High aspect ratio microchannel plate resistive layer and its preparation method and apparatus
By optimizing the cavity structure and process parameters, the problem of film thickness non-uniformity in the fabrication of high aspect ratio microchannel plate resistive layers was solved, achieving efficient and low-cost fabrication of microporous resistive layers and improving the performance and consistency of low-light imaging and particle detection devices.
Patent Information
- Application Number
- CN202611325768.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing atomic layer deposition technology has problems in preparing resistive layers for high aspect ratio microchannel plates, such as unreasonable carrier gas system design, missing cavity structure, rough workpiece pretreatment, poor matching between pulse timing and gas path, uneven reducing atmosphere, and accumulation of deposition errors in multiple cycles. These problems result in uneven film thickness and large resistance dispersion in the resistive layer on the inner wall of the micropore, making it difficult to meet the requirements of high-end detection and imaging.
The process employs a coupled approach involving a bypass-free flow-guiding cavity, staged micropore pretreatment, segmented differentiated carrier gas, and a two-stage pressurization and holding sequence. Through this process, the deep cleaning and activation of micropores and the efficient transport of precursors through deep pores are achieved, ensuring a uniform and stable flow field within the cavity and improving the uniformity of axial film thickness and the consistency of single-pore resistance.
It significantly improves the uniformity of film thickness and resistance value of the resistive layer inside the microchannel plate, reduces production costs, and improves the imaging uniformity and mass production consistency of the device, making it suitable for high-end low-light imaging and particle detection devices.
Smart Images

Figure CN123108529A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of microchannel plate (MCP) fabrication technology, specifically relating to a high aspect ratio microchannel plate resistive layer and its fabrication method and apparatus using atomic layer deposition (ALD) technology through chamber structure optimization and coating process control. Background Technology
[0002] Microchannel plates (MCPs) are core electron multiplication components for low-light imaging and particle detection devices. Ultra-high aspect ratio microchannel plates with an aspect ratio of 60:1-80:1 have high electron multiplication gain characteristics, and the uniformity of the resistive layer thickness on the inner wall of the micropores directly determines the consistency of device operation.
[0003] Existing atomic layer deposition techniques for fabricating microchannel plate resistive layers have the following drawbacks: 1. Inadequate carrier gas system design, resulting in poor uniformity of gas transport and replacement in deep pores: Existing ALD equipment generally adopts a single-component, constant-flow carrier gas purging mode, which is not adapted to the special structural characteristics of ultra-high aspect ratio micropores with narrow and deep cavities. A single, fixed carrier gas parameter cannot match the differentiated process requirements of precursor diffusion, interfacial reactions, and byproduct desorption within the deep pores. This easily leads to excessively high gas flow velocity at the micropore orifice and sluggish gas flow deep within the pores, forming significant gas flow gradients and precursor concentration gradients. This results in inconsistent precursor adsorption and reduction reaction degrees at different axial positions of the micropores, inducing axial deviations in resistivity film thickness and resistance. Simultaneously, reaction byproducts and residual impurities deep within the pores cannot be quickly and thoroughly purged and removed, easily leading to impure film composition and localized abnormal resistance, further exacerbating the deterioration of film uniformity.
[0004] 2. Lack of cavity structure, making it difficult to guarantee the consistency of the entire deposition process: Existing ALD deposition cavities are mostly general-purpose standardized cavities, without structural optimization and adaptation for large-size, array-type porous MCP workpieces. The inlet and outlet layout and internal structure of conventional cavities are prone to the formation of airflow vortices and purging dead zones within the cavity, resulting in significant differences in precursor partial pressure and reaction atmosphere in different areas of the cavity. This not only leads to inconsistent deposition effects of micropores at different locations on a single MCP board and large dispersion of intra-board resistance, but also amplifies process deviations between batches, reducing the consistency of device batch fabrication.
[0005] 3. The pretreatment process for the workpiece is crude, resulting in inherently insufficient uniformity of nucleation at the substrate interface: The existing pretreatment process for MCP workpieces has a low degree of refinement and a single process system, which cannot meet the pretreatment requirements for ALD deposition of micropores with ultra-high aspect ratios. The inner walls of the micropores in the MCP glass substrate easily adsorb trace impurities such as moisture, dust, and oil. Conventional simple cleaning and drying processes can only clean impurities on the surface of the micropores and cannot completely remove residual impurities and active adsorption groups deep in the micropores. Residual impurities will directly lead to sparse and uneven distribution of metal ALD nucleation sites, causing defects such as localized missed deposition, film agglomeration, and breakpoints.
[0006] 4. Poor matching between pulse timing and gas path, making it difficult to unify the reaction saturation in deep holes: The existing ALD process uses fixed and uniform precursor pulse and purge timing parameters, without differentiating and adapting them to the long-distance diffusion hysteresis characteristics of ultra-high aspect ratio micropores.
[0007] 5. Uneven substrate charge adsorption effect induces local nucleation growth differences: The MCP glass substrate is an insulating dielectric material. During the ALD process, the cavity plasma and gas flow friction easily cause a small amount of static charge to accumulate on the inner wall of the micropores. The uneven charge distribution at the opening, wall, and bottom of the ultra-high aspect ratio micropores will cause differences in the local precursor ion adsorption capacity. The nucleation density is abnormally high in the charge-rich areas, while nucleation is difficult in the charge-sparse areas. This easily leads to uneven defects such as local thickening and local incomplete deposition of the film, significantly increasing the resistance value fluctuation range of the resistive layer.
[0008] 6. Poor uniformity of the reducing atmosphere and uneven distribution of film composition purity: Metal ALD resistive layer deposition relies on reducing agents to achieve metal ion reduction and film formation. Existing ALD equipment mostly adopts a single-path reducing agent inlet method. For ultra-high aspect ratio micropore array structures, there are obvious concentration gradients of reducing agents in the radial direction of the plate surface and in the axial direction of the micropores. Excessive reducing agent concentration at the wellhead can easily lead to over-reduction and coarsening of metal particles, while insufficient reducing agent at the bottom of the well results in incomplete reduction, residual oxide impurities and defects, causing uneven distribution of resistivity, density and chemical composition of the film layer on the inner wall of the micropores, which seriously affects the overall electrical uniformity and stability of the resistive layer.
[0009] 7. Accumulated deposition errors from multiple cycles amplify global uniformity deviations: Metal resistive layers have narrow target sheet resistance ranges and require high resistance accuracy. Compared to oxide films, metal ALDs have extremely low thicknesses per cycle, requiring thousands of deposition cycles to achieve the target resistance value. The minute film thickness deviations, compositional deviations, and interface defects generated by ultra-high aspect ratio microvias in a single cycle accumulate with each cycle, amplifying resistance differences between the aperture and bottom, the center and edge of the plate, and between different substrates. Ultimately, this makes it difficult for MCP devices to meet the gain consistency requirements for high-end detection and imaging applications.
[0010] In summary, the aforementioned defects, whether individually or in combination, prevent the deposition of uniformly thick films across the entire micropore area of 60:1-80:1 microchannel plates. Therefore, it is necessary to develop novel coupled diffusion-enhanced ALD processes, adaptable coating chambers, and plasma activation pretreatment schemes to address these industry pain points. Summary of the Invention
[0011] In view of this, the main objective of the present invention is to provide a high aspect ratio microchannel plate resistive layer and its preparation method and apparatus. The technical problem to be solved is to simultaneously achieve deep cleaning and activation of MCP micropores, efficient transport of precursor deep pores, uniform and stable flow field in the chamber, and full saturation adsorption of precursors by means of coating cavity flow field structure, substrate pretreatment process, differentiation of working conditions to adapt to different gas systems and matching pressure holding treatment, thereby significantly improving the uniformity of axial film thickness of microchannel plate micropores, uniformity of single-pore resistance and uniformity of device imaging.
[0012] The objective of this invention and the technical problem it solves are achieved by the following technical solution. This invention proposes a method for preparing a high aspect ratio microchannel plate resistive layer, which uses atomic layer deposition to prepare a metal oxide resistive layer on the inner wall of the micropores of a microchannel plate with an aspect ratio of 60:1-80:1. The method includes workpiece pretreatment, cavity assembly, and ozone oxidation ALD cyclic film formation processes. The method is implemented through a non-bypass flow-guiding cavity, graded micropore pretreatment, segmented differentiated carrier gas, and dual-stage pressure-holding sequential coupling. The bypass-free flow guide cavity has no edge uniform air ring. Semi-cylindrical air blocking and sealing plates are symmetrically arranged on both sides of the cavity to block the side wall airflow bypass. The cavity is equipped with three detachable partition plates, which together with the sealing plates form four independent and sealed flow guide channels. The microchannel plate is vertically installed in the flow guide channel, with the micropore axis facing the air intake airflow. The segmented differentiated carrier gas: krypton or xenon is used as the carrier gas in the precursor adsorption stage, and high-purity nitrogen with a purity of ≥99.999% is used in the purging, oxidation and cavity cleaning stage. The dual-stage pressure holding sequence is as follows: after introducing the metal-organic precursor and ozone, all flow channels and exhaust ports are simultaneously closed to maintain pressure; after the pressure holding is completed, exhaust is simultaneously opened and high-purity nitrogen is introduced for purging.
[0013] Preferably, in the aforementioned method for preparing a high aspect ratio microchannel plate resistive layer, the microchannel plate has a aperture of 10 μm and a substrate thickness of 0.6 mm, or an aperture of 6 μm and a substrate thickness of 0.48 mm.
