Methods and reaction systems for selectively forming films

By using a combination of plasma and co-reactants in the integrated circuit manufacturing process, a film can be selectively formed on the vertical sidewalls of gap features, solving the problem of etching gap features damaging the underlying structure in the prior art and achieving highly efficient etching selectivity.

CN123108537APending Publication Date: 2026-11-17ASM IP HLDG BV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610637233.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2026-05-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the process of integrated circuit manufacturing, existing technologies have difficulty forming a continuous vertical sidewall film in the gap features without damaging the underlying structure, and over-etching can lead to etch damage to the underlying layer.

Method used

By providing plasma and co-reactants in a reaction chamber, combined with deposition and etching processes, films are selectively formed on the vertical sidewalls of gap features. The etching rate is controlled by plasmas of different frequencies and combinations to achieve selective removal of horizontal surfaces and bottom portions.

Benefits of technology

This method enables efficient film formation on the vertical sidewalls of gap features while protecting the underlying structure, avoiding damage caused by over-etching, and improving etching selectivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108537A_ABST
    Figure CN123108537A_ABST
Patent Text Reader

Abstract

A method for selectively forming a film is provided. The method includes providing a substrate in a reaction chamber. The substrate includes a first horizontal surface and a gap feature extending downward from the first horizontal surface. The method includes depositing material layers on the first horizontal surface and in the gap feature by a deposition process. The method includes removing the material layer on the first horizontal surface and the material layer on a second horizontal surface of a bottom portion of the gap feature by an etching process to selectively form a film on the vertical sidewalls of the gap feature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to methods for forming films. More specifically, this invention relates to methods for selectively forming films on the sidewalls of gap features using plasma. Background Technology

[0002] In the manufacturing process of integrated circuits, several processes exist for forming sidewalls in gap features. Sidewalls serve as spacers or to prevent etching of structures from the side surfaces of the gap feature. Typically, sidewalls are formed by forming a conformal film on the surface of the gap feature, followed by asymmetric etching to remove portions formed on the upper surface where the gap feature is formed and portions formed on the bottom surface of the gap feature. However, when using this formation method, over-etching is required to remove the substrates from the sidewalls. Over-etching leads to the etching of the underlying layer, damaging that layer. Furthermore, in gap features with depths ranging from a few nanometers to a few micrometers, it is difficult to achieve a continuous film formed on the vertical sidewalls of the gap feature without forming it on the horizontal surface of the gap feature. Therefore, the development of methods for selectively forming films on the substrate is needed.

[0003] Any discussion set forth in this section (including discussions of problems and solutions) is included in this disclosure for the purpose of providing background information and should not be construed as an admission that any or all of the discussions were known at the time of making this invention or otherwise constitute prior art. Summary of the Invention

[0004] This synopsis is provided to introduce some concepts in a simplified form. These concepts are further described in detail in the following detailed description of embodiments of this disclosure. This synopsis is not intended to identify key or essential features of the claimed subject matter, nor is it intended to limit the scope of the claimed subject matter.

[0005] According to some embodiments of this disclosure, a method for selectively forming a film is provided. The method includes providing a substrate in a reaction chamber. The substrate includes a first horizontal surface and a gap feature extending downward from the first horizontal surface. The method includes depositing material layers on the first horizontal surface and in the gap feature by a deposition process. The method includes removing the material layer on the first horizontal surface and the material layer on a second horizontal surface of a bottom portion of the gap feature by an etching process to selectively form a film on the vertical sidewalls of the gap feature.

[0006] In some embodiments, a first plasma is provided in the reaction chamber during the deposition process.

[0007] In some embodiments, the first plasma includes a single-frequency plasma.

[0008] In some embodiments, the first plasma includes a combination of a first sub-plasma and a pulsed second sub-plasma, and the first sub-plasma is different from the pulsed second sub-plasma.

[0009] In some embodiments, a first plasma and co-reactants are provided in the reaction chamber during the deposition process.

[0010] In some embodiments, the first plasma comprises a single-frequency plasma, and the co-reactants comprise H2, Ar, or a combination thereof.

[0011] In some embodiments, the first plasma includes a combination of a first sub-plasma and a pulsed second sub-plasma, the co-reactants include H2, Ar or a combination thereof, and the first sub-plasma is different from the pulsed second sub-plasma.

[0012] In some embodiments, during the etching process, the etching rate of the material layer on the second horizontal surface of the bottom portion of the gap feature is approximately twice the etching rate of the material layer on the vertical sidewall of the gap feature.

[0013] In some embodiments, a processing procedure is also performed after the deposition process and before the etching process.

[0014] In some embodiments, a first plasma is provided in the reaction chamber during the deposition process, a second plasma is provided in the reaction chamber during the processing process, and the first plasma is different from the second plasma.

[0015] In some embodiments, the second plasma includes a combination of the first sub-plasma and the second sub-plasma, and the first sub-plasma is different from the second sub-plasma.

[0016] In some embodiments, a co-reactant is provided in a reaction chamber during the processing, and the co-reactant comprises H2, Ar, or a combination thereof.

