Method and system for surface modification of alumina caps in antibacterial cosmetics

By constructing a gradient controlled-release structure on the surface of the aluminum alloy cap and using an automated production line system, the contradiction between the release of antibacterial agents and the safety of cosmetic materials was resolved, achieving long-lasting antibacterial and self-cleaning effects on the cap surface and improving the modification uniformity of the three-dimensional parts.

CN123108698APending Publication Date: 2026-11-17NINGBO Z&Z NEW MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611133083.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing antibacterial treatments on the surface of aluminum alloy caps present a contradiction between the release of antibacterial agents and the safety of cosmetic ingredients, and the uneven modification of the inner cavity of three-dimensional parts is difficult to guarantee.

Method used

By constructing a gradient controlled-release structure, silver and copper ions are loaded into the nanopores using a stepwise impregnation process. Combined with step-by-step sealing and hydrophobic treatment, a gradient controlled-release structure with decreasing porosity from the inside to the outside is formed. The non-uniformity of the modification of the three-dimensional part is solved by an automated production line system.

Benefits of technology

It achieves the synergistic effect of long-term release of antibacterial agents and safety of cosmetic materials, improves the antibacterial effect and self-cleaning performance of the cap surface, solves the problem of antibacterial agent migration and contamination, and ensures the uniformity of modification of three-dimensional parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108698A_ABST
    Figure CN123108698A_ABST
Patent Text Reader

Abstract

This invention relates to the technical field of cosmetic packaging materials, and in particular to a method and system for modifying the surface of antibacterial cosmetic alumina pump caps. The method includes: pre-treatment of the aluminum alloy pump cap substrate by degreasing and cleaning; anodizing to generate an alumina thin film layer with a nanoscale porous structure on the pump cap surface; immersion in an acidic pore-expanding solution for pore-expanding treatment; employing a step-by-step impregnation process, first enriching and loading silver ions onto the shallow layer of the nanopores, then enriching and loading copper ions onto the deeper layer; and performing a stepped sealing treatment on the nanopores after loading the antibacterial components, first forming a porous barrier layer in the middle section of the pores with nano-silica particles, then sealing the pores with hot water to narrow the pore openings, forming a gradient controlled-release structure with decreasing porosity from the inside out. This invention improves the antibacterial effect and antibacterial durability of the pump cap surface, and solves the industry problem of antibacterial agent migration and contamination of cosmetic materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the technical field of cosmetic packaging materials, and in particular to a method and system for surface modification of antibacterial cosmetic alumina caps. Background Technology

[0002] Aluminum alloy pump caps are widely used in mid-to-high-end cosmetic packaging due to their lightweight, aesthetic appeal, and recyclability. To improve the surface hardness and corrosion resistance, the industry commonly uses anodizing to create a thin aluminum oxide film. However, this aluminum oxide film naturally possesses a honeycomb-like porous structure, making it highly susceptible to absorbing cosmetic residues and allowing bacteria to grow within the micropores. Each time a consumer presses the pump, bacteria from their fingers remain on the surface, multiplying in the micropores and causing continuous cross-contamination.

[0003] To address the aforementioned issues, relevant existing technologies have been proposed.

[0004] For example, the Chinese patent authorization announcement number is CN116136025B, entitled "Antibacterial liquid for aluminum alloy, antibacterial aluminum alloy parts and preparation method thereof", which achieves antibacterial function through metal salts such as silver and copper, but lacks means to control the release of antibacterial agents.

[0005] For example, Chinese Patent Publication No. CN111647926A, entitled "An Invention Patent on a Method for Preparing Antibacterial Aluminum or Aluminum Alloy by Anodizing", directly deposits antibacterial substances during the anodizing process. Although the process is simplified, it does not have a good effect on the treatment of the inner cavity of three-dimensional parts.

[0006] In addition, some existing solutions mix antibacterial liquid and sealing liquid to treat aluminum alloy parts in one go, attempting to achieve both antibacterial and sealing effects, but the actual antibacterial rate is significantly low.

[0007] Analysis of existing technologies reveals that none of the current solutions resolve the conflict between antibacterial agent release and the safety of cosmetic ingredients. If the antibacterial agent is not controlled by sealing, large amounts of metal ions, especially silver ions, will continue to be released, potentially migrating into the bottle and contaminating the cosmetic ingredient. Conversely, if conventional sealing processes completely seal the pores, the antibacterial agent is trapped inside and cannot reach the surface to exert its antibacterial effect.

[0008] Meanwhile, existing aluminum alloy surface treatment equipment is mostly designed for flat plates or simple profiles, while the cap is a complex three-dimensional part with a top surface, side walls, and an inner cavity. When processed in existing equipment, the uniformity of modification in the inner cavity and deep recesses of the cap is difficult to guarantee due to the Faraday shielding effect and uneven flow of the bath solution. Summary of the Invention

[0009] To address the aforementioned technical problems, this invention provides a method and system for modifying the surface of alumina caps in antibacterial cosmetics by constructing a gradient controlled-release structure to resolve the contradiction between antibacterial agent release and cosmetic material safety.

[0010] The method for surface modification of antibacterial cosmetic alumina caps of the present invention includes the following steps:

[0011] S1: Degreasing and cleaning pretreatment is performed on the aluminum alloy cap substrate to remove surface oil and oxide scale, and obtain a clean and activated aluminum substrate surface;

[0012] S2: The pre-treated caps are anodized to generate an aluminum oxide thin film layer with a nanoscale porous structure on the surface of the caps;

[0013] S3: Immerse the anodized cap in an acidic pore-expanding solution for pore-expanding treatment to increase the pore size of the nanoporous structure;

[0014] S4: A step-by-step impregnation process is used to load shallow fast-acting antibacterial components and deep long-acting antibacterial components into the expanded nanopores respectively;

[0015] S5: Perform a step-by-step sealing process on the nanopores after loading antibacterial components. The step-by-step sealing process includes a semi-sealing process in the middle section of the pores and a narrowing sealing process at the pore opening, so that the nanopores form a gradient controlled-release structure with decreasing porosity from the inside to the outside.

[0016] S6: The surface of the cap after the stepped sealing is hydrophobically treated to form a low surface energy self-cleaning film on the outermost layer of the cap;

[0017] S7: Dry and cure the hydrophobicated caps;

[0018] Between each adjacent processing step from S1 to S6, the cap is cleaned using deionized water.

[0019] Furthermore, the pretreatment process for degreasing and cleaning in step S1 specifically includes:

[0020] S11: Immerse the aluminum alloy cap blank in an alkaline degreasing solution and treat it at a temperature of 40℃ to 60℃ for 2 to 5 minutes to perform alkaline degreasing.

[0021] S12: Immerse the degreased caps in an acidic neutralizing solution and treat at room temperature for 1 to 3 minutes to perform acid washing and neutralization;

[0022] S13: After acid pickling and neutralization, rinse the cap thoroughly with deionized water with a resistivity of not less than 5 MΩ·cm.

[0023] The alkaline degreasing solution is specifically configured as a sodium hydroxide solution, sodium carbonate solution, trisodium phosphate solution, or sodium silicate solution, preferably a sodium hydroxide solution with a mass fraction of 3% to 8%.

[0024] The acid neutralizing solution is specifically configured as a nitric acid solution, a sulfuric acid solution, or a hydrochloric acid solution, preferably a nitric acid solution with a mass fraction of 10% to 20%.

[0025] Furthermore, the anodizing process in step S2 specifically includes:

[0026] After degreasing and cleaning, the button caps are placed in an acidic electrolyte and treated for 25 to 40 minutes at a temperature of 18°C ​​to 22°C and a DC constant voltage of 14V to 18V, so that the thickness of the alumina film formed on the surface of the button cap is 8μm to 15μm and the initial pore size of the nanopores is 10nm to 20nm.

