A cut-resistant ultra-high molecular weight polyethylene fiber, its preparation method, and cut-resistant yarn or fabric.

By using a core-sheath composite structure and gel spinning process, the problems of slippage, filler shedding, and static electricity in ultra-high molecular weight polyethylene fibers during the cutting process have been solved, resulting in fiber products with high cut resistance and long service life, meeting the high standards required for personal protective equipment.

CN123108766APending Publication Date: 2026-11-17TUOSEN (ZHENJIANG) SECURITY TECHNOLOGY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202611534257.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing ultra-high molecular weight polyethylene fibers are prone to problems such as fiber slippage and pull-out, filler agglomeration and insufficient interfacial bonding, electrostatic accumulation and poor dyeing performance during the cutting process, making it difficult to meet the requirements for high cut resistance and service life.

Method used

The core layer is a heterogeneous functional partition structure with a core layer. The core layer is a high-modulus ultra-high molecular weight polyethylene matrix doped with surface-treated inorganic fiber micro powder, while the skin layer is a medium-low molecular weight polyethylene matrix and titanium dioxide particles. The core layer is formed by a gel spinning dual-channel co-extrusion process, and the polyethylene molecular chains are permeated and entangled at the interface to build a stable cut-resistant skeleton and a dense coating layer.

Benefits of technology

It achieves high cut resistance, stable structure, good interface bonding, antistatic properties and colorability, meets EN388:2016 standard, has low spinning breakage rate, long service life and effective cost control.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108766A_ABST
    Figure CN123108766A_ABST
Patent Text Reader

Abstract

This invention discloses a cut-resistant ultra-high molecular weight polyethylene fiber, its preparation method, and cut-resistant yarn or fabric. The fiber is prepared via a gel spinning dual-channel co-extrusion process and includes a core layer and a sheath layer. The core layer contains a weight-average molecular weight ≥ 4.0 × 10⁻⁶. 6 g / mol of first polyethylene and inorganic fiber powder, wherein the inorganic fiber powder is surface treated; the skin layer contains a weight-average molecular weight of 0.5 × 10⁻⁶ g / mol. 6 Up to 3.5×10 6 g / mol of second polyethylene and titanium dioxide particles are coated on the outer surface of the core layer to form a core-skin double-layer composite structure; the weight-average molecular weight of the second polyethylene is lower than that of the first polyethylene. It is prepared by dual-channel co-extrusion gel spinning, where the skin spinning solution and the core spinning solution are extruded through the skin channel and core channel respectively, followed by low-temperature solidification phase separation, super-stretching, and precise heat setting to obtain fibers. The yarn and fabric are prepared from these fibers. This fiber exhibits good cut resistance, strong interfacial bonding, and minimal filler detachment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of high-performance fiber materials technology, specifically to a cut-resistant ultra-high molecular weight polyethylene fiber, its preparation method, and cut-resistant yarn or fabric. Background Technology

[0002] Ultra-high molecular weight polyethylene (UHMWPE) fiber, with its ultra-high strength, low density, and excellent impact and abrasion resistance, is one of the most widely used high-performance fibers in the field of personal protective equipment. The mainstream industrial manufacturing process is gel spinning. Existing commercially available cut-resistant UHMWPE fibers are mainly homogeneous single-layer structures, and performance improvements are mostly achieved by increasing the molecular weight of the matrix, optimizing the single stretching process, or simply blending with inorganic fillers.

[0003] The existing technology has the following shortcomings: homogeneous fibers lack functional partitioning, making them prone to fiber slippage and pull-out during cutting. Local stress concentration can lead to fiber failure, limiting the improvement of cut resistance. Direct blending of inorganic fillers is prone to agglomeration, and the compatibility and bonding force between the filler and the UHMWPE matrix are insufficient, easily causing internal microcracks and a decline in mechanical properties, as well as problems such as surface filler detachment and short service life. The fiber colorability and light-blocking properties are poor, relying heavily on post-dyeing treatment, making it difficult to balance color fastness and protective performance. Static electricity accumulation is also prone to occur during spinning and weaving, leading to problems such as fiber breakage and insufficient fiber cohesion.

[0004] To address the aforementioned issues, existing technologies have proposed several improvement schemes. Chinese patents CN104233497B, CN110205695B, and CN115787121A respectively employ inorganic ultrafine powder, surface-optimized inorganic powder, and a blend of wollastonite and inorganic hard whiskers to improve cut resistance, but these still suffer from filler agglomeration and insufficient interfacial bonding. Chinese patent CN106350882A discloses a scheme for preparing core-sheath composite fibers via gel spinning, but its sheath and core layers use the same type of UHMWPE, and no interfacial transition layer is formed. Chinese patent CN118441463A discloses a post-treatment route for in-situ growth of nano-Al2O3 on the surface of UHMWPE fibers, mainly addressing surface functionalization issues, but not involving the synergistic effect of dyeing, matting, and cut resistance.

[0005] Currently, the national standards for personal protective equipment (GB 39800-2020) and EN388:2016 have raised the requirements for the cut resistance of protective equipment. The market urgently needs a new generation of UHMWPE protective fiber that combines high cut resistance, structural stability, colorability, antistatic properties, and lower cost. The gel spinning process has a high degree of industrial maturity and can be combined with multi-component co-extrusion molding technology, providing a technical basis for the functional design of the core-sheath structure and the directional arrangement of inorganic fillers. Summary of the Invention

[0006] To address the aforementioned technical problems in existing technologies, this invention aims to provide a cut-resistant ultra-high molecular weight polyethylene fiber, its preparation method, and cut-resistant yarn or fabric. By employing a heterogeneous core-sheath functional partition structure, the core layer consists of a high-modulus ultra-high molecular weight polyethylene matrix doped with surface-treated modified inorganic fiber micropowder. Through precise control of the inorganic micropowder content, aspect ratio, axial orientation angle, and axial spacing, a stable, rigid, cut-resistant support skeleton is constructed. The sheath layer uses a medium / low molecular weight polyethylene matrix, compounded with titanium dioxide matting agents of specific particle size and antistatic additives, forming a dense protective coating layer. This solves the technical bottlenecks of traditional homogeneous fibers, such as cutting slippage, filler shedding, poor interfacial bonding, fiber breakage, and low color fastness. The cut-resistant ultra-high molecular weight polyethylene fiber of this invention achieves a cut resistance rating of C or higher (cutting force ≥ 10 N) according to EN388:2016 standard, a spinning breakage rate ≤ 0.12%, and no visible filler shedding was detected after 50 industrial washes. The color fastness to washing reaches ISO 105-C06 standard level 4 or higher.

[0007] To achieve the above objectives, the present invention adopts the following technical solution: a cut-resistant ultra-high molecular weight polyethylene fiber, prepared by a gel spinning dual-channel co-extrusion process, comprising: The core layer contains materials with a weight-average molecular weight ≥ 4.0 × 10⁻⁶. 6 g / mol of first polyethylene and inorganic fiber powder, wherein the inorganic fiber powder is surface-treated inorganic fiber powder; The cortex, containing a weight-average molecular weight of 0.5 × 10⁻⁶. 6 Up to 3.5×10 6 g / mol of second polyethylene and titanium dioxide particles are coated on the outer surface of the core layer to form a skin-core double-layer composite structure; and the interface transition region formed between the core layer and the skin layer; The weight-average molecular weight of the second polyethylene is lower than that of the first polyethylene.

[0008] Furthermore, the core layer is obtained by gel spinning of the core layer spinning solution; based on the total weight of the core layer spinning solution, the content of the first polyethylene is 8-12 wt%, and the content of the inorganic fiber powder is 11-30 wt%; the sheath layer is obtained by gel spinning of the sheath layer spinning solution; based on the total weight of the sheath layer spinning solution, the content of the second polyethylene is 10-15 wt%, and the content of the titanium dioxide particles is 0.5-5.0 wt%.

[0009] Furthermore, the diameter of the fiber is 10-30 μm, and the sheath-core cross-sectional area ratio of the fiber is 1:3-1:5; the surface treatment includes one or more of silane coupling agent treatment or alkylation treatment; Preferably, the core spinning solution and the sheath spinning solution use the same solvent, which is selected from dichloromethane, dichloroethane, carbon tetrachloride, a mixture of dichloromethane and ionic liquid, decahydronaphthalene, or white oil.

