A diamond / Cu-Cr-Zr based composite material with a gradient transition interface, its preparation method and application
By constructing nanoscale pits and microgrooves on the surface of diamond particles to form a metal transition layer and a discontinuous carbide reaction zone, the problem of poor interfacial bonding strength of diamond/copper composite materials is solved, achieving improved material properties with high thermal conductivity and low thermal expansion. This is suitable for heat dissipation and structural stability in high-power semiconductors and high-end molds.
Patent Information
- Application Number
- CN202611536710.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-17
AI Technical Summary
Existing diamond/copper composite materials have poor interfacial bonding strength, are prone to unbonded areas, internal pores and microcracks, and are prone to delamination failure under thermal cycling and mechanical vibration. Existing improvement schemes have failed to effectively solve the problems of interfacial reaction degree and diffusion compatibility.
By constructing nanoscale pits and microgrooves on the surface of diamond particles to form a metal transition layer, and generating discontinuous carbide reaction zones and continuous metal transition zones at the interface, a gradient transition interface is prepared by combining mechanical intercalation and chemical bonding. Combined with hot pressing sintering and aging treatment, the interfacial bonding strength and material density are improved.
It significantly improves the interfacial bonding strength and material density, reduces thermal resistance, enhances mechanical properties, and meets the heat dissipation and structural stability requirements of high-power semiconductors and high-end molds.
Smart Images

Figure CN123108380A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal matrix composites, and more particularly to a diamond / Cu-Cr-Zr based composite material with a gradient transition interface, its preparation method, and its application. Background Technology
[0002] In recent years, as high-end equipment components such as power semiconductors, microwave devices, semiconductor lasers, high-performance computing control chips, and high-heat-fluidity molding dies have been iteratively upgraded towards higher power density, miniaturization, and long-cycle, high-reliability, the heat dissipation problem of electronic devices has become increasingly prominent. As a core thermal management component, the heat dissipation substrate, in addition to possessing excellent thermal conductivity and transport capabilities, should also meet the requirements of thermal expansion compatibility with the functional materials of the chip, sufficient structural mechanical strength, excellent resistance to thermal cycling fatigue, and good machinability and brazing interconnection performance.
[0003] Among numerous candidate materials, diamond possesses ultra-high intrinsic thermal conductivity, low coefficient of thermal expansion, and high hardness; while copper alloys exhibit excellent thermal and electrical conductivity as well as good formability and machinability. Introducing diamond particles into a copper or copper alloy matrix to prepare diamond / copper composite materials can balance high thermal conductivity and low thermal expansion characteristics, meeting the stringent thermal control requirements of high-power, high-end equipment.
[0004] However, diamond is a typical covalent crystal, and the chemical affinity and liquid wettability between the copper and diamond phases are weak. If diamond particles are directly composited with a copper matrix without interface modification, defects such as unbonded areas, internal pores, and microcracks are easily formed at the interface, leading to a significant increase in interfacial thermal resistance. Furthermore, under the alternating thermal loads and mechanical vibration impacts during equipment service, interface delamination and diamond particle peeling failure are easily induced. To address these issues, most existing improvement schemes focus on coating the surface of diamond particles with active metals such as Ti, Cr, W, Mo, and Zr, or generating corresponding carbide transition layers to improve the interfacial bonding. For example, patent CN107916356B discloses a scheme for preparing diamond / copper composite materials by roughening diamond, plating it with tungsten, and then vacuum sintering; patent CN113235020B discloses a technique for preparing gradient diamond / copper composite materials by controlling the volume fraction of diamond using tungsten-plated diamond powder. While the above-mentioned solutions can improve the interfacial bonding effect to some extent, the degree of interfacial reaction of a single tungsten coating, the continuity of the coating, and the diffusion compatibility between the coating and the outer copper substrate still need to be further precisely controlled and optimized.
[0005] In addition, in terms of composite material preparation processes, although high-temperature melting and infiltration, liquid phase sintering, or long-term high-temperature holding processes are beneficial to the densification of the billet, excessively high thermal processes can exacerbate interdiffusion of elements between interfaces, cause coarsening of copper alloy matrix grains, and even damage to the diamond surface structure. Conversely, if a low-temperature sintering process is used, the plastic flow and atomic diffusion driving force of copper powder are insufficient, and pore defects are easily left inside the sintered billet, making it difficult to balance interface control and matrix densification.
[0006] In view of this, it is necessary to design an improved diamond / Cu-Cr-Zr based composite material with a gradient transition interface, as well as its preparation method and application, to solve the above problems. Summary of the Invention
[0007] The purpose of this invention is to provide a diamond / Cu-Cr-Zr based composite material with a gradient transition interface, its preparation method, and its application.
