Phytic acid-based composite activator as well as preparation method and application thereof
By using composite activators prepared by phytic acid, trivalent metal hydroxide and ammonium bicarbonate, the problems of high corrosiveness and poor activation performance of activators in the traditional desulfurization process are solved, and efficient bauxite desulfurization is achieved, which improves the improvement of The quality and recovery of aluminum concentrate and sulfur concentrate are environmentally friendly and safe.
Patent Information
- Application Number
- CN202411091056.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The corrosive activators used in the desulfurization process of existing bauxite cause corrosion to the equipment, and the activation performance of high-sulfur bauxite is poor, affecting the quality of bauxite concentrate.
Using a composite activator based on phytic acid, including phytic acid, trivalent metal hydroxide and ammonium bicarbonate, it is prepared by neutralization reaction and is used for the desulfurization treatment of high-sulfur bauxite to reduce corrosion and improve activation performance.
It effectively reduces the corrosiveness of the activator, improves the activation performance of high-sulfur bauxite, significantly improves the quality of aluminum concentrate and the recovery rate of sulfur concentrate, and is environmentally friendly, safe and reliable.
Smart Images

Figure CN118925942A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of recycling and utilization of ore resources, and in particular to a phytic acid-based composite activator and a preparation method and application thereof. Background Art
[0002] Domestic bauxite is mainly diaspore-type high-sulfur bauxite. Although most of this type of bauxite has a high grade, the sulfur content of this type of bauxite is also very high. Therefore, desulfurization must be carried out before the development and utilization of this type of bauxite resources. At present, the most effective method for desulfurization is flotation. At present, traditional flotation methods generally use sulfuric acid or copper sulfate as an activator for activation.
[0003] However, sulfuric acid is a strong acid with strong corrosiveness, and copper sulfate is also corrosive to a certain extent. The corrosive activator has strong corrosion on the flotation equipment, which is easy to affect the flotation desulfurization process, thereby affecting the indicators of the bauxite concentrate after flotation treatment. When encountering high-sulfur bauxite slurry with a large amount of mud, it is difficult for the highly corrosive sulfuric acid or copper sulfate to activate this type of high-sulfur bauxite slurry, resulting in poor activation performance of this type of activator, which will affect the indicators of the bauxite concentrate after flotation treatment. Summary of the invention
[0004] The present application provides a phytic acid-based composite activator and a preparation method and application thereof, in order to solve the following technical problem: how to reduce the corrosiveness of the activator while improving the activation performance of the activator.
[0005] In a first aspect, the present application provides a phytic acid-based composite activator, wherein the raw materials of the composite activator include phytic acid, trivalent metal hydroxide and ammonium bicarbonate, and the composite activator satisfies:
[0006] (3m+n):q=12:1,
[0007] m:q=(0~4):1, and
[0008] n:q=(0~12):1,
[0009] In the formula, q is the amount of phytic acid;
[0010] m is the amount of substance of the trivalent metal hydroxide;
[0011] n is the amount of ammonium bicarbonate;
[0012] Wherein, the trivalent metal hydroxide includes aluminum hydroxide and / or iron hydroxide.
[0013] Optionally, the composite activator further satisfies:
[0014] m:q=(1~4):1, and
[0015] n:q=(1~12):1,
[0016] In the formula, q is the amount of phytic acid;
[0017] m is the amount of substance of the trivalent metal hydroxide;
[0018] n is the amount of ammonium bicarbonate.
[0019] Optionally, the composite activator further satisfies:
[0020] m:q=(1~3):1, and
[0021] n:q=(3~9):1,
[0022] In the formula, q is the amount of phytic acid;
[0023] m is the amount of substance of the trivalent metal hydroxide;
[0024] n is the amount of ammonium bicarbonate.
[0025] Optionally, the composite activator has a molecular structure as shown in Formula 1;
[0026]
[0027] In Formula 1, m is the amount of substance of the trivalent metal hydroxide, n is the amount of substance of ammonium bicarbonate, and M is a trivalent metal ion;
[0028] The amount m of the trivalent metal hydroxide and the amount n of the ammonium bicarbonate satisfy: (3m+n)=12.
[0029] In a second aspect, the present application provides a method for preparing the composite activator described in the first aspect, the method comprising:
[0030] Phytic acid, trivalent metal hydroxide and ammonium carbonate are mixed and heated to make the phytic acid, the trivalent metal hydroxide and the ammonium carbonate undergo a neutralization reaction to obtain a composite activator.
[0031] Optionally, the terminal temperature of the heating is 25°C to 95°C, and the heating time is 0.5h to 6h.
[0032] In a third aspect, the present application provides an application of a composite activator, wherein the application includes using the composite activator described in the first aspect as a desulfurization reagent used in the desulfurization treatment of high-sulfur bauxite.
[0033] In a fourth aspect, the present application provides a method for desulfurization of high-sulfur bauxite, the method comprising:
[0034] The high-sulfur bauxite is crushed and then ground to obtain high-sulfur bauxite powder;
[0035] Adding a sodium silicate inhibitor to the high-sulfur bauxite powder for a first slurry preparation to obtain a first slurry;
[0036] Adding the composite activator described in the first aspect to the first slurry for second slurry adjustment to obtain a second slurry;
[0037] Adding a xanthate desulfurization collector and a frother to the second slurry to obtain a flotation slurry;
[0038] Passing acidic gas into the flotation pulp to prevent the flotation pulp from being oxidized, and then flotation scraping the flotation pulp after the acidic gas is passed into the flotation pulp to obtain a flotation mixture;
[0039] The flotation mixture is subjected to roughing, cleaning and scavenging to obtain aluminum concentrate and sulfur concentrate respectively;
[0040] The weight m1 of the composite activator and the weight m2 of the first slurry satisfy the relationship: m1:m2≥5×10 -5 :1;
[0041] The xanthate desulfurization collector comprises at least one of the following:
[0042] Ethyl xanthate, butyl xanthate, isobutyl xanthate, amyl xanthate and isopentyl xanthate.
