A core-sheath structure thermoplastic polyurethane-coated yarn and its low-temperature preparation method
The use of a low-temperature melt extrusion process to prepare thermoplastic polyurethane-coated yarns with a core-sheath structure solves the problem of insufficient functionality in traditional synthetic fiber materials, and enables the durable and low-cost industrial production of multifunctional yarns.
Patent Information
- Application Number
- CN202611038840.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-13
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional synthetic fiber materials lack antibacterial, deodorizing, UV-resistant, and antistatic properties, and existing core-sheath composite spinning technology is complex and costly, making it unsuitable for large-scale industrial production.
A low-temperature melt extrusion process is used to coat the core material with a mixture of TPU and functional additives, forming a core-shell structure thermoplastic polyurethane coated yarn. Low-temperature processing avoids heat damage and achieves stable dispersion of functional additives in the TPU skin.
The prepared multifunctional core-sheath structure thermoplastic polyurethane-coated yarn maintains the mechanical properties of the core layer while possessing long-lasting antibacterial, UV-resistant, deodorizing, and antistatic functions. The process is simple, low-cost, and suitable for continuous production.
Smart Images

Figure CN123108795A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of textile materials technology, specifically relating to a core-sheath thermoplastic polyurethane-coated yarn and its low-temperature preparation method, and particularly to a core-sheath thermoplastic polyurethane-coated yarn with antibacterial, anti-ultraviolet, deodorizing and antistatic functions and its preparation method. Background Technology
[0002] Traditional synthetic fibers (such as polyester and nylon) have been widely used in the textile industry due to their high strength, good abrasion resistance, and moderate cost. However, these fiber materials themselves do not possess functional characteristics such as antibacterial, odor-resistant, UV-resistant, and antistatic properties, and their inherent properties, such as a stiff feel and poor resilience, have to some extent limited their promotion and application in the field of high-end functional textiles.
[0003] Functionalization methods for fibers or fabrics typically include finishing and blending spinning. Finishing refers to impregnating or coating woven fabrics with a solution containing functional auxiliaries (such as antibacterial agents, UV stabilizers, etc.). While this method is simple and easy to implement, the functional layer of the resulting fabric mainly adheres to the fiber surface and is easily detached under mechanical forces during washing and friction, resulting in poor durability and difficulty in meeting long-term use requirements. Blending spinning involves blending polymer raw materials with functional auxiliaries before melt spinning. This method results in most of the functional auxiliaries being dispersed within the fiber, leading to a low effective surface concentration and low utilization rate. Furthermore, melt spinning typically requires high processing temperatures (generally exceeding 250°C), which can easily cause the decomposition or deactivation of heat-sensitive functional auxiliaries, leading to functional degradation or even failure.
[0004] In recent years, core-sheath composite spinning technology has attracted attention due to its ability to balance fiber mechanical properties and surface functionality. This technology involves using a specific polymer as a sheath (e.g., thermoplastic polyurethane) to coat the core yarn, and core-spun yarns with various functional properties can be obtained through sheath modification. For example, CN111394848A discloses a process for chemically modifying thermoplastic polyurethane (TPU) (including plasma treatment, graft polymerization, etc.) and then melt-coating it onto the outer layer of the core yarn. However, this method is complex, requires numerous additives, and involves the use of organic solvents, placing high demands on production equipment and environmental control, which is not conducive to large-scale, continuous, and low-cost industrial production.
[0005] To address the aforementioned issues, it is necessary to develop a method for preparing multifunctional TPU core-spun yarn that is more conducive to industrial production. Summary of the Invention
[0006] This application aims to provide a simple and low-cost method for preparing multifunctional thermoplastic polyurethane-coated yarn with a core-sheath structure. The resulting yarn maintains the excellent mechanical properties of the core yarn while also possessing the comfortable and elastic feel of the sheath layer, and can achieve multiple functions such as long-lasting antibacterial, anti-ultraviolet, deodorizing, and antistatic properties.
[0007] To achieve the above objectives, this application provides the following technical solution: A method for preparing a core-sheath structure thermoplastic polyurethane-coated yarn includes the following steps: S1. The mixture of TPU and functional additives is melt-extruded to obtain TPU melt; S2. The TPU melt is conveyed to the coating die head; S3. Pass the core material through the center of the coating die head, so that the TPU melt surrounds the core material to form a complete coating layer, and obtain TPU melt-coated yarn; S4. Cool the TPU melt-coated yarn to obtain the core-sheath structure thermoplastic polyurethane-coated yarn.
[0008] This application also provides the following technical solutions: A core-sheath structure thermoplastic polyurethane-coated yarn is obtained by the aforementioned method for preparing core-sheath structure thermoplastic polyurethane-coated yarn.
[0009] This application also provides the following technical solutions: The aforementioned application of thermoplastic polyurethane-coated yarns with a core-sheath structure in textile manufacturing.
[0010] The technical solution provided in this application has the following beneficial effects: (1) The preparation method of the multifunctional core-sheath structure thermoplastic polyurethane coated yarn provided in this application enables functional additives (such as antibacterial agents, antistatic agents, etc.) to be stably and uniformly dispersed in the TPU skin matrix, and is not easily lost due to external forces such as washing and friction, thereby significantly improving the functional durability of the composite yarn.