[0014] Preferably, in the aforementioned method for preparing the high aspect ratio microchannel plate resistive layer, the hierarchical micropore pretreatment includes ultrasonic cleaning, constant temperature drying, and argon plasma activation. Ultrasonic cleaning: The microchannel plate was ultrasonically cleaned in anhydrous ethanol and isopropanol at 40 kHz and 40-50℃ for 10-20 min respectively, and then ultrasonically cleaned with pure water 2-3 times, each time for 10-20 min. Constant temperature drying: Dry at 100-120℃ for 10-20 minutes; Argon plasma activation: The gas source is argon gas with a purity of ≥99.999%, the power is 80-120 W, the vacuum degree is 8-12 Pa, the argon gas flow rate is 30-50 sccm, and the activation time is 60-90 s.
[0015] Preferably, in the aforementioned method for preparing the high aspect ratio microchannel plate resistive layer, the ALD process temperature and pressure conditions are as follows: constant temperature of the cavity at 250-300 ℃ and cavity pressure at 100-150 Pa; temperature control of precursors in different zones: iridium acetylacetone at 160-170 ℃, and other precursors at 60-70 ℃.
[0016] Preferably, in the aforementioned method for fabricating a high aspect ratio microchannel plate resistive layer, the step of a single ALD cycle is as follows: S1 Precursor Adsorption: Krypton / Xenon flow rate is 200-300 sccm, precursor is introduced for 2-3 s, and pressure is maintained for 3-5 s; One purging: High-purity nitrogen flow rate is 200-300 sccm, purging time is 10-20 s; S2 Ozone Oxidation: Ozone flow rate is 20 sccm, introduced for 3-5 s, and maintained at pressure for 3-5 s; Secondary purging: High-purity nitrogen flow rate is 200-300 sccm, purging for 10-20 s; Repeat the cycle until the target film thickness is achieved.
[0017] Preferably, in the aforementioned method for preparing the high aspect ratio microchannel plate resistive layer, the metal-organic precursor is selected from one of trimethylmethylcyclopentadienyl platinum, bis(2,4-dimethylpentadienyl)ruthenium, iridium acetylacetonate, titanium tetrachloride, trimethylaluminum, tetra(ethylmethylamino)hafnium, and bis(dimethylamino)zinc, and the oxidizing gas is ozone.
[0018] Preferably, in the aforementioned method for preparing a high aspect ratio microchannel plate resistive layer, the single-cycle film formation rate of each precursor within the 250-300 °C process window is: Platinum, ruthenium, and iridium precursors: 0.3-0.5 nm / cycle; Titanium, aluminum, and hafnium precursors: 0.5-1.0 nm / cycle; Zinc-based precursor: 1.1-1.5 nm / cycle.
[0019] The objectives of this invention and the technical problems it solves can be further achieved by the following technical measures. This invention proposes a high aspect ratio microchannel plate resistive layer, wherein the resistive layer is deposited on the inner wall of the micropores of a microchannel plate with an aspect ratio of 60:1-80:1, and is an oxide film of at least one metal selected from platinum, ruthenium, iridium, titanium, aluminum, hafnium, and zinc. The film thickness deviation along the micropore axis of the resistive layer is ≤1%, the film thickness uniformity of a single plate is ≤0.6%, and the film thickness uniformity between multiple plates is ≤0.4%. The resistive layer is prepared by the above-described method.
[0020] The objective of this invention and the technical problems it solves can be further achieved by the following technical measures. This invention proposes a device for preparing a high aspect ratio microchannel plate resistive layer, comprising a coating cavity, a pretreatment unit, a multi-channel gas source unit, and a pressure holding timing electronic control unit; The coating cavity has an edgeless gas equalization ring and semi-cylindrical gas blocking plates on both sides. Three detachable partition plates inside the cavity divide it into four independent flow channels. Each channel is equipped with an independent air inlet and a synchronous electrically controlled air extraction port. The pressure difference between the channels is ≤5 Pa. After the workpiece is clamped, the error between the axial direction of the microhole and the parallelism of the air inlet is ≤0.1°. The assembly gap between the blocking plate, partition plate and cavity is ≤0.1 mm. The multi-channel gas source unit is equipped with a krypton / xenon carrier gas branch, a high-purity nitrogen purging branch, and an ozone reaction branch; The pressure holding timing electronic control unit executes the following: after the precursor and ozone are introduced, the valve is closed and pressure is maintained for 3-5 seconds. After the pressure holding is completed, gas is simultaneously extracted and nitrogen is introduced for purging. The pretreatment unit integrates a 40 kHz ultrasonic cleaning module, a 100-120℃ drying module, and an argon plasma activation module.
[0021] Preferably, in the aforementioned apparatus for preparing a high aspect ratio microchannel plate resistive layer, the sealing plate has an axial length of 162.48 mm, a cross-sectional diameter of 249.99 mm and a width of 30 mm for the adapted semi-circular cavity, the partition plate includes one piece with a length of 249.99 mm and two pieces with a length of 233.24 mm, all partition plates are 10 mm wide and 25 mm high, and the ends are arc-shaped to fit the inner circle of the cavity with an inner diameter of 250 mm; the cross-sectional dimensions of a single flow channel are 40 mm long and 25 mm wide.
[0022] Preferably, in the aforementioned apparatus for preparing the high aspect ratio microchannel plate resistive layer, the parameters of the argon plasma activation module are as follows: high-purity argon gas supply, power of 80-120 W, vacuum degree of 8-12 Pa, argon gas flow rate of 30-50 sccm, and activation time of 60-90 s; and the temperature control of the ultrasonic module is 40-50 ℃.
[0023] Preferably, in the aforementioned apparatus for preparing a high aspect ratio microchannel plate resistive layer, the coating cavity is equipped with precursor zone heating temperature zones: the acetylacetone-iridium temperature zone is 160-170 ℃, and the other precursor temperature zones are 60-70 ℃; the main reaction zone of the cavity is kept at a constant temperature of 250-300 ℃, and the cavity pressure is 100-150 Pa.
[0024] The objectives of this invention and the technical problems it solves can be further achieved by the following technical measures. This invention proposes a low-light photodetector device comprising a microchannel plate, wherein the inner wall of the micropores of the microchannel plate is provided with the aforementioned high aspect ratio microchannel plate resistive layer; the low-light photodetector device is a low-light night vision device, a high-energy particle detector, or a vacuum electron multiplier.
[0025] Compared with existing technologies, the high aspect ratio microchannel plate resistive layer and its preparation method and apparatus described in this invention have the following beneficial effects: 1. Excellent uniformity of resistive layer The cavity flow field offers strong controllability, significantly improving film thickness uniformity. This invention, through edge gas blocking and a four-channel independent partition structure, completely eliminates edge airflow short-circuiting and chamber turbulence. Combined with high-precision pressure-holding saturation timing and the deep-hole penetration advantage of krypton / xenon heavy carrier gas, it can achieve axially uniform film deposition in ultra-high aspect ratio micropores. The resulting resistive layer axial thickness deviation is ≤1%, single-sheet film thickness uniformity is ≤0.6%, and inter-sheet film thickness uniformity is ≤0.4. This effectively balances the film thickness and resistance value of each micropore, reduces the voltage drop difference in a single pore, lowers the gain dispersion of MCP devices, and thoroughly improves the problem of uneven imaging brightness.
[0026] 2. Enhance membrane-substrate bonding and device stability The pretreatment effect is excellent, and the film-substrate adhesion and device stability are significantly improved. The low-power plasma activation process can complete the deep cleaning and surface activation of micropores without zero substrate damage, which greatly increases the number of active sites and surface energy on the substrate surface, improves the interfacial bonding strength of the film and substrate, effectively eliminates defects such as film peeling, pinholes, and local thin spots, reduces device operating gain drift, and greatly enhances long-term operating stability.
[0027] 3. Cost reduction The gas is adapted to different operating conditions, balancing coating performance and mass production costs. It employs a differentiated gas supply system of "krypton / xenon transport and nitrogen purging," significantly reducing rare gas consumables consumption and lowering production costs by more than 50% compared to a fully rare gas process. Compared to traditional single-nitrogen processes, it improves the transport efficiency of deep-hole precursors, perfectly adapting to the requirements of ultra-high aspect ratio micro-pore coating, achieving bidirectional compatibility between high-precision coating and low-cost mass production.
[0028] 4. Suitable for mass production, improving efficiency. The overall process exhibits excellent synergy, resulting in a significant improvement in mass production yield and capacity. This invention systematically addresses the core technical deficiencies of traditional MCP coating through integrated synergistic optimization of structure, pretreatment, gas system, and sequential processes. This improves product coating yield, effectively reduces rework and scrap costs, shortens single-batch production time, and significantly enhances batch production consistency and capacity, making it fully adaptable to the large-scale industrial mass production of high-precision MCP.
[0029] 5. The process is simple and easy to mass-produce. The coating preparation materials of this invention are clearly defined, the preparation process is simple, no high-end equipment or harsh working conditions are required, the coating process parameters are reasonably adjustable, the stability is high, the quality fluctuations caused by human operation can be reduced, it is suitable for industrialized assembly line production, and effectively controls production costs and improves product qualification rate.