[0017] In some embodiments, during the etching process, the etching rate of the material layer on the second horizontal surface of the bottom portion of the gap feature is approximately three times that of the material layer on the vertical sidewall of the gap feature.

[0018] In some embodiments, the first plasma includes a first combination of a first sub-plasma and a second sub-plasma, the second plasma includes a second combination of a third sub-plasma and a fourth sub-plasma, and the first sub-plasma, the second sub-plasma, the third sub-plasma, and the fourth sub-plasma are different.

[0019] In some embodiments, the second sub-plasma of the first combination of the first plasma is a pulsed plasma.

[0020] In some embodiments, a co-reactant is provided in a reaction chamber during the processing, and the co-reactant comprises H2, Ar, or a combination thereof.

[0021] In some embodiments, during the etching process, the etching rate of the material layer on the second horizontal surface of the bottom portion of the gap feature is approximately four times that of the material layer on the vertical sidewall of the gap feature.

[0022] In some embodiments, the frequency of the first plasma is greater than the frequency of the second plasma.

[0023] In some embodiments, the first plasma densifies the material layer on the vertical sidewalls of the gap feature.

[0024] In some embodiments, the second plasma damages the material layer on the first horizontal surface and the material layer on the second horizontal surface at the bottom of the gap feature, such that the material layer on the first horizontal surface and the material layer on the second horizontal surface at the bottom of the gap feature are removed during the etching process.

[0025] According to some embodiments of the present disclosure, a reaction system is provided. The system includes a reaction chamber, a substrate support, a precursor source, a co-reactant source, a plasma power source, and a controller. The substrate support is disposed in the reaction chamber and configured to support a substrate. The precursor source provides a precursor to the reaction chamber. The co-reactant source provides a co-reactant to the reaction chamber. The plasma power source provides plasma to the reaction chamber. The controller is configured to control the precursor, co-reactant, and plasma to perform the methods of some embodiments of the present disclosure. Attached Figure Description

[0026] Embodiments of this disclosure can be best understood from the following detailed description taken in conjunction with the accompanying drawings. It should be noted that, according to industry practice, various features are not drawn to scale. In practice, the dimensions of various elements may be arbitrarily increased or decreased to clearly illustrate the features of the embodiments of this disclosure. It should also be noted that the accompanying drawings illustrate exemplary embodiments of this disclosure. The drawings should not be considered as limiting the scope of this disclosure. This disclosure can also be applied to other embodiments.

[0027] Figure 1 A schematic method for selectively forming a film on a substrate is shown according to some embodiments of the present disclosure.

[0028] Figure 2 A schematic cross-section of a substrate with gap features according to some embodiments of the present disclosure is shown.

[0029] Figure 3 A schematic method for selectively forming a film on a substrate is shown according to some embodiments of the present disclosure.

[0030] Figure 4 Illustrative timing diagrams are shown according to some embodiments of the present disclosure.

[0031] Figure 5 Illustrative timing diagrams are shown according to some embodiments of the present disclosure.

[0032] Figure 6 Illustrative timing diagrams are shown according to some embodiments of the present disclosure.

[0033] Figure 7 Illustrative timing diagrams are shown according to some embodiments of the present disclosure.

[0034] Figure 8 A schematic reaction system for selectively forming a film on a substrate is shown according to some embodiments of the present disclosure. Detailed Implementation

[0035] The following disclosure provides numerous different embodiments or examples for implementing various features of the described subject matter. Specific examples of elements and arrangements are described below to simplify this specification. Of course, these are merely examples and not limiting. For example, in the following description, forming a first feature above or on a second feature can include embodiments where the first and second features are in direct contact, and can also include embodiments where an additional feature is formed between the first and second features such that the first and second features are not in direct contact. Furthermore, reference numerals and / or letters may be repeated in various examples in this disclosure. Such repetition is for simplicity and clarity and does not in itself indicate a relationship between the various embodiments and / or configurations discussed.

[0036] For ease of description, this document uses spatial relative terms such as "below," "below," "lower," "above," and "upper" to describe the relationship between one element or feature and another element or feature as shown in the figure. In addition to the orientations shown in the figure, spatial relative terms are intended to cover different orientations of the device during use or operation. The device may be oriented in other ways (rotated 90 degrees or in other orientations), and the spatial relative descriptors used herein will be interpreted accordingly.

[0037] It should be understood that ordinal numbers used in this disclosure, such as the terms "first," "second," "third," etc., are used to modify elements and do not in themselves imply or indicate that the element (or elements) has any prior ordinal number, nor do they imply the order of one element with another, or the order in which they are manufactured. The use of these ordinal numbers is to clearly distinguish an element with a certain name from another element with the same name. The claims and the description may not use the same terminology. For example, a first element in the description may refer to a second element in the claim.

[0038] In the following description, the terms "about" and "basically" generally refer to + / -10% of the value, or generally + / -5% of the value, or generally + / -3% of the value, or generally + / -2% of the value, or generally + / -1% of the value, or generally + / -0.5% of the value. The expressions "within the range of the first value to the second value" or "between the first value and the second value" mean that the range includes the first value, the second value, and other values ​​in between. The values ​​given in this disclosure are approximate values. That is, the meaning of "about" and "basically" may be implied even if the terms are not specified.