[0008] To achieve the above-mentioned objectives, in a first aspect, the present invention provides a diamond / Cu-Cr-Zr based composite material with a gradient transition interface, comprising:
[0009] Gradient-modified diamond particles, comprising diamond particles and a metal transition layer, wherein a Cu-Cr-Zr alloy matrix is disposed on the surface of the metal transition layer, and the surface of the diamond particles has a surface etching structure, which is at least one of nanoscale pits, microgrooves or protrusions, and at least a portion of the surface etching structure is filled by the metal transition layer, and the two are mechanically interlocked.
[0010] The average depth of the surface etching structure is 10-300 nm, and the surface arithmetic mean roughness Ra is 5-120 nm.
[0011] The metal transition layer includes a continuous metal transition region and a discontinuous carbide reaction region. The total thickness of the metal transition layer is 40-800 nm, the thickness of the continuous metal transition region is 10-700 nm, and the thickness of the discontinuous carbide reaction region is 5-200 nm. The surface coverage of the metal transition layer on the diamond particle is not less than 90%. The discontinuous carbide reaction region is close to the diamond particle, and the continuous metal transition region is used to suppress the diffusion of Cr and Zr in the Cu-Cr-Zr alloy matrix towards the diamond particle.
[0012] Preferably, the surface etching structure is formed by plasma surface etching, and the process parameters of the plasma surface etching are: the gas atmosphere is a mixture of inert gas and oxygen-containing gas, the power is 150-800 W, the working pressure is 5-150 Pa, and the processing time is 5-45 min.
[0013] Preferably, the inert gas is Ar and / or He, the oxygen-containing gas is O2, the volumetric flow rate ratio of the inert gas to the oxygen-containing gas is 3:1-20:1, and the total flow rate is 20-120 sccm.
[0014] Preferably, the composition of the Cu-Cr-Zr alloy matrix, by mass percentage, includes 0.30-1.20% Cr, 0.03-0.50% Zr, 98.1-99.4% Cu, with the balance being unavoidable impurities, and its D50 is 5-45 μm.
[0015] Secondly, the present invention provides a method for preparing a diamond / Cu-Cr-Zr based composite material with a gradient transition interface, comprising the following steps:
[0016] S1. Under mixed plasma conditions, diamond particles are surface etched to form a surface etched structure on the surface of the diamond particles. Then, a metal transition layer is deposited on the surface with the surface etched structure to obtain gradient modified diamond particles.
[0017] S2. The gradient-modified diamond particles obtained in step S1 are mixed with Cu-Cr-Zr alloy powder and pressed into shape to obtain a composite billet.
[0018] S3. Under a protective atmosphere, the composite preform obtained in step S2 is subjected to degassing treatment, hot pressing sintering densification treatment, pressure holding and cooling, and aging treatment in sequence to obtain a diamond / Cu-Cr-Zr based composite material with a gradient transition interface.
[0019] Preferably, in step S2, the mixing process of diamond particles and Cu-Cr-Zr alloy powder is carried out under an inert atmosphere for 0.5-6 h, and the volume fraction of gradient-modified diamond particles in the composite blank is 45-70%.
[0020] Preferably, in step S3, the process parameters for the hot pressing sintering densification treatment are as follows: temperature 750-1200℃, pressure 10-50 MPa, time 20-120 min; the process parameters for the degassing treatment are as follows: temperature 400-650℃, pressure 2-10 MPa, time 30-120 min.
[0021] Preferably, in step S3, the pressure holding and cooling is performed at a pressure of 10-50 MPa, cooling from 750-1200℃ to 300-500℃ at a cooling rate of 5-50℃ / min; the aging treatment is performed at a temperature of 430-520℃ for a time of 1-6 h.
[0022] Preferably, in step S2, the pressure of the pressing process is 150-500 MPa, and the pressing method is one of cold pressing, warm pressing, and cold isostatic pressing.
[0023] Thirdly, the present invention provides an application of diamond / Cu-Cr-Zr based composite material in the preparation of components with heat dissipation or thermal conductivity, wherein the component is one of semiconductor heat sink, electronic packaging substrate, microwave device heat dissipation substrate, wear-resistant thermally conductive component, and chip heat dissipation substrate.