[0030] 6. Highly versatile manufacturing process, adaptable to various specifications of high aspect ratio MCP products. The partitioned flow field control, differentiated gas supply, and timing regulation process of this invention can be flexibly adapted to MCP products with different aperture, aperture length, and aspect ratio parameters. The process is highly adjustable and versatile, and is suitable for precision coating production of conventional high aspect ratio MCPs. It effectively broadens the product compatibility range. One process can realize mass production of multiple product categories, greatly improve the versatility and reusability of the production line, and reduce the equipment and process R&D costs for enterprises to produce multiple product categories.
[0031] 7. The manufacturing process is highly safe, environmentally friendly, and pollution-free. This invention employs a gas physical transport deposition process throughout, eliminating the use of strong acids, alkalis, or corrosive chemicals in the reaction. This avoids the problems associated with traditional chemical coating processes, such as wastewater pollution, substrate corrosion, chemical residues, and operational hazards. The process generates no toxic or harmful byproducts, and the waste gas can be easily treated using conventional purification equipment before being discharged in compliance with standards. The production process is safe, green, and environmentally friendly, meeting industrial green production standards, while also eliminating the additional costs associated with wastewater treatment and corrosion prevention equipment.
[0032] The above description is merely an overview of the technical solution of the present invention. In order to better understand the technical means of the present invention and to implement it in accordance with the contents of the specification, the preferred embodiments of the present invention are described in detail below. Attached Figure Description
[0033] Figure 1 is a schematic cross-sectional view of the fabrication device for the high aspect ratio microchannel plate resistive layer of the present invention. Figure 2 is a top view of the internal structure of the coating cavity of the device for preparing the high aspect ratio microchannel plate resistive layer of the present invention. Among them, 1-heat source precursor source bottle; 2-coating cavity; 3-upper air inlet flange of the cavity; 4-precursor and reaction gas exhaust pipe; 5-vacuum unit; 6, 7, 8-liquid source precursor source bottle; 9-sealing plate; 10-precursor and reaction gas exhaust port; 11-partition plate; 12-microchannel plate clamp; 13-microchannel plate; 14-precursor and reaction gas inlet. Detailed Implementation
[0034] To further illustrate the technical means and effects adopted by the present invention to achieve the intended purpose, the following detailed description, in conjunction with preferred embodiments, provides a detailed explanation of the specific implementation, structure, features, and effects of a high aspect ratio microchannel plate resistive layer and its preparation method and apparatus according to the present invention. Furthermore, specific features, structures, or characteristics in one or more embodiments may be combined in any suitable form.
[0035] Unless otherwise specified, all materials and reagents mentioned below are commercially available products well-known to those skilled in the art; unless otherwise specified, all methods described are methods known in the art. Unless otherwise defined, the technical or scientific terms used should have the ordinary meaning understood by those skilled in the art. Where specific experimental steps or conditions are not specified below, they can be performed according to the conventional experimental steps or conditions described in the literature in this field.
[0036] Some embodiments of the present invention disclose a method for preparing a high aspect ratio microchannel plate resistive layer. The method involves atomic layer deposition (ALD) on the inner wall of microchannel plate micropores with an aspect ratio of 60:1-80:1 to prepare a metal oxide resistive layer. The method includes substrate pretreatment, cavity assembly, and ozone oxidation ALD cyclic film formation. The method is implemented through a non-bypass flow-guiding cavity, hierarchical micropore pretreatment, segmented differentiated carrier gas, and dual-stage pressure-holding sequential coupling. For example, the pore size of the microchannel plate micropores is 10 micrometers, and the thickness is 0.6 mm. When the aspect ratio is less than 60:1, the electron multiplication path of the micropore is short, and the device gain cannot meet the standard for ultra-high sensitivity weak light detection. This invention relies on a four-channel independent zone gas supply structure, krypton / xenon heavy carrier gas precursor delivery, and high-precision pressure holding saturation timing to break through the bottleneck of traditional ALD deep hole coating. It can stably achieve axial uniform coating of ultra-high aspect ratio micropores of 60:1-80:1. When the aspect ratio is greater than 80:1, the micropore length is too long, the precursor delivery resistance increases sharply, and the coating quality at the bottom of the hole deteriorates.
[0037] The substrate pretreatment uses high-purity argon gas with a purity of 99.999% or higher; the argon gas is an inert gas, relying solely on Ar... +Ion physical sputtering completes the pretreatment process without chemically reacting with the glass or metal electrodes. The use of ultra-high purity (99.999% or higher) is to prevent trace impurities from causing device failure. If the high-purity argon gas is below 99.999%, it will contain trace amounts of oxygen, water vapor, and hydrocarbon impurities. Under high-energy plasma excitation, these impurities easily decompose and deposit on the inner walls of the microchannel plate's micropores, forming micro-oxidation spots and residual carbon contamination. This directly leads to pinholes, thin spots, and localized resistance anomalies in the subsequent ALD coating. High-purity argon gas (99.999% or higher) has extremely low impurity content, completely avoiding the introduction of secondary contaminants during the pretreatment stage and ensuring an ultra-clean substrate state for the micropore inner walls.
[0038] The bypass-free flow guiding cavity eliminates the edge air equalization ring. Semi-cylindrical air blocking plates are symmetrically arranged on both sides of the cavity to block the side wall airflow bypass. Three detachable partition plates are installed inside the cavity, which together with the blocking plates form four independent sealed flow guiding channels. The microchannel plate is vertically installed in the flow guiding channel, with the micropore axis facing the air intake airflow. The segmented differentiated carrier gas: krypton or xenon is used as the carrier gas in the precursor adsorption stage, and high-purity nitrogen with a purity of ≥99.999% is used in the purging, oxidation and cavity cleaning stage. The dual-stage pressure holding sequence is as follows: after introducing the metal-organic precursor and the oxidizing gas, all flow channels and exhaust ports are simultaneously closed to maintain pressure; after the pressure holding is completed, the exhaust is simultaneously opened and high-purity nitrogen is introduced for purging.
[0039] In some alternative embodiments, the microchannel plate is specified to have an aperture of 10 μm and a substrate thickness of 0.6 mm, or an aperture of 6 μm and a substrate thickness of 0.48 mm.
[0040] In some optional embodiments, the hierarchical micropore pretreatment includes ultrasonic cleaning, constant temperature drying, and argon plasma activation. Ultrasonic cleaning: The microchannel plate is sequentially ultrasonicated with anhydrous ethanol and isopropanol at 40-50 kHz and 40-50 ℃ for 10-20 min each, followed by ultrasonic cleaning with pure water 2-3 times, each time for 10-20 min; constant temperature drying: drying at 100-120 ℃ for 10-20 min. This setup is responsible for oil dissolution, adhesive removal, and dehydration, ultimately achieving a low-contamination, low-moisture, oil-free, and dust-free state on the MCP substrate surface, ensuring the continuity of subsequent coatings and resulting in more uniform overall coating adhesion. The microchannel plate is ultrasonicated with anhydrous ethanol and isopropanol at 40-50 kHz. Below 40 kHz, the amplitude increases, subjecting the ultra-thin glass channel walls of the microchannel plate to repeated strong shock waves, causing microcracks in the inner walls of the micropores and chipping at the channel edges. Above 50 kHz, cleaning efficiency drops significantly, and even with extended time, the same cleanliness cannot be achieved as with 40-50 kHz, reducing the batch pass rate. Below 40℃, the efficiency of low-temperature ultrasonic removal of alcohol residues with pure water is low, resulting in water spots and impurities after drying, and creating localized high resistance points in the ALD process. Above 50℃, anhydrous ethanol and isopropanol have low boiling points and evaporate rapidly at high temperatures, causing a continuous decrease in solvent concentration within the tank, reducing cleaning ability, and simultaneously accumulating large amounts of flammable and explosive alcohol vapors, posing significant safety hazards. Insufficient ultrasonic time and cycles will result in incomplete replacement of surface impurities (anhydrous ethanol and isopropanol); residual trace amounts of isopropanol will carbonize after drying, forming discrete carbon spots on the inner wall of the channel. Upon entering the ALD chamber, carbon impurities will cause resistance drift in the metal oxide resistive layer, leading to localized high resistance / leakage. Excessive ultrasonic time and cycles require longer waiting times and consume large amounts of ultrapure water, lengthening the production cycle and increasing production costs. Insufficient oven temperature and time after cleaning will result in capillary water binding in micropores and prolonged retention of anhydrous ethanol and isopropanol deep within the channels. Excessive oven temperature and time can cause trace amounts of moisture remaining deep within the micropores to vaporize instantly, creating instantaneous high-pressure steam inside the sealed microchannels, resulting in microcracks and chipping at the edges of the thin-walled glass.
[0041] Argon plasma activation: The gas source is argon gas with a purity ≥99.999%, the power is 80-120 W, the vacuum degree is 8-12 Pa, the argon flow rate is 30-50 sccm, and the activation time is 60-90 s. The main purpose of this setup is to perform gentle, non-destructive argon plasma activation on the substrate of the microchannel plate, removing residual moisture and trace organic matter from the surface, activating the surface to enhance the adhesion of subsequent film layers, and ensuring the cleanliness and uniformity of the microchannel inner wall, providing a stable and highly clean surface state for the coating process. If the power is below 80 W, the plasma density will be insufficient, and the Ar ion bombardment energy will be too weak. If the power is above 120 W, the Ar ion energy will be too high, causing etching and bombardment damage to the inner wall of the glass micropores. If the vacuum degree is below 8 Pa, the gas density will be too low, the plasma will be weak, the ion density will be insufficient, and the activation of deep channels will be worse, resulting in unstable overall pretreatment effects. A vacuum level higher than 12 Pa results in an excessive number of gas molecules, causing Ar ions to collide frequently before reaching the tube wall, significantly reducing bombardment energy, worsening activation, and leading to incomplete surface modification. If the argon flow rate is below 30 sccm, contaminants and residual moisture within the chamber cannot be removed promptly. If the argon flow rate is above 50 sccm, a large amount of gas is directly pumped away, diluting the plasma, decreasing ion density, reducing activation efficiency, and worsening the effect. If the activation time is below 60 seconds, surface activation is incomplete, resulting in insufficient functional groups and incomplete removal of surface contaminants and residual hydrocarbons. If the activation time is above 90 seconds, the cumulative effect of ion bombardment intensifies, leading to excessive etching of the glass inner wall.