[0039] Some embodiments of this disclosure are described below. Additional steps or operations may be provided before, during, and / or after the steps or operations described in these embodiments. In different embodiments, some described steps or operations may be replaced or deleted. Furthermore, it should be understood that in the following embodiments, features from several different embodiments may be replaced, recombinated, and combined to complete another embodiment without departing from the spirit of this disclosure. Features between the various embodiments can be arbitrarily mixed and combined, as long as they do not violate or contradict the spirit of this disclosure.

[0040] In this disclosure, "gas" can include materials that are gaseous at ambient temperature and pressure (NTP), evaporated solids and / or evaporated liquids, and may consist of a single gas or a mixture of gases, depending on the circumstances. Gases other than process gases, i.e., gases not introduced through gas distribution components, multi-port injection systems, other gas distribution devices, etc., can be used, for example, to seal the reaction space, and may include sealing gases, such as rare gases. In some cases, the term "precursor" can refer to a compound that participates in a chemical reaction to produce another compound, and particularly to a compound that constitutes the membrane matrix or the main framework of the membrane. The term "reactant" is used interchangeably with the term "precursor".

[0041] As used herein, the term "substrate" can refer to any one or more underlying materials, including any one or more underlying materials that can be modified or on which devices, circuits, or films can be formed. A "substrate" can be continuous or discontinuous; rigid or flexible; solid or porous; and combinations thereof. A substrate can be in any form, such as powder, plate, or workpiece. Plate-type substrates can include wafers of various shapes and sizes. Substrates can be made of semiconductor materials, including, for example, silicon, silicon germanium, silicon oxide, gallium arsenide, gallium nitride, and silicon carbide.

[0042] For example, substrates in powder form can have applications in pharmaceutical manufacturing. Porous substrates can contain polymers. Examples of workpieces may include medical devices (e.g., stents and syringes), jewelry, tooling devices, components for battery manufacturing (e.g., anodes, cathodes, or separators), or components for photovoltaic cells, etc.

[0043] The continuous substrate can extend beyond the boundary of the processing chamber where the deposition process takes place. In some processes, the continuous substrate can move through the processing chamber, allowing the process to continue until the end of the substrate is reached. The continuous substrate can be supplied from a continuous substrate supply system to allow the continuous substrate to be manufactured and output in any suitable form.

[0044] Non-limiting examples of continuous substrates may include sheets, nonwoven films, rolls, foils, fiber webs, flexible materials, bundles of continuous filaments or fibers (e.g., ceramic fibers or polymer fibers). Continuous substrates may also include carriers or sheets on which non-continuous substrates are mounted.

[0045] As used herein, “atomic layer deposition,” abbreviated as “ALD,” refers to a vapor-phase deposition process in which deposition cycles, such as multiple consecutive deposition cycles, are performed in a reaction space (i.e., one or more reaction chambers). Typically, in an ALD process, during each deposition cycle, a precursor is introduced into the reaction space and adsorbed onto a substrate surface, which may include previously deposited material from previous ALD cycles or other materials, forming at most a monolayer of the precursor that is not readily reacted with any additional excess precursor (i.e., a self-limiting reaction). Subsequently, in some cases, another precursor or reactant may be introduced into the reaction space to convert the chemisorbed precursor into the desired material on the substrate surface. Other reaction steps may be included in the deposition cycle. ALD can occur via a thermal process (thermal ALD), where the reaction is promoted by increasing the substrate temperature relative to ambient temperature; and / or via a plasma-enhanced process (PEALD), where the reaction is promoted by using high-energy plasma materials. As used herein, ALD may also be intended to include processes specified by relevant terms, such as chemical vapor atomic layer deposition, atomic layer epitaxy (ALE), molecular beam epitaxy (MBE), gas-source MBE or organometallic MBE, and chemical beam epitaxy when performed with alternating pulses of reactants.

[0046] As used herein, “chemical vapor deposition,” abbreviated as “CVD,” refers to a vapor deposition process in which a film is deposited on a substrate by exposing the substrate surface to one or more gaseous precursors and reactants, which react and / or decompose on the substrate surface to form the film. The precursors and / or reactants may be provided simultaneously to the reaction space, or in partially or completely separate pulses. In some embodiments, the precursors and / or reactants are provided until a layer of desired thickness is deposited. In some embodiments, a cyclic CVD process may be used with multiple cycles to deposit a thin film of desired thickness. In a cyclic CVD process, the precursors and / or reactants may be provided to the reaction space in non-overlapping or partially or completely overlapping pulses. CVD can occur through a thermal process (thermal CVD), where the reaction is promoted by increasing the substrate temperature relative to ambient temperature; or through a plasma-enhanced CVD process, where the reaction is promoted by using high-energy plasma materials.

[0047] As used herein, the terms “membrane” and / or “layer” can refer to any continuous or discontinuous structure and material, such as materials deposited by the methods disclosed herein. For example, membranes and / or layers can include two-dimensional materials, three-dimensional materials, nanoparticles, or even partial or complete molecular layers or partial or complete atomic layers or atomic and / or molecular clusters. A membrane or layer can include a material or layer with pinholes, which can be at least partially continuous. Alternatively, a membrane or layer can consist entirely of isolated islands.