[0043] Optionally, the weight m3 of the fine-grained high-sulfur bauxite powder in the high-sulfur bauxite powder and the weight m4 of the high-sulfur bauxite powder satisfy the relationship: m3:m4=(0.75-0.85):1, and the particle size of the fine-grained high-sulfur bauxite powder is ≤0.074 mm.
[0044] Optionally, the flotation scraping time is 12 minutes to 20 minutes.
[0045] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0046] An embodiment of the present application provides a phytic acid-based composite activator, wherein the raw materials of the composite activator include phytic acid, trivalent metal hydroxide and ammonium bicarbonate, and the composite activator satisfies: (3m+n):q=12:1, m:q=(0-4):1, and n:q=(0-12):1, wherein q is the amount of phytic acid; m is the amount of trivalent metal hydroxide; n is the amount of ammonium bicarbonate; wherein the trivalent metal hydroxide includes aluminum hydroxide and / or ferric hydroxide. The raw materials of the composite activator may include phytic acid, trivalent metal hydroxide and ammonium bicarbonate, and the composite activator may satisfy: (3m+n):q=12:1, which can promote the presence of sufficient phytic acid in the composite activator, and the sufficient phytic acid can increase the oxidation potential of the pyrite surface in the high-sulfur bauxite, and the hydrophilic substances in the pyrite in the high-sulfur bauxite with the increased surface oxidation potential are easily removed, thereby reducing the content of hydrophilic substances wrapped on the surface of the pyrite in the high-sulfur bauxite to expose the fresh surface of the high-sulfur bauxite; in addition, the composite activator may also satisfy m:q=(0-4):1, and n:q=(0-12):1, and the composite activator may satisfy trivalent metal hydroxide The ratio of the sum of the amount of oxide m and the amount of ammonium bicarbonate n to the amount of phytic acid is 12:1. Ammonium bicarbonate can be used to promote the metal ions of aluminum hydroxide or copper iron hydroxide to be directly adsorbed on the sulfur atoms of pyrite in the high-sulfur bauxite with a fresh surface exposed, so as to avoid the sulfur atoms on the surface of the high-sulfur bauxite occupying other active sites, thereby increasing the number of active sites on the surface of the high-sulfur bauxite, and further improving the activation performance of the activator on the high-sulfur bauxite; in addition, phytic acid, trivalent metal hydroxides and ammonium bicarbonate have low corrosiveness, which can reduce the corrosiveness of the composite activator, thereby achieving the goal of reducing the corrosiveness of the activator while improving the activation performance of the activator. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0048] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0049] Figure 1 A microscopic schematic diagram of a phytic acid-based composite activator provided in an embodiment of the present application;
[0050] Figure 2 A macroscopic schematic diagram of a phytic acid-based composite activator provided in an embodiment of the present application;
[0051] Figure 3 A schematic flow chart of a method for preparing the composite activator provided in an embodiment of the present application;
[0052] Figure 4 A schematic flow chart of a method for desulfurization of high-sulfur bauxite provided in an embodiment of the present application. DETAILED DESCRIPTION
[0053] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0054] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a rigid limitation on the scope of the present application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within the range; for example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range; in addition, whenever a numerical range is indicated in this document, it is meant to include any cited numbers (fractions or integers) within the indicated range.
[0055] In this document, the terms including "including" and "including" mean "including but not limited to". Relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. "And / or" describes the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone; where A and B can be singular or plural. "At least one" means one or more, and "plurality" means two or more; "at least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items; for example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple. Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0056] Figure 1 A microscopic schematic diagram of a phytic acid-based composite activator provided in an embodiment of the present application is exemplarily shown;
[0057] Figure 2 A macroscopic schematic diagram of a phytic acid-based composite activator provided in an embodiment of the present application is exemplarily shown;
[0058] like Figure 1 and Figure 2 As shown, the embodiment of the present application provides a composite activator based on phytic acid, the raw materials of the composite activator include phytic acid, trivalent metal hydroxide and ammonium bicarbonate, and the composite activator satisfies:
[0059] (3m+n):q=12:1,
[0060] m:q=(0~4):1, and
[0061] n:q=(0~12):1,
[0062] In the formula, q is the amount of phytic acid;
[0063] m is the amount of substance of the trivalent metal hydroxide;
[0064] n is the amount of ammonium bicarbonate;
[0065] Wherein, the trivalent metal hydroxide includes aluminum hydroxide and / or iron hydroxide.
[0066] The composite activator may satisfy m:q=0:1, 1:1, 2:1, 3:1 or 4:1.
[0067] The composite activator can satisfy the following ratio: n:q=0:1, 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, 11:1 or 12:1.
[0068] In some optional embodiments, the composite activator further satisfies:
[0069] m:q=(1~4):1, and
[0070] n:q=(1~12):1,
[0071] In the formula, q is the amount of phytic acid;
[0072] m is the amount of substance of the trivalent metal hydroxide;
[0073] n is the amount of ammonium bicarbonate;
[0074] In some optional embodiments, the composite activator further satisfies:
[0075] m:q=(1~3):1, and
[0076] n:q=(3~9):1,
[0077] In the formula, q is the amount of phytic acid;
[0078] m is the amount of substance of the trivalent metal hydroxide;
[0079] n is the amount of ammonium bicarbonate;
[0080] In these embodiments, the composite activator can also satisfy: m:q=(1-4):1, and n:q=(1-12):1, and the composite activator can also satisfy: m:q=(1-3):1, and n:q=(3-9):1, which can promote the presence of sufficient trivalent metal hydroxide and sufficient ammonium carbonate in the composite activator. Sufficient trivalent metal hydroxide and sufficient ammonium carbonate can promote the trivalent metal ions to be directly adsorbed on the sulfur atoms of pyrite in the high-sulfur bauxite with fresh surface exposed, so as to avoid the sulfur atoms on the surface of the high-sulfur bauxite occupying other active sites, thereby increasing the activity of the surface of the high-sulfur bauxite, and further improving the activation performance of the activator on the high-sulfur bauxite.