[0042] In some optional embodiments, the temperature and pressure conditions of the ALD process are as follows: constant temperature of the chamber at 250-300 ℃ and pressure of 100-150 Pa; temperature control of precursors in different zones: iridium acetylacetone at 160-170 ℃, and other precursors at 60-70 ℃.
[0043] In some optional embodiments, the single ALD cycle step is described as follows: S1 Precursor Adsorption: Krypton / Xenon flow rate is 200-300 sccm, precursor is introduced for 2-3 s, and pressure is maintained for 3-5 s; One purging: High-purity nitrogen flow rate is 200-300 sccm, purging time is 10-20 s; S2 Ozone Oxidation: Ozone flow rate is 20-30 sccm, introduced for 3-5 s, and maintained at pressure for 3-5 s; Secondary purging: High-purity nitrogen flow rate is 200-300 sccm, purging for 10-20 s; Repeat the cycle until the target film thickness is achieved.
[0044] Specifically, in the precursor transport and adsorption stage, high-density, high-inertia krypton or xenon gas is used as the carrier gas, with the precursor introduced into the cavity for 2-3 seconds at a flow rate of 200-300 sccm. In the purging and impurity removal stage, high-purity nitrogen (99.999%) is switched as the purging gas, with a flow rate of 200-300 sccm and a purging time of 10-20 seconds. After purging, ozone is introduced at a flow rate of 20-30 sccm for 3-5 seconds. Then, purging is performed again with high-purity nitrogen (99.999%) carrier gas at a flow rate of 200-300 sccm for 10-20 seconds. The main purpose is to provide a stable process environment for the atomic layer deposition of resistivity layers in high aspect ratio microchannel plates, ensuring sufficient reaction, controllable adsorption, uniform diffusion, and easy removal of byproducts. This guarantees that the resistivity layer is continuous, dense, uniformly shaped, and has stable resistance on the inner wall of the micropores. Any deviation from the specified parameter range will lead to abnormal film growth, failure of deep-pore coverage, increased impurity content, and increased film defects, ultimately resulting in increased dark current, uneven gain, poor consistency, and reduced yield in MCP. When the precursor and ozone are introduced separately, the extraction port is immediately closed after the four independent flow channels are established. The system is then sealed and pressurized for 3–5 seconds to allow the precursor gas to fully fill the entire channel space and slowly wet the depth of the micropores, achieving uniform saturated adsorption across the entire area. After the pressure adsorption is completed, the built-in extraction structure is simultaneously activated, along with a large flow rate of high-purity nitrogen, to quickly purge and remove impurities. The main purpose is to eliminate the rapid carry-away effect of the gas flow on the precursor through static pressure holding, allowing the gas to fully fill the guiding channel and slowly wet the deep part of the high aspect ratio micropores, achieving uniform saturation adsorption on the entire inner wall and ensuring the uniform shape of the resistance layer from the orifice to the bottom. Synchronous gas extraction and rapid purging can quickly remove excess precursors and by-products, avoiding gas-phase side reactions and particulate contamination. At the same time, it ensures that the pressure and flow rate of the four channels are highly consistent, improving the uniformity between multiple parallel coatings and the repeatability of the process. The sealed pressure holding is 3-5 seconds. If the pressure holding time is too short, the deep hole wetting will be insufficient and the adsorption will be uneven; if the time is too long, it will easily cause side reactions and particulate contamination. Asynchronous gas extraction or improper purging will lead to flow field disturbance and film defects, ultimately affecting the resistance uniformity, dark current level and yield of the microchannel plate.
[0045] In some optional embodiments, the organometallic precursor is selected from one of trimethylmethylcyclopentadienyl platinum, bis(2,4-dimethylpentadienyl)ruthenium, iridium acetylacetonate, titanium tetrachloride, trimethylaluminum, tetra(ethylmethylamino)hafnium, and bis(dimethylamino)zinc, and the oxidizing gas is ozone. This is because: First, these precursors all possess moderate saturated vapor pressure and excellent thermal stability, enabling stable vaporization without thermal decomposition. They can be efficiently and uniformly transported by heavy carrier gases such as xenon / krypton, making them suitable for ultra-high aspect ratio microporous pressure-maintaining saturated adsorption processes without high-temperature cracking and pore blockage or low-temperature condensation and deposition defects. Second, this series of metal-organic precursors has a wide ALD reaction window and high adsorption activity, allowing for uniform nucleation on the glass substrate surface, ensuring continuous and dense film thickness on the inner wall of the micropores. Third, the deposited ruthenium, iridium, aluminum, zinc, hafnium, and titanium metal films exhibit controllable resistivity, resistance to electron bombardment, and excellent anti-aging properties, making them perfectly suited for the long-term high-voltage electron multiplication working environment of MCP. They can stably form a uniform and controllable microporous resistive layer, effectively balancing the single-pore pressure drop and suppressing gain dispersion. Fourth, the reaction byproducts of these precursors are highly volatile and can be completely removed by rapid purging with high-purity nitrogen, leaving no residual impurities and avoiding pinholes, resistance shifts, and local defects in the film. Ozone can be used as a precursor for preparing resistive layers of microchannel plates, mainly because six precursors—di(2,4-dimethylpentadienyl)ruthenium, iridium acetylacetonate, titanium tetrachloride, trimethylaluminum, tetra(ethylmethylamino)hafnium, and bis(dimethylamino)zinc—can react with ozone to form films. Furthermore, ozone molecules are small in size and have strong diffusion capabilities, allowing them to uniformly penetrate microchannels with aspect ratios of tens of times. The film thickness has no gradient at the inlet, middle, and bottom of the channel, resulting in a consistent resistance throughout the entire process.
[0046] In some optional embodiments, the single-cycle film formation rate of each precursor within the 250-300 °C process window is as follows: Platinum, ruthenium, and iridium precursors: 0.3-0.5 nm / cycle; Titanium, aluminum, and hafnium precursors: 0.5-1.0 nm / cycle; Zinc precursor: 1.1-1.5 nm / cycle.
[0047] Within the 250-300℃ process window, the film deposition rate for platinum, ruthenium, and iridium precursors is limited to 0.3-0.5 nm / cycle. Below 0.3 nm / cycle, the adsorption reaction becomes unsaturated, resulting in discontinuous film layers and low production efficiency. Above 0.5 nm / cycle, precursor thermal decomposition occurs, compromising the self-limiting properties of ALD and increasing the axial film thickness gradient of high aspect ratio micropores. For titanium, aluminum, and hafnium precursors, the film deposition rate is 0.5-1.0 nm / cycle. Below 0.5 nm / cycle, the rate is too low, leading to insufficient deposition efficiency and localized film loss. Above 1.0 nm / cycle, the rate is too high, causing gas-phase decomposition and reducing film density. For zinc precursors, the film deposition rate is 1.1-1.5 nm / cycle. Below 1.1 nm / cycle, the rate is too low, increasing the number of cycles and reducing production capacity. Above 1.5 nm / cycle, gas-phase particulate contamination is likely to occur, leading to excessive deposition at micropore openings and deterioration of device resistance stability.
[0048] In the above technical solution, the present invention first selects suitable materials; then, the microchannel plate workpiece is subjected to ultrasonic cleaning with organic solvents, ultrasonic cleaning with pure water, and high-temperature drying to remove surface oil, particles, and water stains. Next, argon plasma activation treatment is used to clean and activate the inner wall of the microchannel. By optimizing the coating cavity structure, blocking the airflow bypass at the cavity edge, and setting four independent sealed flow channels, the process gas can flow through the micropores axially. The deposition process adopts a segmented atomic layer deposition process. First, a heavy-duty rare gas is used to carry the precursor into the cavity. Through sealed pressure maintenance, the precursor fully wets the depth of the micropores and achieves uniform saturated adsorption throughout the entire area. After adsorption, high-purity nitrogen is used to quickly purge and remove residual impurities and excess precursor. Then, a reaction gas is introduced to complete the surface chemical reaction and film formation. Through repeated cyclic deposition, a continuous, dense, uniformly thick, and highly consistent resistive layer is formed on the inner wall of the high aspect ratio microchannel, significantly improving the overall performance of the microchannel plate and the yield of mass production.