[0024] The beneficial effects of this invention are:
[0025] The preparation method provided by this invention fundamentally solves the problems of poor wettability and easy delamination between diamond and copper alloys through multi-scale interface control and process synergy. Specifically, regarding the interface microstructure, plasma micro-etching is used to construct uniformly distributed micro-pits and grooves on the diamond surface, significantly increasing the specific surface area of the diamond particles and facilitating the mechanical interlocking of the metal transition layer and diamond. By forming an in-situ discontinuous carbide reaction zone and a continuous metal transition zone between the diamond and the alloy matrix, the diffusion of active elements to the diamond side can be effectively constrained by the continuous metal transition zone, avoiding the concentrated precipitation of brittle phases. Regarding densification, pressing molding, combined with a mixed particle size distribution of diamond particles, improves the packing density and uniformity of the blank. The subsequent pressure holding and cooling steps not only eliminate residual thermal stress in the sintered body but also suppress the initiation of microcracks and interface delamination during cooling. In terms of mechanical properties, the Cu-Cr-Zr matrix undergoes aging treatment, resulting in the precipitation of Cr and Zr elements as dispersed precipitates within the grains and at grain boundaries. This produces strong precipitation strengthening and grain boundary pinning effects, endowing the composite material with excellent mechanical properties. Based on the above-mentioned control of microstructure and densification degree, the composite material prepared by this invention achieves synergistic improvement in thermophysical properties, mechanical properties, and cycle stability, making it suitable for applications with extreme requirements for heat dissipation and structural stability, such as high-power semiconductor heat sinks, electronic packaging substrates, microwave device heat dissipation substrates, high-end molds, and wear-resistant thermally conductive components. Attached Figure Description
[0026] Figure 1 A schematic diagram of the structure of the diamond / Cu-Cr-Zr based composite material with a gradient transition interface provided by the present invention;
[0027] Figure 2 This is a flowchart illustrating the preparation method of the diamond / Cu-Cr-Zr based composite material with a gradient transition interface according to the present invention.
[0028] Figure 3 This is a microscopic image of the surface morphology of diamond particles after etching in Example 1 of the present invention;
[0029] Figure 4 This is a Raman image of the diamond particles after etching in Example 1 of the present invention;
[0030] Figure 5 An optical photograph of the composite material obtained in Example 1 of this invention;
[0031] Figure 6 This is a SEM image of the interior of the composite material obtained in Example 1 of the present invention;
[0032] Figure 7 This is an elemental distribution diagram inside the composite material obtained in Example 1 of the present invention;
[0033] Figure 8 This is a diagram showing the discontinuous carbide reaction zone and the continuous metal transition zone at the interface between diamond particles and the metal transition layer in the composite material prepared in Example 1 of the present invention.
[0034] The attached figures are labeled as follows:
[0035] 1. Diamond particles; 2. Surface etching structure; 3. Metal transition layer; 4. Cu-Cr-Zr alloy matrix. Detailed Implementation
[0036] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be described in detail below with reference to the accompanying drawings and specific embodiments.
[0037] It should also be noted that, in order to avoid obscuring the invention with unnecessary details, only the structures and / or processing steps closely related to the present invention are shown in the accompanying drawings, while other details that are not closely related to the present invention are omitted.
[0038] Additionally, it should be noted that the terms “comprising,” “including,” or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.
[0039] Terminology Explanation:
[0040] Continuous metallic transition zone: refers to a metallic enrichment layer that continuously covers the diamond particles circumferentially on a representative interface section and maintains connectivity between adjacent observation areas. The surface and cross-section of the diffusion transition layer are allowed to contain trace pinholes and thickness fluctuation defects. These defects are localized micro-defects that do not disrupt the overall diffusion conductivity, interface bonding, and stress transition function. Specifically, the effective continuous and intact area of the diffusion transition layer accounts for ≥90%, the maximum lateral dimension of a single defect area is ≤5μm, and the total area of defects within the same field of view accounts for ≤10%. Furthermore, pinholes are non-penetrating micropores, without through-hole defects penetrating the substrate, and the thickness fluctuation range does not exceed ±15% of the average thickness of the transition layer.
[0041] Discontinuous carbide reaction zone: refers to the chromium carbide reaction zone at the interface between diamond particles and Cu-Cr-Zr alloy matrix, which is generated by the in-situ reaction of W element with active carbon atoms on the diamond surface after plasma etching modification and high-temperature composite sintering. It is distributed in discrete point, island, or local sheet-like patterns.
[0042] Gradient transition interface: refers to the multi-layer structure from diamond-discontinuous carbide reaction zone-continuous metal transition zone-alloy matrix.
[0043] Please see Figure 1 As shown, the present invention provides a diamond / Cu-Cr-Zr based composite material with a gradient transition interface, comprising:
[0044] Gradient-modified diamond particles, comprising diamond particles 1 and a metal transition layer 3, wherein the surface of the diamond particles 1 has a surface etching structure 2, which is at least one of nanoscale pits, microgrooves or protrusions distributed on the diamond surface, and at least a portion of the surface etching structure 2 is filled by the metal transition layer 3, with a filling ratio greater than 95%, and the two are mechanically interlocked; wherein the average depth of the surface etching structure 2 is 10-300 nm, and the surface arithmetic mean roughness Ra is 5-120 nm.
