration and sedimentation, and ensures uniform dispersion of fillers in the resin matrix.

[0031] Defoamer: Organosilicon defoamer eliminates air bubbles introduced during paint mixing and spraying, avoids pinholes and air bubble defects in the paint film, and ensures the integrity of the paint film.

[0032] Leveling agent: Polyacrylate / silicone leveling agent, improves the leveling of the paint film after construction, eliminates brush marks and orange peel, and forms a continuous and smooth paint film.

[0033] Activated 4Å molecular sieve powder: High-temperature activated 4Å zeolite molecular sieve powder, after removing crystal water, is used to adsorb trace amounts of free water inside component A, alleviating the problem of side reactions between water and isocyanate in component B to generate CO2 bubbles, and improving the storage and construction stability of the system; the activated 4Å molecular sieve powder is pre-dispersed in methylphenylsiloxane oligomer to prepare a dispersion mother liquor, avoiding direct feeding and agglomeration of the powder.

[0034] pH control: The phytic acid-imidazolium complex is an acidic complex salt. A trace amount of organic amine (N-methyldiethanolamine) is used as an adjuster to control the pH of component A to 6.0~7.2, which inhibits the premature self-polymerization and ring-opening of epoxy groups during the storage of component A and ensures the storage stability of the coating. The phytic acid-imidazolium complex can still dissociate at the metal interface on the surface of the rail substrate and generate an iron phytate passivation film in situ.

[0035] Isocyanate-terminated aminosilane composite curing agent: The active amino groups of aminosilane molecules react with excess isocyanate to obtain a composite curing agent with -NCO-terminated groups carrying siloxane groups. The -NCO groups react with the hydroxyl groups of component A resin and the ring-opening hydroxyl groups of diluent epoxy to form a polyurethane crosslinking reaction, thus constructing the main crosslinking network of the paint film. The molecule itself carries hydrolyzable siloxane groups, which on the one hand enhance the bonding of the paint film to the rail interface, and on the other hand can condense with the siloxane components of the system to further improve the crosslinking density, water resistance and salt spray resistance of the paint film.

[0036] Phenylsiloxane crosslinking prepolymer: Phenylsiloxane oligomer prepolymer with silanol groups. The silanol groups can undergo siloxane condensation to form Si-O-Si inorganic crosslinking points, which improve the heat resistance, UV resistance and water vapor and oxygen barrier of the paint film; the phenyl groups improve the compatibility with organic phase and prevent silicon phase precipitation.

[0037] The dual-layer phase change microcapsule has the following structural layers from the inside out: phase change energy storage core sphere → inner layer of high-elastic polyurethane-hybrid siloxane buffer wall layer → outer layer of fluorine-modified phenoloxy-phenylsiloxane dense weather-resistant protective wall layer.

[0038] Double-wall phase change microcapsules (raw material weight parts): core material 63~73 parts; core material modifying agent 2.5~5.0 parts; spherical alumina nanoparticles 1.8~3.6 parts; inner wall material 8~14 parts; outer wall material 12~18 parts.

[0039] Core material: The core material is a compound of heptadecane, octadecane, and eicosane; the mass ratio of heptadecane:octadecane:eicosane is (26~36):(41~51):(14~24); the phase change temperature range is 44~64℃, and the latent heat of phase change is 165~186J / g.

[0040] The combination of three n-alkanes broadens the phase transition temperature range, matching the actual high temperature range of 45~65℃ for rails in summer. When the rail temperature rises and enters the phase transition range, the alkanes undergo a solid-liquid phase transition, absorbing a large amount of ambient heat and storing it as latent heat, thus inhibiting the rail temperature from rising further. At low temperatures, they recrystallize and release heat, buffering the sudden cooling of the rail and reducing the temperature fluctuation range between day and night.