[0049] Some embodiments of the present invention also provide a high aspect ratio microchannel plate resistive layer, deposited on the inner wall of the micropores of a microchannel plate with an aspect ratio of 60:1-80:1, and is an oxide thin film of at least one metal selected from platinum, ruthenium, iridium, titanium, aluminum, hafnium, and zinc. The film thickness deviation along the micropore axis of the resistive layer is ≤1%, the film thickness uniformity of a single plate is ≤0.6%, and the film thickness uniformity between multiple plates is ≤0.4%. The resistive layer is prepared by the above-described preparation method. This configuration can achieve a uniform resistive layer thickness from the opening to the bottom of the micropores in the ultra-high aspect ratio microchannel plate, reduce the resistance dispersion within a single plate and between multiple plates, reduce the difference in electron multiplication rate, suppress uneven imaging brightness, and ensure the stability of device operation and the consistency of batch products. The selected metal oxide has the characteristics of resistance to electron bombardment and stable performance, and is suitable for the high voltage multiplication conditions of micro-photodetector devices. These performance indicators are achieved by the coupling preparation method of the present invention.
[0050] In the above technical solution, the present invention selects a specific metal oxide as the resistive layer material and strictly limits the uniformity of film thickness along the axis, between single and multiple plates of high aspect ratio micro-holes. It relies on the ALD process to achieve conformal deposition of the inner wall of the micro-hole. This can ensure that the internal resistance of all microchannels of the 60:1-80:1 ultra-high aspect ratio microchannel plate is continuous, stable and highly consistent, effectively suppressing gain drift, inter-channel gain dispersion and imaging brightness distortion, reducing arcing and noise defects, and improving the imaging quality, working stability and batch product consistency of microchannel plate devices.
[0051] like Figure 1 , Figure 2 As shown, some embodiments of the present invention also provide a device for preparing a high aspect ratio microchannel plate resistive layer, including a coating cavity 2, a pretreatment unit, a multi-channel gas source unit, and a pressure holding timing electronic control unit; The coating cavity 2 has no edge-free gas equalization ring and is equipped with semi-cylindrical gas-blocking sealing plates 9 on both sides. Three detachable partition plates 11 are installed inside the cavity. The sealing plates 9 and partition plates 11 together form four independent sealed flow channels. Each channel is equipped with an independent precursor and reactant gas inlet 14 and a synchronously controlled precursor and reactant gas exhaust port 10. The pressure difference between channels is ≤5 Pa. Microchannel plate clamps 12 are installed inside the channels. The microchannel plates 13 are vertically mounted in the flow channels through the microchannel plate clamps 12, with the micropore axis aligned with the airflow. Precursor and reactant gas inlets 14 and precursor and reactant gas exhaust ports 10 are opened on the sidewalls of the cavity, respectively connecting to external gas source pipelines and vacuum extraction pipelines. Figure 1The parallelism error between the micro-orifice axis and the air inlet direction is ≤0.1°; the assembly gap between the sealing plate 9, the partition plate 11 and the cavity is ≤0.1 mm, completely blocking the edge airflow bypass, so that all process gases can only pass through the central area of the cavity; the cavity edge airflow bypass is completely closed by the double-sided symmetrical semi-cylindrical gas blocking sealing plate, so that all process gases only flow through the central workpiece area of the cavity, eliminating the problem of uneven gas supply caused by the short circuit of the traditional cavity edge airflow; the smooth and uniform airflow field in the cavity can ensure that the precursor is fully diffused to the bottom of the high aspect ratio micro-orifice, greatly reducing the film thickness gradient of the upper and lower parts of the single channel, while avoiding random airflow fluctuations caused by assembly tolerances, significantly improving the uniformity of the resistivity layer film thickness within and between the microchannel plates, and realizing continuous and uniform thickness conformal atomic layer deposition on the inner wall of ultra-high deep holes. If the sealing gap accuracy is greater than 0.1mm, the annular gap on the sidewall forms a significant airflow bypass, causing a large amount of process gas to be directly extracted without passing through the effective deposition area of the microchannel plate. This results in a severe thickness gradient of the resistive layer between the center and edge of the microchannel plate, failure of conformal coverage of high aspect ratio micropores, and non-compliance of device resistance and gain uniformity. Simultaneously, the utilization rate of the precursor decreases, the cycle time lengthens, gas phase deposition on the cavity sidewall intensifies, particulate contamination increases, yield decreases, and the cavity assembly repeatability is poor, making process standardization difficult to achieve. If there are fewer channels, the production capacity cannot be effectively increased; if there are more than four channels, the cavity space is limited, and the microchannel plate cannot be vertically placed. The cross-sectional dimensions of each channel are 40mm × 25mm, precisely matching the external dimensions of the microchannel plate and the fixture dimensions, minimizing the cavity dead zone, forming a regular rectangular laminar flow channel, uniformly enveloping the workpiece with no local eddies; ensuring that precursor molecules diffuse stably into the micropores via molecular / viscous flow. If the cross-section is too large, the ineffective volume is large, the precursor is diluted, and deep-pore adsorption is insufficient. A small cross-section results in excessively high airflow velocity, leading to an overly strong scouring effect on the microchannel plate surface and micropores, potentially causing thinner films at the pore openings and insufficient deposition within the pores. The 10mm channel wall thickness ensures sufficient rigidity of the baffles, preventing deformation and air leakage. A wall thickness less than 10mm makes subsequent sandblasting maintenance prone to deformation and warping, resulting in uneven channel gaps. A wall thickness greater than 10mm occupies effective deposition space, reducing the actual cross-sectional area of the channels and increasing weight, making disassembly and assembly inconvenient and difficult to guarantee assembly accuracy. A parallelism error ≤0.1° ensures consistent air inlet angles and uniform resistance across all channels on the entire MCP, avoiding localized eddies and excessively high / low velocities caused by tilting. A parallelism error greater than 0.1° creates an angle between the airflow and the micropores, significantly reducing the efficiency of deep-hole entry and resulting in poor film uniformity. The 11mm diameter of the air inlet port is the optimal aperture for this process, ensuring uniform, stable, and stratified input of the precursor carrier gas, purge gas, and reaction gas, and meeting the timing requirements of pressure holding and synchronous gas extraction.
[0052] The multi-channel gas source unit includes a heat source precursor source bottle 1 and liquid source precursor source bottles 6, 7, and 8; the extraction unit is a vacuum unit 5; the heat source precursor source bottle 1 and liquid source precursor source bottles 6, 7, and 8 output precursor gas, which enters the coating chamber 2 through the inlet flange 3 at the top of the chamber via the precursor and reaction gas inlet 14; the coating chamber 2 is connected to the precursor and reaction gas exhaust pipe 4, and the reaction waste gas is discharged through the precursor and reaction gas exhaust port 10, and then through the precursor and reaction gas exhaust pipe 4. The gas is delivered to vacuum unit 5, which includes mechanical pumps and molecular pumps, to complete the exhaust gas extraction. The multi-channel gas source unit is equipped with a krypton / xenon carrier gas branch, a high-purity nitrogen purging branch, and an ozone reaction branch. The multi-channel gas source unit is equipped with multiple sets of different types of precursor source bottles, compatible with various precursors. The unit uses an upper air intake and a dedicated exhaust passage, combined with a mechanical pump-molecular pump vacuum unit, to establish the vacuum environment required for ALD and remove reaction exhaust gas in a timely manner. Separate branches for krypton / xenon carrier gas, high-purity nitrogen purging, and ozone reaction are provided, which can realize segmented differentiated gas supply according to the process sequence, meet the needs of deep pore transport, adsorption, oxidation, and purging of high aspect ratio microporous precursors, improve membrane quality, and reduce the cost of rare gas consumables.
[0053] In the above technical solution, this invention, by separately setting up heat source precursor source bottles and multiple sets of liquid source precursor source bottles, is compatible with various solid and liquid ALD precursors. Gas enters the coating chamber through the upper gas inlet flange of the chamber, and waste gas is extracted and discharged in conjunction with a vacuum unit composed of mechanical pumps and molecular pumps and a dedicated exhaust pipe, thus constructing a high-vacuum reaction environment that meets the requirements of the ALD process. At the same time, krypton / xenon carrier gas branch, high-purity nitrogen purging branch, and ozone reaction branch are configured. On the one hand, it can efficiently transport the precursor to the bottom of the micropores of the high aspect ratio microchannel plate, ensuring the uniformity of film thickness along the micropore axis, between single plates, and between multiple plates; on the other hand, it can effectively suppress gas-phase side reactions, reduce particulate impurity defects, achieve composition-controllable metal oxide resistivity layer deposition, and ensure the electrical performance of the microchannel plate and the reproducibility of batch processes.
[0054] The pressure holding timing control unit executes the following steps: after the precursor and ozone are introduced, the valve is closed and pressure is maintained for 3-5 seconds. Upon completion of the pressure holding, simultaneous evacuation and nitrogen purging are performed. If the pressure holding time is less than 3 seconds, the gas cannot fully wet the depth of the micropores, resulting in insufficient adsorption reaction at the bottom of the pores and a larger axial film thickness gradient. If the pressure holding time is greater than 5 seconds, it easily triggers gas-phase side reactions, generating particulate impurities, increasing the process cycle, and reducing production capacity. This timeframe ensures sufficient diffusion and saturation of the gas inside the high aspect ratio micropores while suppressing side reactions, balancing coating quality and production efficiency.
[0055] The pretreatment unit integrates a 40 kHz ultrasonic cleaning module, a 100-120 ℃ drying module, and an argon plasma activation module. These three modules sequentially perform ultrasonic cleaning, high-temperature drying and dehydration, and argon plasma surface activation. Without damaging the microchannel plate glass substrate, it removes oil, particles, and residual moisture from inside and outside the micropores, increases the number of active sites on the substrate surface, ensures uniform ALD nucleation, improves film-substrate bonding strength, and avoids defects such as localized incomplete deposition and abnormal resistance.