[0048] In this disclosure, the terms “comprising,” “consisting of,” and “having” in some embodiments independently mean “generally or broadly comprising,” “comprising,” “essentially consisting of,” or “consisting of.” It should be understood that when a composition, method, apparatus, etc., is described as comprising certain features, it means that it includes those features, and it does not necessarily exclude the presence of other features, provided they do not render the claims unfeasible. Nevertheless, the expression “comprising” includes the meaning of “consisting of,” that is, when the composition, method, apparatus, etc., under discussion comprises only the listed features, components, and / or steps, and does not contain any other features, components, steps, etc.

[0049] As used herein, the term "carrier gas" can refer to a gas supplied to the reaction chamber along with one or more precursors. For example, a carrier gas may be supplied to the reaction chamber along with one or more precursors used herein. Exemplary carrier gases include N2, H2, and inert gases such as He, Ne, Kr, Ar, and Xe.

[0050] Unlike carrier gases, purge gases can be supplied to the reaction chamber alone (i.e., not with one or more precursors). Nevertheless, gases typically used as carrier gases can also be used as purge gases, even within the same process. For example, in a cyclic deposition-etch process, N2 used as a carrier gas can be supplied with one or more precursors during the deposition pulse, and N2 used as a purge gas can be used to separate the deposition and etching pulses. Therefore, the manner in which a gas is supplied to the reaction chamber determines whether it is used as a purge gas or a carrier gas in a given situation. Thus, as used herein, the term "purge" can refer to the process of supplying an inert or substantially inert gas to the reaction chamber between two interacting gas pulses. For example, a purge, for example using nitrogen, can be provided between precursor and reactant pulses to avoid or at least minimize gas-phase interactions between the precursors and reactants. It should be understood that purging can be achieved temporally, spatially, or both. For example, in the case of time-purge, a purge step can be used, for instance, in a time sequence of providing a first precursor to the reaction chamber, providing a purge gas to the reaction chamber, and providing a second precursor to the reaction chamber, wherein the substrate on which the deposition layer is deposited does not move. For example, in the case of spatial purge, the purge step can take the form of moving the substrate from a first position where the first precursor is continuously supplied through a purge gas curtain to a second position where the second precursor is continuously supplied.

[0051] refer to Figure 1 The illustration shows a schematic method 100 for selectively forming a film on a substrate according to some embodiments of the present disclosure. Method 100 includes: providing a substrate in a reaction chamber (step 110); providing a precursor in a reaction chamber (step 120); providing plasma in a reaction chamber (step 130); and performing an etching process (step 140).

[0052] In step 110, the substrate can be brought to a desired temperature, and the reaction chamber can be brought to a desired pressure, such as a temperature and pressure suitable for subsequent steps. For example, the temperature inside the reaction chamber (e.g., the temperature of the substrate or substrate support) can be between 350°C and 450°C. In some embodiments, the substrate includes one or more gap features, such as trenches.

[0053] In step 120, a precursor for forming a film (material layer) is introduced into the reaction chamber. In some embodiments, the precursor may include a silicon-containing compound and reactants. In some embodiments, the silicon-containing compound may include at least one of the following: silane, silylamine, aminosilane, or silicon halide compound. For example, the precursor may include at least one of the following: silane (SiH4), silane (Si2H6), propane (Si3H8), tetrasilane (Si4H6), etc. 10), N(Si2H5)3, trimethylsilylamine N(SiH3)3, N(SiMe3)(SiHMeNMe2)2, 2,2-dimethylsilyltrisilane (Si(SiH3)4), tridimethylaminosilane (SiH(NMe2)3), bis(diethylamino)silane (SiH2(NEt2)2) (BEDAS), bis(tert-butylamino)silane (SiH2(NHtBu)2) (BTBAS), (diisopropylamino)silane (SiH3(NiPr2)) ( DIPAS), trichlorosilane (Si2Cl3H3), pentachlorosilane (Si2Cl5H), hexachlorosilane (Si2Cl6), octachloropropane (Si3Cl8), dichlorosilane (SiCl2H2), dimethyldichlorosilane (SiCl2Me2), tetrachlorosilane (SiCl4), tetraiodosilane (SiI4), triiodosilane (SiI3H) or diiodosilane (SiI2H2), where Me represents methyl, Et represents ethyl, tBu represents tert-butyl, and iPr represents isopropyl.

[0054] In some embodiments, the reactants may include at least one of the following: N2, NH3, a mixture of N2 and H2, or a combination thereof. In some embodiments, the film (material layer) may be formed by a deposition process such as CVD, ALD, PECVD (plasma-enhanced CVD), PEALD (plasma-enhanced ALD), or other suitable deposition processes.