[0041] Core material modifying additives: 1.8-3.0 parts of methylphenyl silicone oil; 0.6-1.1 parts of γ-mercaptopropyltrimethoxysilane; 0.9-2.0 parts of organically modified nano-montmorillonite.

[0042] Methylphenyl silicone oil improves the interfacial compatibility between alkane core and wall materials, reducing the tendency of core material migration; γ-mercaptopropyltrimethoxysilane acts as an interfacial coupling agent, building a chemical bond interface between inorganic alumina, montmorillonite and organic alkanes; organically modified nano-montmorillonite sheets are dispersed inside the core material, forming a labyrinthine barrier path, further inhibiting the outward permeation of the molten core material.

[0043] Spherical alumina nanoparticles: Spherical alumina nanoparticles are insulating and highly thermally conductive inorganic fillers (particle size 300~500nm). They are uniformly dispersed inside the phase change core material, which improves the thermal conductivity of the core material, accelerates the phase change heat absorption / release response speed, avoids local heat accumulation inside the microcapsules, and improves the overall heat exchange efficiency.

[0044] Inner layer high-elastic polyurethane-hybrid siloxane buffer wall layer: 5-8 parts of toluene diisocyanate modified polyether polyol; 2-4 parts of aminopropyltriethoxysilane; 0.9-1.9 parts of fumed silica.

[0045] The inner wall material adopts a polyurethane-siloxane hybrid system; the polyurethane segments have high elasticity and high elongation at break, which can tolerate the volume expansion caused by the solid-liquid phase change of the core material (the volume change of alkane phase change is about 10~13%), and absorb internal stress through elastic deformation to prevent the shell from cracking directly; aminopropyltriethoxysilane is introduced into the siloxane segments to improve the hydrolysis resistance of the inner wall material, and at the same time builds a silicon oxide chemical bonding interface with the outer wall material to improve the interfacial bonding force between the inner and outer wall materials and prevent interlayer delamination; fumed silica adjusts the viscosity and mechanical strength of the wall material to prevent the wall material from being too soft and creeping.

[0046] Outer fluorine-modified phenolic-phenylsiloxane dense weather-resistant protective wall layer: 7-11 parts of fluorine-modified phenolic resin; 3-5 parts of phenylsiloxane crosslinked prepolymer; 1.0-2.6 parts of nano-kaolin; 0.9-1.9 parts of cerium-doped nano-titanium dioxide.

[0047] The outer wall material is made of fluorinated modified phenolic resin with high CF bond energy, which resists UV free radical attack and significantly improves outdoor weather resistance. The phenylsiloxane prepolymer cross-links to form a dense silicon-oxygen network, blocking water vapor and oxygen from penetrating into the bladder. The nano-kaolin sheet filler forms a labyrinth barrier structure to reduce the medium permeation rate. Cerium-doped nano-titanium dioxide acts as a UV shielding agent, absorbing and scattering UV photons to protect the inner layer and core material from photo-oxidative degradation. The inner and outer layers are bonded by Si-O-Si covalent bonds formed by the condensation of silane components, resulting in a strong interlayer bond that prevents double-layer delamination under thermal cycling conditions.

[0048] Cerium-doped nano-titanium dioxide: Tetrabutyl titanate was dissolved in anhydrous ethanol and acetylacetone was added to inhibit hydrolysis to obtain solution A. Cerium nitrate was dissolved in a deionized water / ethanol mixture and the pH was adjusted with nitric acid to obtain solution B. Solution B was slowly added dropwise to solution A with stirring, and the molar ratio of cerium to titanium was controlled at 0.5%~5%. The deionized water / ethanol mixture was added dropwise to promote hydrolysis and condensation to form Ce-doped TiO2 gel. The gel was dried at 80~100℃ to obtain dry gel powder, and calcined at 400~600℃ for 2~4 hours to allow Ce to condense. 3+ / Ce 4+ After entering the TiO2 surface and near-surface lattice, the calcined product is subjected to sand milling and ball milling to deagglomerate it. The powder D50 is controlled to be less than 500 nm, and it is passed through a 200-300 mesh sieve to obtain cerium-doped nano titanium dioxide powder.