[0010] Furthermore, the interface transition zone is a gradient transition region formed by the mutual penetration and entanglement of the polyethylene molecular chains of the skin layer and the polyethylene molecular chains of the core layer during the co-extrusion process.

[0011] Furthermore, the weight-average molecular weight of the first polyethylene is ≥4.5×10⁻⁶. 6 g / mol, the weight-average molecular weight of the second polyethylene is 1.2–3.0 × 10 g / mol. 6 g / mol; the solvent is decahydronaphthalene or white oil.

[0012] Furthermore, the inorganic fiber powder is selected from one or more of silicon carbide fiber, silicon nitride fiber, carbon fiber, glass fiber, and alumina fiber; the aspect ratio of the inorganic fiber powder is 4 to 10, the angle between the axis of the inorganic fiber powder and the spinning axis is 0 to 10°, and the average axial spacing between the inorganic fiber powders is 50 to 260 μm.

[0013] Furthermore, the inorganic fiber powder is prepared by compounding carbon fiber and alumina fiber in 1-3 parts by mass and 1-3 parts by mass, respectively, and the content of the inorganic fiber powder obtained by compounding is 18-25 wt% of the core spinning solution; the aspect ratio of the carbon fiber is 6-8, and the aspect ratio of the alumina fiber is 4-6; the carbon fiber is surface alkylated with octadecyltrichlorosilane, and the grafting rate is ≥0.8 mmol / g; the alumina fiber is surface alkylated with n-octyltriethoxysilane, and the grafting rate is ≥0.5 mmol / g. Preferably, the titanium dioxide particles have a particle size of 0.2 to 0.5 μm and a content of 2.0 to 3.5 wt% of the skin spinning solution.

[0014] Furthermore, the sheath spinning solution also includes polyethylene glycol monostearate, wherein the polyethylene glycol monostearate has a molecular weight of 1000±100 g / mol and a content of 0.3–1.2 wt% of the sheath spinning solution; Preferably, the sheath spinning solution further includes 0.5–2.0 wt% of a 4-hydroxy-4'-methoxyazobenzene photosensitive derivative, which can achieve reversible gradient color changes of fiber gray, blue, and purple after being irradiated with ultraviolet light with a wavelength of 350–380 nm and an irradiance of 4–6 mW / cm².

[0015] Furthermore, the core spinning solution also includes 0.1–0.8 wt% graphene quantum dots, wherein the graphene quantum dots have a particle size of 2–5 nm and an oxygen content of 8 at.%–12 at.%; the graphene quantum dots form a hydrogen bond-van der Waals synergistic anchoring structure with the surface-treated inorganic fiber micropowder, aligning along the spinning axis to form a conductive path, thereby reducing the fiber volume resistivity to 10 Ω·cm. 4 -10 5 Ω·cm.

[0016] This invention also provides a method for preparing the cut-resistant ultra-high molecular weight polyethylene fiber via gel spinning, comprising the following steps: S1. Preparation of core spinning solution: Dissolve the first polyethylene in a solvent, stir evenly, add the surface-modified inorganic fiber powder, and disperse evenly to obtain the core spinning solution; S2. Preparation of skin spinning solution: Dissolve the second polyethylene in a solvent, add titanium dioxide particles, optionally add antistatic agent and / or photosensitive derivative, stir and disperse evenly to obtain skin spinning solution; S3. Dual-channel co-extrusion spinning: The core spinning solution and the sheath spinning solution are co-extruded and sprayed through a dual-channel co-extrusion device to obtain gel filaments; wherein the volume flow ratio of the core layer to the sheath layer is 3:1 to 5:1; S4. Low-temperature solidification phase separation: The gel fiber enters a solidification bath to cool and solidify, and the solidification bath temperature is -10 to 0℃; S5. Super-high temperature hot stretching: High temperature super-high temperature stretching of solidified filament bundles, stretching temperature 120~145℃, stretching ratio 35~50 times; S6. Heat setting treatment: The stretched fiber is heat set at 140-155℃ for 30-90 s, cooled and wound to obtain the cut-resistant ultra-high molecular weight polyethylene fiber.

[0017] Furthermore, between steps S5 and S6, the method further includes a photosensitive modification treatment step: applying a wavelength of 350–380 nm and an irradiance of 4–6 mW / cm² to the fiber bundle containing the photosensitive derivative. 2Irradiation with ultraviolet light for 30–120 s induces molecular chain isomer rearrangement; the solvent is selected from decahydronaphthalene or white oil; both the skin spinning solution and the core spinning solution are based on polyethylene; during the co-extrusion process, the skin and core layers achieve self-adhesion at the interface through the permeation and entanglement of polyethylene molecular chains.

[0018] The cut-resistant ultra-high molecular weight polyethylene fiber described in this invention can be used to prepare yarns, fabrics, and protective products made from the fabrics. The beneficial technical effects obtained by this invention are as follows:

[0019] 1. The ultra-high molecular weight polyethylene fiber of the present invention has stable cut resistance, reaching above 10 N according to the ISO13997 method, corresponding to level C or above of the EN388 test standard; through molecular weight gradient matching of the core and sheath layers, high-cost ultra-high molecular weight polyethylene is used only in the core layer, while the sheath layer uses low-cost medium and low molecular weight polyethylene, effectively reducing the raw material production cost while ensuring high performance, and making it suitable for large-scale promotion and application.

[0020] 2. The present invention features a continuous coating of a core layer with ultra-high molecular weight polyethylene fiber sheath. This coating utilizes surface-treated modified inorganic micropowder combined with a molecular weight gradient design between the sheath and core, effectively reducing fiber micropowder exposure and shedding. The interfacial transition layer improves the sheath-core bonding strength, reducing delamination, cracking, and thermal shrinkage stress, significantly enhancing the sheath-core interfacial bonding performance. After 50 industrial washes, no filler detachment is observed on the fiber surface, the sheath structure remains intact, and the service life is greatly extended.

[0021] 3. The ultra-high molecular weight polyethylene fiber of the present invention uses medium and low molecular weight polyethylene as the sheath, which is beneficial to forming a uniform and dense coating layer and improving the fiber softness and wearing comfort.

[0022] 4. The ultra-high molecular weight polyethylene fiber of the present invention can further improve its antistatic properties, coloring properties and color fastness by adding a cortex co-composite to the cortex spinning solution. For example, relying on the cortex titanium dioxide matting system, it can stably achieve a variety of colors such as gray, blue, black and military green without the need for post-dyeing, meeting the needs of special scenarios such as high-risk operations, intelligent protective equipment and police concealment equipment.

[0023] 5. This invention employs a dual-channel co-extrusion and gel spinning process, allowing the sheath spinning solution and core spinning solution to be transported independently. While maintaining the high strength and high modulus properties of the ultra-high molecular weight polyethylene core layer, the sheath layer continuously coats the core layer circumferentially, and the inorganic fiber micro powder is confined within the core layer, reducing its surface exposure and shedding. This achieves functionalization of the sheath layer while also ensuring cut resistance, softness, and good interfacial bonding. Attached Figure Description

[0024] Figure 1This is a schematic diagram of the cross-sectional structure of an anti-cut ultra-high molecular weight polyethylene fiber according to an embodiment of the present invention. The dotted and elliptical marks in the core layer represent the cross-sectional morphology of randomly oriented inorganic fiber micropowder, and the dotted marks in the skin layer represent the cross-sectional morphology of titanium dioxide particles.

[0025] Figure 2 This is a partial cross-sectional view of an embodiment of the present invention of cut-resistant ultra-high molecular weight polyethylene fiber, where the short lines in the core layer represent the longitudinal projection of the inorganic fiber micropowder.

[0026] Figure 3 This is a partially enlarged schematic diagram of the sheath-core interface transition zone of an anti-cutting ultra-high molecular weight polyethylene fiber according to an embodiment of the present invention. The thinner curved segment represents the second polyethylene molecular chain, and the thicker curved segment represents the first polyethylene molecular chain.

[0027] Figure 4 This is a longitudinal cross-sectional schematic diagram of a dual-channel co-extrusion spinneret assembly for cut-resistant ultra-high molecular weight polyethylene fiber according to an embodiment of the present invention.

[0028] Figure 5 This is a flowchart of the dual-channel co-extrusion gel spinning process for cut-resistant ultra-high molecular weight polyethylene fiber according to the present invention.