[0055] In step 130, the plasma may be provided by a dual-frequency plasma source comprising a very high frequency (VHF) component (VHF plasma) and a low frequency radio frequency (LRF) component (LRF plasma). In some embodiments, the frequency of the VHF component may be, for example, between 30 MHz and 60 MHz, between 35 MHz and 55 MHz, or between 40 MHz and 50 MHz. In one embodiment, the frequency of the VHF component may be 60 MHz. In some embodiments, the frequency of the LRF component may be, for example, between 300 kHz and 500 kHz, or between 350 kHz and 450 kHz. In one embodiment, the frequency of the LRF component may be 430 kHz. In some embodiments, the VHF component may have a power between about 700 watts (W) and about 1250 watts. In some embodiments, the LRF component may have a power between about 20 watts and about 500 watts, or between about 100 watts and about 500 watts.

[0056] In step 140, the etching process can be a wet etching process. In some embodiments, the etchant can be dilute hydrofluoric acid (dHF).

[0057] It should be noted that the order of steps in method 100 is merely an example. In other embodiments, this order may vary. In some embodiments, additional steps may be provided in the method. For example, in some embodiments, there are additional steps for providing a second precursor. For example, in some embodiments, there are additional steps for providing a purge gas or carrier gas.

[0058] refer to Figure 2 This illustration shows a schematic cross-section of a substrate with a gap feature according to some embodiments of the present disclosure. The substrate 200 includes a first horizontal surface 210 and a gap feature 220 extending downward from the first horizontal surface 210. A material layer 230 is deposited on the first horizontal surface 210 and in the gap feature 220 by a deposition process (step 120). Plasma 235 is provided to densify the material layer 230 on the vertical sidewalls 240 of the gap feature 220 and to damage the material layer 230 on the first horizontal surface 210 of the substrate and on a second horizontal surface 250 of the bottom portion of the gap feature 220 (step 130). In some embodiments, the plasma is a single-frequency plasma (e.g., VHF plasma). In some embodiments, the plasma includes a combination of VHF plasma and pulsed LRF plasma. An etching process is performed to remove the material layer 230 on the first horizontal surface 210 and on the second horizontal surface 250 of the bottom portion of the gap feature 220 to selectively form a film 260 on the vertical sidewalls 240 of the gap feature 220. In some embodiments, material layer 230 and film 260 may include SiN.

[0059] refer to Figure 3 The illustration shows a schematic method 300 for selectively forming a film on a substrate according to some embodiments of the present disclosure. Method 300 includes: providing a substrate in a reaction chamber (step 310); providing a precursor in a reaction chamber (step 320); providing a co-reactant in a reaction chamber (step 330); providing plasma in a reaction chamber (step 340); and performing an etching process (step 350).

[0060] Step 310 is similar to step 110, step 320 is similar to step 120, and step 350 is similar to step 140. Therefore, they will not be described again here.

[0061] In step 330, a co-reactant comprising H2, Ar, or a combination thereof may be provided in the reaction chamber to enhance the etch selectivity of the material layer during the deposition process.

[0062] In some embodiments, the plasma provided in step 340 is a single-frequency plasma (e.g., VHF plasma) during the deposition process (step 341). In some embodiments, a plasma comprising N2 may be used during the deposition process. In some embodiments, the plasma provided in step 340 includes a combination of VHF plasma and pulsed LRF plasma during the deposition process (step 341).

[0063] refer to Figure 4 The diagram illustrates a schematic timing sequence 400 according to some embodiments of the present disclosure. Timing sequence 400 includes a precursor 410, a co-reactant 420, and a VHF plasma 430. During the deposition process, the precursor 410 is provided prior to the VHF plasma 430, and the co-reactant 420 is provided continuously throughout the timing sequence.

[0064] In such Figure 4 In the illustrated embodiment, the VHF plasma 430 is a single-frequency plasma, and the co-reactant 420 is Ar. The etching rate (e.g., wet etching rate) of the material layer 230 on the second horizontal surface 250 of the bottom portion of the gap feature 220 is approximately twice the etching rate (e.g., wet etching rate) of the material layer 230 on the vertical sidewall 240 of the gap feature 220.

[0065] In some embodiments, the plasma provided in step 340 includes a first plasma and a second plasma. The first plasma is different from the second plasma. The first plasma is provided in the reaction chamber during the deposition process (step 341), and the second plasma is provided in the reaction chamber during the processing process (step 342). The processing process (step 342) is performed after the deposition process (step 341) and before the etching process (step 350).

[0066] refer to Figure 5 The diagram illustrates a schematic timing sequence 500 according to some embodiments of the present disclosure. Timing sequence 500 includes a precursor 510, a co-reactant 520, a VHF plasma 530, and an LRF plasma 540. The precursor 510 is provided prior to the VHF plasma 530 during the deposition process, and the co-reactant 520, VHF plasma 530, and LRF plasma 540 are provided during the processing.

[0067] In such Figure 5In the illustrated embodiment, the first plasma is VHF plasma 530 during the deposition process, and the second plasma includes a combination of VHF plasma 530 and LRF plasma 540 during the processing. In this embodiment, a co-reactant 520 comprising H2 is provided in the reaction chamber during the processing. The etching rate (e.g., wet etching rate) of the material layer 230 on the second horizontal surface 250 of the bottom portion of the gap feature 220 is approximately three times the etching rate (e.g., wet etching rate) of the material layer 230 on the vertical sidewall 240 of the gap feature 220.