[0011] (2) The preparation method of the multifunctional core-sheath structure thermoplastic polyurethane coated yarn provided in this application can adopt a low temperature processing technology (not higher than 200°C), which can effectively avoid thermal damage to the core material caused by high temperature during the coating process and thermal decomposition or deactivation of functional additives, thereby helping to retain the mechanical properties of the core material (such as high strength and high modulus characteristics) and the multifunctionality of the sheath material.
[0012] (3) The preparation method of the multifunctional core-sheath structure thermoplastic polyurethane-coated yarn provided in this application does not require complicated processes and equipment, and does not involve the use of organic solvents. It has the advantages of low cost, environmental friendliness and easy continuous production. Figure 1 ).
[0013] (4) The multifunctional core-sheath structure thermoplastic polyurethane-coated yarn provided in this application has a core-sheath composite structure. The TPU sheath not only provides the yarn with excellent elasticity and soft touch, but also introduces a variety of functional additives to give the composite yarn a variety of functions (such as antibacterial, UV-resistant, odor-resistant and antistatic properties), thereby achieving a synergistic improvement in the comfort and functionality of the composite yarn. Attached Figure Description
[0014] Figure 1 A process flow diagram of the method for preparing the core-sheath structure thermoplastic polyurethane-coated yarn provided in this application. Invention Details 1. Terminology Explanation All patents and other publications cited herein are incorporated herein in their entirety. In the event of any conflict between any description of terminology herein and any document incorporated herein by reference, this document shall prevail.
[0015] Numerical ranges can be represented by a hyphen "-" or a tilde "~". Unless otherwise stated, the range should be understood to encompass both the endpoint values and any values in between. There are no particular restrictions on the type of numeric values within the range, including but not limited to integers, decimals, fractions, percentages, etc., unless explicitly excluded by the context or a particular numeric type is technically unavailable. The type of numeric values within the range is not limited by the specific representation of the endpoints.
[0016] The terms “including,” “containing,” and similar expressions have a non-restrictive meaning.
[0017] "Optional" is used to indicate that a certain feature (including but not limited to components, steps, parameters or structures) may be present in some embodiments, but may not appear in other embodiments, thereby providing technical flexibility for different implementations without departing from the core concept of the present invention.
[0018] A “combination” of the enumeration items refers to any two or more of the enumeration items that coexist or are used together, including but not limited to any two-item combination, any three-item combination, any more items, and any combination of all the enumeration items, unless the context explicitly excludes it or a particular combination is technically impossible.
[0019] In this application, the use of labels such as a), b), i), ii), 1), 2), S1, S2, etc. to number the method steps is only for the convenience of description and reading, and does not mean that the corresponding steps must be performed in the order of the numbers, unless it is clearly stated in the text that there is a logical or temporal relationship between specific steps.
[0020] When the content or amount of each raw material or component is provided in the form of "%", unless otherwise specified, it is assumed to be a mass percentage (wt%).
[0021] "Thermoplastic polyurethane" or "TPU" refers to a thermoplastic polyurethane material formed by polymerization / addition reaction of oligomeric polyols, polyisocyanates, and chain extenders. The polyol molecule contains two or more free hydroxyl groups. The polyisocyanate molecule contains two or more isocyanate groups. The molecular structure of TPU consists of alternating hard and soft segments: the soft segments are formed from oligomeric polyols, such as polyether polyols (e.g., polytetramethylene ether glycol (PTMEG)), polyester polyols (e.g., poly(1,4-butanediol adipate) (PBA)), polycarbonate polyols (e.g., poly(hexamethylene carbonate) glycol (PHC), poly(trimethylene carbonate) glycol (PTC)), and polycaprolactone polyols (e.g., polycaprolactone glycol); the hard segments are formed by the reaction of polyisocyanates (e.g., diphenylmethane diisocyanate (MDI), toluene diisocyanate (TDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI)) with small molecule chain extenders (e.g., short-chain diols, including but not limited to ethylene glycol (EG), 1,3-propanediol (PDO), 1,4-butanediol (BDO), 1,6-hexanediol (HDO)). TPU can be molded using conventional thermoplastic processing methods, such as extrusion, injection molding, blow molding, calendering, and melt spinning. Its mechanical properties can be adjusted according to its composition, molecular weight, and the ratio of hard to soft segments. Typical characteristics include good elasticity, abrasion resistance, high impact resistance, oil resistance, and chemical resistance. Based on the different chemical structures of the soft segments, TPU can be mainly classified into polyester type, polyether type, and polycarbonate type. Based on the different types of isocyanates used, TPU can also be classified into aromatic TPU and aliphatic TPU.
[0022] "Fiber material" refers to long, spinnable materials used in yarns, fabrics, and related textiles, including but not limited to natural fibers, regenerated fibers, and synthetic fibers. Exemplary natural fibers include cotton, wool, and silk. Exemplary regenerated fibers include viscose, lyocell, and acetate fibers. "Synthetic fiber" refers to fibers whose main component is one or more artificially synthesized polymers. Exemplary synthetic fibers include polyester, polyamide, polyurethane, polyolefin, polyacrylonitrile, and polyaramid fibers. Fiber material can consist of one or more monofilaments of one or more different types. The specifications of fiber material are typically expressed as a combination of "linear density / number of monofilaments." "Linear density" refers to the mass of a unit length of fiber material, measured in denier (D), defined as the mass (in grams) of 9000 meters of fiber material. For example, 9000 meters of 75D fiber material has a mass of approximately 75 grams. "Number of monofilaments" refers to the number of monofilaments in the fiber material, usually indicated by "F." For example, 36F fiber material consists of 36 monofilaments.