[0029] Wherein, 1: core layer; 2: sheath layer; 3: interface transition zone; 101: inorganic fiber micro powder; 102: first polyethylene molecular chain; 103: core layer spinning solution; 201: titanium dioxide particles; 202: second polyethylene molecular chain; 203: sheath layer spinning solution; 4: spinneret assembly box; 401: sheath layer spinning solution inlet; 402: core layer spinning solution inlet; 403: sheath layer flow channel; 404: core layer flow channel; 405: sheath-core composite flow channel; 406: spinneret hole; 5: gelatin filament. Detailed Implementation

[0030] To make the objectives, technical solutions, and advantages of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are some preferred embodiments of this application, but not all embodiments. In addition, for clarity and brevity, descriptions of known functions and structures are omitted in the embodiments.

[0031] In this article, the term "and / or" is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can mean: A exists alone, B exists alone, and A and B exist simultaneously. In this article, the term " / and" describes another type of relationship between related objects, indicating that two relationships can exist. For example, A / and B can mean: A exists alone, and A and B exist alone.

[0032] It should be noted that the accompanying drawings are only for illustrating the structure of the present invention. The thickness of each layer, the size, quantity and distribution density of the micropowder, as well as the thickness, shape and entanglement of the molecular chains in the drawings do not represent the actual size and proportion. The specific dimensions and parameters of the present invention shall be based on the textual description in the specification.

[0033] In this invention, for ease of description, polyethylene is classified into the following two grades according to its weight-average molecular weight (Mw): First type of polyethylene (ultra-high molecular weight polyethylene): Mw ≥ 4.0 × 10 6 g / mol, preferably ≥ 4.5 × 10 6 g / mol, used for the core layer; Secondary polyethylene (relatively low molecular weight polyethylene): Mw is 0.5 × 10 6 Up to 3.5×10 6 g / mol, preferably 0.8 × 10 g / mol. 6 Up to 3.0×10 6 g / mol, used for the cortex; The molecular weight of the second polyethylene is always lower than that of the first polyethylene.

[0034] It should be noted that "relatively low molecular weight" in this article is a comparative term relative to the first polyethylene core layer and does not represent its absolute classification standard in the field of polyethylene.

[0035] Unless otherwise stated, all weight-average molecular weights mentioned herein refer to values ​​determined by high-temperature gel permeation chromatography (HT-GPC).

[0036] (a) Cut-resistant ultra-high molecular weight polyethylene fiber This invention provides a cut-resistant ultra-high molecular weight polyethylene fiber, wherein the fiber has a core-sheath structure, such as... Figure 1 As shown, the structure includes a core layer 1 and a sheath layer 2, which are formed by a dual-channel co-extrusion process of gel spinning, namely core spinning solution 103 and sheath spinning solution 203. The sheath layer 2 continuously coats the outer surface of the core layer 1 in the circumferential direction to form a core-sheath double-layer composite structure, and an interface transition zone 3 is formed between the core layer 1 and the sheath layer 2. The diameter of the cut-resistant ultra-high molecular weight polyethylene fiber of the present invention is 10-30 μm, and the cross-sectional area ratio of the core layer to the sheath layer is 3:1 to 5:1, that is, the core-sheath cross-sectional area ratio of the fiber is 1:3 to 1:5.

[0037] The core spinning solution 103 comprises a first polyethylene, inorganic fiber powder 101, and other core components, while the sheath spinning solution 203 comprises a second polyethylene, titanium dioxide particles 201, and other sheath components. The other sheath components and the other core components can be the same or different components, and are independently selected from additives capable of improving the processing performance of the corresponding layer or imparting additional functions to the corresponding layer. The weight-average molecular weight of the second polyethylene is lower than that of the first polyethylene.

[0038] (ii) Core spinning solution 1. First polyethylene The first polyethylene is ultra-high molecular weight polyethylene with a weight-average molecular weight ≥ 4.0 × 10⁻⁶. 6 g / mol, preferably ≥4.5×10 6 g / mol; the first polyethylene content is 8–12 wt% based on the total weight of the core spinning solution.

[0039] 2. Inorganic fiber powder like Figure 1 and Figure 2 As shown, inorganic fiber powder 101 is dispersed in the core layer 1. Since the inorganic fiber powder 101 is obtained by cutting and / or grinding inorganic fibers, it has a significant aspect ratio and is randomly dispersed in the core layer 1. Therefore, in a cross-section perpendicular to the fiber axis, the inorganic fiber powder 101 may appear as dots or ellipses depending on its orientation. These dot or elliptical markings are only used to indicate the cross-sectional shape of the inorganic fiber powder and do not represent its actual size and quantity.

[0040] The inorganic fiber powder 101 is selected from one or more of silicon carbide fiber, silicon nitride fiber, carbon fiber, glass fiber, and alumina fiber; the content of inorganic fiber powder 101 is 11-30 wt% based on the total weight of the core spinning solution. The inorganic fiber powder 101 is subjected to surface treatment, which is selected from one or more of silane coupling agent treatment or alkylation treatment.

[0041] The longer the fibers and the smaller the spacing of the inorganic fiber micro powder 101, the better the cut resistance, but the worse the flexibility; the larger the angle, the easier it is for the powder to fall off during subsequent processing. In this invention, the aspect ratio of the inorganic fiber micro powder 101 is set to 4-10, the angle between the axial direction and the spinning axis is 0-10°, and the average axial spacing is 50-260 μm.

[0042] This invention constructs a highly stable, cut-resistant skeleton structure by synergistically combining the content, aspect ratio, axial orientation angle, and axial spacing of the inorganic fiber powder 101 in the core layer 1. Through the above-mentioned adjustment and combination of parameters of the inorganic fiber powder 101, the high performance and low volatility properties of the ultra-high molecular weight polyethylene fiber of this invention can be achieved.

[0043] In some embodiments, the inorganic fiber powder 101 is made of silicon carbide fiber, and the silicon carbide fiber is surface-treated with a silane coupling agent, wherein the silane coupling agent is KH-550 (amino), KH-560 (epoxy), or KH-570 (methacryloyloxy). In other embodiments, the inorganic fiber powder 101 is prepared by compounding carbon fiber and alumina fiber in a mass ratio of 1-3 parts and 1-3 parts respectively, and the content of the inorganic fiber powder obtained by compounding is 18-25 wt% of the core spinning solution. The aspect ratio of the carbon fiber is 6-8, and the aspect ratio of the alumina fiber is 4-6; the carbon fiber is surface-alkylated with octadecyltrichlorosilane, with a grafting rate ≥0.8 mmol / g; the alumina fiber is surface-alkylated with n-octyltriethoxysilane, with a grafting rate ≥0.5 mmol / g.

[0044] Different inorganic fiber micropowders are treated with differentiated surface treatment methods. After surface treatment modification, the inorganic fiber micropowders achieve high-strength interfacial compatibility between the inorganic filler and the polyethylene matrix, preventing filler detachment and microcrack propagation. Compared to single-component inorganic fiber micropowders, carbon fiber has the advantage of strong cut resistance, but adding low amounts of carbon fiber results in high viscosity of the spinning solution, while adding high amounts is difficult. By compounding with alumina fiber, the viscosity of the spinning solution is improved, and the overall content of carbon fiber + alumina is higher than that of adding carbon fiber alone, achieving better cut resistance than using single-component inorganic fiber micropowder.

[0045] 3. Other components of the core layer In some embodiments, the core spinning solution further includes 0.1–0.8 wt% graphene quantum dots, the graphene quantum dots having a particle size of 2–5 nm; the oxygen content of the graphene quantum dots, as determined by XPS, is 8 at.%–12 at.%; the graphene quantum dots form a hydrogen bond-van der Waals co-anchoring structure with the surface-treated inorganic fiber micropowder 101, aligning along the spinning axis to form a conductive path, which can reduce the fiber volume resistivity to 10 Ω·cm. 4 -10 5 Ω·cm.

[0046] (III) Cortical spinning solution 1. Second polyethylene The second polyethylene is a relatively low molecular weight polyethylene with a weight-average molecular weight of 0.5–3.5 × 10⁻⁶. 6 g / mol, preferably 1.2–3.0 × 10⁻⁶ g / mol. 6 g / mol. The content of the second polyethylene is 10–15 wt% based on the total weight of the cortex spinning solution.