[0045] More specifically, the metal transition layer 3 includes metals such as W, Cr, Ni, Ti, Ag, Mo, and Cu, and includes a continuous metal transition region and a discontinuous carbide reaction region. The total thickness of the metal transition layer 3 is 40-800 nm, the thickness of the continuous metal transition region is 10-700 nm, and the thickness of the discontinuous carbide reaction region is 5-200 nm. The coverage of the metal transition layer 3 on the surface of the diamond particles is not less than 90%. The discontinuous carbide reaction region is close to the diamond particles and is used to provide local chemical bonding. The continuous metal transition region is used to suppress the diffusion of Cr and Zr from the Cu-Cr-Zr alloy matrix to the diamond side.
[0046] The Cu-Cr-Zr alloy matrix 4 is disposed on the surface of the metal transition layer 3. Its composition, by mass percentage, includes 0.30-1.20% Cr, 0.03-0.50% Zr, 98.1-99.4% Cu, with the balance being unavoidable impurities.
[0047] On the other hand, please see Figure 2 As shown, the present invention also provides a method for preparing the above-mentioned composite material, which includes the following steps:
[0048] S1. Under mixed plasma conditions, diamond particles are surface etched to form a surface etched structure on the surface of the diamond particles, thereby obtaining diamond particles with a surface etched structure. A metal transition layer is deposited on the surface of the surface etched structure to obtain gradient modified diamond particles.
[0049] S2. The gradient-modified diamond particles obtained in step S1 are mixed with Cu-Cr-Zr alloy powder and pressed into shape to obtain a composite billet.
[0050] S3. Under a protective atmosphere, the composite preform obtained in step S2 is subjected to degassing treatment, hot pressing sintering densification treatment, pressure holding and cooling, and aging treatment in sequence to obtain a diamond / Cu-Cr-Zr based composite material with a gradient transition interface.
[0051] In some embodiments, in step S1, the mixed plasma is obtained by mixing an inert gas and an oxygen-containing gas, wherein the inert gas is Ar and / or He, the oxygen-containing gas is O2, the volumetric flow rate ratio of the two is 3:1-20:1, and the total flow rate is 20-120 sccm.
[0052] In some embodiments, in step S1, the diamond particles adopt a mixed particle size distribution, including first diamond particles with a particle size of 200-800 μm and second diamond particles with a particle size of 25-200 μm, wherein the volume ratio of the first diamond particles to the second diamond particles is 1:1-10:1. Specifically, the diamond particles need to be pretreated before use, which is achieved by sequentially sieving, degreasing, washing, and vacuum drying. The above pretreatment methods are conventional techniques in the art, and since they are not improvements of this invention, they are not limited here. In other embodiments, the diamond particles may also be made from a single particle size.
[0053] In some embodiments, the surface etching process conditions in step S1 are as follows: plasma power of 150-800 W, working pressure of 5-150 Pa, and processing time of 5-45 min.
[0054] In some embodiments, in step S2, the Cu-Cr-Zr alloy powder comprises, by mass percentage, 0.30-1.20% Cr, 0.03-0.50% Zr, and 98.1-99.4% Cu, with the balance being unavoidable impurities, and the powder has a D50 of 5-45 μm. Preferably, the Cr content is 0.50-0.90%, the Zr content is 0.05-0.20%, the Cu content is 98.5-99.5%, and the balance is unavoidable impurities.
[0055] In some embodiments, in step S2, the mixing process of diamond particles and Cu-Cr-Zr alloy powder is carried out under an inert atmosphere, such as nitrogen or helium, for 0.5-6 h. The volume fraction of gradient-modified diamond particles in the composite preform is 45-70%. When the volume fraction is less than 45%, it is difficult to fully utilize the high thermal conductivity and low thermal expansion of diamond. When the volume fraction is greater than 70%, the continuous phase of the copper alloy is reduced, and the difficulty of powder forming and densification increases.
[0056] In some embodiments, in step S2, the pressing pressure is 50-500 MPa, and the pressing method is one of cold pressing, warm pressing, and cold isostatic pressing.
[0057] In some embodiments, the process parameters for degassing in step S3 are as follows: temperature 400-650℃, pressure 2-10 MPa, time 30-120 min. This stage is used to remove adsorbed gases and residual organic matter from the green body.
[0058] In some embodiments, in step S3, the process parameters for interfacial diffusion are as follows: temperature 700-850℃, pressure 8-20 MPa, and holding time 15-40 min. Within this temperature range, the metal transition layer and the diamond surface undergo an interfacial reaction.
[0059] In some embodiments, in step S3, the process parameters for hot pressing sintering densification are as follows: temperature 750-1200℃, pressure 10-50 MPa, time 20-120 min. During this process, a discontinuous carbide reaction zone can be formed on the side of the metal transition layer close to the diamond.