[0023] "Polyester fiber" refers to a synthetic fiber with one or more polyesters as its main component, optionally also containing one or more other polymers and / or functional auxiliaries and / or common impurities (e.g., residues of reactants or reagents). The polyester content in the polyester fiber is greater than 50% (mass fraction), preferably not less than 85%. Exemplary polyesters include polyethylene terephthalate (PET), polypropylene terephthalate (PTT), polybutylene terephthalate (PBT), polycyclohexanedimethyl terephthalate (PCT), polylactic acid (PLA), etc. "Polyester" refers to polyester fiber with a PET content of not less than 85%.
[0024] "Polyamide fiber," also known as "nylon" or "polyamide fiber," refers to a synthetic fiber with one or more polyamides as the main component, and optionally also containing one or more other polymers and / or functional auxiliaries and / or common impurities (e.g., residues of reactants or reagents). The polyamide content in the polyamide fiber is more than 50% (mass fraction), preferably not less than 85%. Polyamides (PAs) can be obtained through three methods: Method 1, by polycondensation of diamines (such as ethylenediamine, butanediamine, pentanediamine, hexamethylenediamine, decanediamine, trimethylhexanediamine, isophoronediamine, m-phenylenediamine, terephthalic acid, etc.) with diacids (such as oxalic acid, succinic acid, adipic acid, sebacic acid, dodecanoic acid, terephthalic acid, isophthalic acid, 1,4-cyclohexanedicarboxylic acid, etc.); Method 2, by ring-opening polymerization of lactams (such as caprolactam, laurolactam, etc.); Method 3, by polycondensation of amino acids (such as 6-aminohexanoic acid, 9-aminononanoic acid, 11-aminoundecanoic acid, 12-aminododecanoic acid, etc.). Polyamides obtained through Method 1 can be represented by "PAxy", where x and y represent the number of carbon atoms in the diamine and diacid residues, respectively. Polyamides obtained through Method 2 or 3 can be represented by "PAx", where x represents the number of carbon atoms in the lactam or amino acid residue. Exemplary polyamides include polycaprolactam (PA6), polyhexamethylene adipamide (PA66), polyundecanoamide (PA11), polydodecanoamide (PA12), etc.
[0025] "Functional additives" refer to functional components added to impart, enhance, or improve specific functions of materials (such as antibacterial properties, dispersibility, flowability / processability, antioxidant properties, stability, weather resistance, flame retardancy, interfacial compatibility, etc.), including but not limited to antibacterial agents, antioxidants, ultraviolet absorbers, light stabilizers, coupling agents, dispersants, plasticizers, flame retardants, etc.
[0026] "Antibacterial agent" refers to a functional additive with antibacterial activity. The antibacterial activity refers to the property of inhibiting, killing, or preventing the growth, reproduction, or colonization of one or more microorganisms (e.g., bacteria, fungi, etc.) on a material surface or in a matrix. Antibacterial agents can exert their effects by releasing bactericidal active substances (release-type antibacterial agents), or by achieving contact antibacterial or bactericidal properties in contact with the substrate after bonding (contact-type antibacterial agents), or a combination of both mechanisms. Exemplary antibacterial agents include, but are not limited to, small molecule organic antibacterial agents (e.g., phenolic compounds, amine compounds, chlorinated organic compounds, bromine-containing organic compounds, etc.) and soluble metal ion-based antibacterial agents (e.g., Ag-releasing antibacterial agents). + Cu 2+ Zn 2+Antimicrobial agents include plasma salts or complexes, metal oxides with antibacterial activity (e.g., zinc oxide, titanium dioxide, zirconium oxide, copper oxide, etc.), natural antimicrobial agents (e.g., chitosan and its derivatives), antimicrobial polymers (e.g., quaternized polymers, antimicrobial peptide-modified polymers, etc.), and composite systems formed by loading or encapsulating any of the aforementioned active components onto a carrier. The decomposition of organic matter in sweat by surface microorganisms produces odor components; therefore, the application of antimicrobial agents can often reduce or inhibit body odor.
[0027] "Nano metal oxides" refer to metal oxide particles with an average particle size or main size at the nanoscale (1-1000 nm, preferably 1-100 nm). Examples of nano metal oxides that can be used as antibacterial agents or other functional additives include, but are not limited to, nano zinc oxide (ZnO), nano copper oxide (CuO), nano titanium oxide (TiO2), nano zirconium dioxide (ZrO2), and nano tin dioxide (SnO2). The antibacterial mechanisms of these nano-metal oxides include one or more of the following: i) Metal ions released from the partial dissolution of nano-metal oxides in humid or acidic environments can exert antibacterial effects by disrupting bacterial cell membranes, interfering with enzyme systems, and disturbing intracellular homeostasis; ii) Nano-metal oxides can catalyze the generation of reactive oxygen species (ROS) under light (especially ultraviolet / near-ultraviolet) or in the presence of surface defects, thereby increasing microbial cell membrane permeability, metabolic disorders, and cell death, providing additional UV resistance and antibacterial functions; iii) Nano-metal oxides can directly contact microbial cell walls / cell membranes, especially sharp edges or positively charged surfaces can pierce or electrostatically adsorb onto negatively charged bacterial cell membranes, leading to localized physical damage to the membrane (e.g., pore formation or impaired membrane integrity). To improve their dispersibility, compatibility, stability, and specific functionality in organic material matrices, the nano-metal oxides can be surface-modified.