[0047] 2. Titanium dioxide particles like Figure 1 and Figure 2 As shown, titanium dioxide particles 201 are added to the sheath 2 as an anti-glossing agent to achieve anti-glossing treatment of the fiber. The content of titanium dioxide particles 201 is 0.5-5.0 wt% based on the total weight of the sheath spinning solution 203. Preferably, the content of titanium dioxide particles 201 is 2.0-3.5 wt% of the sheath spinning solution 203.

[0048] The titanium dioxide particles 201 have a particle size of 0.2 to 0.5 μm. If the particle size of the added titanium dioxide particles 201 is too small (nano), it will result in insufficient matting, a shiny finished product, and obvious reflection in the protective fabric. If the particle size of the added titanium dioxide particles 201 is too large, the powder will be poorly dispersed, the spinning solution will easily clog the spinneret, the fiber surface will be rough, and microcracks will easily form under stress.

[0049] More preferably, the titanium dioxide particles are modified by forming an organosilicon hydrophobic coating layer on the TiO2 surface using a treatment agent. The treatment agent is a non-polar silane coupling agent, such as alkylsilane, like octyltriethoxysilane, which reduces surface polarity, improves wetting and compatibility with the polyethylene matrix, inhibits agglomeration, and retains the matting effect. As one embodiment, for titanium dioxide particles with a diameter of 0.2–0.3 μm, modification with octyltriethoxysilane followed by a small amount added to the skin spinning solution 203 can achieve low gloss without compromising compatibility with the polyethylene matrix, balancing matting, mechanical properties, and spinning processability.

[0050] 3. Other components of the cortex In some embodiments, the sheath spinning solution 203 further includes polyethylene glycol monostearate, wherein the polyethylene glycol monostearate has a molecular weight of 1000±100 g / mol and a content of 0.3–1.2 wt% of the sheath spinning solution. Through the synergistic formulation of titanium dioxide matting agent and polyethylene glycol monostearate antistatic agent in the sheath spinning solution 203, the problems of coloring, static electricity, and weaving processing are solved simultaneously.

[0051] In some other embodiments, the skin spinning solution 203 further includes 0.5–2.0 wt% of a 4-hydroxy-4'-methoxyazobenzene photosensitizing derivative, wherein the 4-hydroxy-4'-methoxyazobenzene photosensitizing derivative is subjected to an irradiance of 4–6 mW / cm at a wavelength of 350–380 nm. 2 After being irradiated with ultraviolet light, the fiber can achieve reversible gradient color change of gray, blue and purple, and the bonding energy of the core-sheath interface can be improved by 25-40%.

[0052] The core spinning solution 103 and the skin spinning solution 203 use the same solvent, which is selected from dichloromethane, dichloroethane, carbon tetrachloride, dichloromethane and ionic liquid compound, decahydronaphthalene or white oil, preferably decahydronaphthalene or white oil.

[0053] In the core-sheath structure of the present invention, the core layer 1 and the sheath layer 2 are designed with a gradient based on the molecular weight of polyethylene and coupled with a functional partition structure. The core layer 1 provides high-strength cut resistance, while the sheath layer 2, as a covering layer, provides other additional functions, such as the addition of polyethylene glycol monostearate to achieve protective and antistatic properties. Thus, the ultra-high molecular weight polyethylene fiber of the present invention has both cost advantages and excellent performance.

[0054] (iv) Interface transition area like Figure 3 As shown, the interface transition zone 3 is a gradient transition region formed by the mutual penetration and entanglement of the second polyethylene molecular chain 202 of the skin layer 2 and the first polyethylene molecular chain 102 of the core layer 1 during co-extrusion, rather than an abrupt geometric interface. Within the interface transition zone 3, the first polyethylene molecular chain 102 and the second polyethylene molecular chain 202 are entangled with each other. This illustration is only used to show the entanglement state and interfacial bonding relationship of different molecular chains in the interface transition zone and does not represent the actual size, number, or entanglement density of the molecular chains.

[0055] The formation of the interface transition zone 3 is based on the following two conditions: First, the skin layer 2 and the core layer 1 belong to the same polyethylene system, and the polyethylene molecular chains are thermodynamically completely compatible; Second, the skin layer spinning solution 203 and the core layer spinning solution 103 use the same solvent, which eliminates the obstacle of interfacial tension between solvents to the diffusion of molecular chains.

[0056] Furthermore, during the dual-channel co-extrusion process, the two polyethylene spinning solutions converge and are extruded together within the spinneret. At the interface, the polyethylene molecular chains undergo cross-interfacial diffusion and interpenetration under the plasticizing effect of solvent molecules in a gel state. During the subsequent equilibration and resting of the gel filaments, molecular chain diffusion is further enhanced. Finally, during the super-stretching stage, the intertwined polyethylene molecular chains at the interface are oriented along the fiber axis, forming a continuous entangled network that spans the sheath-core interface. This entangled network anchors the sheath and core layers into a unified whole, preventing sheath-core delamination during subsequent drafting, weaving, and use.

[0057] It is particularly important to note that the interfacial self-entanglement mechanism of this invention is fundamentally different from the heterogeneous polymer skin-core system in the prior art. For example, in the prior art, composite fibers with ultra-high molecular weight polypropylene as the skin and ultra-high molecular weight polyethylene as the core have limited interfacial bonding strength because the skin and core are different types of polymers, requiring the introduction of an interfacial compatibilizer. This invention, however, utilizes the fact that the skin and core belong to the same polyethylene system and use the same solvent to achieve mutual penetration and entanglement of interfacial molecular chains, obtaining excellent skin-core bonding strength without any interfacial agent.

[0058] (v) Dual-channel co-extrusion spinneret assembly The cut-resistant ultra-high molecular weight polyethylene fiber of this invention is produced using a gel spinning process and a dual-channel co-extrusion device. Alternatively, such as... Figure 4 As shown, the spinneret in this dual-channel co-extrusion equipment includes a spinneret housing 4, which has a sheath spinning solution inlet 401 and a core spinning solution inlet 402. The spinneret housing 4 contains a core flow channel 404 and a sheath flow channel 403 surrounding the core flow channel 404. Because... Figure 4 The diagram shows a longitudinal cross-section. The annular skin channel 403 is represented as two channels located on both sides of the core channel 404.

[0059] The lower ends of both the core layer flow channel 404 and the skin layer flow channel 403 are connected to the core-skin composite flow channel 405. A spinneret is provided below the core-skin composite flow channel 405, and spinneret holes 406 penetrating its thickness are opened on the spinneret. The spinneret holes 406 are narrow channels.

[0060] The sheath spinning solution 203 enters the sheath-core composite flow channel 405 sequentially through the sheath spinning solution inlet 401 and the sheath flow channel 403, while the core spinning solution 103 enters the sheath-core composite flow channel 405 sequentially through the core spinning solution inlet 402 and the core flow channel 404. Within the sheath-core composite flow channel 405, the core spinning solution 103 is located at the center, and the sheath spinning solution 203 circumferentially covers the core spinning solution 103, forming a coaxial laminar flow structure. The two are extruded through the spinneret orifice 406 in a coaxial laminar flow state to form a cut-resistant ultra-high molecular weight polyethylene fiber gel filament 5 with a sheath-core coaxial structure.

[0061] It should be noted that the attached diagram is only a schematic diagram of the structure, and the dimensions and proportions of each flow channel, spinneret orifice and fiber in the diagram do not represent the actual dimensions and proportions.

[0062] (vi) Preparation method This invention also provides a method for preparing the cut-resistant ultra-high molecular weight polyethylene fiber via gel spinning, such as... Figure 5 As shown, it includes the following steps: S1. Preparation of core spinning solution: The first polyethylene is dissolved in a solvent, stirred evenly, and then surface-treated inorganic fiber powder is added. The mixture is dispersed evenly at 145-169°C to obtain the core spinning solution. S2. Preparation of skin spinning solution: The second polyethylene is dissolved in a solvent, titanium dioxide particles are added, and an antistatic agent and / or a photosensitive derivative are optionally added. The solution is stirred and dispersed evenly at 135-150°C to obtain the skin spinning solution. S3. Dual-channel co-extrusion spinning: The core spinning solution and the sheath spinning solution are co-extruded and sprayed out through a dual-channel co-extrusion device to obtain gelatin raw yarn 5; S4. Low-temperature solidification phase separation: The gelatin filament 5 enters a solidification bath to cool and solidify, and the solidification bath temperature is -10 to 0℃; S5. Super-high temperature hot stretching: High temperature super-high temperature stretching of solidified filament bundles, stretching temperature 120~145℃, stretching ratio 35~50 times; S6. Heat setting treatment: The stretched fiber is heat set at 140-155℃ for 30-90 s, cooled and wound to obtain the cut-resistant ultra-high molecular weight polyethylene fiber.