[0060] In some embodiments, in step S3, the pressure holding cooling is to cool from 750-1200°C to 300-500°C at a cooling rate of 5-50°C / min under a pressure of 10-50 MPa, followed by depressurization.
[0061] In some embodiments, in step S3, the aging treatment temperature is 430-520℃ and the time is 1-6 h. During the aging treatment process, some Cr and Zr elements in the alloy matrix are dispersedly precipitated to form a dispersed nanoscale strengthening phase, thereby achieving dispersion strengthening of the matrix.
[0062] The following specific embodiments further illustrate the diamond / Cu-Cr-Zr based composite material with a gradient transition interface proposed in this invention, its preparation method, and its application:
[0063] Example 1
[0064] This embodiment provides a method for preparing a diamond / Cu-Cr-Zr based composite material with a gradient transition interface, comprising the following steps:
[0065] Single-peak diamond particles with a diameter of 150 μm were selected and ultrasonically cleaned sequentially with acetone, anhydrous ethanol, and deionized water for 15 min each, followed by vacuum drying at 90 °C for 2 h to obtain pretreated diamond particles. These diamond particles were then placed in a drum-type plasma treatment chamber, and Ar and O2 were introduced at a volumetric flow rate ratio of 8:1, a total flow rate of 40 sccm, a working pressure of 45 Pa, and a plasma power of 350 W for 20 min to prepare a surface etched structure on the diamond particles. The surface etched structure had an average depth of 70 nm and a surface arithmetic mean roughness Ra of 50 nm. A 250 nm thick W layer was then prepared on the surface of the diamond particles with the surface etched structure using a drum-type magnetron sputtering method to obtain gradient-modified diamond particles.
[0066] Gradient-modified diamond particles were mixed with Cu-Cr-Zr alloy powder and mixed under Ar atmosphere for 2 h. The mixture was then cold-pressed at 380 MPa to obtain a composite preform. The Cu-Cr-Zr alloy powder contained 0.65% Cr, 0.10% Zr, and 99.15% Cu, with the remainder being unavoidable impurities. The powder D50 was 18 μm, and the volume fraction of modified diamond particles in the composite preform was 60%.
[0067] The composite preform was placed in a vacuum hot press furnace and heated at a rate of 10°C / min, first to 520°C and held at 5 MPa for 60 min, then to 880°C and held at 20 MPa for 45 min, and finally to 1030°C with the pressure gradually increased to 60 MPa and held for 90 min for hot pressing. During this process, a discontinuous carbide reaction zone was formed on the side of the metal transition layer near the diamond, and a continuous metal transition zone was formed on the side away from the diamond. The thickness of the metal transition layer was 200 nm, the thickness of the continuous metal transition zone was 100 nm, and the thickness of the discontinuous carbide reaction zone was 100 nm. Then, the preform was cooled to 430°C at a rate of 2°C / min under 30 MPa pressure, then depressurized and cooled to room temperature, and aged at 470°C for 2 h to obtain the diamond / Cu-Cr-Zr based composite material.
[0068] It should be noted that, unless otherwise specified, the reagents and raw materials used in the embodiments of the present invention can all be obtained through commercial purchase.
[0069] The surface microstructure of the diamond particles after surface etching in this embodiment is shown in the following figure. Figure 3 As shown in the figure, the polyhedral diamond particles are generally golden yellow, with numerous regular pit-like surface etching structures (mostly polygonal or square depressions) distributed on their surface. This surface etching structure effectively increases the specific surface area and roughness of the diamond surface, significantly enhancing the mechanical interlocking between the metal transition layer and the diamond, thereby greatly improving the interfacial bonding strength and the overall stability of the composite material.
[0070] Raman images of diamond particles after surface etching are shown below. Figure 4 As shown, it is at 1332.3 cm. -1 The presence of a single sharp characteristic peak without any graphite impurities, consistent with the Raman peak position of pure diamond particles, indicates that the surface etching process effectively increases the surface mechanical interlocking effect without causing diamond graphitization or structural degradation.
[0071] Optical photographs of composite materials, such as Figure 5 As shown, the results indicate that diamond particles are uniformly distributed within the copper-chromium-zirconium matrix; the SEM image of the composite material is shown below. Figure 6 As shown, the corresponding element distribution diagram is as follows: Figure 7 As shown, Figure 6 This demonstrates good wettability between diamond and the copper-chromium-zirconium matrix, which can reduce the thermal resistance between diamond particles and copper-chromium-zirconium. Figure 7 The elements are uniformly distributed in the diamond particles and the copper-chromium-zirconium matrix, and the transition metal W is mainly coated on the diamond side.
[0072] The diagram shows the discontinuous carbide reaction zone and the continuous metal transition zone at the interface between diamond particles and the metal transition layer in the composite material. Figure 8 As shown, the results indicate that the diamond and the copper-chromium-zirconium matrix are tightly bonded through a discontinuous carbide reaction zone and a continuous metal transition zone, thereby reducing the overall thermal resistance.