[0028] Surface modification refers to the process of introducing functional groups, forming coatings, or binding compounds on the surface of solid materials to alter their physical and / or chemical properties, such as energy state, hydrophilicity / hydrophobicity, and reactivity. Surface modification can be achieved through mechanisms such as covalent bonding (including coordination bonding), electrostatic interactions, hydrogen bonding, or physical adsorption between the material and the modifier. Common processes for surface modification of inorganic powders (especially metal oxides) can be categorized into wet, dry, and gas-phase methods, depending on the operating method and medium. Wet methods typically involve mixing and stirring metal oxides and modifiers in an aqueous phase or organic solvent, allowing the modifier to adsorb or chemically react with the particle surface under appropriate temperature conditions, followed by separation, washing, and drying to obtain surface-modified particles. The dry method typically refers to applying a liquid containing a modifier to the surface of metal oxide powder in a dry state by atomization, spraying, or dripping while stirring (or airflowing) the powder in equipment such as a high-speed mixer or fluidized bed. This causes the modifier to deposit on the particle surface and form a coating layer, which is then obtained through heat treatment or curing to obtain the modified product. The gas-phase method typically refers to introducing the modifier into a reaction chamber or fluidized bed containing metal oxide powder using an inert gas (such as nitrogen) as a carrier gas. This allows the modifier to adsorb or chemically react with the particle surface in the gas phase to achieve coating or bonding.
[0029] "Silane coupling agent" refers to an organosilicon compound containing at least one hydrolyzable silicon-based functional group (e.g., -SiX3, where X is an alkoxy group) and one or more organic moieties. After hydrolysis, the hydrolyzable silicon group can condense with hydroxyl groups on the surface of inorganic materials such as metal oxides to form stable Si-OM covalent bonds (M representing a metal), thereby achieving chemical bonding with the inorganic surface. The organic moieties may contain one or more functional groups capable of chemically reacting with the organic material (e.g., organic polymer) matrix (e.g., amino groups, epoxy groups) and groups primarily providing compatibility (e.g., olefinic groups, methacryloxy groups, long-chain alkyl groups, etc.). Exemplary silane coupling agents include, but are not limited to: aminosilanes (e.g., N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane), epoxysilanes (e.g., 3-glycidoxypropyltrimethoxysilane), methacryloxysilanes (e.g., 3-methacryloyloxypropyltrimethoxysilane), mercaptosilanes (e.g., 3-mercaptopropyltrimethoxysilane), vinylsilanes (e.g., vinyltrimethoxysilane), isocyanate or carboxylic anhydride-functionalized silanes (e.g., 3-isocyanopropyltriethoxysilane, 3-(triethoxysilyl)propylsuccinic anhydride), and alkyl / arylsilanes (e.g., methyltrimethoxysilane, phenyltrimethoxysilane, octyltriethoxysilane).
[0030] "Average particle size" refers to the statistical average of a group of particle sizes. The average particle size of nanoparticles can be obtained by common particle size measurement methods, such as dynamic light scattering (DLS), scanning electron microscopy (SEM), transmission electron microscopy (TEM), or other known particle size analysis techniques. Unless otherwise specified, the average particle size of nanoparticles provided in this application refers to the size obtained by measuring and statistically averaging a certain number (preferably at least 200) of particles using TEM.
[0031] "Antistatic agent" refers to a functional additive used to reduce or eliminate static electricity accumulation and electrostatic discharge on or in the volume of a material surface. Antistatic agents achieve their antistatic function through mechanisms such as reducing the surface or volume resistivity of the material, increasing charge migration channels, and improving conductivity or hygroscopic conductivity. Exemplary antistatic agents include, but are not limited to, the following categories: ionic or hygroscopic low-molecular-weight compounds, such as quaternary ammonium salts, sulfonates, fatty acid esters, ethoxylated amines, etc., which typically migrate easily to the material surface and form a conductive layer by adsorbing ambient moisture; conductive polymers, including intrinsically conductive polymers (e.g., polyaniline, polypyrrole, etc.) and their doped systems; conductive fillers, such as carbon-based materials (e.g., carbon black, carbon fiber, carbon nanotubes, graphene), metal powders, metal oxides (e.g., antimony tin oxide), etc., which achieve volume conductivity and electrostatic dissipation by forming conductive pathways in the matrix; functional ionic media, such as ionic liquids, solid electrolytes, etc., which provide ion migration channels to reduce resistance; and composite antistatic systems, obtained by compounding any two or more of the aforementioned antistatic components.
[0032] Multi-walled carbon nanotubes (MWCNTs) are hollow tubular nanomaterials composed of two or more concentric cylindrical graphene layers. MWCNTs typically have diameters on the nanometer scale and lengths on the micrometer scale or longer, exhibiting extremely high aspect ratios. MWCNTs can form highly efficient and non-migrating three-dimensional conductive networks within a material matrix through interlocking, providing continuous electron migration pathways for electrostatic charges, significantly reducing the material's volume resistivity, and thus achieving rapid and long-lasting electrostatic dissipation.