[0068] refer to Figure 6 The diagram illustrates a schematic timing sequence 600 according to some embodiments of the present disclosure. Timing sequence 600 includes a precursor 610, a co-reactant 620, a VHF plasma 630, and an LRF plasma 640. The precursor 610 is provided prior to the VHF plasma 630 and the LRF plasma 640 during the deposition process, and the co-reactant 620, VHF plasma 630, and LRF plasma 640 are provided during the processing.

[0069] In such Figure 6 In the illustrated embodiment, during the deposition process, the first plasma comprises a first combination of VHF plasma 630 and LRF plasma 640, and during the processing, the second plasma comprises a second combination of VHF plasma 630 and LRF plasma 640. The first combination differs from the second combination. The LRF plasma 640 of the first combination of the first plasma is a pulsed plasma. The pulse frequency is approximately 2.5 kHz. In this embodiment, a co-reactant comprising H2 is provided in the reaction chamber during the processing. The etching rate (e.g., wet etching rate) of the material layer 230 on the second horizontal surface 250 of the bottom portion of the gap feature 220 is approximately four times the etching rate (e.g., wet etching rate) of the material layer 230 on the vertical sidewall 240 of the gap feature 220.

[0070] refer to Figure 7 The diagram illustrates a schematic timing sequence 700 according to some embodiments of the present disclosure. Timing sequence 700 includes a precursor 710, a VHF plasma 720, and an LRF plasma 730. The precursor 710 is provided prior to the VHF plasma 720 during the deposition process, and the LRF plasma 730 is provided during the processing.

[0071] In such Figure 7In the illustrated embodiment, the first plasma is VHF plasma 720 during the deposition process, and the second plasma is LRF plasma 730 during the processing. In this embodiment, the etching rate (e.g., wet etching rate) of the material layer 230 on the second horizontal surface 250 of the bottom portion of the gap feature 220 is approximately four times the etching rate (e.g., wet etching rate) of the material layer 230 on the vertical sidewall 240 of the gap member 220.

[0072] It should be noted that timing sequences 400, 500, 600, and 700 are examples. In other embodiments, the duration and start point of the precursor, co-reactant, VHF plasma, and / or LRF plasma can vary. For example, in some embodiments, co-reactants 420, 520, and 620 can be continuous. In other embodiments, co-reactants 420, 520, and 620 can be pulsed. In some embodiments, VHF plasmas 430, 530, 630, and 720 can be continuous. In other embodiments, VHF plasmas 430, 530, 630, and 720 can be pulsed. In some embodiments, LRF plasmas 540, 640, and 730 can be continuous. In other embodiments, LRF plasmas 540, 640, and 730 can be pulsed.

[0073] In some embodiments, the first selectivity (selectivity 1) is defined as: (wet etching rate of the material layer 230 on the second horizontal surface 250 of the bottom portion of the gap feature 220) / (wet etching rate of the material layer 230 on the vertical sidewall 240 of the gap feature 220 at a height of 90 mm from the second horizontal surface 250). The second selectivity (selectivity 2) is defined as: (wet etching rate of the material layer 230 on the second horizontal surface 250 of the bottom portion of the gap feature 220) / (wet etching rate of the material layer 230 on the vertical sidewall 240 of the gap feature 220 at a height of 120 mm from the second horizontal surface 250). The etchant used in the etching process can be dilute hydrofluoric acid (dHF).

[0074] In some embodiments, VHF plasma is provided during the deposition of the material layer, and no co-reactant and LRF plasma are provided during the deposition process. In some embodiments, VHF plasma and co-reactant are provided during the deposition of the material layer, and no LRF plasma is provided during the deposition process. In some embodiments, a first VHF plasma is provided during the deposition of the material layer, and a second VHF plasma, LRF plasma, and co-reactant are provided during the processing. In some embodiments, VHF plasma is provided during the deposition of the material layer, and LRF plasma is provided during the processing. In some embodiments, a first VHF plasma and a first LRF plasma are provided during the deposition of the material layer, and a second VHF plasma, a second LRF plasma, and co-reactant are provided during the processing. In some embodiments, the LRF plasma is pulsed, and the pulse frequency may be between 1 kHz and 10 kHz, between 2.5 kHz and 7.5 kHz, or between 3 kHz and 6 kHz.

[0075] In some embodiments, the power of the VHF plasma can be between 500W and 1800W, between 1000W and 1500W, or between 700W and 1250W. In some embodiments, the power of the LRF plasma can be between 10W and 700W, between 20W and 500W, or between 50W and 100W.

[0076] In some embodiments, the co-reactant may be Ar, H2, or a combination thereof. In some embodiments, the flow rate of the co-reactant may be between 1 slm (standard liters per minute) and 10 slm, between 2 slm and 8 slm, or between 3 slm and 6 slm. In some embodiments, the flow rate of the co-reactant may be between 100 sccm (standard cubic centimeters per minute) and 600 sccm, between 200 sccm and 500 sccm, or between 300 sccm and 400 sccm.