[0081] In some optional embodiments, the composite activator has a molecular structure as shown in Formula 1;
[0082]
[0083] In Formula 1, m is the amount of substance of the trivalent metal hydroxide, n is the amount of substance of ammonium bicarbonate, and M is a trivalent metal ion;
[0084] The amount m of the trivalent metal hydroxide and the amount n of the ammonium bicarbonate satisfy: (3m+n)=12;
[0085] In this embodiment, the composite activator can have a molecular structure as shown in Formula 1, and the amount of the trivalent metal hydroxide and the amount of the ammonium carbonate can satisfy: (3m+n)=12; it can be explained that the phytic acid, trivalent metal hydroxide and ammonium carbonate in the composite activator react fully, thereby forming a stable composite activator.
[0086] Figure 3 A schematic flow chart of a method for preparing the composite activator provided in an embodiment of the present application is shown exemplarily;
[0087] Based on a general invention, such as Figure 3 As shown, the present embodiment provides a method for preparing the composite activator, the method comprising:
[0088] S1. Phytic acid, trivalent metal hydroxide and ammonium carbonate are mixed and heated to allow the phytic acid, the trivalent metal hydroxide and the ammonium carbonate to undergo a neutralization reaction to obtain a composite activator.
[0089] This method is a method for preparing the above-mentioned composite activator. The specific composition of the composite activator can refer to the above-mentioned embodiment. Since the preparation method adopts part or all of the technical solutions of the above-mentioned embodiment, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiment, which will not be repeated here one by one.
[0090] In some optional embodiments, the terminal temperature of the heating is 25° C. to 95° C., and the heating time is 0.5 h to 6 h.
[0091] In these embodiments, the terminal temperature of heating can be 25° C. to 95° C., and the heating time can be 0.5 h to 6 h, which can promote the neutralization reaction between phytic acid, copper hydroxide and ammonium carbonate to obtain a sufficient amount of composite activator.
[0092] The endpoint temperature of the heating may be 25°C, 35°C, 45°C, 55°C, 65°C, 75°C, 85°C or 95°C.
[0093] The heating time can be 0.5h, 1.0h, 1.5h, 2.0h, 2.5h, 3.0h, 3.5h, 4.0h, 4.5h, 5.0h, 5.5h or 6.0h.
[0094] Based on a general inventive concept, an embodiment of the present application provides an application of a composite activator, wherein the application includes using the composite activator as a desulfurization reagent for desulfurization treatment of high-sulfur bauxite.
[0095] This application is realized based on the above-mentioned composite activator. The specific composition of the composite activator can refer to the above-mentioned embodiment. Since this application adopts part or all of the technical solutions of the above-mentioned embodiment, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiment, which will not be described one by one here.
[0096] Figure 4 A schematic diagram of a desulfurization method for high-sulfur bauxite provided in an embodiment of the present application is shown as an example;
[0097] Based on a general inventive concept, such as Figure 4 As shown, the embodiment of the present application provides a desulfurization method for high-sulfur bauxite, the method comprising:
[0098] S1. crushing the high-sulfur bauxite and then grinding it to obtain high-sulfur bauxite powder;
[0099] S2. adding a sodium silicate inhibitor to the high-sulfur bauxite powder for a first slurry adjustment to obtain a first slurry;
[0100] S3. adding the composite activator to the first slurry for a second slurry adjustment to obtain a second slurry;
[0101] S4. adding a xanthate desulfurization collector and a frother to the second slurry to obtain a flotation slurry;
[0102] S5. introducing acidic gas into the flotation pulp to prevent the flotation pulp from being oxidized, and then flotation scraping the flotation pulp after introducing acidic gas to obtain a flotation mixture;
[0103] The flotation mixture is subjected to roughing, cleaning and scavenging to obtain aluminum concentrate and sulfur concentrate respectively;
[0104] The weight m1 of the composite activator and the weight m2 of the first slurry satisfy the relationship: m1:m2≥5×10 -5 :1;
[0105] The xanthate desulfurization collector comprises at least one of the following:
[0106] Ethyl xanthate, butyl xanthate, isobutyl xanthate, amyl xanthate and isopentyl xanthate.
[0107] This method is implemented based on the above-mentioned composite activator. The specific composition of the composite activator can refer to the above-mentioned embodiment. Since this method adopts part or all of the technical solutions of the above-mentioned embodiment, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiment, which will not be repeated here one by one.
[0108] It should be noted that the sodium silicate inhibitor can effectively inhibit the floating of aluminosilicate minerals in the high-sulfur bauxite powder. In addition, the sodium silicate inhibitor can disperse the high-sulfur bauxite mud in the first slurry.
[0109] It should be noted that the addition of the composite activator can promote the copper ions of copper hydroxide to be directly adsorbed on the sulfur atoms of pyrite in the high-sulfur bauxite with fresh surface exposed, so as to avoid the sulfur atoms on the surface of the high-sulfur bauxite occupying other active sites, thereby increasing the number of active sites on the surface of the high-sulfur bauxite. A sufficient number of active sites can significantly affect the effect of pyrite in the high-sulfur bauxite and the xanthate desulfurization collector. When the concentration of the xanthate desulfurization collector is high, some copper-xanthate compounds and a hydrophobic dixanthate layer will be generated on the surface of pyrite in the high-sulfur bauxite. These copper-xanthate compounds and dixanthate layers The capture ability of xanthate desulfurization collectors on pyrite in high-sulfur bauxite is improved; in addition, the ammonium ions in the composite activator can promote the electrochemical reaction of the xanthate collectors on the surface of pyrite in high-sulfur bauxite and generate a hydrophobic double xanthate layer, which can improve the capture ability of the xanthate desulfurization collectors on pyrite in high-sulfur bauxite; in addition, the ammonium ions in the composite activator will also combine with water molecules to obtain hydrated molecules of ammonia, which will reduce the stability of the solid-liquid interface hydration layer of the flotation tailings and the xanthate desulfurization collectors, thereby dispersing the high-sulfur bauxite sludge whose surface of pyrite in high-sulfur bauxite is covered by hydrophilic substances.