[0049] Radiation-reflective cooling composite pigments and fillers (parts by weight of raw materials): 5-10 parts rutile titanium dioxide; 2-4 parts nano-modified sodium lanthanum molybdate; 3-5 parts flaky barite powder.

[0050] Rutile titanium dioxide has high reflectivity to visible and near-infrared sunlight, reducing the heat input of solar radiation received by the rails; nano-modified sodium lanthanum molybdate has a high hemispherical emissivity in the 8~13μm "atmospheric window", radiating the heat accumulated in the rails to the cosmic cold source in the form of infrared radiation, realizing radiative cooling; the stacked layers of platy barite extend the water and oxygen penetration path, improve the barrier properties of the paint film, and at the same time enhance the resistance to wind and sand erosion and wear resistance.

[0051] Auxiliary fillers (parts by weight of raw materials): 1-2 parts of fumed silica; 3-4 parts of precipitated barium sulfate.

[0052] Fumed silica provides thixotropic properties, preventing coatings from settling during storage and sagging during application; precipitated barium sulfate improves the hardness and abrasion resistance of the paint film, optimizing its mechanical properties.

[0053] Example 1 In this embodiment, the phase change microcapsules of the double-walled material of the present invention are prepared.

[0054] The weight percentages of each raw material are as follows: core material 68 parts (31 parts heptadecane, 46 parts octadecane, 23 parts eicosane); core material modifying agent 3.8 parts (2.4 parts methyl phenyl silicone oil, 0.8 parts γ-mercaptopropyltrimethoxysilane, 1.6 parts organically modified nano-montmorillonite); spherical alumina nanopowder 2.7 parts; inner wall material 11 parts (6.5 parts toluene diisocyanate modified polyether polyol, 3 parts aminopropyltriethoxysilane, 1.5 parts fumed silica); outer wall material 14.5 parts (9 parts fluorine-modified phenolic resin, 4 parts phenylsiloxane crosslinked prepolymer, 1.8 parts nano-kaolin, 1.7 parts cerium-doped nano-titanium dioxide).

[0055] Preparation steps: Heptadecane, octadecane, and eicosane were added to a reaction vessel, heated to 52°C and stirred until completely melted. Methylphenyl silicone oil and γ-mercaptopropyltrimethoxysilane were added and stirred for 25 minutes. Then, organically modified nano-montmorillonite and 300-500 nm spherical alumina nanoparticles were added and sheared at high speed for 40 minutes to obtain a uniform modified phase change core material oil phase.

[0056] Take deionized water, add a small amount of styrene-maleic anhydride copolymer as an emulsifier, adjust the pH of the system to 4.5-5.5, stir to dissolve, and obtain a continuous aqueous phase.

[0057] The modified phase change core material oil phase is slowly added to the aqueous phase, and high-speed homogenization emulsification is carried out at a shear speed of 8000~10000 r / min for 35 min to form an O / W stable emulsion. The emulsion droplet size is controlled at 15~35 μm.

[0058] Maintaining the emulsion temperature at 55°C, toluene diisocyanate-modified polyether polyol was added dropwise to the emulsion. After stirring and dispersing evenly, aminopropyltriethoxysilane was added dropwise, and the temperature was slowly raised to 62°C. The reaction was maintained at this temperature for 2.5 hours. Then, fumed silica was added, and stirring was continued for 1 hour to complete the polymerization and molding of the inner wall material, resulting in a microcapsule intermediate with an inner shell.