[0077] In some embodiments, during the etching process, selectivity 1 can be between 1.0 and 4.0, between 1.6 and 4.0, between 2.2 and 4.0, or between 3.9 and 4.0. In some embodiments, during the etching process, selectivity 2 can be between 1.0 and 4.4, between 2.1 and 4.4, between 3.2 and 4.4, or between 4.1 and 4.4.

[0078] In some embodiments, selectivity may be increased to about 4.0, about 4.1, or about 4.4. Higher selectivity results in a better ability to remove material layers on horizontal surfaces and to form material layers on the vertical sidewalls of the gap feature.

[0079] refer to Figure 8 This illustrates a reaction system for selectively forming films on a substrate according to some embodiments of the present disclosure. The reaction system 800 can be used to perform one or more steps or sub-steps as described herein and / or to form one or more structures or portions thereof as described herein.

[0080] The reaction system 800 may include a pair of parallel and facing conductive plate electrodes 802, 804 within the interior 811 (reaction zone) of the reaction chamber 803. Plasma can be excited within the reaction chamber 803 by applying VHF power (e.g., 60 MHz) and LRF power (e.g., 430 kHz) from a plasma power source 825 to one electrode (e.g., electrode 804) and electrically grounding the other electrode (e.g., electrode 802). A temperature regulator may be provided in the lower electrode 802, and the temperature of the substrate 801 placed thereon may be maintained at a desired temperature. Electrode 802 may serve as a substrate support. Electrode 804 may serve as a gas distribution device, such as a spray plate. Precursor gas from precursor source 830, co-reactant gas (if any) from co-reactant source 831, purge gas from purge source 832, etc., may be introduced into the reaction chamber 803 via one or more of gas lines 820, gas line 821, and gas line 822 and through electrode 804 (spray plate). Although three gas lines are shown, the reaction system 800 may include any suitable number of gas lines.

[0081] In the reaction chamber 803, a circular pipe 813 with an exhaust line 807 can be provided, through which gases in the interior 811 of the reaction chamber 803 can be discharged. Additionally, a transfer chamber 805 located below the reaction chamber 803 can be provided with a sealing gas line 824 to introduce sealing gas into the interior 811 of the reaction chamber 803 via the interior 816 (transfer zone) of the transfer chamber 805. A separation plate 814 for separating the reaction zone and the transfer zone (a gate valve is omitted from this figure; this gate valve is used to transfer the wafer in and out of the transfer chamber 805) can be provided in the transfer chamber. The transfer chamber can also be provided with an exhaust line 806. In some embodiments, deposition and processing steps can be performed in the same reaction space, allowing two or more (e.g., all) steps to be performed consecutively without exposing the substrate to air or other oxygen-containing atmospheres.

[0082] In some embodiments, a flow-through system (FPS) can be used to achieve continuous flow of inert gas or carrier gas to reaction chamber 803. The carrier gas line may be provided with a bypass line having a precursor reservoir (bottle), and the main line and bypass line can be switched. The bypass line is closed when only carrier gas is intended to be supplied to the reaction chamber, while the main line can be closed when both carrier gas and precursor gas are intended to be supplied to the reaction chamber. The carrier gas can then flow through the bypass line and exit from the bottle along with the precursor gas. In this way, the carrier gas can flow continuously into the reaction chamber, and the precursor gas can be carried in pulses by switching between the main line and the bypass line, with minimal pressure fluctuations in the reaction chamber.

[0083] The reaction system 800 includes one or more controllers 826 that are programmed or otherwise configured to perform one or more method steps as described herein. As those skilled in the art will understand, the controllers are connected to various power sources, heating systems, pumps, robots, and gas flow controllers or valves of the reactor.

[0084] In some embodiments, a multi-chamber reactor (for processing two or more segments or compartments of a wafer disposed close to each other) may be used, wherein reactant gases and rare gases may be supplied through a shared pipeline, while precursor gases may be supplied through a non-shared pipeline.

[0085] According to some embodiments of this disclosure, plasmas (including VHF and LRF plasmas) and co-reactants (including H2 and Ar) are used to achieve desired selectivity of the film. Ion orientation can be controlled by different combinations of VHF and LRF plasmas to densify the film on the vertical sidewalls of the gap feature and to damage the film on the horizontal surface of the substrate and the horizontal surface of the bottom portion of the gap feature. Furthermore, a combination of continuous and pulsed plasmas can help control ion orientation, allowing ions to reach a greater depth to the horizontal surface of the gap feature. Co-reactants can increase ion flux during deposition and / or processing to help achieve the desired selectivity. Therefore, film selectivity can be controlled to selectively form the film on the vertical sidewalls of the gap feature rather than on the horizontal surface of the substrate and the horizontal surface of the bottom portion of the gap feature.