[0073] Example 2
[0074] This embodiment provides a method for preparing a diamond / Cu-Cr-Zr based composite material with a gradient transition interface, comprising the following steps:
[0075] A first diamond particle with a particle size of 200-300 μm and a second diamond particle with a particle size of 25-50 μm were compounded at a volume ratio of 4:1. The mixture was then ultrasonically cleaned sequentially with acetone, anhydrous ethanol, and deionized water for 15 min each, and vacuum dried at 90℃ for 2 h to obtain pretreated diamond particles. These diamond particles were placed in a drum-type plasma treatment chamber, and Ar and O2 were introduced at a volume flow ratio of 10:1, a total flow rate of 80 sccm, a working pressure of 60 Pa, and a plasma power of 420 W for 18 min to prepare a surface etched structure on the diamond particles. The surface etched structure had an average depth of 100 nm and a surface arithmetic mean roughness Ra of 60 nm. A 320 nm thick W layer was then prepared on the surface of the diamond particles with the surface etched structure using a drum-type magnetron sputtering method to obtain gradient-modified diamond particles.
[0076] Gradient-modified diamond particles were mixed with Cu-Cr-Zr alloy powder and mixed under Ar atmosphere for 2 h. The mixture was then cold-pressed at 380 MPa to obtain a composite preform. The Cu-Cr-Zr alloy powder contained 0.80% Cr, 0.15% Zr, and 98.95% Cu, with the remainder being unavoidable impurities. The volume fraction of modified diamond particles in the composite preform was 65%.
[0077] The composite preform was placed in a vacuum hot press furnace and heated at a rate of 12℃ / min. First, it was heated to 550℃ and held at 6 MPa for 60 min, then held at 900℃ and 25 MPa for 60 min, and finally heated to 980℃ and the pressure was gradually increased to 70 MPa for 120 min for hot pressing. During this process, a discontinuous carbide reaction zone was formed on the side of the metal transition layer near the diamond, and a continuous metal transition zone was formed on the side away from the diamond. The thickness of the metal transition layer was 250 nm, the thickness of the continuous metal transition zone was 140 nm, and the thickness of the discontinuous carbide reaction zone was 110 nm. Then, it was cooled to 430℃ under 30 MPa pressure, depressurized, cooled to room temperature, and aged at 460℃ for 3 h to obtain the diamond / Cu-Cr-Zr based composite material.
[0078] Example 3
[0079] This embodiment provides a method for preparing a diamond / Cu-Cr-Zr based composite material with a gradient transition interface, comprising the following steps:
[0080] Diamond particles with a D50 of 100 μm were selected and ultrasonically cleaned sequentially with acetone, anhydrous ethanol, and deionized water for 15 min each, followed by vacuum drying at 90 °C for 2 h to obtain pretreated diamond particles. These diamond particles were then placed in a drum-type plasma treatment chamber, and Ar and O2 were introduced at a volumetric flow rate ratio of 12:1, a total flow rate of 100 sccm, a working pressure of 30 Pa, and a plasma power of 260 W for 12 min to prepare a surface etched structure on the diamond particles. The average depth of the etched structure was 150 nm, and the surface arithmetic mean roughness Ra was 80 nm. A 150 nm thick W layer was then prepared on the surface of the diamond particles with the surface etched structure using a drum-type magnetron sputtering method to obtain gradient-modified diamond particles.
[0081] Gradient-modified diamond particles were mixed with Cu-Cr-Zr alloy powder and mixed under Ar atmosphere for 2 h. The mixture was then cold-pressed at 380 MPa to obtain a composite preform. The Cu-Cr-Zr alloy powder contained 0.50% Cr, 0.08% Zr, and 99.32% Cu, with the remainder being unavoidable impurities. The powder D50 was 18 μm, and the volume fraction of modified diamond particles in the composite preform was 50%.
[0082] The composite preform was placed in a vacuum hot press furnace and heated at a rate of 15℃ / min, first to 520℃ and 5 MPa for 60 min, then to 880℃ and 20 MPa for 45 min, and finally to 900℃ with the pressure gradually increased to 50 MPa for 60 min for hot pressing. During this process, a discontinuous carbide reaction zone was formed on the side of the metal transition layer near the diamond, and a continuous metal transition zone was formed on the side away from the diamond. The thickness of the metal transition layer was 300 nm, the thickness of the continuous metal transition zone was 180 nm, and the thickness of the discontinuous carbide reaction zone was 120 nm. Then, the preform was cooled to 430℃ under 30 MPa pressure, depressurized, cooled to room temperature, and aged at 450℃ for 2 h to obtain the diamond / Cu-Cr-Zr based composite material.