[0033] "Composite yarn" refers to yarn composed of two or more different materials. "Core-sheath structure" refers to the concentric wrapping structure of a composite yarn, including a core layer (innermost layer) and a sheath layer (outermost layer), and optionally one or more intermediate layers between the core and sheath layers. The core-sheath structure integrates the performance advantages of different materials into a single yarn, achieving a combination of multiple functional or mechanical properties within a single yarn structure. The sheath layer can be a continuous, complete wrapping layer, or a discontinuous or segmented wrapping layer. "Core material" refers to the material constituting the core layer, primarily contributing to the basic mechanical properties of the yarn (e.g., tensile strength, elastic recovery, and overall strength). "Sheath material" refers to the material constituting the sheath layer, primarily contributing to the surface properties of the yarn (e.g., feel, appearance, dyeability) and additional surface functionalities (e.g., antibacterial properties, UV protection, antistatic properties). The properties, thickness, and interfacial bonding between the sheath material and the core material can also regulate the overall mechanical and performance properties of the yarn.
[0034] A "coating die" is an extrusion molding assembly used to form a coating layer around a core material by depositing molten coating material (such as a skin material). The coating die has internal channels or openings to guide the flow of the molten material. The cross-sectional shape of the coating die can be designed as a cross, Y, triangle, polygon, circle, ellipse, or other regular or irregular geometry. The "center of the coating die" is not limited to the strict geometric center of the component, but refers to the axial area through which the core material passes and receives the molten coating. A cross-shaped coating die has a four-way symmetrical channel design, which not only allows the melt to act uniformly and synchronously around the core material, but also helps maintain the centered position of the core material during the coating process, thereby ensuring the uniformity of the yarn's mechanical properties.
[0035] 2. Implementation Plan One embodiment of this application is as follows: A method for preparing a core-sheath structure thermoplastic polyurethane-coated yarn includes the following steps: S1. The mixture of TPU and functional additives is melt-extruded to obtain TPU melt; S2. The TPU melt is conveyed to the coating die head; S3. Pass the core material through the center of the coating die head, so that the TPU melt surrounds the core material to form a complete coating layer, and obtain TPU melt-coated yarn; S4. Cool the TPU melt-coated yarn to obtain the core-sheath structure thermoplastic polyurethane-coated yarn.
[0036] In some specific implementations, the Shore hardness of the TPU is 80-95A.
[0037] In some specific implementations, the Shore hardness of the TPU is 85A.
[0038] In some specific implementations, the TPU has a Shore hardness of 90A.
[0039] In some specific implementations, the functional additive includes one or more antibacterial agents.
[0040] In some specific implementations, the functional additives include one or more antistatic agents.
[0041] In some specific implementations, the functional additive consists of an antibacterial agent and an antistatic agent.
[0042] In some specific embodiments, the antibacterial agent comprises one or more nano-metal oxides; wherein each nano-metal oxide is optionally surface-modified.
[0043] In some specific implementations, each nanometal oxide is independently nanozinc oxide, nano copper oxide, nano titanium dioxide, nano zirconium dioxide, or nano tin dioxide.
[0044] In some specific implementations, the surface modification uses a silane coupling agent as the modifier.
[0045] In some specific embodiments, the silane coupling agent is N-(2-aminoethyl)-3-aminopropyltrimethoxysilane.
[0046] In some specific implementations, the antibacterial agent consists of a surface-modified nano-metal oxide.
[0047] In some specific implementations, the average particle size of the surface-modified nano-metal oxide is 20-50 nm.
[0048] In some specific implementations, the amount of antibacterial agent used is 5-9 wt% of the TPU amount.
[0049] In some specific implementations, the antistatic agent is carbon nanotubes or graphene.
[0050] In some specific implementations, the antistatic agent is a multi-walled carbon nanotube.
[0051] In some specific implementations, the amount of antistatic agent is 0.5-2 wt% of the TPU amount.
[0052] In some specific implementations, the TPU and functional additives are dried separately or simultaneously before use; the drying is preferably carried out at 75-95°C; and the drying time is preferably 4-6 hours.
[0053] In some specific embodiments, the melt extrusion is carried out at a temperature below 200°C, preferably 160-195°C.
[0054] In some specific implementations, the packaging mold head is any one of the following shapes: cross-shaped, Y-shaped, regular pentagon, regular hexagon, circular, and elliptical, preferably cross-shaped or Y-shaped.
[0055] In some specific implementations, the TPU melt is delivered to the coating die head via a metering pump.
[0056] In some specific implementations, the core material is composed of one or more synthetic fibers.
[0057] In some specific implementations, the synthetic fiber is polyester or nylon.
[0058] In some specific implementations, the linear density of the core layer material is 50-300D, preferably 75-150D.
[0059] In some specific implementations, the core material has 24-288F monofilaments, preferably 36-96F.
[0060] In some specific implementations, the core material has specifications of 75D / 36F or 150D / 96F.
[0061] In some specific implementations, the core material is preheated before use.
[0062] In some specific implementations, the preheating treatment is carried out at 60-90°C.
[0063] In some specific implementations, the core material is cleaned before use.
[0064] In some specific implementations, the cleaning process includes dust removal and / or degreasing.
[0065] In some specific implementations, the core material passes through the center of the covering die head under constant tension; the tension is preferably 5-80 cN, more preferably 8-50 cN.
[0066] In some specific implementations, the cooling of the TPU melt-coated yarn is carried out at 5-20°C.