[0059] The microcapsule intermediate was filtered and washed with water to separate the aqueous phase. It was then transferred to a xylene dispersion system, heated to 62°C, and a pre-dissolved mixture of fluorinated modified phenolic resin and phenylsiloxane crosslinked prepolymer was added dropwise over 1.5 hours. Subsequently, nano-kaolin and cerium-doped nano-titanium dioxide powder were added, stirred and dispersed, and the system was adjusted to a weakly acidic state using glacial acetic acid to promote siloxane condensation and crosslinking. The reaction was maintained at this temperature for 3.5 hours, during which siloxane condensation occurred in the inner and outer wall layers to form Si-O-Si covalent bonds.

[0060] After the reaction was completed and cooled to room temperature, the solid particles were separated by filtration, washed, dried under vacuum at 60°C, and passed through a 200-mesh sieve to obtain the finished product of double-walled phase change microcapsules.

[0061] The resulting microcapsules have a phase transition temperature of 44~64℃ and a latent heat of phase transition of 174J / g; after 500 cycles of heating and cooling at -20~70℃, the capsule shell does not crack and there is no leakage of the core material.

[0062] Example 2 In this embodiment, the rail phase change coating of the present invention is prepared.

[0063] This embodiment uses the double-layer wall material phase change microcapsules prepared in Example 1. The components are as follows by mass: Component A: 29 parts of fluorinated modified phenolic resin, 10 parts of methylphenylsiloxane oligomer, 5 parts of monoepoxy isobutyl glycidyl ether reactive diluent; 0.2 parts of tris(dimethylaminomethyl)phenol; 1.7 parts of phytic acid-imidazolium compound; 1.2 parts of organosilicon modified polymer wetting and anchoring agent; 0.5 parts of polyolefin wax powder; 1.5 parts of polyacrylate dispersant; 0.6 parts of organosilicon defoamer; 0.7 parts of polyacrylate-organosilicon compound leveling agent; 0.4 parts of activated 4Å molecular sieve powder; A total of 47 functional fillers were used: 28 parts of the double-walled phase change microcapsules prepared in Example 1; 15 parts of radiation-reflective cooling composite pigments and fillers (7.5 parts of rutile titanium dioxide, 3 parts of nano-modified sodium lanthanum molybdate, and 4.5 parts of flake barite powder); and 4 parts of auxiliary fillers (1.5 parts of fumed silica and 2.5 parts of precipitated barium sulfate). Component B: 23 parts isocyanate-terminated aminosilane composite curing agent; 8 parts phenylsiloxane crosslinked prepolymer.

[0064] In this embodiment, the equivalent ratio of total hydroxyl groups in component A to -NCO in component B is 1:0.95~1.15.

[0065] Preparation steps: An activated 4Å molecular sieve powder was pre-dispersed in methylphenylsiloxane oligomers to prepare a dispersion mother liquor.

[0066] Fluorine-modified phenolic resin, activated 4Å molecular sieve powder-methylphenylsiloxane oligomer dispersion mother liquor, and monoepoxy isobutyl glycidyl ether reactive diluent were added to the paint mixing tank and stirred at low speed for 20 min at a speed of 300~400 r / min to obtain a homogeneous resin matrix.

[0067] Phytic acid-imidazolium complex, tris(dimethylaminomethyl)phenol, organosilicon modified polymer wetting and anchoring agent, polyolefin wax powder, dispersant, defoamer, and leveling agent were added sequentially to the resin matrix. The mixture was stirred at 500 r / min for 25 min until the additives were completely dispersed. A trace amount of organic amine regulator was used during the process to control the pH at 6.0~7.2.

[0068] First, add rutile titanium dioxide, nano-modified sodium lanthanum molybdate, flake barite powder, fumed silica, and precipitated barium sulfate. Disperse the mixture in a high-speed disperser at 800~1000 r / min for 30 min, and then mill it to a fineness ≤45 μm. After milling, cool the mixture to below 45℃, and add the double-layer wall material phase change microcapsules obtained in Example 1 under low-speed stirring. Stir at 400~500 r / min for 20 min to avoid high-speed shearing damaging the microcapsule shells. Detect the fineness and viscosity, filter and package to obtain component A.