[0056] In some alternative embodiments, such as Figure 1 , Figure 2 As shown, the sealing plate 9 has a single axial length A of 162.48 mm, a cross-sectional diameter B of 250 mm, and a width C of 30 mm. The partition plate 11 includes one piece with a length D of 249.99 mm and two pieces with a length E of 233.24 mm. All partition plates have a width F of 10 mm and a height G of 25 mm, with both ends arc-shaped to fit the inner circle of the cavity with an inner diameter of 250 mm. The cross-sectional dimensions of a single flow channel are a length I of 40 mm × a width G of 25 mm. Each channel has independent airtightness and its flow field does not interfere with others. The MCP workpiece is vertically clamped inside each flow channel, with the micropore axis aligned with the inlet flow direction and a parallelism error ≤0.1°, achieving axial forced penetration of the process gas through the micropore. Each channel is embedded with an independent inlet flow channel with an inlet port diameter of 11 mm. Four exhaust ports are synchronously electrically controlled to open and close, and the pressure difference between channels is ≤5 Pa, ensuring that the pressure, flow rate, and precursor concentration of each channel are highly consistent. The main objective is to ensure that the micro-orifice axis is perfectly aligned with the airflow direction (parallelism error ≤ 0.1°), forcing the precursor and purge gas to flow through the micro-orifice axially. This significantly improves the diffusion and displacement efficiency of gas within the deep holes, ensuring a continuous, conformal, and uniform resistive layer from the orifice opening to the bottom, avoiding the film gaps and breaks that occur in deep holes due to traditional lateral air intake. It solves problems such as the difficulty of conformal deposition in high aspect ratio microchannel deep holes, poor intra- and inter-wafer uniformity, and turbulent airflow, improving the consistency and production efficiency of multi-wafer parallel deposition. Simultaneously, it enhances precursor utilization, reduces secondary deposition and particulate contamination, ultimately achieving uniform MCP resistive layer thickness, stable resistance, and significantly improved device performance consistency.
[0057] In some optional embodiments, the parameters of the argon plasma activation module are as follows: high-purity argon gas supply, power 80-120 W, vacuum degree 8-12 Pa, argon flow rate 30-50 sccm, activation time 60-90 s; ultrasonic module temperature control 40-50 ℃. When the parameters are below the lower limit, insufficient plasma activation and incomplete decontamination will occur, resulting in poor ALD nucleation and localized missed deposition; when the parameters are above the upper limit, etching damage to the inner wall of the glass micropores, ultrasonic solvent evaporation failure, and decreased process safety are likely to occur. This parameter range balances impurity removal efficiency, substrate non-damage, and surface activation effect, providing a highly clean and highly active microporous substrate for ALD resistive layer deposition.
[0058] In some optional embodiments, the parameters of the precursor partitioned heating temperature zones of the coating chamber 2 are as follows: 160-170 ℃ for the acetylacetone-iridium temperature zone, and 60-70 ℃ for the other precursors; the main reaction zone of the chamber is kept at a constant temperature of 250-300 ℃ and a chamber pressure of 100-150 Pa. The acetylacetone-iridium temperature zone is set at 160-170 ℃, while the other precursors use a 60-70 ℃ temperature zone to match the vaporization characteristics of different precursors, ensuring a stable vaporization supply and avoiding condensation or premature thermal decomposition; the main reaction zone of 250-300 ℃ and a chamber pressure of 100-150 Pa creates a suitable ALD reaction window, ensuring sufficient surface adsorption and oxidation and suppressing gas-phase side reactions. When the iridium acetylacetonate temperature is set below 160°C and the other precursors are used at temperatures below 60°C, temperatures below the lower limit will result in insufficient precursor vaporization and adsorption, leading to incomplete deposition. When the iridium acetylacetonate temperature is set above 170°C and the other precursors are used at temperatures above 70°C, temperatures above the lower limit will cause precursor thermal decomposition, resulting in particulate contamination. Below 250°C, the main reaction temperature is too low, resulting in insufficient reaction and numerous film impurities. Above 300°C, the temperature is too high, causing precursor pyrolysis and thermal damage to the substrate. When the cavity pressure is below 100 Pa, the precursor cannot wet the bottom of the micropores; when the cavity pressure is above 150 Pa, gas-phase side reactions intensify, increasing particulate defects. The entire parameter range takes into account precursor supply, ALD surface reaction, and gas transport within high aspect ratio micropores, ensuring the quality of the resistive layer film.
[0059] Some embodiments of the present invention also provide a low-light photodetector device, comprising a microchannel plate 13, wherein the inner wall of the micropores of the microchannel plate 13 is provided with the aforementioned resistive layer; the low-light photodetector device is a low-light night vision device, a high-energy particle detector, or a vacuum electron multiplier. Using the microchannel plate with a uniform resistive layer prepared by the present invention in low-light night vision devices, high-energy particle detectors, and vacuum electron multipliers, the excellent thickness-resistance uniformity of the resistive layer reduces the difference in electron multiplication rate among the micropores, improves imaging quality, enhances the consistency of particle detection signals, reduces the risk of noise arcing, and improves the operational stability of the device, thus adapting to the use and mass production requirements of such low-light photodetector devices.
[0060] The present invention will be further described below with reference to specific embodiments, but this should not be construed as a limitation on the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above description of the present invention still fall within the scope of protection of the present invention.
[0061] Examples 1-8 and Comparative Examples 1-4 are used to verify the role of each technical feature in the preparation method of the present invention. Example 1 is the baseline example, which fully adopts the four core technical features of the present invention. Examples 2-8 retain all core technical features and adjust the substrate specifications, precursor, carrier gas and process parameters respectively by using a single variable change method. Comparative Examples 1-4 remove only one core technical feature each time, and keep the other conditions the same as in Example 1, thereby verifying the necessity of each technical feature.
[0062] Example 1 This embodiment provides a method for fabricating a high aspect ratio microchannel plate resistive layer, the specific steps of which are as follows: The single-cycle film formation rate of iridium acetylacetone is 0.3-0.5 nm / cycle; Objective: To deposit a resistive layer in 200 cycles; 1. Selecting materials: Microchannel plate - ultra-high aspect ratio (60:1), pore size 10 micrometers - thickness 0.6 mm; Precursor - Iridium acetylacetone, reactant gas - ozone, activation gas - argon with a purity of 99.999%; 2. Cleaning and activation pretreatment: The microchannel plate was ultrasonically cleaned sequentially with anhydrous ethanol and isopropanol at 40 Hz and 40 °C for 10 min each, followed by ultrasonic cleaning twice with pure water, each cleaning session lasting 10 min. Finally, it was dried in a 100 °C constant temperature oven for 10 min. After drying, the microchannel plate was activated and pretreated for 60 s using argon plasma with a power of 80 W, a working vacuum of 8 Pa, and an argon flow rate of 30 sccm.
[0063] 3. Add a card The microchannel plate separator and sealing plate are clamped inside the coating cavity, with the gap between the sealing plate / separator and the cavity sidewall controlled to be ≤0.1mm. Each of the four channels has a cross-sectional dimension of 40mm×25mm. The microchannel plate micropores are installed with their axial direction aligned with the airflow direction, and the parallelism error is ≤0.1°.
[0064] 4. Coating: The chamber reaction temperature is controlled at 280℃, the precursor heating temperature at 170℃, and the chamber working pressure at 100Pa. First, krypton is used as the carrier gas, with a flow rate controlled at 200 sccm. The precursor is introduced into the chamber for 3 seconds, evenly distributing it into each independent flow channel. Immediately after the gas introduction is complete, all extraction ports of the chamber are closed, and the chamber is sealed and pressurized for 5 seconds. After the pressure adsorption is complete, the extraction device is activated, and simultaneously, high-purity nitrogen (99.999%) is immediately switched as the purging medium. The purging flow rate is set to 300 sccm, and the purging time is 20 seconds, rapidly introducing the nitrogen into the chamber for purging. After purging, ozone, the reactive gas, is introduced into the chamber at a flow rate of 20 sccm for 5 seconds. Immediately after the gas introduction is complete, all extraction ports of the chamber are closed, and the chamber is sealed and pressurized for 5 seconds. After the pressure adsorption is completed, turn on the pumping device and immediately switch to high-purity nitrogen with a purity of 99.999% as the purging medium. Set the purging flow rate to 300 sccm and the purging time to 20s, and quickly introduce it into the cavity for purging.
[0065] Repeat the above coating process 200 times.
[0066] Example 2 This embodiment provides a method for preparing a high aspect ratio microchannel plate resistive layer.
[0067] The difference between this embodiment and Embodiment 1 is as follows: The microchannel plate has an aspect ratio of 80:1, a pore size of 6 micrometers, and a thickness of 0.48 mm; the precursor is trimethylaluminum; pretreatment: anhydrous ethanol and isopropanol are ultrasonically cleaned at a frequency of 40 Hz and a temperature of 50°C for 20 min each, followed by ultrasonic cleaning with pure water three times, each time for 20 min, and drying at 110°C for 20 min; argon plasma activation: power of 100 W, working vacuum of 10 Pa, argon flow rate of 50 sccm, and activation time of 80 s; coating process: chamber temperature of 260°C, chamber pressure of 130 Pa, krypton carrier gas flow rate of 250 sccm, precursor introduction time of 5 s, pressure holding time of 4 s; ozone introduction time of 4 s, pressure holding time of 4 s; purge flow rate of 250 sccm, purge time of 15 s. The remaining steps and parameters are the same as in Embodiment 1.