[0086] While some embodiments and advantages of this disclosure have been described in detail, it should be understood that various changes, substitutions, and modifications can be made herein without departing from the spirit and scope of this disclosure as defined by the appended claims. Features of the various embodiments can be used in any combination, provided they do not depart from the spirit and scope of this disclosure. Furthermore, the scope of this application is not intended to be limited to the specific embodiments of the processes, machines, manufactures, compositions of matter, apparatuses, methods, and steps described in the specification. Those skilled in the art will readily understand from this disclosure that, according to this disclosure, existing or later-developed processes, machines, manufactures, compositions of matter, apparatuses, methods, or steps that perform substantially the same function or achieve substantially the same result as the corresponding embodiments described herein can be utilized. Therefore, the appended claims are intended to include such processes, machines, manufactures, compositions of matter, apparatuses, methods, or steps within their scope. Moreover, each claim constitutes a separate embodiment, and the scope of protection claimed by this disclosure includes combinations of claims and embodiments. The scope of protection of this disclosure is limited by the scope of the appended claims. No embodiment or claim of this disclosure is required to satisfy all the purposes, advantages, and features disclosed in this disclosure.

Claims

1. A method for selectively forming a film, comprising: A substrate is provided in a reaction chamber, wherein the substrate includes a first horizontal surface and a gap feature extending downward from the first horizontal surface; A material layer is deposited on the first horizontal surface and in the interstitial features through a deposition process; and The material layer on the first horizontal surface and the material layer on the second horizontal surface of the bottom portion of the gap feature are removed by an etching process to selectively form a film on the vertical sidewall of the gap feature.

2. The method for selectively forming a film according to claim 1, wherein, A first plasma is provided in the reaction chamber during the deposition process.

3. The method for selectively forming a film according to claim 2, wherein, The first plasma includes single-frequency plasma.

4. The method for selectively forming a film according to claim 2, wherein, The first plasma comprises a combination of a first sub-plasma and a pulsed second sub-plasma, and the first sub-plasma is different from the pulsed second sub-plasma.

5. The method for selectively forming a film according to claim 1, wherein, During the deposition process, a first plasma and co-reactants are provided in the reaction chamber.

6. The method for selectively forming a film according to claim 5, wherein, The first plasma comprises a single-frequency plasma, and the co-reactants comprise H2, Ar, or a combination thereof.

7. The method for selectively forming a film according to claim 5, wherein, The first plasma comprises a combination of a first sub-plasma and a pulsed second sub-plasma, the co-reactants comprising H2, Ar, or a combination thereof, and the first sub-plasma is different from the pulsed second sub-plasma.

8. The method for selectively forming a film according to claim 5, wherein, During the etching process, the etching rate of the material layer on the second horizontal surface of the bottom portion of the gap feature is approximately twice that of the material layer on the vertical sidewall of the gap feature.

9. The method for selectively forming a film according to claim 1, further comprising performing a processing step after the deposition process and before the etching process.

10. The method for selectively forming a film according to claim 9, wherein, A first plasma is provided in the reaction chamber during the deposition process, and a second plasma is provided in the reaction chamber during the processing, wherein the first plasma is different from the second plasma.

11. The method for selectively forming a film according to claim 10, wherein, The second plasma includes a combination of a first sub-plasma and a second sub-plasma, and the first sub-plasma is different from the second sub-plasma.

12. The method for selectively forming a film according to claim 11, wherein, During the processing, co-reactants are provided in the reaction chamber, and the co-reactants include H2, Ar, or a combination thereof.

13. The method for selectively forming a film according to claim 11, wherein, During the etching process, the etching rate of the material layer on the second horizontal surface of the bottom portion of the gap feature is approximately three times that of the material layer on the vertical sidewall of the gap feature.

14. The method for selectively forming a film according to claim 10, wherein, The first plasma includes a first combination of a first sub-plasma and a second sub-plasma, the second plasma includes a second combination of a third sub-plasma and a fourth sub-plasma, and the first sub-plasma, the second sub-plasma, the third sub-plasma and the fourth sub-plasma are different.

15. The method for selectively forming a film according to claim 14, wherein, The second sub-plasma of the first combination of the first plasma is a pulsed plasma.

16. The method for selectively forming a film according to claim 14, wherein, During the processing, co-reactants are provided in the reaction chamber, and the co-reactants include H2, Ar, or a combination thereof.

17. The method for selectively forming a film according to claim 14, wherein, During the etching process, the etching rate of the material layer on the second horizontal surface of the bottom portion of the gap feature is approximately four times that of the material layer on the vertical sidewall of the gap feature.

18. The method for selectively forming a film according to claim 10, wherein, The frequency of the first plasma is greater than the frequency of the second plasma.

19. The method for selectively forming a film according to claim 10, wherein, The first plasma densifies the material layer on the vertical sidewall of the gap feature.

20. The method for selectively forming a film according to claim 10, wherein, The second plasma damages the material layer on the first horizontal surface and the material layer on the second horizontal surface at the bottom of the gap feature, such that the material layer on the first horizontal surface and the material layer on the second horizontal surface at the bottom of the gap feature are removed during the etching process.

21. A reaction system, comprising: Reaction chamber; A substrate support, located in the reaction chamber and configured to support the substrate; The precursor source provides the precursor to the reaction chamber; Co-reactant source, which provides co-reactants to the reaction chamber; A plasma power source that supplies plasma to the reaction chamber; as well as A controller configured to control the precursor, co-reactant, and plasma to perform the method as described in claim 1.