[0027] The acidic electrolyte is specifically configured as a sulfuric acid solution, an oxalic acid solution, or a phosphoric acid solution, preferably a sulfuric acid solution with a mass fraction of 15% to 20%.

[0028] Furthermore, the hole enlargement process in step S3 is specifically configured as follows:

[0029] The anodized caps are immersed in an acidic pore-expanding solution and treated at a temperature of 25°C to 35°C for 3 to 8 minutes to expand the pore size of the nanopores from the initial anodized pore size to 50 to 80 nm.

[0030] The acidic pore-expanding solution is specifically configured as a phosphoric acid solution or an oxalic acid solution, preferably a phosphoric acid solution with a mass fraction of 5% to 10%.

[0031] Furthermore, the step-by-step impregnation process in step S4 specifically includes the following steps:

[0032] S41: The first step of impregnation involves immersing the expanded cap in the silver salt solution in the first impregnation tank for 5 to 10 minutes at room temperature, so that silver ions are enriched and loaded in the shallow region of the nanopores through physical adsorption and electrostatic interaction.

[0033] S42: After completing the first step of impregnation, rinse the cap with deionized water with a resistivity of not less than 5 MΩ·cm for 30 to 60 seconds;

[0034] S43: After rinsing, place the cap in a weakly alkaline solution with a pH of 8.5 to 9.5 for 1 to 3 minutes to reduce some of the silver ions loaded in the shallow layer of the pores to nano-silver elemental.

[0035] S44: The second step is immersion. The rinsed cap is immersed in the copper salt aqueous solution in the second immersion tank and soaked at room temperature for 8 to 15 minutes. Due to the difference in diffusion rate between copper ions and silver ions, copper ions are enriched and loaded in the deep region of the nanopores.

[0036] The silver salt aqueous solution is specifically configured as a silver nitrate solution, a silver acetate solution, or a silver sulfate solution, preferably a silver nitrate solution with a mass concentration of 0.5 g / L to 2 g / L;

[0037] The copper salt aqueous solution is specifically configured as copper gluconate solution, copper sulfate solution or copper acetate solution, preferably a copper gluconate solution with a mass concentration of 5 g / L to 15 g / L.

[0038] The weakly alkaline solution is specifically configured as a sodium carbonate solution, a sodium bicarbonate solution, or an ammonia solution, preferably a sodium carbonate solution, with its concentration adjusted to a pH value between 8.5 and 9.5.

[0039] Furthermore, the stepped sealing process in step S5 specifically includes:

[0040] S51: First-stage sealing: The caps processed in step S4 are immersed in nano-silica sol, wherein the silica particles in the nano-silica sol have a diameter of 5nm to 15nm and a pH value of 2 to 4. The caps are immersed at room temperature for 5 to 10 minutes to enrich and deposit the nano-silica particles in the middle section of the nano-pores, forming a permeable inorganic porous barrier layer.

[0041] S52: After the first stage of sealing is completed, the cap is preheated at 80°C to 100°C for 5 to 10 minutes to allow the nano-silica particles deposited in the middle section of the nanopores to undergo a dehydration condensation reaction and form a cross-linked network.

[0042] S53: Second stage of sealing. After the first stage of sealing is completed, the cap is placed in high-purity deionized water with a resistivity of not less than 18 MΩ·cm at 95℃ to 98℃ for 15 to 20 minutes. The volume expansion effect generated by the hydration of the alumina pore wall causes the pore diameter of the nanopores to shrink to 10nm to 30nm.

[0043] By combining the inorganic porous barrier layer of the first-stage sealing with the pore narrowing structure of the second-stage sealing, a release rate gradient is formed for the antibacterial components in the shallow and deep layers.

[0044] The nano-silica sol is preferably an acidic silica sol solution with a mass fraction of 5% to 10%.

[0045] Furthermore, the hydrophobicity treatment process in step S6 is specifically configured as follows:

[0046] After the step-sealed caps are applied, they are immersed or sprayed in a fluorinated silane coupling agent solution for 1 to 3 minutes to allow a fluorinated silane coating to adhere to the surface of the caps.

[0047] The fluorinated silane coupling agent solution is preferably a heptadecafluorodecyltrimethoxysilane ethanol solution with a mass fraction of 0.5% to 2%.

[0048] Furthermore,

[0049] The drying and curing process in step S7 is specifically as follows:

[0050] After hydrophobication treatment, the caps are baked at 100°C to 120°C for 20 to 30 minutes to allow the fluorinated silane coating to crosslink and cure on the cap surface, forming a hydrophobic and oleophobic film.

[0051] Furthermore, it also includes production auxiliary processes, which include the following two processes:

[0052] During the operation of each wet treatment tank corresponding to steps S1 to S6, the liquid level, temperature and concentration parameters of each tank liquid are monitored in real time by an online sensor group. When any parameter deviates from the set range, the corresponding treatment tank is automatically replenished with concentrate or deionized water to maintain the stability of the tank liquid composition.

[0053] The silver-containing bath solution discharged after impregnation in step S4 is introduced into the ion exchange resin recovery device to adsorb and recover the free silver ions in the bath solution. The recovered bath solution is returned to step S4 for reuse. The resin after adsorption saturation is regenerated by elution with dilute nitric acid, and the eluent is returned to step S4 for recycling.

[0054] A surface modification system for antibacterial cosmetic alumina caps, used to realize a method for modifying the surface of antibacterial cosmetic alumina caps, comprises:

[0055] Multiple processing tanks are arranged sequentially along the process flow direction. Each processing tank includes at least a pretreatment tank group, an anodizing tank, a hole-expanding tank, a first immersion tank, a weak alkali treatment tank, a second immersion tank, a silica sol treatment tank, a hot water sealing tank, and a hydrophobic treatment tank. A cleaning tank is provided between each adjacent processing tank. Each processing tank is equipped with a temperature control device, which is electrically connected to the central control system and is used to independently adjust the temperature of the solution in each processing tank according to the instructions of the central control system.

[0056] An automatic trolley transport system is equipped with a rotating hanger for attaching button caps. During the immersion process in the tank, the rotating hanger rotates continuously around its own axis at a speed of 5 rpm to 15 rpm, so that the surfaces of the button caps at different positions on the hanger are alternately exposed to the flow direction of the tank liquid, thereby eliminating the contact differences between the three-dimensional structure of the button caps and the tank liquid.

[0057] A tank liquid monitoring and automatic replenishment system, the tank liquid monitoring and automatic replenishment system includes an online sensor group installed in each processing tank and an automatic replenishment pump group connected to each processing tank, wherein the online sensor group of the first immersion tank is provided with a silver ion selective electrode.

[0058] A silver ion recovery device is connected to the first impregnation tank and is used to adsorb and recover free silver ions in the solution of the first impregnation tank, and return the recovered solution to the first impregnation tank.

[0059] A preheating crosslinking treatment device is provided, which is disposed between the silica sol treatment tank and the hot water sealing tank. The preheating crosslinking treatment device is preferably a heating oven or heating channel structure, used to preheat the caps after silica sol treatment, so that a crosslinking network is formed between the nano-silica particles deposited in the middle section of the nanopores.

[0060] A drying and curing device is provided downstream of the hydrophobic treatment tank. The drying and curing device is a multi-temperature zone tunnel drying and curing oven that is sequentially divided into a preheating zone, a curing zone, and a cooling zone along the conveying direction.

[0061] The central control system is electrically connected to the automatic trolley transport system, the tank liquid monitoring and automatic replenishment system, the silver ion recovery device and the drying and curing equipment, and is used to control the operating parameters of each system. The temperature of each area is independently controlled by the central control system.