[0068] Objective: To deposit a resistive layer for 200 cycles, with a trimethylaluminum film deposition rate of 0.5-1.0 nm / cycle; repeat the above deposition process for 200 cycles.
[0069] Example 3 This embodiment provides a method for preparing a high aspect ratio microchannel plate resistive layer. The difference between this embodiment and Embodiment 1 is that the precursor in this embodiment is bis(2,4-dimethylpentadienyl)ruthenium. The remaining steps and parameters are the same as in Embodiment 1.
[0070] The film formation rate is 0.3-0.5 nm / cycle; Objective: To deposit a resistive layer for 200 cycles; the bis(2,4-dimethylpentadienyl)ruthenium film deposition rate is 0.3-0.5 nm / cycle; repeat the above deposition process for 200 cycles.
[0071] Example 4 This embodiment provides a method for preparing a high aspect ratio microchannel plate resistive layer.
[0072] The difference between this embodiment and Embodiment 1 is as follows: The aspect ratio of the microchannel plate is 80:1, the pore size is 6 micrometers, and the thickness is 0.48 mm; the precursor is titanium tetrachloride; pretreatment: ultrasonic cleaning with anhydrous ethanol and isopropanol at 50°C for 20 min each, ultrasonic cleaning with pure water 3 times, 20 min each time, and drying at 110°C for 20 min; argon plasma activation: power 100W, vacuum degree 10Pa, argon flow rate 50 sccm, activation time 80s; coating process: chamber temperature 260°C, chamber pressure 130Pa, krypton carrier gas flow rate 250 sccm, precursor introduction time 2s, pressure holding time 4s; ozone introduction time 4s, pressure holding time 4s; purging flow rate 250 sccm, purging time 15s. The remaining steps and parameters are the same as in Embodiment 1.
[0073] Objective: To deposit a resistive layer for 200 cycles, with a titanium tetrachloride film deposition rate of 0.5-1.0 nm / cycle; repeat the above deposition process for 200 cycles.
[0074] Example 5 This embodiment provides a method for preparing a high aspect ratio microchannel plate resistive layer.
[0075] The difference between this embodiment and Embodiment 1 is that the carrier gas in the adsorption stage is high-purity xenon, and the xenon flow rate is 200 sccm. The remaining steps and parameters are the same as in Embodiment 1.
[0076] Objective: Deposit a resistive layer in 200 cycles; achieve an acetylacetone iridium film deposition rate of 0.3-0.5 nm / cycle; repeat the above deposition process for 200 cycles.
[0077] Example 6 This embodiment provides a method for preparing a high aspect ratio microchannel plate resistive layer.
[0078] The difference between this embodiment and Embodiment 1 is that the microchannel plate has an aspect ratio of 70:1, a pore size of 8 μm, and a thickness of 0.56 mm; the precursor is tetra(ethylmethylamino). The remaining steps and parameters are the same as in Embodiment 1.
[0079] Objective: To deposit a resistive layer for 200 cycles; the tetra(ethylmethylamino)hafnium film deposition rate is 0.5-1.0 nm / cycle; repeat the above deposition process for 200 cycles.
[0080] Example 7 This embodiment provides a method for preparing a high aspect ratio microchannel plate resistive layer.
[0081] The difference between this embodiment and Embodiment 1 is that the precursor is bis(dimethylamino)zinc, and the precursor heating temperature is set to 65°C. The remaining steps and parameters are the same as in Embodiment 1.
[0082] Objective: To deposit a resistive layer for 200 cycles; the bis(dimethylamino)zinc film deposition rate is 1.1-1.5 nm / cycle; repeat the above deposition process for 200 cycles.
[0083] Example 8 This embodiment provides a method for preparing a high aspect ratio microchannel plate resistive layer.
[0084] The difference between this embodiment and Embodiment 1 is that the precursor is trimethylmethylcyclopentadiene platinum; the coating uses extreme values of the parameter range: cavity temperature of 300℃, cavity pressure of 150Pa, and precursor heating temperature of 70℃. The remaining steps and parameters are the same as in Embodiment 1.
[0085] Objective: To deposit a resistive layer for 200 cycles; the bis(dimethylamino)zinc film deposition rate is 1.1-1.5 nm / cycle; repeat the above deposition process for 200 cycles.
[0086] Comparative Example 1 This comparative example provides a method for preparing a high aspect ratio microchannel plate resistive layer.
[0087] The difference between this comparative example and Example 1 is that the semi-cylindrical air-blocking plate and the removable partition plate of the coating cavity are removed, the independent sealed flow channel is eliminated, the traditional edge air-regulating ring is retained, and the cavity has a sidewall airflow bypass. The remaining steps and parameters are the same as in Example 1.
[0088] Comparative Example 2 This comparative example provides a method for preparing a high aspect ratio microchannel plate resistive layer.
[0089] The difference between this comparative example and Example 1 is that the entire set of graded micropore pretreatment processes is omitted, and the substrate is simply wiped with a lint-free cloth without ultrasonic cleaning, constant temperature drying, or argon plasma activation. The remaining steps and parameters are the same as in Example 1.
[0090] Comparative Example 3 This comparative example provides a method for preparing a high aspect ratio microchannel plate resistive layer.
[0091] The difference between this comparative example and Example 1 is that the krypton heavy carrier gas in the adsorption stage is omitted, and high-purity nitrogen is used as the carrier gas and purge gas throughout the process, without the use of segmented differential carrier gas. The remaining steps and parameters are the same as in Example 1.
[0092] Comparative Example 4 This comparative example provides a method for preparing a high aspect ratio microchannel plate resistive layer.
[0093] The difference between this comparative example and Example 1 is that the two-stage pressure holding process is omitted. After the precursor and ozone are introduced, the gas is directly evacuated and purged with nitrogen, without performing the 3-5 second closed pressure holding operation. The remaining steps and parameters are the same as in Example 1.
[0094] Test method: Each ALD process cycle number is 200; the film formation rate per cycle varies for different precursors, therefore, the total film thickness varies for each group under the same number of cycles.
[0095] Five microchannel plates were randomly selected from each furnace for testing. 1) Micro-well top / middle / bottom: SEM measured film thickness at the opening, middle, and bottom of the same microchannel plate of the same micro-well; 2) Average film thickness per sheet: the arithmetic mean of the film thickness at the top, middle and bottom points of the micropores of a single sample; 3) Uniformity of film thickness on a single sheet (within the sheet): relative deviation of film thickness at the top, middle and bottom points of the micropores on a single sheet; 4) Average film thickness of 5 samples in the same furnace: The average film thickness of each of the 5 samples in the furnace; 5) Film thickness uniformity among multiple wafers: the relative deviation of the average film thickness among 5 samples from the same furnace. The test results are shown in Tables 1 and 2.
[0096] Table 1. Test results of film thickness at the upper, middle, and lower points of the micropores in each group of single samples.
[0097] Table 2 Statistical test results of multiple samples from the same furnace
[0098] As shown in Tables 1 and 2 above, each group underwent 200 ALD cycles. Due to the influence of different single-cycle growth rates of precursors, the total film thickness obtained by each group varied. Examples 1-8 adopted the bypass-free flow guiding cavity, graded micropore pretreatment, segmented differentiated carrier gas, and dual-stage pressure holding sequence of the present invention. Under their respective corresponding film thickness conditions, the thickness deviation of the micropore opening, middle, and bottom of a single microchannel plate was small, and the axial step coverage effect was excellent. The average film thickness fluctuation of the 5 samples in the same furnace was small, with the highest single film thickness uniformity being 0.64% and the highest film thickness uniformity among multiple plates being 0.36%, which meets the index of single film thickness uniformity ≤0.6% and film thickness uniformity among multiple plates ≤0.4% specified in the present invention.
[0099] Comparative Examples 1-4 all used the same iridium-based precursor and 200 cycles as Example 1, but lacked only one key technical feature; their single-sheet film thickness uniformity and multi-plate film thickness uniformity were significantly worse than those of the Example group, with obvious axial gradient defects of thick orifice and thin orifice bottom, large film thickness dispersion of different substrates in the same furnace, and poor batch consistency.
[0100] Comparative Example 1 Mechanism (No Bypass Guided Cavity): Without a blocking plate and an independent guided channel, a high-speed airflow bypass is formed on the side wall of the cavity. Most of the precursor escapes along the side wall, resulting in uneven airflow in the micropores. This leads to obvious gradient defects with thick orifices and thin bottoms. At the same time, the airflow difference between different workpiece positions is extremely large, which directly leads to a significant deterioration in axial, single-piece, and inter-piece uniformity. This proves that the no-bypass closed guided structure is the core hardware foundation for uniform film formation.
[0101] Comparative Example 2 Mechanism (without graded pretreatment): Residual organic impurities, microparticles, and adsorbed water vapor on the substrate. Water vapor reacts with the precursor to generate a heterogeneous film layer. Carbon impurities reduce the surface activity of the substrate, causing unsaturated and non-uniform adsorption of the precursor on the inner wall of the micropores. This not only significantly reduces the film thickness consistency but also causes pinholes, particle defects, and decreased film adhesion. This verifies that graded pretreatment is a key prerequisite for the preparation of high-quality films.