[0083] Example 4
[0084] This embodiment provides a method for preparing a diamond / Cu-Cr-Zr based composite material with a gradient transition interface, comprising the following steps:
[0085] Single-peak diamond particles with a diameter of 150 μm were selected and ultrasonically cleaned sequentially with acetone, anhydrous ethanol, and deionized water for 15 min each, followed by vacuum drying at 90 °C for 2 h to obtain pretreated diamond particles. The diamond particles were then placed in a drum-type plasma treatment chamber, and Ar and O2 were introduced at a volume flow rate ratio of 8:1, a total flow rate of 120 sccm, a working pressure of 45 Pa, and a plasma power of 350 W for 20 min to prepare a surface etched structure on the diamond particles with an average depth of 180 nm and a surface arithmetic mean roughness Ra of 100 nm. A W layer with a thickness of 400 nm was prepared on the surface of the diamond particles with the surface etched structure using a drum-type magnetron sputtering method to obtain gradient-modified diamond particles.
[0086] Gradient-modified diamond particles were mixed with Cu-Cr-Zr alloy powder and mixed under Ar atmosphere for 2 h. The mixture was then cold isostatically pressed at 380 MPa to obtain a composite preform. The Cu-Cr-Zr alloy powder contained 0.70% Cr, 0.12% Zr, and 99.08% Cu, with the remainder being unavoidable impurities. The powder D50 was 18 μm, and the volume fraction of modified diamond particles in the composite preform was 58%.
[0087] The composite preform was placed in a vacuum hot press furnace and heated at a rate of 18°C / min, first to 520°C and 5 MPa for 60 min, then to 880°C and 20 MPa for 45 min, and finally to 850°C with the pressure gradually increased to 65 MPa for 100 min for hot pressing. During this process, a discontinuous carbide reaction zone was formed on the side of the metal transition layer near the diamond, and a continuous metal transition zone was formed on the side away from the diamond. The thickness of the metal transition layer was 320 nm, the thickness of the continuous metal transition zone was 200 nm, and the thickness of the discontinuous carbide reaction zone was 120 nm. Then, the preform was cooled to 430°C under 30 MPa pressure, depressurized, cooled to room temperature, and aged at 470°C for 2 h to obtain the diamond / Cu-Cr-Zr based composite material.
[0088] Comparative Example 1
[0089] The only difference between this comparative example and Example 1 is that the plasma surface etching step in Example 1 is omitted. All other experimental parameters and steps are the same as in Example 1, and will not be repeated here.
[0090] Comparative Example 2
[0091] The only difference between this comparative example and Example 1 is that the aging treatment step in Example 1 is omitted. All other experimental parameters and steps are the same as in Example 1, and will not be repeated here.
[0092] Comparative Example 3
[0093] The only difference between this comparative example and Example 1 is that the step of depositing the metal transition layer W in Example 1 is omitted. All other experimental parameters and steps are the same as in Example 1, and will not be repeated here.
[0094] The performance results of the composite materials obtained in Examples 1 to 4 and Comparative Examples 1 to 3 are shown in Table 1. The results show that the composite materials prepared by the present invention (Examples 1-4) have higher density, with a maximum density of 99.3%. Compared with the comparative examples, the thermal conductivity is significantly improved, with Example 2 reaching a thermal conductivity of 682 W / (m·K), while the interfacial thermal resistance is significantly reduced. In terms of mechanical properties, the flexural strength of the sample samples in the examples is all higher than 248 MPa, which is far superior to the comparative sample samples, with Example 2 reaching a flexural strength of 296 MPa. In the reliability test of 1000 cycles of thermal cycling from -55 to 150℃, the thermal conductivity retention rate of the composite materials obtained in Examples 1-4 after 1000 cycles is ≥90%, which is significantly better than the comparative group (83%-87%). The above results indicate that the preparation method proposed in this invention can effectively improve the interfacial bonding state between the filler and the matrix, reduce the interfacial thermal resistance, and significantly improve the mechanical strength and temperature cycling stability of the material while obtaining high thermal conductivity, meeting the requirements of heat dissipation materials for high-power electronic devices.
[0095] The composite materials prepared in Example 2 and Comparative Example 2 were applied to a high-power electronic module with a power of up to 1100W as a chip heat dissipation substrate. The surface temperature of the chip when the high-power chip was running at full load is shown in Table 2. The results show that the composite material prepared in Example 2 can effectively conduct and dissipate heat when used as a heat dissipation plate, significantly reducing the chip operating temperature and ensuring the stable and reliable operation of the module under high-temperature conditions.
[0096] Table 1. Performance results of the composite materials obtained in Examples 1 to 4 and Comparative Examples 1 to 3
[0097]
[0098] Table 2. Chip temperature when the composite material is used as a heat sink in Example 2 and Comparative Example 2.