[0062] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0063] This invention employs a stepwise impregnation process, first loading silver ions onto the shallow layer of nanopores and then loading copper ions onto the deeper layer, forming a dual-source antibacterial system with rapid shallow-layer action and long-lasting deep-layer action. Silver ions rapidly kill surface bacteria in the shallow layer of the pores, while copper ions are continuously released as reserves in the deeper layer. The two work synergistically to inhibit bacteria and greatly improve the antibacterial effect.

[0064] Through a stepped sealing process, a porous barrier layer is first formed in the middle section of the pores using nano-silica particles, and then the pores are narrowed by hot water hydration, creating a gradient controlled-release structure with decreasing porosity from the inside out. This structure allows the antibacterial agent to be released at an extremely low rate, improving the long-lasting antibacterial properties of the cap surface and solving the industry problem of antibacterial agent migration and contamination of cosmetic materials.

[0065] A weak alkaline reduction treatment was added after the first impregnation step and before the second impregnation step, which reduced some of the silver ions already loaded in the shallow layer of the pores to nano-silver in situ, forming a composite antibacterial form of silver ions plus nano-silver, which further improved the water resistance and antibacterial durability of silver.

[0066] After the silica sol semi-sealing, a preheating cross-linking treatment was added, which caused the nano-silica particles deposited in the middle section of the pores to undergo a dehydration condensation reaction to form a cross-linking network. This upgraded the porous barrier layer from physical stacking to chemical bonding, significantly improving the structural strength and controlled release stability of the barrier layer.

[0067] A fluorinated silane hydrophobic and oleophobic film is formed on the outermost layer of the applicator cap through hydrophobic treatment, giving the surface of the applicator cap a self-cleaning function. Cosmetic residues are not easy to adhere to, reducing the nutrient source for bacterial growth from the source.

[0068] The automated production line system uses a rotating fixture design to make the caps continuously rotate in the bath, with each surface alternately exposed to the direction of the bath flow. This solves the problem of uneven modification of the inner cavity and deep recesses of three-dimensional parts caused by the Faraday shielding effect. Attached Figure Description

[0069] Figure 1 This is a flowchart of the method of the present invention;

[0070] Figure 2 This is a system architecture diagram of the present invention;

[0071] Figure 3 This is a flowchart of the pretreatment process for degreasing and cleaning in step S1 of the present invention.

[0072] Figure 4 This is a flowchart of the step-by-step impregnation process in step S4 of the present invention;

[0073] Figure 5 This is a flowchart of the stepped sealing process in step S5 of the present invention. Detailed Implementation

[0074] The specific embodiments of the present invention will be described in further detail below with reference to the accompanying drawings and examples. The following examples are for illustrative purposes only and are not intended to limit the scope of the invention.

[0075] like Figures 1 to 5 As shown:

[0076] Example 1:

[0077] The method for surface modification of antibacterial cosmetic alumina caps of the present invention includes the following steps:

[0078] S1: Degreasing and cleaning pretreatment is performed on the aluminum alloy cap substrate to remove surface oil and oxide scale, and obtain a clean and activated aluminum substrate surface;

[0079] S2: The pre-treated caps are anodized to generate an aluminum oxide thin film layer with a nanoscale porous structure on the surface of the caps;

[0080] S3: Immerse the anodized cap in an acidic pore-expanding solution for pore-expanding treatment to increase the pore size of the nanoporous structure;

[0081] S4: A step-by-step impregnation process is used to load shallow fast-acting antibacterial components and deep long-acting antibacterial components into the expanded nanopores respectively;

[0082] S5: Perform a step-by-step sealing process on the nanopores after loading antibacterial components. The step-by-step sealing process includes a semi-sealing process in the middle section of the pores and a narrowing sealing process at the pore opening, so that the nanopores form a gradient controlled-release structure with decreasing porosity from the inside to the outside.

[0083] S6: The surface of the cap after the stepped sealing is hydrophobically treated to form a low surface energy self-cleaning film on the outermost layer of the cap;

[0084] S7: Dry and cure the hydrophobicated caps;

[0085] Between each adjacent processing step from S1 to S6, the cap is cleaned using deionized water.

[0086] In this embodiment, through the sequential implementation of the above seven steps, a complete functional structure is constructed on the cap surface, from the porous alumina substrate to the antibacterial component loading layer, then to the stepped sealing controlled release layer, and finally to the hydrophobic self-cleaning outer layer.

[0087] In step S4, stepwise impregnation achieves spatial partitioning loading of silver ions in the shallow layer and copper ions in the deep layer, laying the foundation for subsequent gradient controlled release. Step S5, through two-stage pore sealing, forms a gradient structure with decreasing porosity from the inside out, providing structural assurance for the precise controlled release of the antibacterial agent. This embodiment serves as the basic framework of the entire method, and the sequence and functional coordination between the steps form a complete process logic chain. Subsequent embodiments optimize and refine the specific process parameters based on this embodiment.

[0088] In Example 1, it is important to note that the specific process parameters in each step, such as bath concentration, treatment temperature, and treatment time, should be appropriately selected and adjusted according to the material and size of the cap and the performance requirements of the final product. Deionized water rinsing between adjacent processes must be thorough and complete to prevent cross-contamination between different bath solutions from affecting the stability of subsequent processes. The resistivity of the deionized water used for rinsing after acid pickling neutralization and after the first-step immersion should not be lower than 5 MΩ·cm. For the hot water sealing process, it is recommended to use high-purity water with a resistivity of not less than 18 MΩ·cm to ensure the purity of the hydrated sealing product. Ordinary deionized water is sufficient for rinsing between other processes.

[0089] Example 2:

[0090] As a preferred embodiment of the first embodiment, the pretreatment process for degreasing and cleaning in step S1 specifically includes:

[0091] S11: Immerse the aluminum alloy cap blank in an alkaline degreasing solution and treat it at a temperature of 40°C to 60°C for 2 to 5 minutes to perform alkaline degreasing; the alkaline degreasing solution is specifically set as sodium hydroxide solution, sodium carbonate solution, trisodium phosphate solution or sodium silicate solution, preferably a sodium hydroxide solution with a mass fraction of 3% to 8%.

[0092] S12: Immerse the degreased caps in an acidic neutralizing solution and treat them at room temperature for 1 to 3 minutes to perform acid washing and neutralization. The acidic neutralizing solution is specifically set as a nitric acid solution, a sulfuric acid solution, or a hydrochloric acid solution, preferably a nitric acid solution with a mass fraction of 10% to 20%.

[0093] S13: After acid pickling and neutralization, rinse the cap thoroughly with deionized water with a resistivity of not less than 5 MΩ·cm.

[0094] Preferably, the anodizing process in step S2 specifically includes:

[0095] The button caps, after degreasing and cleaning, are placed in an acidic electrolyte and treated for 25 to 40 minutes at a temperature of 18°C ​​to 22°C and a DC constant voltage of 14V to 18V, so that the thickness of the alumina film formed on the surface of the button cap is 8μm to 15μm and the initial pore size of the nanopores is 10nm to 20nm. The acidic electrolyte is specifically set as a sulfuric acid solution, oxalic acid solution or phosphoric acid solution, preferably a sulfuric acid solution with a mass fraction of 15% to 20%.

[0096] Preferably, the hole enlargement process in step S3 is specifically configured as follows:

[0097] The anodized caps are immersed in an acidic expanding solution and treated at a temperature of 25°C to 35°C for 3 to 8 minutes to expand the pore size of the nanopores from the initial anodized pore size to 50 to 80 nm. The acidic expanding solution is specifically a phosphoric acid solution or an oxalic acid solution, preferably a phosphoric acid solution with a mass fraction of 5% to 10%.

