A method for automatically repairing enlarged inner diameter and melt damage in the downcomer tube of an RH furnace
By generating a high-melting-point oxide protective layer, the problems of increased inner diameter and melting loss of the downcomer tube in the RH furnace were solved, achieving long-term protection and improved safety of the downcomer tube, and extending the maintenance cycle.
Patent Information
- Application Number
- CN202611392109.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-09
- Publication Date
- 2026-11-17
AI Technical Summary
The existing RH furnace downcomer tubes are prone to leakage due to increased inner diameter and melting loss under high temperature molten steel and vacuum conditions. Existing sprayed refractory materials have poor adhesion, short maintenance cycle and safety hazards.
By generating a high-melting-point oxide protective layer during the production interval of the RH furnace, including vacuum tank cold steel oxidation treatment, aluminum alloy addition, and the formation of a circulating adhesive protective layer, Al2O3 particles are generated and solidified on the inner wall of the downcomer to form a dense protective layer.
It achieves long-term protection of the inner wall of the downcomer, reduces melting loss, extends service life, eliminates safety hazards, and improves production continuity.
Smart Images

Figure CN123108237A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of ladle refining technology in the metallurgical industry, specifically relating to a method for repairing and protecting against the problem of enlarged inner diameter and melting loss in the downcomer of an RH furnace. Background Technology
[0002] The RH furnace is a key piece of equipment for secondary steel refining. Its downcomer is constantly exposed to high-temperature molten steel and vacuum conditions, making it prone to leakage due to increased inner diameter and melting loss, leading to production interruptions. The current mainstream maintenance method is high-pressure gas injection of refractory materials, such as refractory slurry, but this method has the following drawbacks: 1. Poor adhesion: The refractory material applied by spraying is easily detached during the scouring and splashing of molten steel, requiring frequent spraying. 2. Moisture Hazard: Refractory mortar containing moisture may cause splashing or even explosion when it comes into contact with molten steel; 3. Short maintenance cycle: The sprayed layer cannot adhere stably for a long time, making it difficult to meet the needs of high-frequency production.
[0003] Therefore, there is an urgent need for a maintenance technology that can provide long-term protection for the inner wall of the downcomer, reduce melting loss, and eliminate safety hazards. Summary of the Invention
[0004] To address the issues of poor adhesion, unstable maintenance results, and safety risks associated with existing spraying techniques, this invention proposes a method for automatically repairing and strengthening the inner wall of downcomer pipes by generating a high-melting-point oxide protective layer in situ. The technical solution adopted in this invention is as follows: A method for automatically repairing enlarged inner diameter and melt damage in the downcomer of an RH furnace, the method comprising the following steps: S1. Vacuum bath cold steel oxidation treatment During the production interval of the RH furnace, oxygen or a mixture of oxygen and coal gas is blown into the cold steel in the vacuum tank, causing the cold steel to oxidize and generate ferrous oxide (FeO). The molten cold steel and ferrous oxide form a semi-fluid that eventually condenses mostly at the bottom of the vacuum tank and inside the downcomer, forming an oxide layer substrate. S2. Aluminum alloy addition and alumina formation During the steelmaking stage, when the downcomer is inserted into the molten steel until the vacuum level drops to 20 kPa and the circulation has not yet formed, 30 kg to 120 kg more aluminum alloy is added to the vacuum tank according to the composition. The aluminum reacts with FeO and oxygen in the molten steel to generate high-concentration aluminum oxide (Al2O3) particles. S3. Circulating Adhesion Protective Layer As the vacuum level decreases to ≤20 kPa, the molten steel gradually forms a circulation. Al2O3 particles enter the downcomer along with the molten steel. Since the melting point of Al2O3 is 2057℃, which is much higher than the temperature of molten steel (1500~1620℃), it solidifies and adheres to the inner wall and lower end of the downcomer, forming a dense protective layer that fills the melting loss area and reduces the inner diameter.
[0005] Furthermore, in step S1, the oxygen flow rate for blowing oxygen into the vacuum tank for cooling the steel is 700~1200 m³ / h. 3 / h.
[0006] Further, in step S1, the oxygen-to-coal ratio of the oxygen-to-gas mixture is 1.2~1.8, and the flow rate is 400~600 m³ / s. 3 / h.
[0007] Furthermore, in step S2, the Al content of the aluminum alloy added to the vacuum tank is ≥90%.
[0008] The beneficial effects of this invention are: by generating a high-melting-point oxide protective layer in situ, this invention improves the service life and production continuity of the downcomer, provides long-term protection for the inner wall of the downcomer, reduces melting loss, and eliminates safety hazards. Attached Figure Description
[0009] Figure 1 Schematic diagram of RH furnace for cooling steel; Figure 2 A schematic diagram of aluminum addition during the post-processing of cold steel in an RH furnace; The labels in the diagram are as follows: 1—Vacuum trough, 2—RH furnace top lance, 3—Cold steel in the vacuum trough, 4—Ferrous oxide condensed at the bottom of the vacuum trough and in the downcomer, 5—Downcomer, 6—Rising pipe, 7—Ladle, 8—Feeding pipe, 9—Aluminum alloy particles, 10—Ferrous oxide floating in the vacuum trough, 11—Drive gas, 12—Al2O3 adhering to the downcomer, 13—Slag in the ladle, 14—Molten steel. Detailed Implementation
[0010] The present invention will be further described in detail below with reference to embodiments. A method for automatically repairing the enlarged inner diameter and melting loss of the downcomer tube in an RH furnace includes the following steps: 1. Vacuum bath cold steel oxidation stage: After the RH furnace is shut down, oxygen is blown into the remaining cold steel at the bottom of the furnace at a flow rate of 700~1200 m³ / h. 3 / h or an oxygen-coal gas mixture, with an oxygen-to-coal ratio of 1.2~1.8 and a gas flow rate of 500~700 m³ / h. 3 / h, FeO layer 4 is generated.