[0099]
[0100] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention.
Claims
1. A diamond / Cu-Cr-Zr based composite material with a gradient transition interface, characterized in that, include: Gradient-modified diamond particles, comprising diamond particles and a metal transition layer, wherein a Cu-Cr-Zr alloy matrix is disposed on the surface of the metal transition layer, and the surface of the diamond particles has a surface etching structure, which is at least one of nanoscale pits, microgrooves or protrusions, and at least a portion of the surface etching structure is filled by the metal transition layer, and the two are mechanically interlocked. The average depth of the surface etching structure is 10-300 nm, and the surface arithmetic mean roughness Ra is 5-120 nm. The metal transition layer includes a continuous metal transition region and a discontinuous carbide reaction region. The total thickness of the metal transition layer is 40-800 nm, the thickness of the continuous metal transition region is 10-700 nm, and the thickness of the discontinuous carbide reaction region is 5-200 nm. The surface coverage of the metal transition layer on the diamond particle is not less than 90%. The discontinuous carbide reaction region is close to the diamond particle, and the continuous metal transition region is used to suppress the diffusion of Cr and Zr in the Cu-Cr-Zr alloy matrix towards the diamond particle.
2. The diamond / Cu-Cr-Zr based composite material according to claim 1, characterized in that, The surface etching structure is formed by plasma surface etching. The process parameters for plasma surface etching are as follows: the gas atmosphere is a mixture of inert gas and oxygen-containing gas, the power is 150-800 W, the working pressure is 5-150 Pa, and the processing time is 5-45 min.
3. The diamond / Cu-Cr-Zr based composite material according to claim 2, characterized in that, The inert gas is Ar and / or He, the oxygen-containing gas is O2, the volumetric flow rate ratio of the inert gas to the oxygen-containing gas is 3:1-20:1, and the total flow rate is 20-120 sccm.
4. The diamond / Cu-Cr-Zr based composite material according to claim 1, characterized in that, The composition of the Cu-Cr-Zr alloy matrix, by mass percentage, includes 0.30-1.20% Cr, 0.03-0.50% Zr, 98.1-99.4% Cu, with the balance being unavoidable impurities, and its D50 is 5-45 μm.
5. A method for preparing a diamond / Cu-Cr-Zr based composite material with a gradient transition interface as described in any one of claims 1-4, characterized in that, Includes the following steps: S1. Under mixed plasma conditions, diamond particles are surface etched to form a surface etched structure on the surface of the diamond particles. Then, a metal transition layer is deposited on the surface with the surface etched structure to obtain gradient modified diamond particles. S2. The gradient-modified diamond particles obtained in step S1 are mixed with Cu-Cr-Zr alloy powder and pressed into shape to obtain a composite billet. S3. Under a protective atmosphere, the composite preform obtained in step S2 is subjected to degassing treatment, hot pressing sintering densification treatment, pressure holding and cooling, and aging treatment in sequence to obtain a diamond / Cu-Cr-Zr based composite material with a gradient transition interface.
6. The preparation method according to claim 5, characterized in that, In step S2, the mixing process of diamond particles and Cu-Cr-Zr alloy powder is carried out under an inert atmosphere for 0.5-6 h, and the volume fraction of gradient-modified diamond particles in the composite blank is 45-70%.
7. The preparation method according to claim 5, characterized in that, In step S3, the process parameters for the hot pressing sintering densification treatment are as follows: temperature 750-1200℃, pressure 10-50 MPa, time 20-120 min; the process parameters for the degassing treatment are as follows: temperature 400-650℃, pressure 2-10 MPa, time 30-120 min.
8. The preparation method according to claim 5, characterized in that, In step S3, the pressure holding and cooling is performed at a pressure of 10-50 MPa, cooling from 750-1200℃ to 300-500℃ at a cooling rate of 5-50℃ / min; the aging treatment is performed at a temperature of 430-520℃ for a time of 1-6 h.
9. The preparation method according to claim 5, characterized in that, In step S2, the pressure of the pressing process is 150-500 MPa, and the pressing method is one of cold pressing, warm pressing, or cold isostatic pressing.
10. The application of a diamond / Cu-Cr-Zr based composite material as described in any one of claims 1 to 4 or a diamond / Cu-Cr-Zr based composite material prepared by any one of claims 5 to 9 in the preparation of a component with heat dissipation or thermal conductivity, wherein the component is one of a semiconductor heat sink, an electronic packaging substrate, a microwave device heat dissipation substrate, a wear-resistant thermally conductive component, and a chip heat dissipation substrate.
Citation Information
Patent Citations
A method for preparing a diamond / copper composite material with high thermal conductivity
CN107916356B
A gradient diamond / copper composite material and its preparation method
CN113235020B