[0063] The solvents used in steps S1 and S2 are the same; alternatively, the solvent is selected from dichloromethane, dichloroethane, carbon tetrachloride, a mixture of dichloromethane and ionic liquids, decahydronaphthalene, or white oil. As one implementation method, when the solvent is white oil, based on its high boiling point and low volatility, the solidified filament bundle is extracted with n-hexane / xylene between steps S4 and S5, and then dried after extraction. As another implementation, when the solvent is decahydronaphthalene, extraction is not required, and the solvent can be evaporated and removed in step S5 without additional extraction and drying steps.

[0064] Both the sheath spinning solution and the core spinning solution are based on polyethylene. During the co-extrusion process, the sheath 2 and the core 1 achieve self-adhesion at the interface transition zone 3 through the penetration and entanglement of polyethylene molecular chains.

[0065] Preferably, when a photosensitive derivative is added to the cortex spinning solution, this step is performed after step S5 and before step S6. The method further includes a photosensitive modification treatment step: applying a photosensitive modification treatment to the fiber bundle containing the photosensitive derivative at a wavelength of 365 nm and an irradiance of 5 mW / cm². 2 Exposure to ultraviolet light for 30–120 s induces molecular chain isomer rearrangement.

[0066] In step S3, the core spinning solution and the sheath spinning solution are respectively fed into the dual-channel co-extrusion equipment by metering pumps. The extrusion speed can be conventionally adjusted by those skilled in the art according to parameters such as the viscosity of the spinning solution, the diameter of the spinneret orifice and the linear density of the target fiber, as long as the sheath spinning solution and the core spinning solution can form a stable coaxial laminar flow in the composite zone.

[0067] The cross-sectional area ratio of the core and sheath layers is controlled by adjusting the volumetric flow rate ratio of the core layer flow channel and the sheath flow channel. The preferred volumetric flow rate ratio of the core layer to the sheath spinning solution is 3:1 to 5:1.

[0068] (vii) Performance indicators The fibers obtained by the preparation method described above have one or more of the following performance indicators: 1. Cut-resistant performance Test according to EN388:2016 (or ISO 13997): Cutting force ≥ 10 N, preferably ≥ 15 N, more preferably ≥ 20 N; The cut resistance rating is C or higher.

[0069] 2. Fiber mechanical properties Tensile strength: 18–25 cN / dtex; Elongation at break: 2–3.1%; Modulus: 800~950 cN / dtex.

[0070] 3. Core-skin structure The ratio of the skin to the core cross-sectional area is 1:3 to 1:5.

[0071] 4. Spinnability The single filament breakage rate during spinning is ≤ 0.12%, preferably ≤ 0.08%; Stretchability > 10.

[0072] 5. Durability Filler retention: After 50 industrial washes, the filler shedding rate is ≤ 0.5%, or no pitting or shedding marks are found on the fiber surface by SEM observation; Color fastness: The color fastness to washing, as tested according to ISO 105-C06, is ≥ grade 4.

[0073] (viii) Yarns and fabrics The cut-resistant ultra-high molecular weight polyethylene fiber of the present invention can be made into yarn using conventional twisting, plying, covering, or blending methods in the art, and can be made into fabric using conventional knitting, weaving, or nonwoven methods. The linear density, twist, and ply count of the yarn, as well as the fabric structure, areal density, and number of layers, can be adjusted according to the cut resistance level and usage requirements.

[0074] The yarn or fabric may be made solely from the cut-resistant ultra-high molecular weight polyethylene fiber of the present invention, or it may be mixed with other fibers without affecting the cut-resistant performance. Example 1

[0075] A cut-resistant ultra-high molecular weight polyethylene fiber, with a fiber diameter of 12 μm and a core-sheath cross-sectional area ratio of 1:3.4, comprises: First type of polyethylene: weight average molecular weight 5.2 × 10⁻⁶ 6 g / mol ultra-high molecular weight polyethylene; Inorganic fiber powder: carbon fiber modified with octadecyltrichlorosilane; wherein the carbon fiber has an aspect ratio of 7.2, an axial angle of 3°, and an average axial spacing of 120 μm; Second polyethylene: weight-average molecular weight is 2.1 × 10⁻⁶ 6 g / mol of relatively low molecular weight polyethylene; Titanium dioxide particles: 0.35 μm.

[0076] Of these, based on the total weight of the core spinning solution, the first polyethylene content is 10.0 wt% and the inorganic fiber powder content is 22.0 wt%; based on the total weight of the sheath spinning solution, the second polyethylene content is 12.5 wt% and the titanium dioxide particle content is 3.0 wt%. The solvent for both the core and sheath spinning solutions is decahydronaphthalene.

[0077] The cut-resistant ultra-high molecular weight polyethylene fiber of this embodiment is prepared by the following method: S1. Preparation of core spinning solution: Select the first polyethylene, dissolve it in decahydronaphthalene solvent at a ratio of 10.0 wt%, add 22.0 wt% carbon fiber modified by octadecyltrichlorosilane, and disperse it uniformly at high speed at 145℃ to obtain the core spinning solution.

[0078] S2. Preparation of the skin spinning solution: Select the second polyethylene, dissolve it in decahydronaphthalene solvent at a ratio of 12.5 wt%, add 3.0 wt% titanium dioxide particles with a particle size of 0.35 μm, and stir and disperse evenly at 135℃ to obtain the skin spinning solution.

[0079] S3, Dual-channel co-extrusion spinning: The volumetric flow rate ratio of the core spinning solution to the sheath spinning solution is controlled at 3.4:1, and the solutions are co-extruded synchronously to obtain gelatin filaments.

[0080] S4. Solidification and molding: Set the solidification bath temperature to -5℃ to complete phase separation and molding.

[0081] S5. Hot stretching treatment: stretching temperature 135℃, stretching ratio 50 times.

[0082] S6. Heat setting treatment: Heat set at 148℃ for 60 seconds, then cool and rewind to obtain the finished fiber. Example 2

[0083] A cut-resistant ultra-high molecular weight polyethylene fiber, with a fiber diameter of 15 μm and a core-sheath cross-sectional area ratio of 1:4, comprising: First type of polyethylene: weight average molecular weight 4.8 × 10⁻⁶ 6 g / mol ultra-high molecular weight polyethylene; Inorganic fiber powder: alumina fiber modified with n-octyltriethoxysilane, wherein the alumina fiber has an aspect ratio of 5.3, an axial angle of 5°, and an average axial spacing of 180 μm; Second polyethylene: weight-average molecular weight is 0.95 × 10⁻⁶ 6 g / mol of relatively low molecular weight polyethylene; Titanium dioxide particles: 0.28μm.

[0084] Of these, based on the total weight of the core spinning solution, the first polyethylene content is 9.5 wt% and the inorganic fiber powder content is 18.5 wt%; based on the total weight of the sheath spinning solution, the second polyethylene content is 11 wt% and the titanium dioxide particle content is 2.2 wt%. The solvent for both the core and sheath spinning solutions is white oil.

[0085] In this embodiment, the dual-channel co-extrusion volume ratio is set to 4:1, the stirring temperature of the sheath spinning solution is 150°C, the stirring temperature of the core spinning solution is 169°C, the coagulation bath temperature is -2°C, the 47-fold overstretch is performed at 130°C, and the filaments are heat-set at 142°C for 45 seconds. Between steps S4 and S5, the solidified filaments are extracted with hexane / xylene and then dried. The remaining steps are the same as in Example 1. Example 3

[0086] A cut-resistant ultra-high molecular weight polyethylene fiber, with a fiber diameter of 25 μm and a core-sheath cross-sectional area ratio of 1:5, comprising: First type of polyethylene: weight average molecular weight 4.0 × 10⁻⁶ 6 g / mol ultra-high molecular weight polyethylene; Inorganic fiber micro powder: silicon carbide fiber modified with silane coupling agent KH-550; wherein, the silicon carbide fiber has an aspect ratio of 4, an axial angle of 0°, and an average axial spacing of 250 μm; Second polyethylene: weight-average molecular weight is 0.5 × 10⁻⁶ 6 g / mol of relatively low molecular weight polyethylene; Titanium dioxide particles: 0.2 μm.