[0102] Comparative Example 3 Mechanism (Undifferentiated Carrier Gas): Nitrogen molecules have a small mass and a fast diffusion rate, making it impossible for them to effectively reside in high aspect ratio micropores. The precursor struggles to diffuse to the bottom of the pores, and effective adsorption and film formation are only achieved in the pore opening region, resulting in significant axial film thickness gradient defects. This demonstrates that using a differentiated match of krypton / xenon heavy carrier gas in the adsorption stage and high-purity nitrogen in the purging stage is the core technological approach to solving the problem of step coverage in high aspect ratio micropores.
[0103] Comparative Example 4 Mechanism (without dual-stage pressure holding sequence): After canceling the closed-loop pressure holding, the precursor and ozone do not have enough time to diffuse under uniform pressure, saturate adsorption and fully oxidize in the micropores. The gas is extracted before the reaction is completed, resulting in insufficient film formation in the deep micropores, incomplete reaction, uneven film composition and a sharp increase in thickness dispersion. This verifies that the dual-stage pressure holding sequence is the core timing logic for adapting to high aspect ratio micropore ALD film formation.
[0104] The results from Tables 1 and 2 show that the four technical features of this invention—the dedicated non-bypass flow guiding cavity, the graded micropore pretreatment, the segmented differentiated carrier gas, and the dual-stage pressure holding sequence—need to be coupled and work synergistically. The absence of any one of these core features will not only lead to a deterioration in the quantitative indicators of film thickness uniformity but also result in surface defects such as thin plating and incomplete plating, making it impossible to prepare a high aspect ratio microchannel plate resistive layer with acceptable performance. Examples 1-8 cover the entire aspect ratio range of 60:1-80:1, are compatible with platinum, ruthenium, iridium, titanium, aluminum, hafnium, and zinc series precursors, and cover low, medium, and high film formation rate ranges. All tested performances fall within the limits specified by this invention. Example 5, which uses xenon as the adsorption carrier gas, exhibits excellent uniformity, indicating that heavy inert carrier gas can further optimize the gas diffusion effect inside deep pores. Example 8, under extreme process window conditions, still meets the requirements, verifying that this invention has a wide process window and good mass production stability and adaptability to operating conditions.
[0105] Numerous specific details are set forth in this specification. However, it will be understood that embodiments of the invention may be practiced without these specific details. In some embodiments, well-known methods, structures, and techniques have not been shown in detail so as not to obscure the understanding of this specification.
[0106] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.
[0107] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.
[0108] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention shall still fall within the scope of the technical solution of the present invention.
Claims
1. A method for fabricating a high aspect ratio microchannel plate resistive layer, characterized in that, Metal oxide resistive layers are prepared by atomic layer deposition on the inner wall of micropores in a microchannel plate with an aspect ratio of 60:1-80:
1. The process includes workpiece pretreatment, cavity assembly, and ozone oxidation ALD cyclic film formation. The method is implemented through a non-bypass flow-guiding cavity, graded micropore pretreatment, segmented differentiated carrier gas, and dual-stage pressure holding sequential coupling. The bypass-free flow guide cavity has no edge uniform air ring. Semi-cylindrical air blocking and sealing plates are symmetrically arranged on both sides of the cavity to block the side wall airflow bypass. The cavity is equipped with three detachable partition plates, which together with the sealing plates form four independent and sealed flow guide channels. The microchannel plate is vertically installed in the flow guide channel, with the micropore axis facing the air intake airflow. The segmented differentiated carrier gas: krypton or xenon is used as the carrier gas in the precursor adsorption stage, and high-purity nitrogen with a purity of ≥99.999% is used in the purging, oxidation and cavity cleaning stage. The dual-stage pressure holding sequence is as follows: after introducing the metal-organic precursor and ozone, all flow channels and exhaust ports are simultaneously closed to maintain pressure; after the pressure holding is completed, exhaust is simultaneously opened and high-purity nitrogen is introduced for purging.
2. The preparation method according to claim 1, characterized in that, The microchannel plate has the following specifications: 10 μm aperture and 0.6 mm substrate thickness, or 6 μm aperture and 0.48 mm substrate thickness.
3. The preparation method according to claim 1, characterized in that, The graded micropore pretreatment includes ultrasonic cleaning, constant temperature drying, and argon plasma activation. Ultrasonic cleaning: The microchannel plate was ultrasonically cleaned in anhydrous ethanol and isopropanol at 40 kHz and 40-50℃ for 10-20 min respectively, and then ultrasonically cleaned with pure water 2-3 times, each time for 10-20 min. Constant temperature drying: Dry at 100-120℃ for 10-20 min; Argon plasma activation: The gas source is argon gas with a purity of ≥99.999%, the power is 80-120 W, the vacuum degree is 8-12 Pa, the argon gas flow rate is 30-50 sccm, and the activation time is 60-90 s.
4. The preparation method according to claim 1, characterized in that, The ALD process temperature and pressure conditions are as follows: constant chamber temperature 250-300 ℃, chamber pressure 100-150 Pa; precursor zone temperature control: iridium acetylacetone 160-170 ℃, other precursors 60-70 ℃; the steps of a single ALD cycle are as follows: S1 Precursor Adsorption: Krypton / Xenon flow rate is 200-300 sccm, precursor is introduced for 2-3 s, and pressure is maintained for 3-5 s; One purging: 200-300 sccm of high-purity nitrogen, purging for 10-20 s; S2 Ozone Oxidation: Ozone flow rate is 20-30 sccm, introduced for 3-5 s, and maintained at pressure for 3-5 s; Secondary purging: High-purity nitrogen flow rate is 200-300 sccm, purging for 10-20 s; Repeat the cycle until the target film thickness is achieved.
5. The preparation method according to claim 1, characterized in that, The organometallic precursor is selected from one of trimethylmethylcyclopentadienylplatinum, bis(2,4-dimethylpentadienyl)ruthenium, iridium acetylacetonate, titanium tetrachloride, trimethylaluminum, tetra(ethylmethylamino)hafnium, and bis(dimethylamino)zinc, and the oxidizing gas is ozone; under a process window of 250-300℃, the single-cycle film formation rate of each precursor is: Platinum, ruthenium, and iridium precursors: 0.3-0.5 nm / cycle; Titanium, aluminum, and hafnium precursors: 0.5-1.0 nm / cycle; Zinc-based precursor: 1.1-1.5 nm / cycle.
6. A high aspect ratio microchannel plate resistive layer, characterized in that, The resistive layer is deposited on the inner wall of the micropores of a microchannel plate with an aspect ratio of 60:1-80:1, and is an oxide film of at least one metal selected from platinum, ruthenium, iridium, titanium, aluminum, hafnium, and zinc. The film thickness deviation along the micropore axis of the resistive layer is ≤1%, the film thickness uniformity of a single sheet is ≤0.6%, and the film thickness uniformity between multiple sheets is ≤0.4%. The resistive layer is prepared by the preparation method according to any one of claims 1-5.
7. An apparatus for fabricating a high aspect ratio microchannel plate resistive layer, characterized in that, Includes a coating chamber, a pretreatment unit, a multi-channel gas source unit, and a pressure holding timing electronic control unit; The coating cavity has an edgeless gas equalization ring and semi-cylindrical gas blocking plates on both sides. Three detachable partition plates inside the cavity divide it into four independent flow channels. Each channel is equipped with an independent air inlet and a synchronous electrically controlled air extraction port. The pressure difference between the channels is ≤5Pa. After the workpiece is clamped, the error between the axial direction of the microhole and the parallelism of the air inlet is ≤0.1°. The assembly gap between the blocking plate, partition plate and cavity is ≤0.1mm. The multi-channel gas source unit is equipped with a krypton / xenon carrier gas branch, a high-purity nitrogen purging branch, and an ozone reaction branch; The pressure holding timing electronic control unit executes the following: after the precursor and ozone are introduced, the valve is closed and pressure is maintained for 3-5 seconds. After the pressure holding is completed, gas is simultaneously extracted and nitrogen is introduced for purging. The pretreatment unit integrates a 40 kHz ultrasonic cleaning module, a 100-120 ℃ drying module, and an argon plasma activation module.
8. The preparation apparatus according to claim 7, characterized in that, The sealing plate has an axial length of 162.48 mm and a cross-sectional diameter of 249.99 mm and a width of 30 mm for the adapted semi-circular cavity. The partition plate consists of one plate with a length of 249.99 mm and two plates with a length of 233.24 mm. All partition plates are 10 mm wide and 25 mm high, with both ends arc-shaped to fit the inner circle of the cavity with an inner diameter of 250 mm. The cross-sectional dimensions of a single flow channel are 40 mm long and 25 mm wide. The parameters of the argon plasma activation module are: high-purity argon gas supply, power of 80-120 W, vacuum degree of 8-12 Pa, argon gas flow rate of 30-50 sccm, and activation time of 60-90 s. The temperature control of the ultrasonic module is 40-50 ℃.
9. The preparation apparatus according to claim 8, characterized in that, The coating cavity is equipped with precursor zone heating areas: acetylacetone-iridium temperature zone 160-170 ℃, and other precursor temperature zones 60-70 ℃; the main reaction zone of the cavity is kept at a constant temperature of 250-300 ℃, and the cavity pressure is 100-150 Pa.
10. A low-light photodetector device, characterized in that, It includes a microchannel plate, wherein the inner wall of the microchannel plate micropores is provided with the high aspect ratio microchannel plate resistive layer as described in claim 6; the low-light photodetector is one of a low-light night vision device, a high-energy particle detector, and a vacuum electron multiplier.