[0067] One embodiment of this application is as follows: A core-sheath structure thermoplastic polyurethane-coated yarn is obtained by any of the aforementioned methods for preparing core-sheath structure thermoplastic polyurethane-coated yarns.
[0068] In some specific implementations, the weight of the sheath layer of the thermoplastic polyurethane-coated yarn with the sheath-core structure accounts for 15-35% of the total weight of the yarn, preferably 20-30%.
[0069] One embodiment of this application is as follows: Application of any of the aforementioned core-sheath structure thermoplastic polyurethane-coated yarns in textile manufacturing.
[0070] In some specific implementations, the textile has at least one of the following functions: antibacterial, UV resistant, odor-resistant, and antistatic.
[0071] In some specific implementations, the textiles simultaneously possess antibacterial, UV-resistant, odor-resistant, and antistatic properties.
[0072] In some specific implementations, the textiles are clothing, outdoor or sports equipment, home textile products, industrial textiles, or functional technical fabrics.
[0073] In some specific implementation schemes, the clothing may be casual wear, sportswear, work clothes, underwear, or children's clothing.
[0074] In some specific implementations, the outdoor or sports equipment includes backpacks, tents, sunshades, waterproof jackets, or sports protective gear.
[0075] In some specific implementations, the household textile products are bedding, curtains, furniture coverings or decorative fabrics, carpets or towels.
[0076] In some specific implementations, the industrial textiles are filter materials, conveyor belts, tarpaulins, or industrial wiping cloths.
[0077] In some specific implementations, the technical functional fabric is a medical protective textile, antistatic clothing, UV-resistant shielding material, or smart textile. 3. Detailed Implementation The raw materials used in this application can be purchased or synthesized in-house. The following specific embodiments are used to further describe the implementation of the present invention and do not limit the scope of the invention.
[0079] Example 1 75D / 36F polyester yarn is passed through a tension controller via a 90°C preheated roller and then through a cross-shaped wrapping die. TPU particles (Covestro Texin 985, Shore A hardness 85A) are mixed with nano-zinc oxide (average particle size 40 nm) modified with a silane coupling agent (N-(2-aminoethyl)-3-aminopropyltrimethoxysilane), wherein the amount of nano-zinc oxide is 5% of the amount of TPU and the amount of multi-walled carbon nanotubes is 2% of the amount of TPU. After drying the TPU mixture at 75℃ for 5 hours, it was fed into a single-screw extruder (temperature settings: zone 1 165℃, zone 2 180℃, zone 3 190℃, die head 195℃) for melt extrusion. The screw speed of the single-screw extruder was controlled at 40-50 rpm, and the traction speed was controlled at 180-220 m / min, so that the TPU melt uniformly coated the surface of the core yarn. The resulting TPU sheath layer accounted for approximately 20% of the total weight of the composite yarn. The TPU melt was pumped into the coating die. The screw speed and traction speed were adjusted, and the yarn dryness was maintained uniformly using a diameter gauge. After cooling in a 20℃ water bath, the coated yarn was dried, oiled, and wound up to obtain a multifunctional core-sheath structure thermoplastic polyurethane coated yarn. Testing showed that the surface of the coated yarn was continuous and intact, with no obvious core exposure or glue breakage. It exhibited good softness, resilience, and abrasion resistance, and also possessed excellent antibacterial, deodorizing, UV-resistant, and antistatic properties.
[0080] Example 2 150D / 96F nylon yarn is passed through a tension controller via a 60°C preheated roller and then through a cross-shaped wrapping die. TPU granules (BASF Elastollan B, Shore A hardness 90A) are mixed with silane coupling agent-modified nano-zinc oxide (average particle size 40 nm), where the amount of nano-zinc oxide is 9% of the TPU amount, and the amount of multi-walled carbon nanotubes is 0.5% of the TPU amount. After drying the TPU mixture at 75°C for 5 hours, the extruder screw speed is controlled at 35–45 rpm, and the traction speed is controlled at 170–190 m / min. The resulting TPU sheath accounts for approximately 25% of the total weight of the composite yarn and is fed into a single-screw extruder (temperature settings: zone 1 160°C, zone 2 175°C, zone 3 185°C, die head 190°C) for melt extrusion. The TPU melt is then pumped into the wrapping die via a metering pump. The screw speed and traction speed are adjusted, and the yarn uniformity is maintained using a diameter gauge. After being cooled in a 5°C water bath, the coated yarn is dried, oiled, and wound up to obtain a multifunctional thermoplastic polyurethane-coated yarn with a core-sheath structure. The resulting yarn has a uniform and continuous coating layer that is firmly bonded to the core layer, exhibiting high abrasion resistance and dimensional stability, while maintaining excellent antibacterial, deodorizing, UV-resistant, and antistatic properties.
[0081] Example 3 100D / 48F polyester filament was selected as the core layer material. The core layer yarn was regulated by a tension controller, passed through an 80℃ preheated roller, and then through a cross-shaped covering die. The TPU granules were made of polyether-type TPU with a Shore hardness of 90A, mixed with silane coupling agent-modified nano-zinc oxide, where the amount of nano-zinc oxide was 7% of the TPU mass, and the amount of multi-walled carbon nanotubes was 1% of the TPU mass. The mixed TPU material was dried at 75℃ for 5 hours and then fed into a single-screw extruder. The temperatures in each zone were controlled at 165℃, 180℃, 188℃, and the die head at 193℃ for melt extrusion. The TPU melt was delivered to the covering die by a metering pump and uniformly coated onto the surface of the core layer yarn. The resulting sheath layer accounted for approximately 25% of the total weight of the composite yarn. After being cooled in a 15℃ circulating cooling water bath, the yarn was dried, oiled, and wound to obtain a multifunctional core-sheath structure thermoplastic polyurethane-coated yarn. Testing revealed that the resulting yarn exhibits uniform coverage, good softness, resilience, and overall mechanical properties, while also maintaining excellent antibacterial and antistatic properties.