[0011] 2. Aluminum alloy addition stage: After refilling the molten steel 14, when the downcomer 5 is inserted into the molten steel 14 and the vacuum level drops to 20 kPa, aluminum alloy particles 9 are added through the feeding pipe 8, with an additional 30 kg to 120 kg of aluminum added according to the composition.
[0012] 3. Protective layer formation stage: As the vacuum level continues to decrease, the circulation of molten steel 14 intensifies, and Al2O3 particles adhere uniformly to the inner wall of the downcomer along with the circulation, forming a protective layer 12.
[0013] Furnace-cooled steel Figure 1 As shown, oxygen is blown into the cold steel 3 in the vacuum tank through the RH furnace top lance, causing the cold steel to oxidize and generate ferrous oxide 4, i.e., O2 + 2Fe = 2FeO; the molten cold steel and ferrous oxide form a semi-fluid that eventually condenses mostly at the bottom of the vacuum tank and in the downcomer, forming an oxide layer substrate.
[0014] The post-processing of furnace-cooled steel is as follows Figure 2 As shown, the downcomer 5 is inserted into the molten steel 14 to begin processing. As the vacuum level in the vacuum tank 1 decreases, the molten steel 14 is forced into the vacuum tank 1 by atmospheric pressure and melts the oxide layer that was previously solidified at the bottom of the vacuum tank and inside the downcomer, which floats on the molten steel 14 in the vacuum tank 1. During this period, aluminum alloy particles 9 are added through the feed pipe 8 and react with the ferrous oxide floating in the vacuum tank 1: 2Al + 3FeO = 3Fe + Al2O3. As the vacuum level decreases, molten steel circulation is formed, and Al2O3 enters the downcomer 5 along with the molten steel 14 and adheres to the inside and lower end of the downcomer 5, thereby achieving the purpose of automatic repair and strengthening.
[0015] In an industrial trial at a steel plant using a 350-ton RH furnace, the following results were observed after applying this method: Downcomer inner diameter recovery rate: For downcomers whose diameter was originally 750 mm but was expanded to 850 mm, 30 mm to 50 mm can be recovered each time this method is used; Maintenance cycle: The original high-intensity maintenance for each furnace has been extended to once every 5 furnaces; Repair rate of melt damage: 50mm~100mm can be restored each time this method is used.
[0016] The above content is only used to illustrate the technical solution of the present invention. Simple modifications or equivalent substitutions made by those skilled in the art to the technical solution of the present invention do not depart from the essence and scope of the technical solution of the present invention.
Claims
1. A method for automatically repairing enlarged inner diameter and melt damage in the downcomer tube of an RH furnace, characterized in that: The method includes the following steps: S1. Vacuum bath cold steel oxidation treatment During the production interval of the RH furnace, oxygen or a mixture of oxygen and coal gas is blown into the cold steel in the vacuum tank, causing the cold steel to oxidize and generate ferrous oxide (FeO). The molten cold steel and ferrous oxide form a semi-fluid that eventually condenses mostly at the bottom of the vacuum tank and inside the downcomer, forming an oxide layer substrate. S2. Aluminum alloy addition and alumina formation During the steelmaking stage, when the downcomer is inserted into the molten steel until the vacuum level drops to 20 kPa and the circulation has not yet formed, 30 kg to 120 kg more aluminum alloy is added to the vacuum tank according to the composition. The aluminum reacts with FeO and oxygen in the molten steel to generate high-concentration aluminum oxide (Al2O3) particles. S3. Circulating Adhesion Protective Layer As the vacuum level decreases to ≤20 kPa, the molten steel gradually forms a circulation. Al2O3 particles enter the downcomer along with the molten steel, solidify and adhere to the inner wall and lower end of the downcomer, forming a dense protective layer that fills the melting loss area and reduces the inner diameter.
2. The method for automatically repairing the enlarged inner diameter and melt damage of the downcomer tube in an RH furnace according to claim 1, characterized in that: In step S1, the oxygen flow rate for blowing oxygen into the vacuum tank for cooling steel is 700~1200 m³ / h. 3 / h.
3. The method for automatically repairing the enlarged inner diameter and melt damage of the downcomer tube in an RH furnace according to claim 1, characterized in that: In step S1, the oxygen-to-coal ratio of the oxygen-to-gas mixture is 1.2-1.8, and the flow rate is 400-600 m³ / s. 3 / h.
4. The method for automatically repairing the enlarged inner diameter and melt damage of the downcomer tube in an RH furnace according to claim 1, characterized in that: In step S2, the aluminum alloy with an Al content ≥90% is added to the vacuum tank.