[0110] It should be noted that the acid gas may be a mixed gas of carbon dioxide gas and nitrogen gas, the volume fraction of carbon dioxide gas in the acid gas may be 0% to 50%, and the volume fraction of nitrogen gas in the acid gas may be 50% to 100%.
[0111] It should be noted that the addition of the acidic gas can prevent oxygen from oxidizing the surface of pyrite in high-sulfur bauxite. In addition, the carbon dioxide in the acidic gas will also form H2CO3 and HCO3 in the flotation pulp. - 、CO3 2- Plasma, these ions can further promote the electrochemical reaction of xanthate collectors on the surface of pyrite in high-sulfur bauxite and generate a hydrophobic double xanthate layer. In addition, these ions can also increase the ability of pyrite in high-sulfur bauxite to adsorb xanthate collectors.
[0112] It should be noted that the first slurry mixing and the second slurry mixing are only set to distinguish operations, rather than to mark the order of operations; the first slurry mixing and the second slurry mixing can be performed by stirring to promote sufficient mixing of the various materials.
[0113] In some optional embodiments, the weight m3 of the fine-grained high-sulfur bauxite powder in the high-sulfur bauxite powder and the weight m4 of the high-sulfur bauxite powder satisfy the relationship: m3:m4=(0.75-0.85):1, and the particle size of the fine-grained high-sulfur bauxite powder is ≤0.074 mm.
[0114] In these embodiments, the weight m3 of the fine-grained high-sulfur bauxite powder and the weight m4 of the high-sulfur bauxite powder in the high-sulfur bauxite powder can satisfy the relationship: m3:m4=(0.75-0.85):1, and the particle size of the fine-grained high-sulfur bauxite powder is generally ≤0.074mm, which can promote the effective combination of sodium silicate inhibitors, composite activators, xanthate desulfurization collectors and foaming agents with the high-sulfur bauxite powder, thereby obtaining a sufficient amount of aluminum concentrate and sulfur concentrate.
[0115] The weight m3 of the fine-grained high-sulfur bauxite powder and the weight m4 of the high-sulfur bauxite powder in the high-sulfur bauxite powder may satisfy the relationship: m3:m4=0.75, 0.76, 0.77, 0.78, 0.79, 0.80, 0.81, 0.82, 0.83, 0.84 or 0.85.
[0116] In some optional embodiments, the flotation scraping time is 13min to 18min;
[0117] In these embodiments, the flotation scraping time may be 13 minutes to 18 minutes, which can promote the flotation scraping to be fully carried out, so that the impurities floating in the flotation pulp after the acid gas are removed by the flotation scraping method.
[0118] The flotation scraping time can be 13 minutes, 14 minutes, 15 minutes, 16 minutes, 17 minutes or 18 minutes.
[0119] The present application is further described below in conjunction with specific examples. The experimental methods in the following examples that do not specify specific conditions are usually measured according to industry standards; if there are no corresponding industry standards, they are carried out according to common international standards, conventional conditions, or conditions recommended by the manufacturer.
[0120] Example 1
[0121] A composite activator, the raw materials of the composite activator include phytic acid, trivalent metal hydroxide and ammonium bicarbonate, and based on 1 mol of phytic acid, the composite activator satisfies:
[0122] (3m+n):q=12:1,
[0123] m:q = 4:1, and
[0124] n:q=0:1,
[0125] In the formula, q is the amount of phytic acid, 1 mol;
[0126] m is the amount of substance of trivalent metal hydroxide, 4 mol;
[0127] n is the amount of ammonium bicarbonate, 0 mol;
[0128] Wherein, the trivalent metal hydroxide is aluminum hydroxide.
[0129] The composite activator has a molecular structure as shown in Formula 1,
[0130]
[0131] In formula 1, m is the amount of trivalent metal hydroxide, which is 4; n is the amount of ammonium bicarbonate, which is 0; M is the trivalent metal ion Al 3+ ;
[0132] The raw ore of a high-sulfur bauxite mine in Henan was selected, and its sulfur content was 2.41%.
[0133] like Figure 3 As shown, a method for preparing a composite activator comprises:
[0134] S1. Phytic acid, trivalent metal hydroxide and ammonium bicarbonate are mixed and heated to neutralize the phytic acid, trivalent metal hydroxide and ammonium bicarbonate to obtain a composite activator.
[0135] The end point temperature of heating was 25°C and the heating time was 0.5 h.
[0136] like Figure 4 As shown, a desulfurization method for high-sulfur bauxite comprises:
[0137] S1. crushing the high-sulfur bauxite to 3 mm and then grinding it to obtain high-sulfur bauxite powder;
[0138] S2. adding a sodium silicate inhibitor to the high-sulfur bauxite powder at a mass ratio of 1500 g / t and stirring for 3 min to perform a first slurry to obtain a first slurry;
[0139] S3. The composite activator was added to the first slurry at a mass ratio of 80 g / t and stirred for 3 min for a second slurry to obtain a second slurry;
[0140] S4. The xanthate desulfurization collector was added to the second slurry at a mass ratio of 700 g / t and the frother at a mass ratio of 300 g / t and stirred for 6 min to obtain a flotation slurry;
[0141] S5. A mixture of CO2 and N2 is passed into the flotation pulp to prevent the flotation pulp from being oxidized, and then the flotation pulp after the acid gas is passed is flotated and scraped to obtain a flotation mixture;
[0142] S6. roughing, concentrating and scavenging the flotation mixture to obtain aluminum concentrate and sulfur concentrate, respectively;
[0143] The weight of the composite activator m1 and the weight of the first slurry m2 satisfy the relationship: m1:m2≥8×10 -5 :1;
[0144] The xanthate desulfurization collector is amyl xanthate.