[0069] In a dry nitrogen-protected reactor, isocyanate-terminated aminosilane composite curing agent is added, followed by phenylsiloxane crosslinking prepolymer. The mixture is stirred at 450 rpm for 30 minutes until homogeneous. The -NCO content is then measured, and the mixture is sealed and packaged to obtain component B.

[0070] During railway track maintenance, weigh and mix component A and component B at a mass ratio (A:B) of 100:31 (the equivalent ratio of total hydroxyl groups to -NCO is 1:0.95~1.15), and stir evenly. The rail web is treated with degreasing and rust removal (Sa1 grade, no thick layer, peeling, or flaky rust), and no primer is required. Apply the coating to the surface of the rail web by spraying or brushing. The ambient temperature is 20~35℃, the relative humidity is ≤65%, there is no condensation on the rail surface, the dry film thickness is controlled at 120~160μm, and it is cured at room temperature.

[0071] In this embodiment, the coating film was prepared under a solar irradiance of 1000 W / m. 2 In a windless laboratory simulation, the temperature of the rail can be reduced by 10~15℃; under experimental conditions, the paint film does not crack after 500 cycles of hot and cold cycles from -20℃ to 70℃; the adhesion of the paint film on the slightly rusted rail substrate can reach level 1, meeting the requirements for rapid construction during nighttime skylights and long-term outdoor service.

[0072] Comparative Example 1 In this comparative example, no double-wall material phase change microcapsules were added; only reflective-radiative cooling was used.

[0073] In this comparative example, the phase change microcapsules of the double-layer wall material were removed, and the corresponding mass parts were allocated to the radiation-reflective refrigeration composite pigment and filler. The radiation-reflective refrigeration composite pigment and filler was adjusted to 43 parts, while the remaining A and B components remained unchanged, which is basically the same as in Example 2. The preparation process and construction process of A and B components are exactly the same as in Example 2.

[0074] Comparative Example 2 In this comparative example, ordinary single-walled phase change microcapsules with covalently bonded double-layered shells were used.

[0075] Using the same inner wall material as in Example 1, the outer fluorine-modified phenoloxy-phenylsiloxane protective wall layer is omitted, and no outer coating is performed, only the inner polyurethane-hybrid siloxane single-layer shell is retained; the rest of the coating formulation, preparation, and application conditions are the same as in Example 2.

[0076] Comparative Example 3 No phytic acid-imidazolium metal passivation complexing agent or substrate wetting and anchoring agent was added in this comparative example.

[0077] The formula remains the same as in Example 2, except that the phytic acid-imidazolium compound and the organosilicon-modified polymer wetting and anchoring agent are removed; the other raw materials, preparation process and construction process remain unchanged; the rail substrate needs to be completely sandblasted to remove rust and coated with epoxy primer before applying this coating.

[0078] The coatings obtained in Example 2 and each comparative example were subjected to performance tests.

[0079] Test conditions: Simulated solar irradiance 1000W / m 2 The test was conducted in a windless environment; the substrate was a rail web sample with loose rust; the dry film thickness of the paint was 120~160μm; the thermal cycling conditions were -20℃ to 70℃ for 500 cycles; the temperature drop was the maximum steady-state temperature difference between the bare rail substrate and the coated sample. The test results are as follows:

[0080] The test results show that: Comparative Example 1, without phase change microcapsules, lacks a latent heat of phase change peak reduction mechanism and relies solely on reflection and infrared radiation, resulting in a significant decrease in the cooling rate. This demonstrates that the double-walled phase change microcapsules play a key peak reduction role in the triple synergistic temperature control.

[0081] Comparative Example 2 uses ordinary single-wall phase change microcapsules without bilayer covalent bonded shells. After thermal cycling, the shell cracks and leaks, and the coating bubbles and fails, verifying the necessity of the bilayer wall and interlayer Si-O-Si covalent bond structure of the present invention for resistance to thermal cycling.