[0087] Of these, based on the total weight of the core spinning solution, the first polyethylene content is 8.0 wt% and the inorganic fiber powder content is 11.0 wt%; based on the total weight of the sheath spinning solution, the second polyethylene content is 10.0 wt% and the titanium dioxide particle content is 0.5 wt%. The solvent for both the core and sheath spinning solutions is decahydronaphthalene.

[0088] In this embodiment, the dual-channel co-extrusion volume ratio is set to 5:1, the stirring temperature of the outer layer spinning solution is 140℃, the stirring temperature of the core layer spinning solution is 155℃, the coagulation bath temperature is -10℃, the stretching is 37 times under 130℃, and the heat setting is 142℃ for 45 s. The remaining steps are the same as in Embodiment 1. Example 4

[0089] A cut-resistant ultra-high molecular weight polyethylene fiber, with a fiber diameter of 30 μm and a core-sheath cross-sectional area ratio of 1:5, comprising: First type of polyethylene: weight average molecular weight 4.5 × 10 6 g / mol ultra-high molecular weight polyethylene; Inorganic fiber micro powder: silicon nitride fibers modified with silane coupling agent KH-560; wherein, the silicon nitride fibers have an aspect ratio of 10, an axial angle of 10°, and an average axial spacing of 110 μm; Second polyethylene: weight average molecular weight is 3.5 × 10⁻⁶ 6 g / mol of relatively low molecular weight polyethylene; Titanium dioxide particles: 0.5μm.

[0090] Of these, based on the total weight of the core spinning solution, the first polyethylene content is 12.0 wt% and the inorganic fiber powder content is 30.0 wt%; based on the total weight of the sheath spinning solution, the second polyethylene content is 15 wt% and the titanium dioxide particle content is 5.0 wt%. The solvent for both the core and sheath spinning solutions is decahydronaphthalene.

[0091] In this embodiment, the dual-channel co-extrusion volume ratio is set to 5:1, the coagulation bath temperature is 0℃, the stretching is 35 times under 130℃, and the heat setting is 142℃ for 45 seconds. The remaining steps are the same as in Embodiment 1. Example 5

[0092] A cut-resistant ultra-high molecular weight polyethylene fiber, with a fiber diameter of 10 μm and a core-sheath cross-sectional area ratio of 1:3, comprising: First type of polyethylene: weight average molecular weight 4.5 × 10 6 g / mol ultra-high molecular weight polyethylene; Inorganic fiber micro powder: a blend of octadecyltrichlorosilane-modified carbon fiber and silicon carbide fiber in a mass ratio of 8:2; wherein the carbon fiber has an aspect ratio of 6, an axial angle of 8°, and an average axial spacing of 260 μm; Second polyethylene: weight average molecular weight is 3.5 × 10⁻⁶ 6 g / mol of relatively low molecular weight polyethylene; Titanium dioxide particles: Octyltriethoxysilane modified titanium dioxide particles, 0.2 μm in diameter.

[0093] Of these, based on the total weight of the core spinning solution, the first polyethylene content is 12.0 wt% and the inorganic fiber powder content is 25.0 wt%; based on the total weight of the sheath spinning solution, the second polyethylene content is 15 wt% and the titanium dioxide particle content is 5.0 wt%. The solvent for both the core and sheath spinning solutions is decahydronaphthalene.

[0094] In this embodiment, the dual-channel co-extrusion volume ratio is set to 3:1, the coagulation bath temperature is 0℃, the stretching is 37 times under 130℃, and the heat setting is 142℃ for 45 seconds. The remaining steps are the same as in Embodiment 1. Example 6

[0095] A cut-resistant ultra-high molecular weight polyethylene fiber, with a fiber diameter of 15 μm and a core-sheath cross-sectional area ratio of 1:4.8, comprises: First polyethylene: weight-average molecular weight 5×10 6 g / mol ultra-high molecular weight polyethylene; Inorganic fiber micro powder: octadecyltrichlorosilane modified glass fiber micro powder and alumina micro powder are compounded in a mass ratio of 6.5:3.5; wherein the glass fiber has an aspect ratio of 8, an axial angle of 10°, and an average axial spacing of 250 μm; Second polyethylene: weight average molecular weight is 3.5 × 10⁻⁶ 6 g / mol of relatively low molecular weight polyethylene; Titanium dioxide particles: Octyltriethoxysilane modified titanium dioxide particles, with a diameter of 0.3 μm.

[0096] Of these, based on the total weight of the core spinning solution, the first polyethylene content is 12.0 wt% and the inorganic fiber powder content is 18.0 wt%; based on the total weight of the sheath spinning solution, the second polyethylene content is 15 wt% and the titanium dioxide particle content is 5.0 wt%. The solvent for both the core and sheath spinning solutions is decahydronaphthalene.

[0097] In this embodiment, the dual-channel co-extrusion volume ratio is set to 4.8:1, the coagulation bath temperature is -5℃, the stretching is 47 times under 130℃, and the heat setting is 142℃ for 45 seconds. The remaining steps are the same as in Embodiment 1. Example 7

[0098] Based on Example 1, the inorganic fiber micropowder was prepared by compounding octadecyltrichlorosilane-modified carbon fiber and alumina fiber at a mass ratio of 2:1. Based on the total weight of the core spinning solution, the total content of the inorganic fiber micropowder was 23.0 wt.%, of which the carbon fiber grafting rate was 0.85 mmol / g and the aspect ratio was 6.5, and the alumina fiber grafting rate was 0.52 mmol / g and the aspect ratio was 4.8. Other components of the sheath spinning solution were added, specifically 0.8 wt.% PEG-1000 monostearate antistatic agent, while the remaining process parameters remained unchanged. Example 8

[0099] Based on Example 2, the inorganic fiber micro powder was made by compounding octadecyltrichlorosilane-modified carbon fiber and alumina fiber in a mass ratio of 7:3, with a total content of 20.5 wt.%, a carbon fiber grafting rate of 0.82 mmol / g, and an alumina fiber grafting rate of 0.54 mmol / g; based on the total weight of the cortex spinning solution, the content of titanium dioxide particles was 2.8 wt.% and the content of antistatic additives was 0.6 wt.%.

[0100] In this embodiment, the dual-channel co-extrusion volume ratio is set to 4.2:1, 138℃, and 47 times stretching, while other parameters remain unchanged. Example 9

[0101] Based on Example 1, 1.2 wt.% of 4-hydroxy-4'-methoxyazobenzene was added to the cortex spinning solution to give it intelligent color-changing properties. In this example, after step S5 and before S6, a wavelength of 365 nm and 5 mW / cm² was used. 2 Expose to ultraviolet light for 90 seconds, with all other parameters remaining unchanged. Example 10

[0102] Based on Example 2, 0.5 wt.% graphene quantum dots were added to the core spinning solution to give this example antistatic strengthening properties, with a particle size of 3.2 nm and an oxygen content of 9.7 at.%, while the rest of the process remained unchanged. Example 11

[0103] The cut-resistant ultra-high molecular weight polyethylene fiber obtained in Example 1 was twisted to obtain a yarn with a linear density of 200 D and a twist of 80 twists / meter. The yarn was woven on an 18-needle flat knitting machine, and the cutting force of the fabric was tested according to ISO13997. The cutting force retention rate after bending and washing was 99.1%.

[0104] Examples 1 to 10 above provide specific settings for the sheath, core layer, and preparation process. To facilitate comparison of the basic properties of the fibers obtained in each example, the fibers obtained in each example were tested using a unified sample preparation and testing method, as follows: Cut resistance: The fiber is made into a standard knitted sample with consistent specifications, and the cutting force is measured according to ISO 13997:1999 standard, expressed in N; in addition, 200D filaments made from the fiber are made into gloves on an 18-needle glove knitting machine, and the cut resistance rating of the finished product is verified according to EN 388.

[0105] Tensile properties: The tensile strength and elongation at break of the fiber or yarn shall be determined in accordance with ISO 2062 or GB / T 3916. Tensile strength is expressed in cN / dtex, elongation at break is expressed in % and modulus is expressed in cN / dtex.