[0145] The weight m3 of the fine-grained high-sulfur bauxite powder and the weight m4 of the high-sulfur bauxite powder satisfy the relationship: m3:m4=0.80:1, and the particle size of the fine-grained high-sulfur bauxite powder is ≤0.074mm.
[0146] The flotation scraping time is 13 minutes.
[0147] Example 2
[0148] A composite activator, the raw materials of the composite activator include phytic acid, trivalent metal hydroxide and ammonium bicarbonate, and based on 1 mol of phytic acid, the composite activator satisfies:
[0149] (3m+n):q=12:1,
[0150] m:q = 1:1, and
[0151] n:q=9:1,
[0152] In the formula, q is the amount of phytic acid, 1 mol;
[0153] m is the amount of substance of trivalent metal hydroxide, 1 mol;
[0154] n is the amount of ammonium bicarbonate, 9 mol;
[0155] Wherein, the trivalent metal hydroxide is aluminum hydroxide.
[0156] The composite activator has a molecular structure as shown in Formula 1,
[0157]
[0158] In formula 1, m is the amount of aluminum hydroxide or ferric hydroxide, which is 1; n is the amount of ammonium bicarbonate, which is 9; M is the trivalent metal ion Al 3+ ;
[0159] A magnetic aluminum concentrate slurry was selected, and its sulfur content was 5.74%.
[0160] like Figure 3 As shown, a method for preparing a composite activator comprises:
[0161] S1. Phytic acid, trivalent metal hydroxide and ammonium bicarbonate are mixed and heated to neutralize the phytic acid, trivalent metal hydroxide and ammonium bicarbonate to obtain a composite activator.
[0162] The final temperature of heating was 50°C and the heating time was 2 h.
[0163] like Figure 4 As shown, a desulfurization method for high-sulfur bauxite comprises:
[0164] S1. Add 1.5 L of magnetic aluminum concentrate slurry with a mass concentration of 28% to a flotation machine and stir for 3 min for the first slurry adjustment to obtain a first slurry;
[0165] S2. The composite activator was added to the first slurry at a mass ratio of 150 g / t and stirred for 3 min for a second slurry to obtain a second slurry;
[0166] S3. The xanthate desulfurization collector was added to the second slurry at a mass ratio of 900 g / t and the frother at a mass ratio of 450 g / t and stirred for 6 min to obtain a flotation slurry;
[0167] S4. A mixture of CO2 and N2 is passed into the flotation pulp as an acidic gas to prevent the flotation pulp from being oxidized, and then the flotation pulp after the acidic gas is passed is subjected to flotation scraping to obtain a flotation mixture;
[0168] S5. roughing, concentrating and scavenging the flotation mixture to obtain aluminum concentrate and sulfur concentrate, respectively;
[0169] The weight of the composite activator m1 and the weight of the first slurry m2 satisfy the following relationship: m1:m2≥15×10 -5 :1;
[0170] The xanthate desulfurization collector is butyl xanthate.
[0171] The weight m3 of the fine-grained high-sulfur bauxite powder and the weight m4 of the high-sulfur bauxite powder satisfy the relationship: m3:m4=0.75:1, and the particle size of the fine-grained high-sulfur bauxite powder is ≤0.074mm.
[0172] The flotation scraping time is 17.0min.
[0173] Example 3
[0174] A composite activator, the raw materials of the composite activator include phytic acid, trivalent metal hydroxide and ammonium bicarbonate, and based on 1 mol of phytic acid, the composite activator satisfies:
[0175] (3m+n):q=12:1,
[0176] m:q = 2:1, and
[0177] n:q=6:1,
[0178] In the formula, q is the amount of phytic acid, 1 mol;
[0179] m is the amount of substance of trivalent metal hydroxide, 2 mol;
[0180] n is the amount of ammonium bicarbonate, 6 mol;
[0181] Wherein, the trivalent metal hydroxide is aluminum hydroxide.
[0182] The composite activator has a molecular structure as shown in Formula 1,
[0183]
[0184] In formula 1, m is the amount of aluminum hydroxide or ferric hydroxide, which is 2; n is the amount of ammonium bicarbonate, which is 6; M is the trivalent metal ion Al 3+ ;
[0185] The raw ore of a high-sulfur bauxite mine in Guizhou was selected, and its sulfur content was 5.05%.
[0186] like Figure 3 As shown, a method for preparing a composite activator comprises:
[0187] like Figure 3 As shown, a method for preparing a composite activator comprises:
[0188] S1. Phytic acid, trivalent metal hydroxide and ammonium bicarbonate are mixed and heated to neutralize the phytic acid, trivalent metal hydroxide and ammonium bicarbonate to obtain a composite activator.
[0189] The final temperature of heating was 50°C and the heating time was 3 h.
[0190] like Figure 4 As shown, a desulfurization method for high-sulfur bauxite comprises:
[0191] S1. crushing the high-sulfur bauxite to 3 mm and then grinding it to obtain high-sulfur bauxite powder;
[0192] S2. adding a sodium silicate inhibitor to the high-sulfur bauxite powder at a mass ratio of 2000 g / t and stirring for 3 min to perform a first slurry to obtain a first slurry;
[0193] S3. The composite activator is added to the first slurry at a mass ratio of 100 g / t and stirred for 3 min for a second slurry to obtain a second slurry;
[0194] S4. The xanthate desulfurization collector was added to the second slurry at a mass ratio of 900 g / t and the frother at a mass ratio of 400 g / t and stirred for 6 min to obtain a flotation slurry;
[0195] S5. A mixture of CO2 and N2 is passed into the flotation pulp to prevent the flotation pulp from being oxidized, and then the flotation pulp after the acid gas is passed is flotated and scraped to obtain a flotation mixture;
[0196] S6. roughing, concentrating and scavenging the flotation mixture to obtain aluminum concentrate and sulfur concentrate, respectively;
[0197] The weight of the composite activator m1 and the weight of the first slurry m2 satisfy the relationship: m1:m2≥10×10 -5 :1;
[0198] The xanthate desulfurization collector is amyl xanthate.