[0098] More preferably, the step-by-step impregnation process in step S4 specifically includes the following steps:

[0099] S41: The first step of impregnation involves immersing the expanded cap in the silver salt aqueous solution in the first impregnation tank for 5 to 10 minutes at room temperature, so that silver ions are enriched and loaded in the shallow region of the nanopores through physical adsorption and electrostatic interaction. The silver salt aqueous solution is specifically set as silver nitrate solution, silver acetate solution or silver sulfate solution, preferably a silver nitrate solution with a mass concentration of 0.5 g / L to 2 g / L.

[0100] S42: After completing the first step of impregnation, rinse the cap with deionized water with a resistivity of not less than 5 MΩ·cm for 30 to 60 seconds;

[0101] It should be noted that the deionized water rinsing operation in this step only removes the free silver ions that have not been adsorbed on the surface of the cap and the opening of the pores. The silver ions already loaded in the shallow pore area are combined with the alumina pore walls through electrostatic attraction and coordination bonds. Their desorption free energy is much higher than the shear force of the water flow. Therefore, this cleaning operation will not have a substantial impact on the total amount of silver ions that have been enriched and loaded in the shallow pore area.

[0102] The purpose of this rinsing operation is to remove residual free silver ions to prevent cross-contamination of the bath solution, rather than to wash away already adsorbed silver ions. In actual production, the cleaning effect and the maintenance of the adsorption capacity can be balanced by controlling the rinsing time, water flow intensity, and number of rinsing cycles.

[0103] S43: After rinsing, place the cap in a weakly alkaline solution with a pH of 8.5 to 9.5 for 1 to 3 minutes to reduce some of the silver ions loaded in the shallow layer of the pores to nano-silver elemental.

[0104] It should be noted that this reduction treatment only converts a portion of the silver ions already loaded in the shallow layer of the pores into nano-silver; the majority of the silver ions remain in an ionic state in the shallow pore region. Due to the short reduction time of only 1 to 3 minutes, the reduction reaction occurs only in the outermost layer of the shallow pore region. After the silver ions are reduced to silver atoms, their size changes from approximately 0.2 nm to approximately 0.29 nm. This size change is negligible relative to the pore diameter (50 nm to 80 nm) and will not cause physical blockage of the main pore space. Subsequently, copper ions can still diffuse normally along the pore walls to the deeper regions during the second impregnation process.

[0105] The purpose of this reduction treatment is to form a composite antibacterial morphology of "silver ions + nano-silver" to enhance the antibacterial durability, rather than to seal the pores. Room temperature is sufficient for the reduction treatment; no additional heating is required.

[0106] S44: The second step is immersion. The rinsed cap is immersed in the copper salt aqueous solution in the second immersion tank and soaked at room temperature for 8 to 15 minutes. Due to the difference in diffusion rate between copper ions and silver ions, copper ions are enriched and loaded in the deep region of the nanopores. The copper salt aqueous solution is specifically set as copper gluconate solution, copper sulfate solution or copper acetate solution, preferably copper gluconate solution with a mass concentration of 5 g / L to 15 g / L.

[0107] Preferably, the stepped sealing process in step S5 specifically includes:

[0108] S51: First-stage sealing: The caps processed in step S4 are immersed in nano-silica sol, wherein the silica particles in the nano-silica sol have a diameter of 5nm to 15nm and a pH value of 2 to 4. The caps are immersed at room temperature for 5 to 10 minutes to enrich and deposit the nano-silica particles in the middle section of the nanopores, forming a permeable inorganic porous barrier layer. The nano-silica sol is preferably an acidic silica sol solution with a mass fraction of 5% to 10%.

[0109] S52: After the first stage of sealing is completed, the cap is preheated at 80°C to 100°C for 5 to 10 minutes to allow the nano-silica particles deposited in the middle section of the nanopores to undergo a dehydration condensation reaction and form a cross-linked network.

[0110] S53: Second stage of sealing. After the first stage of sealing is completed, the cap is placed in high-purity deionized water with a resistivity of not less than 18 MΩ·cm at 95℃ to 98℃ for 15 to 20 minutes. The volume expansion effect generated by the hydration of the alumina pore wall causes the pore diameter of the nanopores to shrink to 10nm to 30nm.

[0111] By combining the inorganic porous barrier layer of the first-stage sealing with the pore narrowing structure of the second-stage sealing, a release rate gradient is formed for the antibacterial components in the shallow and deep layers.

[0112] Preferably, the hydrophobicity treatment process in step S6 is specifically configured as follows:

[0113] After the step-sealed caps are applied, they are immersed or sprayed in a fluorinated silane coupling agent solution for 1 to 3 minutes to coat the surface of the caps with a fluorinated silane coating. The fluorinated silane coupling agent solution is preferably a heptadecafluorodecyltrimethoxysilane ethanol solution with a mass fraction of 0.5% to 2%.

[0114] More preferably, the drying and curing process in step S7 specifically includes:

[0115] After hydrophobication treatment, the caps are baked at 100°C to 120°C for 20 to 30 minutes to allow the fluorinated silane coating to crosslink and cure on the cap surface, forming a hydrophobic and oleophobic film.

[0116] Regarding the distribution of substances within the nanopores, it should be noted that in this invention, the distribution of silver ions, nano-silver elements, and copper ions along the depth direction within the nanopores, i.e. from the pore opening to the bottom, is "relatively enriched" rather than "absolutely stratified."

[0117] Specifically, silver ions are mainly concentrated in the shallow region of the nanopores (from the pore opening to a depth of approximately 2 μm), but not all silver ions are strictly confined to this region; some silver ions may diffuse into the middle or deeper regions. Copper ions are mainly concentrated in the deep region of the nanopores (approximately 2 μm to 8 μm depth), but a small amount of copper ions may also be present in the shallow region. Nano-silica particles are mainly concentrated and deposited in the middle region of the nanopores (approximately 3 μm to 5 μm depth). There are certain gradual transition zones of concentration between the regions, rather than strictly defined physical boundaries. This gradual distribution is an inevitable result of the competition between adsorption and diffusion rates in the stepwise impregnation process, as well as the pre-occupation adsorption effect. It does not affect the realization of the "rapid effect in the shallow layer and long-lasting effect in the deep layer" antibacterial function, nor does it affect the controlled release effect of the gradient controlled release structure.

[0118] The terms "shallow layer," "middle section," and "deep layer" in this invention refer to the relative enrichment locations and main functional areas of various substances in the pore depth direction.

[0119] The technical effects of the solution in Embodiment 2 are as follows:

[0120] Based on the basic implementation scheme of Example 1, the present invention is implemented within the above-mentioned preferred parameter range. The process parameters of each step cooperate and work together to ensure the complete construction of the gradient controlled release structure.

[0121] The combined use of alkaline degreasing and acid pickling neutralization in the pretreatment step ensured the cleanliness and activation state of the aluminum substrate surface, providing a uniform reaction interface for anodizing. In the anodizing step, the coordinated control of electrolyte concentration, temperature, voltage, and processing time ensured that the thickness of the alumina film and the initial pore size were within a suitable matching range. The pore enlargement step precisely expanded the pore size to 50nm to 80nm, providing sufficient space for subsequent antibacterial agent loading while preserving the integrity of the pore structure for stepped sealing. The coordinated use of silver salt aqueous solution concentration, copper salt aqueous solution concentration, and immersion time in each step of the step-by-step impregnation process further enhanced the quality of the anodizing process. This process ensures a gradient distribution of silver ions enriched in the shallow layer and copper ions enriched in the deep layer. The weak base reduction step promptly converts some silver ions into nano-silver element after silver ion loading, forming a composite antibacterial morphology where ionic and elemental states coexist. The synergistic coordination of silica sol concentration, particle size, pH value, preheating temperature, and time in the step-sealing step improves the permeability of the porous barrier layer and the integrity of the cross-linked network. The temperature and time of hot water sealing precisely control the degree of pore narrowing. The temperature and time coordination of the hydrophobic treatment and drying curing steps result in a relatively complete coverage and sufficient cross-linking of the fluorinated silane coating.