[0082] Example 4 75D / 48F nylon 66 filament was selected as the core layer material. The core layer yarn was preheated at 70℃ and then passed through a cross-shaped covering die. The TPU used was a Shore A hardness 85A polyether-type TPU, with silane coupling agent-modified nano-zinc oxide and nano-titanium dioxide added as composite antibacterial agents. The mass ratio of nano-zinc oxide to nano-titanium dioxide was 2:1, and the total addition amount was 8% of the TPU mass. 0.8% graphene was also added. After uniform mixing, the mixture was dried at 75℃ for 5 hours, followed by melt coating (under the same conditions as in Example 1). The resulting sheath layer accounted for approximately 25% of the total weight of the composite yarn. The coated yarn was cooled with circulating water at 10℃ and then wound into shape. The resulting TPU-coated yarn has a continuous and intact sheath layer, exhibiting excellent antibacterial properties, as well as good UV shielding and antistatic properties, making it suitable for outdoor sports and functional protective fabrics.
[0083] Example 5 150D / 96F polyester filament was selected as the core layer material. The core layer yarn was preheated at 70℃ and then passed through a cross-shaped covering die. The TPU used was a 90A Shore A polyester TPU, with silane coupling agent-modified nano-copper oxide added as an antibacterial agent at 6% of the TPU mass, along with 1.5% multi-walled carbon nanotubes. The mixture was dried at 75℃ for 5 hours and then melt-coated (under the same conditions as in Example 1). The weight of the sheath layer was controlled to be approximately 30% of the total yarn weight. After cooling with circulating water at 10℃, the yarn was wound to obtain the TPU-coated yarn. The resulting yarn exhibits high abrasion resistance and bending resistance, while maintaining excellent antibacterial, deodorizing, and antistatic effects, making it suitable for shoe uppers, bag fabrics, and highly abrasion-resistant functional textiles.
[0084] Example 6 75D / 36F polyester filament was selected as the core material. The core yarn was preheated at 80℃ and then passed through a Y-shaped covering die. The TPU used was a Shore A 80A polyether-type TPU, with 5% nano-zinc oxide modified with a silane coupling agent and 1% graphene added. After uniform mixing, it was dried at 75℃ for 5 hours, followed by melt coating (under the same conditions as in Example 1). The sheath layer accounted for approximately 20% of the total yarn weight. After cooling with circulating water at 10℃, drying, and winding, the TPU-coated yarn was obtained. The resulting yarn has a softer hand feel and excellent elastic recovery properties, while also possessing antibacterial, deodorizing, UV-resistant, and antistatic properties, making it suitable for close-fitting clothing, sports knitwear, and elastic fabrics.
[0085] Example 7 100D / 72F nylon 6 filament was selected as the core material and preheated at 75℃ before being passed through a Y-shaped covering die. The TPU used was a polycarbonate-type TPU with a Shore hardness of 88A, with silane coupling agent-modified nano-tin dioxide added as an antibacterial agent at 6.5% of the TPU mass, along with 1.2% multi-walled carbon nanotubes. The mixture was dried at 80℃ for 5 hours and then melt-extruded using a single-screw extruder, with temperatures controlled at 165℃, 178℃, 188℃, and 192℃ at the die head. The TPU melt was metered and pumped to the covering die, with the sheath layer accounting for approximately 30% of the total yarn weight. The covered yarn was cooled in a 12℃ circulating cooling water bath, dried, oiled, and wound up. The resulting TPU sheath layer was continuous and uniform, firmly bonded to the core layer, and exhibited excellent hydrolysis resistance, antibacterial properties, and antistatic properties, making it suitable for outdoor footwear and functional protective fabrics.
[0086] Comparative Example 1 75D / 36F polyester filament of the same specifications as in Example 1 was selected as the core layer material. The TPU used was the same polyether-type TPU as in Example 1, with a Shore hardness of 85A. However, no antibacterial agents were added; only 2 wt% of multi-walled carbon nanotubes were added. The remaining preparation process was the same as in Example 1. Performance testing was performed on the obtained TPU-coated yarn. The results showed that the obtained yarn still had good coating integrity and mechanical properties, but its inhibitory ability against Staphylococcus aureus and Escherichia coli was significantly reduced.
[0087] Comparative Example 2 The same raw materials and processes as in Example 1 were used, but multi-walled carbon nanotubes were not added. Instead, 5 wt% of silane coupling agent was added to modify nano-zinc oxide, while the other preparation conditions remained the same. The resulting TPU-coated yarn exhibited good antibacterial properties, but its surface resistivity was significantly increased, and its static dissipation ability decreased.
[0088] Comparative Example 3 The same core material and TPU as in Example 1 were used, but no functional additives were added to the TPU; only ordinary TPU melt coating was performed. The resulting yarn has basic softness and abrasion resistance, but its antibacterial, deodorizing, antistatic, and UV-resistant properties are significantly lower than those of the Example 1.