[0199] The weight m3 of the fine-grained high-sulfur bauxite powder and the weight m4 of the high-sulfur bauxite powder satisfy the relationship: m3:m4=0.85:1, the particle size of the fine-grained high-sulfur bauxite powder is ≤0.074mm, and the particle size of the fine-grained high-sulfur bauxite powder is
[0200] ≤0.074mm.
[0201] The flotation scraping time is 20.0min.
[0202] Example 4
[0203] A composite activator, the raw materials of the composite activator include phytic acid, trivalent metal hydroxide and ammonium bicarbonate, and based on 1 mol of phytic acid, the composite activator satisfies:
[0204] (3m+n):q=12:1,
[0205] m:q = 3:1, and
[0206] n:q=3:1,
[0207] In the formula, q is the amount of phytic acid, 1 mol;
[0208] m is the amount of substance of trivalent metal hydroxide, 3 mol;
[0209] n is the amount of ammonium bicarbonate, 3 mol;
[0210] Wherein, the trivalent metal hydroxide is aluminum hydroxide.
[0211] The composite activator has a molecular structure as shown in Formula 1,
[0212]
[0213] In formula 1, m is the amount of aluminum hydroxide or iron hydroxide, which is 3; n is the amount of ammonium bicarbonate, which is 3;
[0214] like Figure 3 As shown, a method for preparing a composite activator comprises:
[0215] S1. Phytic acid, trivalent metal hydroxide and ammonium bicarbonate are mixed and heated to neutralize the phytic acid, trivalent metal hydroxide and ammonium bicarbonate to obtain a composite activator.
[0216] The final temperature of heating was 75°C and the heating time was 4 h.
[0217] A decarbonized bauxite slurry was selected, and its sulfur content was 4.41%.
[0218] like Figure 4 As shown, a desulfurization method for high-sulfur bauxite comprises:
[0219] S1. 1.5 L of decarbonized bauxite slurry having a mass concentration of 27% was added to a flotation machine and stirred for 3 min for a first slurry adjustment to obtain a first slurry;
[0220] S2. The composite activator is added to the first slurry at a mass ratio of 100 g / t and stirred for 3 min for a second slurry preparation to obtain a second slurry;
[0221] S3. The xanthate desulfurization collector was added to the second slurry at a mass ratio of 800 g / t and the frother at a mass ratio of 400 g / t and stirred for 6 min to obtain a flotation slurry;
[0222] S5. A mixture of CO2 and N2 is passed into the flotation pulp to prevent the flotation pulp from being oxidized, and then the flotation pulp after the acid gas is passed is flotated and scraped to obtain a flotation mixture;
[0223] S6. roughing, concentrating and scavenging the flotation mixture to obtain aluminum concentrate and sulfur concentrate, respectively;
[0224] The weight of the composite activator m1 and the weight of the first slurry m2 satisfy the relationship: m1:m2≥10×10 -5 ;
[0225] The weight m3 of the fine-grained high-sulfur bauxite powder and the weight m4 of the high-sulfur bauxite powder satisfy the relationship: m3:m4=0.85:1, and the particle size of the fine-grained high-sulfur bauxite powder is ≤0.074mm.
[0226] The xanthate desulfurization collector is butyl xanthate.
[0227] The flotation scraping time is 16.0min.
[0228] Example 5
[0229] A composite activator, the raw materials of the composite activator include phytic acid, trivalent metal hydroxide and ammonium bicarbonate, and based on 1 mol of phytic acid, the composite activator satisfies:
[0230] (3m+n):q=12:1,
[0231] m:q = 4:1, and
[0232] n:q=0:1,
[0233] In the formula, q is the amount of phytic acid, 1 mol;
[0234] m is the amount of substance of trivalent metal hydroxide, 4 mol;
[0235] n is the amount of ammonium bicarbonate, 0 mol;
[0236] Wherein, the trivalent metal hydroxide is ferric hydroxide.
[0237] The composite activator has a molecular structure as shown in Formula 1,
[0238]
[0239] In formula 1, m is the amount of aluminum hydroxide or iron hydroxide, which is 4; n is the amount of ammonium bicarbonate, which is 0; M is the trivalent metal ion Fe 3+ ;
[0240] like Figure 3 As shown, a method for preparing a composite activator comprises:
[0241] S1. Phytic acid, trivalent metal hydroxide and ammonium bicarbonate are mixed and heated to neutralize the phytic acid, trivalent metal hydroxide and ammonium bicarbonate to obtain a composite activator.
[0242] The final temperature of heating was 95°C and the heating time was 6 h.
[0243] The raw ore of a high-sulfur bauxite mine in Chongqing was selected, and its sulfur content was 4.08%.
[0244] like Figure 4 As shown, a desulfurization method for high-sulfur bauxite comprises:
[0245] S1. crushing the high-sulfur bauxite to 3 mm and then grinding it to obtain high-sulfur bauxite powder;
[0246] S2. adding a sodium silicate inhibitor to the high-sulfur bauxite powder at a mass ratio of 1500 g / t and stirring for 3 min to perform a first slurry to obtain a first slurry;
[0247] S3. The composite activator is added to the first slurry at a mass ratio of 100 g / t and stirred for 3 min for a second slurry to obtain a second slurry;
[0248] S4. The xanthate desulfurization collector was added to the second slurry at a mass ratio of 700 g / t and the frother at a mass ratio of 300 g / t and stirred for 6 min to obtain a flotation slurry;
[0249] S5. A mixture of CO2 and N2 is passed into the flotation pulp to prevent the flotation pulp from being oxidized, and then the flotation pulp after the acid gas is passed is flotated and scraped to obtain a flotation mixture;
[0250] S6. roughing, concentrating and scavenging the flotation mixture to obtain aluminum concentrate and sulfur concentrate, respectively;
[0251] The weight of the composite activator m1 and the weight of the first slurry m2 satisfy the relationship: m1:m2≥10×10 -5 ;
[0252] The xanthate desulfurization collector is amyl xanthate.