[0122] It is important to note the following during the implementation of Example 2: Each process parameter should be strictly controlled within the preferred range. Exceeding the range may lead to problems such as mismatch between pore size and antibacterial agent particle size, insufficient antibacterial agent loading, incomplete sealing layer structure, or insufficient cross-linking.

[0123] In particular, the pH value and soaking time of the weak alkali reduction treatment need to be precisely controlled. If the pH value is too low, the reduction will be insufficient; if it is too high, it may lead to excessive reduction of silver ions, forming large-diameter silver particles. The temperature and time of the preheating crosslinking treatment also need to be precisely controlled. If the temperature is too low or the time is insufficient, the crosslinking will be insufficient; if it is too high or too long, it may damage the porous structure of the deposited silica sol. The temperature and concentration of each bath solution should be kept stable to avoid large fluctuations that may affect product consistency. The resistivity of the deionized water used for cleaning should not be lower than 5 MΩ·cm, and the cleaning time should be sufficient but not too long to avoid excessive elution of adsorbed silver ions.

[0124] Example 3:

[0125] As another preferred embodiment of the first embodiment, it also includes a production auxiliary process, which includes the following two processes:

[0126] During the operation of each wet processing tank corresponding to steps S1 to S6, an online sensor array monitors the liquid level, temperature, and concentration parameters of each tank solution in real time. Specifically, a pH meter monitors the pH of the tank solution, a conductivity meter monitors the concentration changes, and a temperature sensor monitors the temperature. A silver ion selective electrode is installed in the first immersion tank to accurately monitor the silver ion concentration. Data from each sensor is transmitted to the central control system in real time. When any parameter deviates from the set range, the central control system automatically starts the replenishment pump to replenish the corresponding processing tank with concentrated solution or deionized water to maintain the stability of the tank solution composition.

[0127] Preferably, the silver-containing bath solution discharged after impregnation in step S4 is introduced into an ion exchange resin recovery device. This device is filled with a strongly acidic cation exchange resin. When the silver-containing bath solution circulates through the resin column, the free silver ions are adsorbed and retained by the resin, achieving a recovery rate of over 90%. The adsorbed and recovered bath solution is returned to step S4 for reuse, reducing the amount of fresh silver salt required for replenishment. After adsorption saturation, the resin is regenerated by elution with dilute nitric acid, and the eluted silver ions are returned to the first impregnation tank for recycling in the form of silver nitrate.

[0128] In this embodiment, the online monitoring and automatic replenishment process of the bath solution enables real-time monitoring and automatic adjustment of the process parameters of each treatment tank, avoiding batch-to-batch quality differences caused by fluctuations in bath solution composition, and ensuring the stability and consistency of product performance under long-term continuous production conditions. The silver ion recovery and recycling process uses ion exchange resin to adsorb and recover free silver ions in the silver-containing bath solution, achieving a silver recycling rate of over 90%, significantly reducing the consumption cost of silver nitrate and the treatment cost of silver-containing wastewater. The parallel implementation of these two auxiliary processes upgrades the entire production process from "experience-dependent" to "data-driven," providing technical support for large-scale continuous production.

[0129] The following points should be noted during the implementation of Example 3: Online sensors need to be calibrated regularly to ensure the accuracy of monitoring data. The silver ion selective electrode, as a dedicated sensor for the first impregnation tank, requires regular maintenance. The replenishment pump of the automatic replenishment system should be set with a reasonable replenishment cycle and volume based on the tank liquid consumption rate to avoid over- or under-replenishment. The ion exchange resin needs to have its adsorption capacity tested regularly according to the actual production load and throughput. After saturation, it should be eluted and regenerated promptly to prevent silver ions from penetrating the resin column and causing loss. The concentration of the acid used during elution and regeneration should be controlled within an appropriate range. Too low a concentration will result in incomplete elution, while too high a concentration may damage the resin structure. Technicians can adjust the concentration based on actual operation and results.

[0130] Example 4:

[0131] The antibacterial cosmetic alumina cap surface modification system of the present invention is used to implement the method of antibacterial cosmetic alumina cap surface modification. A preferred embodiment of the system is as follows:

[0132] The antibacterial cosmetic alumina cap surface modification system used in this embodiment includes: a pretreatment tank group, an anodizing tank, a pore-expanding tank, a first immersion tank, a weak alkali treatment tank, a second immersion tank, a silica sol treatment tank, a hot water sealing tank, and a hydrophobication treatment tank arranged sequentially along the process flow direction. Cleaning tanks are provided between each adjacent treatment tank. The system is also equipped with an automatic trolley transport system, a tank solution monitoring and automatic replenishment system, a silver ion recovery device, a preheating crosslinking treatment device, a drying and curing equipment, and a central control system. The automatic trolley transport system is equipped with a rotating hanger that continuously rotates at a speed of 5 to 15 rpm during the immersion process in each tank.

[0133] The above system is used to perform surface modification treatment on the alumina caps of pump heads for cosmetic packaging bottles. The caps have an outer diameter of 30mm, a height of 15mm, and are made of 6063 aluminum alloy. The specific implementation steps are as follows:

[0134] Pre-treatment process: The aluminum alloy mandrel blank is mounted on a rotating fixture of an automated conveyor system. The automated conveyor first sends the fixture into the pre-treatment tank assembly. The mandrel is immersed in a 3% sodium hydroxide solution in an alkaline degreasing tank at 40°C for 5 minutes for alkaline degreasing. Subsequently, the mandrel is placed in an acidic neutralization tank and immersed in a 10% nitric acid solution at room temperature for 3 minutes for acid pickling and neutralization. After acid pickling and neutralization, the mandrel is thoroughly rinsed with deionized water with a resistivity of not less than 5 MΩ·cm.

[0135] Anodizing process: The pretreated caps are placed in an anodizing tank and immersed in a 15% sulfuric acid electrolyte. The caps are treated at 18°C ​​and 14V DC constant voltage for 40 minutes to produce an alumina film with a thickness of 8μm±0.5μm and an initial pore size of 10nm±1nm on the surface of the caps.

[0136] Hole expansion process: The anodized caps are sent into the hole expansion tank and immersed in a 5% phosphoric acid solution. They are then treated at 25°C for 8 minutes to expand the pore size of the nanopores from the initial anodized pore size to 50nm±2nm.

[0137] Step-by-step impregnation process: The enlarged pore caps are placed in the first impregnation tank and immersed in a 0.5 g / L silver nitrate solution at room temperature for 10 minutes, allowing silver ions to accumulate and load in the shallow region of the nanopores through physical adsorption and electrostatic interaction. After the first impregnation step, the caps are placed in a cleaning tank and rinsed with deionized water for 60 seconds. Then, the caps are placed in a weak alkali treatment tank and immersed in a sodium carbonate solution with a pH of 8.5 for 3 minutes, reducing some of the silver ions already loaded in the shallow pores to nano-silver. Finally, the caps are placed in the second impregnation tank and immersed in a 5 g / L copper gluconate solution at room temperature for 15 minutes, allowing copper ions to accumulate and load in the deeper region of the nanopores.