[0089] Comparative Example 4 Using 75D / 36F polyester filament of the same specifications as in Example 1, the yarn was impregnated with a finishing solution containing 5 wt% nano zinc oxide and 1 wt% antistatic agent. After drying and setting, the functional yarn was obtained. Testing showed that the initial antibacterial performance was high, but the antibacterial rate decreased significantly, and the antistatic performance decreased rapidly, indicating that the functional layer obtained after finishing was prone to peeling off and had poor durability.
[0090] Example 8 In this embodiment, the yarns prepared in the aforementioned embodiments and comparative examples were subjected to mechanical property tests, and knitted into standard-sized samples under the same weaving process for functional index testing and durability testing after 20 standard washes. All performance tests were conducted in accordance with the relevant national or industry standards. Specifically, antibacterial properties were tested according to GB / T 20944.3, UV resistance was tested according to GB / T 18830, and surface resistivity was tested according to GB / T 12703.4. Each test was performed in parallel at least three times, and the data listed in Table 1 are the average of the three test results.
[0091] Table 1. Performance Test Results
[0092] As shown in Table 1, the TPU-coated yarn provided in this application, while maintaining the excellent mechanical properties of the core material, achieves a synergistic improvement in multiple functions such as antibacterial, antistatic, UV protection, and deodorization by introducing antibacterial and antistatic agents into the TPU skin layer. Example 4, due to the use of a nano-zinc oxide and nano-titanium dioxide composite system, achieved the highest UPF (ultraviolet resistance) value; Example 5, using nano-copper oxide as an antibacterial agent, maintained excellent antibacterial properties while exhibiting better abrasion resistance; Example 6, using low-hardness polyether-type TPU and a Y-shaped coating die, resulted in superior softness and elastic recovery. In contrast, Comparative Example 1 lacked an antibacterial agent, resulting in a significant decrease in antibacterial performance; Comparative Example 2 lacked conductive fillers, leading to an increase in surface resistivity of approximately five orders of magnitude; Comparative Example 3 did not add any functional additives and only possessed the basic properties of ordinary TPU-coated yarn; Comparative Example 4, using a traditional finishing process, although exhibiting good initial antibacterial performance, showed a significant decrease in antibacterial rate after 20 washes, indicating that its durability was far lower than that of the solution in this application. Therefore, this application achieves a balance between mechanical properties and multiple functions by using a TPU skin to stably encapsulate functional additives, and also has excellent durability and industrial application value.
[0093] This invention does not impart yarn functionality through fabric finishing or functional sizing coating. Instead, it uses a continuous TPU sheath as a functional carrier to stably retain functional additives within the sheath. Through a core-sheath structure, it achieves a partitioned design where the core layer provides mechanical properties and the sheath layer provides functional properties, thereby obtaining a covered yarn that is both durable and multifunctional.
[0094] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention without departing from the principles and spirit of the present invention.
Claims
1. A method for preparing a core-sheath structure thermoplastic polyurethane-coated yarn, characterized in that, Includes the following steps: S1. After mixing thermoplastic polyurethane with functional additives, melt extrusion is carried out at a temperature below 200°C to form TPU melt; S2. The TPU melt is conveyed to the coating die head; S3. Pass the core material through the center of the coating die head, so that the TPU melt continuously coats the core material and forms a complete skin layer, thereby obtaining a TPU-coated yarn with a skin-core structure. The functional additives are distributed in the dermis; S4. Cool and solidify the core-sheath structure yarn to obtain the core-sheath structure thermoplastic polyurethane-coated yarn.
2. The preparation method according to claim 1, characterized in that, The functional additives include an antibacterial agent, which is a nano-metal oxide modified with a silane coupling agent. The silane coupling agent is N-(2-aminoethyl)-3-aminopropyltrimethoxysilane. The average particle size of the nano-metal oxide is 20-50 nm. The amount of the antibacterial agent is 5-9 wt% of the amount of thermoplastic polyurethane.
3. The preparation method according to claim 1, characterized in that, The functional additives include an antistatic agent, which is a carbon nanotube or graphene, and the amount of the antistatic agent is 0.5-2 wt% of the amount of thermoplastic polyurethane.
4. The preparation method according to claim 1, characterized in that, The melt extrusion is carried out at a temperature of 160-195°C.
5. The preparation method according to claim 1, characterized in that, The cross-sectional shape of the covering mold head is cross-shaped or Y-shaped.
6. The preparation method according to claim 1, characterized in that, The core material is preheated before use, and the preheating treatment is carried out at 60-90°C.
7. The preparation method according to claim 1, characterized in that, The core material is polyester or nylon.
8. A core-sheath structure thermoplastic polyurethane-coated yarn, characterized in that, The yarn is obtained by the method for preparing the core-sheath structure thermoplastic polyurethane-coated yarn according to any one of claims 1-7.
9. The core-sheath structure thermoplastic polyurethane-coated yarn according to claim 8, characterized in that, The weight of the sheath layer in the thermoplastic polyurethane-coated yarn with a sheath-core structure accounts for 15-35% of the total weight of the yarn.
10. The application of the core-sheath structure thermoplastic polyurethane-coated yarn of claim 8 in the preparation of textiles.
Citation Information
Patent Citations
Modified thermoplastic polyurethane coated yarn and preparation method thereof
CN111394848A