[0253] The weight m3 of the fine-grained high-sulfur bauxite powder and the weight m4 of the high-sulfur bauxite powder satisfy the relationship: m3:m4=0.80:1, and the particle size of the fine-grained high-sulfur bauxite powder is ≤0.074mm.
[0254] The flotation scraping time is 15 minutes.
[0255] Comparative Example 1
[0256] Comparative Example 1 and Example 1 are compared. The difference between Comparative Example 1 and Example 1 is:
[0257] Only oxalic acid was used as the composite activator.
[0258] Comparative Example 2
[0259] Comparing Comparative Example 2 with Example 2, the difference between Comparative Example 1 and Example 2 is:
[0260] Only sulfuric acid was used as the composite activator.
[0261] Comparative Example 3
[0262] Comparing Comparative Example 3 with Example 3, the difference between Comparative Example 1 and Example 3 is:
[0263] Only sulfuric acid was used as the composite activator.
[0264] Comparative Example 4
[0265] Comparing Comparative Example 4 with Example 4, the difference between Comparative Example 1 and Example 4 is:
[0266] Only copper sulfate was used as the composite activator.
[0267] Comparative Example 5
[0268] Comparing Comparative Example 5 with Example 5, the difference between Comparative Example 1 and Example 5 is:
[0269] Only copper sulfate was used as the composite activator.
[0270] Related experiments and effect data:
[0271] The performance parameters of the aluminum concentrate and sulfur concentrate obtained in each embodiment and comparative example are shown in Table 1.
[0272]
[0273]
[0274] It can be seen from Table 1 that the sulfur content of the aluminum concentrate obtained in Example 1 can be reduced to 0.29%, the sulfur content of the sulfur concentrate can reach 29.98%, and the recovery rate of sulfur recovered by the sulfur concentrate in Example 1 is 88.81%; while the sulfur content of the aluminum concentrate obtained in Comparative Example 1 can be reduced to 0.36%, the sulfur content of the sulfur concentrate can reach 24.29%, and the recovery rate of sulfur recovered by the sulfur concentrate in Comparative Example 1 is only 86.35%.
[0275] The sulfur content of the aluminum concentrate obtained in Example 2 can be reduced to 0.46%, the sulfur content of the sulfur concentrate can reach 37.28%, and the recovery rate of sulfur recovered through the sulfur concentrate in Example 2 is 93.13%; while the sulfur content of the aluminum concentrate obtained in Comparative Example 2 can be reduced to 0.58%, the sulfur content of the sulfur concentrate can reach 34.39%, and the recovery rate of sulfur recovered through the sulfur concentrate in Comparative Example 2 is only 91.44%.
[0276] The sulfur content of the aluminum concentrate obtained in Example 3 can be reduced to 0.51%, the sulfur content of the sulfur concentrate can reach 38.22%, and the recovery rate of sulfur recovered through the sulfur concentrate in Example 3 is 90.57%; while the sulfur content of the aluminum concentrate obtained in Comparative Example 3 can be reduced to 0.68%, the sulfur content of the sulfur concentrate can reach 32.74%, and the recovery rate of sulfur recovered through the sulfur concentrate in Comparative Example 3 is only 88.37%.
[0277] The sulfur content of the aluminum concentrate obtained in Example 4 can be reduced to 0.33%, the sulfur content of the sulfur concentrate can reach 33.84%, and the recovery rate of sulfur recovered through the sulfur concentrate in Example 4 is 93.42%; while the sulfur content of the aluminum concentrate obtained in Comparative Example 4 can be reduced to 0.40%, the sulfur content of the sulfur concentrate can reach 30.57%, and the recovery rate of sulfur recovered through the sulfur concentrate in Comparative Example 4 is only 92.13%.
[0278] The sulfur content of the aluminum concentrate obtained in Example 5 can be reduced to 0.41%, the sulfur content of the sulfur concentrate can reach 36.09%, and the recovery rate of sulfur recovered through the sulfur concentrate in Example 5 is 90.98%; while the sulfur content of the aluminum concentrate obtained in Comparative Example 5 can be reduced to 0.51%, the sulfur content of the sulfur concentrate can reach 33.79%, and the recovery rate of sulfur recovered through the sulfur concentrate in Comparative Example 5 is only 88.84%.
[0279] In summary, a composite activator provided in an embodiment of the present application can reduce the content of hydrophilic substances coated on the surface of pyrite in high-sulfur bauxite to expose the fresh surface of the high-sulfur bauxite. In addition, ammonium bicarbonate can be used to promote the direct adsorption of trimetallic ions such as aluminum hydroxide or iron hydroxide on the sulfur atoms of pyrite in the high-sulfur bauxite with the fresh surface exposed, thereby increasing the number of active sites on the surface of the high-sulfur bauxite, thereby improving the activation performance of the activator on the high-sulfur bauxite; in addition, phytic acid, trivalent metal hydroxides and ammonium bicarbonate have low corrosiveness, which can reduce the corrosiveness of the composite activator, thereby achieving the improvement of the activation performance of the activator while reducing the corrosiveness of the activator.