[0138] The stepped sealing process involves immersing the cap in a silica sol treatment tank with a mass fraction of 5%, a silica particle size of 5 nm, and a pH of 2 in an acidic silica sol at room temperature for 10 minutes. This allows the nano-silica particles to accumulate and deposit in the middle section of the nanopores, forming a permeable inorganic porous barrier layer. The cap is then placed in a heating channel structure and preheated at 80°C for 10 minutes. This causes a dehydration condensation reaction between the nano-silica particles deposited in the middle section of the nanopores, forming a cross-linked network. Finally, the cap is immersed in a hot water sealing tank at 95°C in deionized water for 20 minutes. Utilizing the volume expansion effect caused by the hydration of the alumina pore walls, the pore diameter of the nanopores shrinks to 10 nm ± 1 nm.

[0139] Hydrophobication process: The stepped sealing caps are sent into the hydrophobication treatment tank and immersed in a 0.5% (w / w) heptadecafluorodecyltrimethoxysilane ethanol solution for 3 minutes to coat the surface of the caps with a fluorinated silane coating.

[0140] Drying and curing process: Finally, the cap is sent into the drying and curing equipment and baked at 100°C for 30 minutes to allow the fluorinated silane coating to cross-link and cure on the surface of the cap, forming a stable hydrophobic and oleophobic film.

[0141] In this embodiment, under the above parameter combination conditions, each process parameter is at the lower or upper limit of the preferred range. Although all steps of the method of the present invention can be fully realized and a gradient controlled-release structure can be formed, the production efficiency is slightly lower and the energy consumption is slightly higher compared with other parameter combinations of the present invention due to the lower processing temperature, longer processing time, and lower bath concentration. However, the product quality stability and consistency are good. The capped sample obtained in this embodiment is marked as sample A, and its surface has a uniform metallic luster.

[0142] Example 5:

[0143] The only difference between this embodiment and embodiment four is the value of each process parameter; the specific implementation steps are the same as in embodiment four.

[0144] The aluminum alloy cap used in this embodiment is the same as that used in Embodiment 4, and the surface modification system used is also exactly the same.

[0145] The difference between this implementation process and that of Example 4 is as follows:

[0146] Pretreatment steps: In the alkaline degreasing step, the sodium hydroxide solution has a mass fraction of 8%, the treatment temperature is 60℃, and the treatment time is 2 minutes. In the acid washing and neutralization step, the nitric acid solution has a mass fraction of 20%, and the treatment time is 1 minute at room temperature.

[0147] Anodizing process: The mass fraction of sulfuric acid electrolyte is 20%, the processing temperature is 22℃, the voltage is 18V, the processing time is 25 minutes, the oxide film thickness is 15μm±1μm, and the initial pore size is 20nm±1nm.

[0148] Pore ​​expansion process: The mass fraction of phosphoric acid solution is 10%, the treatment temperature is 35℃, the treatment time is 3 minutes, and the pore diameter after expansion is 80nm±3nm.

[0149] The process involves a multi-step impregnation process: In the first impregnation step, the silver nitrate concentration is 2 g / L, and the soaking time is 5 minutes. The subsequent water rinse lasts 30 seconds. In the weak alkali reduction treatment, the solution pH is 9.5, and the soaking time is 1 minute. In the second impregnation step, the copper gluconate concentration is 15 g / L, and the soaking time is 8 minutes.

[0150] Stepped sealing process: The silica sol treatment tank contains 10% acidic silica sol by mass, with silica particle size of 15nm, pH value of 4, and soaking time of 5 minutes. The preheating crosslinking treatment temperature is 100℃, and the treatment time is 5 minutes. The hot water sealing temperature is 98℃, the soaking time is 15 minutes, and the diameter of the pore after shrinkage is 30nm±2nm.

[0151] Hydrophobication treatment process: The mass fraction of the fluorinated silane coupling agent solution is 2%, and the treatment time is 1 minute.

[0152] Drying and curing process: The drying and curing temperature is 120℃, and the processing time is 20 minutes.

[0153] The technical advantages of this embodiment are as follows: Under the above parameter combination conditions, each process parameter is at the upper or lower limit of the preferred range. The processing temperature is higher, the processing time is shorter, and the tank solution concentration is higher, resulting in higher production efficiency compared to Embodiment 4. However, due to the higher processing temperature and shorter processing time, the precision requirements for tank solution temperature and concentration control are more stringent. The capped sample obtained in this embodiment is marked as Sample B, and its surface also exhibits a uniform metallic luster.

[0154] Comparative Example 1:

[0155] This comparative example uses the traditional anodizing process to treat aluminum alloy caps without any antibacterial modification treatment.

[0156] The specific steps are as follows: The aluminum alloy cap blank undergoes degreasing and cleaning pretreatment with the same parameters as in Example 4; it is then placed in sulfuric acid electrolyte and anodized for 30 minutes at 20°C and 16V DC constant voltage; after anodizing, it is directly sealed with hot water at 96°C for 20 minutes; no hole-expanding treatment, antibacterial impregnation treatment, stepped sealing treatment, or hydrophobic treatment are performed. The cap sample obtained in this comparative example is marked as Sample C.

[0157] Comparative Example 2:

[0158] This comparative example uses a one-step process with an antibacterial sealing mixture to treat aluminum alloy caps.

[0159] The specific steps are as follows: The aluminum alloy cap blank is pretreated with degreasing and cleaning, using the same pretreatment parameters as in Example 4; it is then anodized in sulfuric acid electrolyte at 20°C and 16V DC constant voltage for 30 minutes, using the same anodizing parameters as in Example 4; pore enlargement is performed using the same pore enlargement parameters as in Example 4 (5% phosphoric acid mass fraction, 25°C for 8 minutes, resulting in a pore diameter of approximately 50nm after enlargement). After pore enlargement, the cap is immersed in an antibacterial sealing mixture for a one-step impregnation and sealing treatment. This mixture is prepared by mixing antibacterial solution and sealing solution at a volume ratio of 1:1. The antibacterial solution contains 0.5g / L silver nitrate and 5g / L copper gluconate, while the sealing solution contains 5g / L nickel acetate. The pH of the mixture is approximately 5.5 to 6.0, the treatment temperature is 85°C, and the treatment time is 20 minutes. After treatment, the cap is removed, rinsed with deionized water, and then air-dried. This comparative example does not undergo weak alkali reduction treatment, preheating crosslinking treatment, step-by-step sealing treatment, or hydrophobication treatment. The capped sample prepared in this comparative example is labeled as sample D.

[0160] The cap samples prepared in Examples 4 and 5 and the two comparative examples were subjected to the following performance tests:

[0161] I. Test methods are shown in Table 1:

[0162] Table 1:

[0163]

[0164] II. The test results are as follows:

[0165] Performance tests were conducted on Example 4 (Sample A), Example 5 (Sample B), Comparative Example 1 (Sample C), and Comparative Example 2 (Sample D) according to the above test methods. The test results are shown in Table 2.

[0166] Table 2:

[0167]

[0168] III. Results Analysis:

[0169] 1. Antibacterial performance analysis:

[0170] In Examples 4 and 5, the inhibition rates against Staphylococcus aureus reached 99.5% and 99.8%, respectively, and the inhibition rates against Escherichia coli reached 99.2% and 99.6%, respectively. This excellent antibacterial performance stems from the dual-source antibacterial system constructed by the stepwise impregnation process of this invention. Simultaneously, the weak alkali reduction treatment converts some silver ions in the shallow pores into nano-silver, forming a composite antibacterial morphology of "silver ions + nano-silver." The synergistic effect of contact bactericidal and leaching bactericidal mechanisms further enhances the antibacterial efficiency.

[0171] After 10,000 simulated pressing tests, the antibacterial rates of Examples 4 and 5 remained above 95.8% and 96.5%, respectively. This excellent antibacterial durability stems from the gradient controlled-release structure constructed with a step-sealed pore structure, which allows silver and copper ions to be released at extremely low rates, ensuring a continuous supply of antibacterial components during long-term use.