[0082] In Comparative Example 3, after removing the phytic acid-imidazolium passivating complexing agent and wetting anchoring agent, the adhesion of the slightly rusted rail surface decreased to level 3, making it impossible to apply directly to the substrate. A primer must be used instead, which confirms that the additive system achieves the technical effect of in-situ passivation and rust prevention, as well as direct coating for mechanical anchoring.

[0083] This invention is not limited to the preferred embodiments described above. Anyone can derive other products in various forms under the guidance of this invention. However, regardless of any changes made in their shape or structure, any technical solution that is the same as or similar to this invention falls within the protection scope of this invention.

Claims

1. A phase change coating for steel rails, characterized in that: Includes component A and component B; Component A comprises resin, pigments, fillers, and functional additives; component B is a curing and crosslinking component. By weight: Component A: 24-34 parts of fluorinated modified phenolic resin, 7-13 parts of methyl phenyl siloxane oligomer, 3-7 parts of monoepoxy isobutyl glycidyl ether reactive diluent, 0.1-0.3 parts of epoxy ring-opening catalyst, 1.2-2.2 parts of phytic acid-imidazolium compound, 0.8-1.6 parts of organosilicon modified polymer wetting and anchoring agent, 0.4-0.8 parts of polyolefin wax powder, 1.0-2.0 parts of dispersant, 0.3-0.9 parts of defoamer, 0.4-1.1 parts of leveling agent, and 0.3-0.5 parts of activated 4Å molecular sieve powder; Component B: 19-27 parts of isocyanate-terminated aminosilane composite curing agent, 6-10 parts of phenylsiloxane crosslinking prepolymer; The total amount of functional fillers added is 38-56 parts; of which, 23-33 parts are double-wall material phase change microcapsules, 11-19 parts are radiation-reflective refrigeration composite pigments and fillers, and 4-6 parts are auxiliary fillers. The pH of component A is controlled at 6.0~7.2 using an organic amine regulator, and the total hydroxyl content of component A to the equivalent of -NCO in component B is 1:0.95~1.

15.

2. The rail phase change coating according to claim 1, characterized in that, The preparation method of the phytic acid-imidazolium complex is as follows: 50-70 wt% phytic acid was slowly added dropwise to a 2-methylimidazolium ethanol solution and stirred to complex; the molar ratio of phytic acid to 2-methylimidazolium was 1:6-8; ethanol and free water were removed by vacuum distillation, and the mixture was dried under vacuum and pulverized through a 300-400 mesh sieve.

3. The rail phase change coating according to claim 1, characterized in that: The aforementioned double-walled phase change microcapsule comprises, from the inside out, a phase change energy storage core sphere, an inner high-elastic polyurethane-hybrid siloxane buffer wall layer, and an outer fluorine-modified phenoloxy-phenyl siloxane dense weather-resistant protective wall layer; the inner and outer wall layers are bonded by siloxane condensation to form Si-O-Si covalent bonds. By weight, the raw materials for the double-wall phase change microcapsules include: 63-73 parts of core material, 2.5-5.0 parts of core material modifying agent, 1.8-3.6 parts of spherical alumina nanoparticles, 8-14 parts of inner wall material, and 12-18 parts of outer wall material.

4. The rail phase change coating according to claim 3, characterized in that: The core material is a compound of heptadecane, octadecane, and eicosane; the mass ratio of heptadecane:octadecane:eicosane is (26~36):(41~51):(14~24); the phase change temperature range is 44~64℃, and the latent heat of phase change is 165~186J / g.

5. The rail phase change coating according to claim 3, characterized in that: The core material modifying agent includes 1.8-3.0 parts of methylphenyl silicone oil, 0.6-1.1 parts of γ-mercaptopropyltrimethoxysilane, and 0.9-2.0 parts of organically modified nano-montmorillonite.