[0280] In addition, the composite activator provided in the embodiment of the present application uses only phytic acid, trivalent metal hydroxide and ammonium bicarbonate as raw materials, so the composite activator has good environmental compatibility. In addition, the composite activator does not need to use highly toxic chemicals such as lead nitrate, nor does it use highly corrosive liquid strong acids such as sulfuric acid. Therefore, the composite activator provided in the embodiment of the present application is also green, environmentally friendly and safe to use.
[0281] In addition, the application of a composite activator provided in an embodiment of the present application can be used as a desulfurization reagent used in the desulfurization treatment of high-sulfur bauxite, which can reduce the sulfur content in the obtained aluminum concentrate to below 0.60%, and can also increase the sulfur recovery rate in the sulfur concentrate to 88.00%.
[0282] In addition, a desulfurization method for high-sulfur bauxite provided in an embodiment of the present application uses a composite activator with low cost and strong adaptability, and can be widely used to remove impurities such as sulfur from high-sulfur bauxite or low-sulfur bauxite with a sulfur content of less than 6%; in addition, the composite activator is applied to the flotation desulfurization process of bauxite, and then after one roughing selection, two fine selections, three scavenging selections or one roughing selection, three fine selections, three scavenging selections, most of the sulfur impurities in the sulfur-containing bauxite can be floated out, and the aluminum concentrate obtained after fine selection can meet the requirements of the raw material indicators required for alumina production, and the sulfur concentrate after scavenging meets the requirements of sulfuric acid raw materials.
[0283] The above is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. It will be apparent to those skilled in the art that various modifications to these embodiments are possible, and the general principles defined in the present application can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to these embodiments shown in the present application, but will conform to the widest scope consistent with the principles and novel features applied for by the present application.
Claims
1. A composite activator based on phytic acid, It is characterized in that The raw materials of the composite activator include phytic acid, trivalent metal hydroxide and ammonium bicarbonate, and the composite activator satisfies: (3m+n):q=12:1, m:q=(0~4):1, and n:q=(0~12):1, In the formula, q is the amount of phytic acid; m is the amount of substance of the trivalent metal hydroxide; n is the amount of ammonium bicarbonate; Wherein, the trivalent metal hydroxide includes aluminum hydroxide and / or iron hydroxide.
2. The composite activator according to claim 1, It is characterized in that The composite activator also satisfies: m:q=(1~4):1, and n:q=(1~12):1, In the formula, q is the amount of phytic acid; m is the amount of substance of the trivalent metal hydroxide; n is the amount of ammonium bicarbonate.
3. The composite activator according to claim 1, It is characterized in that The composite activator also satisfies: m:q=(1~3):1, and n:q=(3~9):1, In the formula, q is the amount of phytic acid; m is the amount of substance of the trivalent metal hydroxide; n is the amount of ammonium bicarbonate.
4. The composite activator according to claim 1, It is characterized in that The composite activator has a molecular structure as shown in Formula 1; In Formula 1, m is the amount of substance of the trivalent metal hydroxide, n is the amount of substance of ammonium bicarbonate, and M is a trivalent metal ion; The amount m of the trivalent metal hydroxide and the amount n of the ammonium bicarbonate satisfy: (3m+n)=12.
5. A method for preparing the composite activator according to any one of claims 1 to 4, It is characterized in that The method comprises: Phytic acid, trivalent metal hydroxide and ammonium carbonate are mixed and heated to make the phytic acid, the trivalent metal hydroxide and the ammonium carbonate undergo a neutralization reaction to obtain a composite activator.
6. The method according to claim 5, It is characterized in that The terminal temperature of the heating is 25° C. to 95° C., and the heating time is 0.5 h to 6 h.
7. Application of a composite activator, It is characterized in that The application includes using the composite activator as described in any one of claims 1 to 4 as a desulfurization reagent used in the desulfurization treatment of high-sulfur bauxite.
8. A method for desulfurization of high-sulfur bauxite, It is characterized in that The method comprises: The high-sulfur bauxite is crushed and then ground to obtain high-sulfur bauxite powder; Adding a sodium silicate inhibitor to the high-sulfur bauxite powder for a first slurry preparation to obtain a first slurry; Adding the composite activator according to any one of claims 1 to 4 to the first slurry for second slurry adjustment to obtain a second slurry; Adding a xanthate desulfurization collector and a frother to the second slurry to obtain a flotation slurry; Passing acidic gas into the flotation pulp to prevent the flotation pulp from being oxidized, and then flotation scraping the flotation pulp after the acidic gas is passed into the flotation pulp to obtain a flotation mixture; The flotation mixture is subjected to roughing, cleaning and scavenging to obtain aluminum concentrate and sulfur concentrate respectively; The weight m1 of the composite activator and the weight m2 of the first slurry satisfy the relationship: m1:m2≥5×10 -5 :1; The xanthate desulfurization collector comprises at least one of the following: Ethyl xanthate, butyl xanthate, isobutyl xanthate, amyl xanthate and isopentyl xanthate.
9. The desulfurization method according to claim 8, It is characterized in that The weight m3 of the fine-grained high-sulfur bauxite powder in the high-sulfur bauxite powder and the weight m4 of the high-sulfur bauxite powder satisfy the relationship: m3:m4=(0.75-0.85):1, and the particle size of the fine-grained high-sulfur bauxite powder is ≤0.074mm.
10. The desulfurization method according to claim 8, It is characterized in that The flotation scraping time is 12 minutes to 20 minutes.
Citation Information
Patent Citations
Flotation impurity-removing method for asbestos-containing talcose ore
CN102225370A
Combined gangue mineral inhibitor and preparation method and application thereof
CN110773324A
Refractory low-grade nickel-cobalt sulfide ore flotation reagent system and application thereof
CN115318446A
Inositol hexaphosphate-protein complex degrading bacterium and application thereof
CN116218723A
ID2019S00428A
Cited By
Flotation desulfurization activating agent as well as preparation method and application thereof
CN119140285A
A flotation desulfurization activator, its preparation method and application
CN119140285B