[0172] A comparison of Examples 4 and 5 shows that the antibacterial rate of Example 5 is slightly higher than that of Example 4. This is because the concentrations of silver nitrate and copper gluconate in Example 5 are higher (2 g / L vs 0.5 g / L, 15 g / L vs 5 g / L), resulting in a greater antibacterial dose loaded into the pores. Additionally, the hydrophobic treatment in Example 5 is more thorough, leading to better self-cleaning performance and reducing interference from contaminant adhesion on the antibacterial effect. However, the diameter of the pore after shrinkage in Example 5 is 30 nm, slightly larger than the 10 nm in Example 4, resulting in slightly lower controlled-release precision. Therefore, its silver and copper migration amounts are slightly higher than those in Example 4.

[0173] Comparative Example 1, using traditional anodizing, exhibits almost no antibacterial function, with an inhibition rate of only 10.5% against Staphylococcus aureus and 7.2% against Escherichia coli. After 10,000 presses, the inhibition rate further decreased to 8.8%. This demonstrates that simple anodizing combined with conventional hot water sealing cannot provide effective antibacterial properties. The porous structure of the alumina film merely serves to adsorb residues, instead providing conditions for bacterial growth.

[0174] Comparative Example 2, employing a one-step mixed antibacterial impregnation method followed by conventional nickel acetate complete sealing, showed a significantly lower antibacterial rate, with only 32.8% inhibition of Staphylococcus aureus and 26.1% inhibition of Escherichia coli. This is because the one-step mixed impregnation method causes silver and copper ions to compete for adsorption sites within the pores, resulting in a mixed distribution of the two ions. More importantly, the conventional nickel acetate complete sealing thoroughly closes the pores, trapping most silver and copper ions inside and preventing their release. Only a very small number of ions can reach the cap surface to exert their antibacterial effect. Although the silver and copper migration rates in Comparative Example 2 were both low, this was achieved at the expense of antibacterial function.

[0175] 2. Controlled-release performance analysis:

[0176] The silver migration levels in Examples 4 and 5 were below 0.005 ppm and 0.008 ppm, respectively, and the copper migration levels were below 0.008 ppm and 0.010 ppm, respectively, all far below the heavy metal limits required by the "Cosmetic Safety Technical Specifications". This excellent controlled-release effect stems from the gradient controlled-release structure constructed by the step-sealing method. The porous barrier layer formed by the silica sol semi-sealing and the pore narrowing structure formed by the hot water sealing work together functionally. The porous structure of the barrier layer allows ions to pass through at an extremely low rate, while the narrowing structure performs a secondary throttling on the ions passing through the barrier layer. The release resistance formed by the combination of the two is much greater than that of a single sealed structure.

[0177] In contrast, although Comparative Example 2 used nickel acetate to completely seal the pores, resulting in very low silver and copper migration, the cost was the near loss of antibacterial function. This clearly demonstrates that "complete sealing" is not the right approach to solving the problem. The "gradient controlled release" scheme of this invention achieves a more ideal balance between maintaining long-lasting antibacterial effects and ensuring the safety of the material.

[0178] The migration rate in Example 5 is slightly higher than that in Example 4, mainly because its orifice diameter after shrinkage is 30nm±2nm, which is larger than that in Example 4 (10nm±1nm). This results in relatively less physical resistance for ions to pass through, leading to a slightly higher release rate. However, the migration rates in both examples are far below the safety limits, indicating that the controlled-release structure of the present invention has high process tolerance and can maintain good controlled-release performance within a certain range of parameter fluctuations.

[0179] 3. Self-cleaning performance analysis:

[0180] The water contact angles of Examples 4 and 5 reached 112° and 118° respectively, both exhibiting good hydrophobic properties. The contact angle of Example 5 was higher than that of Example 4, mainly because its fluorinated silane coupling agent solution had a higher concentration, a higher surface fluorine coverage, and a lower surface energy. After hydrophobic treatment, the surface of the pump cap possesses a self-cleaning function similar to the "lotus leaf effect," making it difficult for cosmetic residues to adhere, reducing the nutrient source for bacterial growth from the source, and improving the tactile quality and hygiene of the pump cap.

[0181] The water contact angle of Comparative Example 1 was 62°, and that of Comparative Example 2 was 55°; neither of them exhibited hydrophobic properties. This is because neither Comparative Example 1 nor Comparative Example 2 underwent any hydrophobic treatment, and their surfaces retained the original hydrophilic properties of alumina.

[0182] After cosmetic corrosion tests, Examples 4 and 5 showed no change in appearance, while Comparative Example 1 showed slight discoloration. This indicates that the present invention provides more comprehensive protection for the cap substrate through a multi-layer composite structure consisting of an anodic oxide film layer, an antibacterial component loading layer, a stepped sealing layer, and a hydrophobic outer layer.

[0183] 4. Comprehensive comparison between the examples and comparative examples:

[0184] Although Example 4 has slightly lower production efficiency and slightly higher energy consumption, it has sufficient processing time, allowing for more complete reactions in each step, resulting in good product quality stability and consistency.

[0185] Example 5 has higher production efficiency, but due to the higher concentration and temperature, and shorter processing time, it requires more stringent control over the temperature and concentration of the bath solution. Improper control may lead to batch-to-batch quality fluctuations.

[0186] In summary, Examples 4 and 5, under different parameter combinations, achieved a balance between long-lasting antibacterial effect and minimal migration contamination, demonstrating that the technical solution of this invention has a wide range of process adaptability and good industrialization prospects. Comparative Examples 1 and 2, on the other hand, revealed defects such as poor antibacterial function and the sealing of the antibacterial agent, respectively, confirming the inventiveness and practicality of the combined technical solution of "stepwise impregnation + weak alkali reduction + stepwise sealing + preheating crosslinking" of this invention.

[0187] IV. In conclusion:

[0188] The above test results and analysis fully demonstrate that this invention achieves spatial partitioning loading of silver ions in the shallow layer of pores and copper ions in the deep layer of pores through a stepwise impregnation process; constructs a composite antibacterial morphology of "silver ions + nano-silver" through weak alkali reduction treatment; constructs a gradient controlled-release structure with decreasing porosity from the inside to the outside through stepwise pore sealing; enhances the structural strength of the porous barrier layer through preheating crosslinking treatment; and endows the cap surface with self-cleaning function through hydrophobic treatment. The synergistic cooperation among these steps achieves a balance between "long-lasting antibacterial effect" and "zero migration contamination," effectively resolving the contradiction between antibacterial agent release and cosmetic material safety in existing technologies, and achieving excellent technical results.

[0189] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for modifying the surface of an antibacterial cosmetic alumina cap, characterized in that, Includes the following steps: S1: Degreasing and cleaning pretreatment is performed on the aluminum alloy cap substrate to remove surface oil and oxide scale, and obtain a clean and activated aluminum substrate surface; S2: The pre-treated caps are anodized to generate an aluminum oxide thin film layer with a nanoscale porous structure on the surface of the caps; S3: Immerse the anodized cap in an acidic pore-expanding solution for pore-expanding treatment to increase the pore size of the nanoporous structure; S4: A step-by-step impregnation process is used to load shallow fast-acting antibacterial components and deep long-acting antibacterial components into the expanded nanopores respectively; S5: Perform a step-by-step sealing process on the nanopores after loading antibacterial components. The step-by-step sealing process includes a semi-sealing process in the middle section of the pores and a narrowing sealing process at the pore opening, so that the nanopores form a gradient controlled-release structure with decreasing porosity from the inside to the outside. S6: The surface of the cap after the stepped sealing is hydrophobically treated to form a low surface energy self-cleaning film on the outermost layer of the cap; S7: Dry and cure the hydrophobicated caps; Between each adjacent processing step from S1 to S6, the cap is cleaned using deionized water.