6. The rail phase change coating according to claim 3, characterized in that: The inner high-elastic polyurethane-hybrid siloxane buffer wall layer raw materials include 5-8 parts of toluene diisocyanate modified polyether polyol, 2-4 parts of aminopropyltriethoxysilane, and 0.9-1.9 parts of fumed silica. The outer fluorine-modified phenolic-phenylsiloxane dense weather-resistant protective wall layer raw materials include 7-11 parts of fluorine-modified phenolic resin, 3-5 parts of phenylsiloxane crosslinked prepolymer, 1.0-2.6 parts of nano-kaolin, and 0.9-1.9 parts of cerium-doped nano-titanium dioxide.

7. The rail phase change coating according to claim 1, characterized in that: The radiation-reflective cooling composite pigment and filler comprises, by weight, 5-10 parts of rutile titanium dioxide, 2-4 parts of nano-modified sodium lanthanum molybdate, and 3-5 parts of flaky barite powder.

8. The rail phase change coating according to claim 1, characterized in that: The auxiliary filler comprises, by weight, 1-2 parts of fumed silica and 3-4 parts of precipitated barium sulfate.

9. The method for preparing bilayer wall material phase change microcapsules according to any one of claims 1-8, characterized in that, Includes the following steps: S11. Heptadecane, octadecane, and eicosane are heated and melted, core material modifiers are added and stirred, and then spherical alumina nanoparticles are added and sheared at high speed to obtain the modified phase change core material oil phase. S12. Prepare an aqueous phase containing styrene-maleic anhydride copolymer emulsifier, and adjust the pH to 4.5~5.5; add the oil phase to the aqueous phase, homogenize and emulsify at high speed to obtain an O / W emulsion; S13, emulsion insulation, toluene diisocyanate modified polyether polyol and aminopropyltriethoxysilane are added dropwise, the reaction is heated and then fumed silica is added and stirred to complete the polymerization of the inner wall material and obtain the microcapsule intermediate; S14. Filter and wash the S13 microcapsule intermediate to separate the aqueous phase; then transfer it to an anhydrous low-polarity organic solvent dispersion system, heat and dropwise add a mixture of fluorinated modified phenolic resin and phenylsiloxane crosslinked prepolymer, then add nano-kaolin and cerium-doped nano-titanium dioxide; adjust the system to be weakly acidic, keep the reaction at a certain temperature, and the inner and outer wall layers undergo siloxane condensation to form Si-O-Si covalent bonds; S15. Cooling, filtering, washing, vacuum drying, and sieving to obtain the finished product of double-walled phase change microcapsules.

10. The method for preparing rail phase change coatings using double-layer wall material phase change microcapsules according to claim 9, characterized in that, Includes the preparation of component A and component B; Preparation steps for component A: S21, activated 4Å molecular sieve powder is pre-dispersed in methylphenylsiloxane oligomer to prepare a dispersion mother liquor; S22. Fluorine-modified phenolic resin, S11 dispersion mother liquor, and monoepoxy isobutyl glycidyl ether reactive diluent are mixed and stirred at low speed to obtain the resin matrix. S23. Add phytic acid-imidazolium complex, epoxy ring-opening catalyst, organosilicon modified polymer wetting and anchoring agent, dispersant, defoamer, and leveling agent to the S12 resin matrix, stir and disperse, and adjust the pH to 6.0~7.2 with organic amine. S24, with the addition of radiation-reflective cooling composite pigments and fillers, and auxiliary fillers, for high-speed dispersion; Add double-walled phase change microcapsules under low-speed stirring, filter and package to obtain component A; Preparation steps for component B: S31. Under dry nitrogen protection conditions, add isocyanate-terminated aminosilane composite curing agent, add phenylsiloxane crosslinking prepolymer, stir and mix evenly, detect the -NCO content, seal and package to obtain component B.