[0106] Core-sheath cross-sectional area ratio: The core-sheath cross-sectional area ratio is calculated by observing the fiber cross-section with a scanning electron microscope, measuring the sheath thickness and core diameter.

[0107] Interface status: Observe whether the interface between the cortex and core is continuous by cross-sectional SEM, or observe the interface layering after a set bending cycle.

[0108] Filler shedding: After repeatedly bending and washing the fibers a specified number of times, observe the exposure and shedding of surface micro-powder.

[0109] The sample preparation conditions and testing environment for the above indicators are kept consistent.

[0110] The basic performance parameters of each embodiment were measured according to the above test methods, and the results are shown in Table 1. The results of the special performance parameters of embodiments 8 to 10 are shown in Table 2.

[0111] Table 1 Basic performance parameters of each embodiment Table 2 Special performance parameters of Examples 8-10 serial number index Test Results Example 8 Antistatic properties <![CDATA[Volume resistivity 8.7×10 5 Ω·cm]]> Example 9 Intelligent color change The fiber is initially gray, turns dark blue after 90 seconds of irradiation, and turns purple after 120 seconds of continuous irradiation; the color gradation can be reversibly adjusted. Example 10 Antistatic properties <![CDATA[Volume resistivity 9.0×10 4 Ω·cm]]> To further illustrate the technical effects of the present invention, the following comparative examples are provided. Unless otherwise specified, the preparation methods and testing conditions of each comparative example are the same as those of Example 1, with only the corresponding technical features adjusted. Comparative Example 1

[0112] The skin and core layers use ultra-high molecular weight polyethylene with the same weight-average molecular weight, specifically 5.2 × 10⁻⁶. 6 g / mol, with the other conditions the same as in Example 1. Comparative Example 2

[0113] The core layer and process are the same as in Example 1, except that the skin layer is made of ultra-high molecular weight polypropylene, specifically 5.2 × 10⁻⁶. 6The content of ultra-high molecular weight polypropylene and titanium dioxide particles was the same as in Example 1, g / mol. The solvent for the skin spinning solution was tetrahydronaphthalene, and no additional agents to promote interfacial compatibility were added. Comparative Example 3

[0114] Particle / whisker filler to replace fiber powder The core layer spinning solution uses rod-shaped SiO2 whiskers instead of inorganic fiber powder, while maintaining the same filler content; otherwise, it is the same as in Example 1. Comparative Example 4

[0115] All components of the skin spinning solution and core spinning solution in Example 1, including ultra-high molecular weight polyethylene, medium and low molecular weight polyethylene, inorganic fiber micro powder and titanium dioxide particles, were uniformly mixed in the same amounts as in Example 1, and homogeneous fibers were prepared by conventional single-channel gel spinning. Comparative Example 5

[0116] 5a: The weight-average molecular weight of the second polyethylene contained in the cortex spinning solution is 4 × 10⁻⁶. 6 g / mol, the rest is the same as in Example 1.

[0117] 5b: The weight-average molecular weight of the second polyethylene contained in the cortex spinning solution is 4 × 10⁻⁶. 5 g / mol, the rest is the same as in Example 1. Comparative Example 6

[0118] The inorganic fiber powder in the core spinning solution was not surface-treated, and the rest was the same as in Example 1.

[0119] The performance testing methods for Comparative Examples 1 to 6 were the same as those for Example 1. The key settings differences and performance comparison results between Example 1 and each comparative example are shown in Table 3.

[0120] Table 3 Performance comparison between Example 1 and Comparative Examples 1-6 serial number Differences from Example 1 EN388 level Tensile strength (cN / dtex) Interface status Stretchability Modulus (cN / dtex) Surface after bending / washing Example 1 benchmark scheme F 20.2 Combine well 50 850 No obvious inorganic fiber powder shedding Comparative Example 1 The skin layer was replaced with ultra-high molecular weight polyethylene with the same weight average molecular weight. F 20.4 Combine well 45 855 No obvious inorganic fiber powder shedding Comparative Example 2 The skin layer was replaced with ultra-high molecular weight polypropylene. F 19.2 The core-skin structure is obvious. 42 844 No obvious inorganic fiber powder shedding Comparative Example 3 Core layer replaced with granular filler C 18.4 Combine well 50 603 Surface filler powder is easy to fall off Comparative Example 4 All components were mixed, and a single-channel gel spinning method was used to prepare the product. F 20.0 / 44 846 There was obvious shedding of inorganic fiber powder. Comparative Example 5a The second polyethylene weight-average molecular weight is higher than the upper limit. F 19.5 Easy to stratify 46 855 No obvious inorganic fiber powder shedding Comparative Example 5b The second polyethylene weight-average molecular weight is below the lower limit. E 18.3 Easy to stratify 50 848 There was obvious shedding of inorganic fiber powder. Comparative Example 6 Inorganic fiber powder does not undergo surface treatment. F 19.8 Combine well 50 840 There was obvious shedding of inorganic fiber powder. As shown in Table 3, compared with Example 1, each comparative example only changed one technical feature, and the rest of the settings were the same as in Example 1. Compared with Example 1, the skin layer of Comparative Example 1 uses ultra-high molecular weight polyethylene with the same molecular weight as the core layer. Its skin layer coating integrity and maximum draw ratio are both lower than those of Example 1, indicating that medium and low molecular weight skin layers are beneficial to improving coating uniformity and spinnability.

[0121] Comparative Example 2 used ultra-high molecular weight polypropylene (UHMWPP) as the sheath layer. Due to the poor compatibility between UHMWPP and the core layer UHMWPE, and its high molecular weight and low melt flowability, it was difficult to form a thin, uniform, and continuous coating layer. This weakened the sheath-core interface bonding, leading to delamination after bending and a decrease in fiber softness and spinnability. These results indicate that using medium- to low-molecular-weight polyethylene (MMWPE) as the sheath layer is beneficial for improving sheath integrity, interfacial bonding, softness, and spinnability.

[0122] Comparative Example 3 replaced the fibrous powder in the core layer with granular filler. Granular filler has a smaller specific surface area and aspect ratio, resulting in weaker mechanical interaction with the matrix. It is more prone to exposure and detachment after bending and washing, leading to a more significant decrease in cutting force. These results indicate that fibrous powder is superior to granular filler in terms of pull-out resistance and durable cut resistance.

[0123] Comparative Example 4 involved mixing all components and then spinning using a single-channel gel spinning process. The resulting fibers did not form a continuous core-sheath structure; the hard filler was dispersed throughout the fiber cross-section, and the sheath could not provide isolation and protection for the core and filler. This resulted in increased fiber surface exposure and shedding, and decreased spinnability. These results demonstrate that dual-channel co-extrusion and a core-sheath partitioned structure are necessary to achieve the technical effects of this invention.

[0124] In Comparative Example 5a, the weight-average molecular weight of the second polyethylene was higher than the upper limit. This resulted in reduced melt flowability of the skin layer, making it difficult to uniformly coat the core layer, leading to decreased skin layer thickness uniformity and spinnability, and reduced fiber softness. These results indicate that the upper limit of the weight-average molecular weight of the second polyethylene plays a crucial role in the integrity of the skin layer coating and its processing performance.

[0125] In Comparative Example 5b, the weight-average molecular weight of the second polyethylene was below the lower limit. Although the skin's fluidity was improved, its mechanical strength and abrasion resistance were insufficient, making it prone to damage during stretching, bending, or washing, leading to exposure of the core layer micropowder and decreased cutting stability. These results indicate that the lower limit of the weight-average molecular weight of the second polyethylene plays a crucial role in the skin's protective performance and durability.

[0126] The fiber powder in Comparative Example 6, without surface treatment, showed decreased dispersion uniformity and cutting stability, indicating that surface pretreatment is beneficial for improving interfacial bonding and performance stability.

[0127] In summary, the molecular weight of the cortex, the interfacial layer, the morphology and location of the fiber micropowder, the cortex functional additives, and the surface treatment of the micropowder all affect the integrity of the fiber coating, interfacial bonding, cut resistance, and spinnability. Under the synergistic effect of the above characteristics, Example 1 maintains a high cut resistance level while also possessing good softness, durability, and processing stability.