2. The method for surface modification of antibacterial cosmetic alumina caps as described in claim 1, characterized in that, The degreasing and cleaning pretreatment process in step S1 specifically includes: S11: Immerse the aluminum alloy cap blank in an alkaline degreasing solution and treat it at a temperature of 40℃ to 60℃ for 2 to 5 minutes to perform alkaline degreasing. S12: Immerse the degreased caps in an acidic neutralizing solution and treat at room temperature for 1 to 3 minutes to perform acid washing and neutralization; S13: After acid pickling and neutralization, rinse the cap thoroughly with deionized water with a resistivity of not less than 5 MΩ·cm.

3. The method for surface modification of antibacterial cosmetic alumina caps as described in claim 1, characterized in that, The anodizing process in step S2 specifically includes: After degreasing and cleaning, the button caps are placed in an acidic electrolyte and treated for 25 to 40 minutes at a temperature of 18°C ​​to 22°C and a DC constant voltage of 14V to 18V, so that the thickness of the alumina film formed on the surface of the button cap is 8μm to 15μm and the initial pore size of the nanopores is 10nm to 20nm.

4. The method for surface modification of antibacterial cosmetic alumina caps as described in claim 1, characterized in that, The hole-expansion process in step S3 is specifically set as follows: The anodized caps are immersed in an acidic pore-expanding solution and treated at a temperature of 25°C to 35°C for 3 to 8 minutes to expand the pore size of the nanopores from the initial anodized pore size to 50 to 80 nm.

5. The method for surface modification of antibacterial cosmetic alumina caps as described in claim 1, characterized in that, The step-by-step impregnation process in step S4 specifically includes the following steps: S41: The first step of impregnation involves immersing the expanded cap in the silver salt solution in the first impregnation tank for 5 to 10 minutes at room temperature, so that silver ions are enriched and loaded in the shallow region of the nanopores through physical adsorption and electrostatic interaction. S42: After completing the first step of impregnation, rinse the cap with deionized water with a resistivity of not less than 5 MΩ·cm for 30 to 60 seconds; S43: After rinsing, place the cap in a weakly alkaline solution with a pH of 8.5 to 9.5 for 1 to 3 minutes to reduce some of the silver ions loaded in the shallow layer of the pores to nano-silver elemental. S44: The second step is immersion. The rinsed cap is immersed in the copper salt aqueous solution in the second immersion tank and soaked at room temperature for 8 to 15 minutes. Due to the difference in diffusion rate between copper ions and silver ions, copper ions are enriched and loaded in the deep region of the nanopores.

6. The method for surface modification of antibacterial cosmetic alumina caps as described in claim 1, characterized in that, The stepped sealing process in step S5 specifically includes: S51: First-stage sealing: The caps processed in step S4 are immersed in nano-silica sol, wherein the silica particles in the nano-silica sol have a diameter of 5nm to 15nm and a pH value of 2 to 4. The caps are immersed at room temperature for 5 to 10 minutes to enrich and deposit the nano-silica particles in the middle section of the nano-pores, forming a permeable inorganic porous barrier layer. S52: After the first stage of sealing is completed, the cap is preheated at 80°C to 100°C for 5 to 10 minutes to allow the nano-silica particles deposited in the middle section of the nanopores to undergo a dehydration condensation reaction and form a cross-linked network. S53: Second stage of sealing. After the first stage of sealing is completed, the cap is placed in high-purity deionized water with a resistivity of not less than 18 MΩ·cm at 95℃ to 98℃ for 15 to 20 minutes. The volume expansion effect generated by the hydration of the alumina pore wall causes the pore diameter of the nanopores to shrink to 10nm to 30nm. By combining the inorganic porous barrier layer of the first-stage sealing with the pore narrowing structure of the second-stage sealing, a release rate gradient is formed for the antibacterial components in the shallow and deep layers.

7. The method for surface modification of antibacterial cosmetic alumina caps as described in claim 1, characterized in that, The hydrophobication process in step S6 is specifically configured as follows: After the step-sealed caps are applied, they are immersed or sprayed in a fluorinated silane coupling agent solution for 1 to 3 minutes to allow a fluorinated silane coating to adhere to the surface of the caps.

8. The method for surface modification of antibacterial cosmetic alumina caps as described in claim 1, characterized in that, The drying and curing process in step S7 is specifically as follows: After hydrophobication treatment, the caps are baked at 100°C to 120°C for 20 to 30 minutes to allow the fluorinated silane coating to crosslink and cure on the cap surface, forming a hydrophobic and oleophobic film.

9. The method for surface modification of antibacterial cosmetic alumina caps as described in claim 1, characterized in that, It also includes auxiliary production processes, which include the following two processes: During the operation of each wet treatment tank corresponding to steps S1 to S6, the liquid level, temperature and concentration parameters of each tank liquid are monitored in real time by an online sensor group. When any parameter deviates from the set range, the corresponding treatment tank is automatically replenished with concentrate or deionized water to maintain the stability of the tank liquid composition. The silver-containing bath solution discharged after impregnation in step S4 is introduced into the ion exchange resin recovery device to adsorb and recover the free silver ions in the bath solution. The recovered bath solution is returned to step S4 for reuse. The resin after adsorption saturation is regenerated by elution with dilute nitric acid, and the eluent is returned to step S4 for recycling.

10. A surface modification system for antibacterial cosmetic alumina caps for implementing the method of any one of claims 1 to 9, characterized in that, include: Multiple processing tanks are arranged sequentially along the process flow direction. Each processing tank includes at least a pretreatment tank group, an anodizing tank, a hole-expanding tank, a first immersion tank, a weak alkali treatment tank, a second immersion tank, a silica sol treatment tank, a hot water sealing tank, and a hydrophobic treatment tank. A cleaning tank is provided between each adjacent processing tank. Each processing tank is equipped with a temperature control device, which is electrically connected to the central control system and is used to independently adjust the temperature of the solution in each processing tank according to the instructions of the central control system. An automatic trolley transport system is equipped with a rotating hanger for attaching button caps. During the immersion process in the tank, the rotating hanger rotates continuously around its own axis at a speed of 5 rpm to 15 rpm, so that the surfaces of the button caps at different positions on the hanger are alternately exposed to the flow direction of the tank liquid, thereby eliminating the contact differences between the three-dimensional structure of the button caps and the tank liquid. A tank liquid monitoring and automatic replenishment system, the tank liquid monitoring and automatic replenishment system includes an online sensor group installed in each processing tank and an automatic replenishment pump group connected to each processing tank, wherein the online sensor group of the first immersion tank is provided with a silver ion selective electrode. A silver ion recovery device is connected to the first impregnation tank and is used to adsorb and recover free silver ions in the solution of the first impregnation tank, and return the recovered solution to the first impregnation tank. A preheating crosslinking treatment device is provided between the silica sol treatment tank and the hot water sealing tank. It is used to preheat the caps after silica sol treatment to form a crosslinking network between the nano-silica particles deposited in the middle section of the nanopores. A drying and curing device is provided downstream of the hydrophobic treatment tank. The drying and curing device is a multi-temperature zone tunnel drying and curing oven that is sequentially divided into a preheating zone, a curing zone, and a cooling zone along the conveying direction. The central control system is electrically connected to the automatic trolley transport system, the tank liquid monitoring and automatic replenishment system, the silver ion recovery device and the drying and curing equipment, and is used to control the operating parameters of each system. The temperature of each area is independently controlled by the central control system.

Citation Information

Patent Citations

  • Anodic oxidation preparation method of antibacterial aluminum alloy

    CN111647926A

  • Antibacterial solution for aluminum alloy, antibacterial aluminum alloy member, and method for producing same

    CN116136025B