[0128] In summary, this invention solves the technical problems of traditional homogeneous ultra-high molecular weight polyethylene fibers, such as poor cut resistance, filler shedding, weak interfacial bonding, electrostatic fraying, and poor colorability, by precisely controlling the structural parameters of inorganic micropowder, the molecular weight gradient of the core and sheath, the ratio of functional additives, and the dual-channel co-extrusion gel spinning process. The fibers of this invention achieve a cut resistance rating of EN388 C or higher, exhibit high color fastness, excellent weaving performance, and can selectively achieve intelligent photosensitive color changing and low-impedance electrostatic functions. They are suitable for applications in industrial protection, police equipment, tactical protection, aerospace, and other fields. The manufacturing process is simple and controllable, with moderate cost, making it suitable for large-scale industrial production.

[0129] The above description is merely a preferred embodiment or an example of the present invention and is not intended to limit the present invention. For those skilled in the art, the composite materials and their preparation process in the present invention are not limited thereto. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principle of the present invention should be included within the protection scope of the present invention.

Claims

1. A cut-resistant ultra-high molecular weight polyethylene fiber, prepared by a gel spinning dual-channel co-extrusion process, characterized in that, include: The core layer contains materials with a weight-average molecular weight ≥ 4.0 × 10⁻⁶. 6 g / mol of first polyethylene and inorganic fiber powder, wherein the inorganic fiber powder is surface-treated inorganic fiber powder; The cortex, containing a weight-average molecular weight of 0.5 × 10⁻⁶. 6 Up to 3.5×10 6 g / mol of second polyethylene and titanium dioxide particles are coated on the outer surface of the core layer to form a skin-core double-layer composite structure; and the interface transition region formed between the core layer and the skin layer; The weight-average molecular weight of the second polyethylene is lower than that of the first polyethylene.

2. A cut-resistant ultra-high molecular weight polyethylene fiber according to claim 1, characterized in that, The core layer is formed by gel spinning of the core layer spinning solution; based on the total weight of the core layer spinning solution, the content of the first polyethylene is 8-12 wt%, and the content of the inorganic fiber powder is 11-30 wt%. The skin layer is obtained by gel spinning of the skin layer spinning solution; based on the total weight of the skin layer spinning solution, the content of the second polyethylene is 10-15 wt%, and the content of the titanium dioxide particles is 0.5-5.0 wt%. The surface treatment includes one or more of silane coupling agent treatment or alkylation treatment; The fiber diameter is 10-30 μm, and the core-sheath cross-sectional area ratio of the fiber is 1:3-1:

5.

3. A cut-resistant ultra-high molecular weight polyethylene fiber according to claim 2, characterized in that, The interface transition zone is a gradient transition region formed by the mutual penetration and entanglement of the polyethylene molecular chains of the skin layer and the polyethylene molecular chains of the core layer during co-extrusion; and / or, The core spinning solution and the sheath spinning solution use the same solvent, which is selected from dichloromethane, dichloroethane, carbon tetrachloride, a mixture of dichloromethane and ionic liquid, decahydronaphthalene, or white oil.

4. A cut-resistant ultra-high molecular weight polyethylene fiber according to claim 3, characterized in that, The weight-average molecular weight of the first polyethylene is ≥4.5×10⁻⁶. 6 g / mol, the weight-average molecular weight of the second polyethylene is 1.2–3.0 × 10 g / mol. 6 g / mol; the solvent is decahydronaphthalene or white oil.

5. A cut-resistant ultra-high molecular weight polyethylene fiber according to claim 4, characterized in that, The inorganic fiber powder is selected from one or more of silicon carbide fiber, silicon nitride fiber, carbon fiber, glass fiber, and alumina fiber; the aspect ratio of the inorganic fiber powder is 4 to 10, the angle between the axis of the inorganic fiber powder and the spinning axis is 0 to 10°, and the average axial spacing between the inorganic fiber powders is 50 to 260 μm.

6. A cut-resistant ultra-high molecular weight polyethylene fiber according to claim 5, characterized in that, The inorganic fiber powder is prepared by compounding carbon fiber and alumina fiber in weight ratios of 1-3 parts and 1-3 parts respectively, and the content of the inorganic fiber powder obtained by compounding is 18-25 wt% of the core spinning solution; the aspect ratio of the carbon fiber is 6-8, and the aspect ratio of the alumina fiber is 4-6; the carbon fiber is surface alkylated with octadecyltrichlorosilane, with a grafting rate ≥0.8 mmol / g; the alumina fiber is surface alkylated with n-octyltriethoxysilane, with a grafting rate ≥0.5 mmol / g; and / or, The titanium dioxide particles have a particle size of 0.2 to 0.5 μm and a content of 2.0 to 3.5 wt% of the skin spinning solution.

7. A cut-resistant ultra-high molecular weight polyethylene fiber according to claim 6, characterized in that, The sheath spinning solution further includes polyethylene glycol monostearate, wherein the polyethylene glycol monostearate has a molecular weight of 1000±100 g / mol and a content of 0.3–1.2 wt% of the sheath spinning solution; and / or, The sheath spinning solution further includes 0.5–2.0 wt% of a 4-hydroxy-4'-methoxyazobenzene photosensitizing derivative; and / or, The core spinning solution also includes 0.1–0.8 wt% graphene quantum dots, the graphene quantum dots having a particle size of 2–5 nm and an oxygen content of 8 at.%–12 at.%; the graphene quantum dots form a hydrogen bond-van der Waals synergistic anchoring structure with the surface-treated inorganic fiber micropowder, and are oriented along the spinning axis to form a conductive path.

8. A method for preparing cut-resistant ultra-high molecular weight polyethylene fiber according to any one of claims 1 to 7, characterized in that, Includes the following steps: S1. Preparation of core spinning solution: The first polyethylene is dissolved in a solvent, stirred evenly at 145-169°C, and then surface-modified inorganic fiber powder is added and dispersed evenly to obtain the core spinning solution. S2. Preparation of skin spinning solution: The second polyethylene is dissolved in a solvent, titanium dioxide particles are added, and an antistatic agent and / or a photosensitive derivative are optionally added. The solution is stirred and dispersed evenly at 135-150°C to obtain the skin spinning solution. S3. Dual-channel co-extrusion spinning: The core spinning solution and the sheath spinning solution are co-extruded and sprayed through a dual-channel co-extrusion device to obtain gel filaments; wherein the volume flow ratio of the core layer to the sheath layer is 3:1 to 5:1; S4. Low-temperature solidification phase separation: The gel fiber enters a solidification bath to cool and solidify, and the solidification bath temperature is -10 to 0℃; S5. Super-high temperature hot stretching: High temperature super-high temperature stretching of solidified filament bundles, stretching temperature 120~145℃, stretching ratio 35~50 times; S6. Heat setting treatment: The stretched fiber is heat set at 140-155℃ for 30-90 s, cooled and wound to obtain the cut-resistant ultra-high molecular weight polyethylene fiber.

9. The method for preparing cut-resistant ultra-high molecular weight polyethylene fiber according to claim 8, characterized in that, Between step S5 and step S6, the method further includes a photosensitive modification treatment step: For fiber bundles containing the aforementioned photosensitive derivative, an irradiance of 4–6 mW / cm is applied at a wavelength of 350–380 nm. 2 Irradiation with ultraviolet light for 30–120 s induces molecular chain isomer rearrangement; the solvent is selected from decahydronaphthalene or white oil; both the skin spinning solution and the core spinning solution are based on polyethylene; during the co-extrusion process, the skin and core layers achieve self-adhesion at the interface through the permeation and entanglement of polyethylene molecular chains.

10. A cut-resistant yarn or fabric, characterized in that, The cut-resistant yarn or the fabric includes cut-resistant ultra-high molecular weight polyethylene fiber as described in any one of claims 1-7.

Citation Information

Patent Citations

  • A method for preparing high-cut-resistant ultra-high molecular weight polyethylene fiber and its application

    CN104233497B

  • Cutting-resistant ultra high molecular weight polyethylene fiber, preparation method and application thereof

    CN106350882A

  • A high-cut-resistant ultra-high molecular weight polyethylene fiber and its preparation method

    CN110205695B

  • Cutting-resistant ultra-high molecular weight polyethylene fiber as well as preparation method and application thereof

    CN115787121A

  • Preparation method of ultra-high molecular weight polyethylene composite fiber material

    CN118441463A