Layered composite fabrics, their preparation methods and textiles
By using a layered composite fabric structure and the synergistic design of a through-capillary array and breathable pores, the shortcomings of the fabric in terms of moisture absorption and perspiration wicking, breathability and heat dissipation, and softness and comfort are solved, and the stability and comfort of the fabric are achieved after washing and stretching.
Patent Information
- Application Number
- CN202611511793.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing fabrics cannot simultaneously achieve moisture wicking, breathability, heat dissipation, and soft comfort. The pore response of irregularly shaped fibers is slow, and the pores of traditional woven fabrics are prone to deformation or tearing after washing and stretching.
The fabric adopts a layered composite structure, including a first weft-knitted fabric layer, a second weft-knitted fabric layer and an intermediate layer. The intermediate layer is connected to the two weft-knitted fabric layers to form a through-capillary array and ventilation holes. The ventilation holes are formed by the surrounding yarns being drawn together by floats. The floats are fixed to the loops of the loop or tucked structure, and the connecting area provides support.
It enables rapid migration and evaporation of sweat without external mechanical pressure, maintains the stability of the pore edges, and balances moisture absorption and wicking, breathability and heat dissipation, soft and comfortable feel, and dimensional stability.
Smart Images

Figure CN123108818A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of textile technology, and in particular to a layered composite fabric, its preparation method, and textile products. Background Technology
[0002] As consumers continue to demand higher sleep quality, the functional needs of home textile fabrics are becoming increasingly prominent. Summer bedding fabrics need to meet the following core requirements simultaneously: moisture wicking – quickly wicking away body sweat to keep the fabric dry; breathability and heat dissipation – promoting air circulation and reducing the perceived temperature upon contact; softness and comfort – the fabric can conform to the body's curves while also possessing good durability.
[0003] However, existing fabrics often struggle to simultaneously achieve moisture wicking, breathability, heat dissipation, and softness and comfort.
[0004] For example, related technologies often utilize the capillary effect of irregularly shaped fibers such as cross-shaped and Y-shaped fibers to impart moisture-wicking properties to fabrics. However, the opening of the pores of irregularly shaped fibers depends entirely on the increase of ambient temperature and humidity. At normal temperatures or during the initial stage of sweating, the pores of irregularly shaped fibers remain closed, failing to provide immediate and continuous efficient air convection. This passive response mechanism exhibits a significant lag in breathability and heat dissipation during periods of heavy sweating in summer, easily leading to a stuffy feeling. Furthermore, compared to round cross-section fibers, irregularly shaped fibers have a higher specific surface area, resulting in higher contact friction and cohesion between fibers. The relative sliding space of fibers within the yarn is restricted, making it difficult for the fabric to undergo soft deformation, resulting in a stiffer feel that fails to meet the softness requirements of home textile products.
[0005] Another related technology involves alternating loop-forming and loop-gathering knitting on a double-sided circular knitting machine, causing some loops to stretch and suspend, thereby forming tiny mesh holes on both sides of the fabric. However, the edges of the mesh holes are formed naturally only by the stretched loops. After the fabric undergoes multiple washes and tumbling or daily stretching, the yarns at the edges of the ventilation holes are prone to slippage, causing the hole shape to become unstable and the hole diameter to continuously expand, making it difficult to maintain dimensional stability.
[0006] In summary, there is an urgent need for a composite fabric that can balance moisture wicking, breathability and heat dissipation, softness and comfort, and dimensional stability of weft-knitted fabrics. Summary of the Invention
[0007] This application provides a layered composite fabric, its preparation method, and a textile to solve the above-mentioned problems.
[0008] To achieve the above objectives, the technical solution of this application is as follows: The first aspect of this application provides a layered composite fabric, comprising: The first weft-knitted fabric layer and the second weft-knitted fabric layer, both of which have loops and loops; An intermediate layer is located between the first weft-knitted fabric layer and the second weft-knitted fabric layer. At multiple connection areas, the intermediate layer is connected to the first weft-knitted fabric layer and the second weft-knitted fabric layer. The intermediate layer has a tucked structure and a looped structure. The tucked structure includes loops and suspension arcs. The suspension arcs of adjacent rows of tucked structures are staggered and superimposed along the thickness direction to form a capillary array that runs through the thickness direction. The first weft-knitted fabric layer, the intermediate layer, and / or the second weft-knitted fabric layer are all covered with ventilation holes. The ventilation holes are formed by pulling the surrounding yarns together with floats. The two ends and the middle of the floats are fixed to the root of the loop post of the corresponding fabric layer or the loop of the tucked structure. If adjacent fabric layers are covered with the ventilation holes, the ventilation holes penetrate the adjacent corresponding fabric layers.
[0009] In one embodiment of this application, the layered composite fabric satisfies at least one of the following requirements (1)-(3): (1) The equivalent diameter of the capillary is 10-300 μm, preferably 50-150 μm; (2) The pore size of the vent is 0.8-4.0 mm, preferably 1.2-2.5 mm; (3) The equivalent diameter of the connecting area is 1-5 mm.
[0010] In one embodiment of this application, the layered composite fabric satisfies at least one of the following (4)-(6): (1) At all the connection areas, the looped arc of the intermediate layer is connected to the looped arc of the first weft knitted fabric layer and the second weft knitted fabric layer, thus connecting the intermediate layer with the first weft knitted fabric layer and the second weft knitted fabric layer. (2) At all the said connecting areas, the intermediate layer is connected to the first weft-knitted fabric layer and the second weft-knitted fabric layer by connecting yarn; (3) Along the direction from the center to the edge of the ventilation hole, the intermediate layer is divided into a first area and a second area. The distribution density of the tucked structure in the first area is greater than that in the second area. At all the connecting areas, the hanging arc of the tucked structure in the first area is connected to the loop arc of the first weft-knitted fabric layer and the second weft-knitted fabric layer, connecting the intermediate layer with the first weft-knitted fabric layer and the second weft-knitted fabric layer. Alternatively, at all the connecting areas in the first area, the intermediate layer is connected to the first weft-knitted fabric layer and the second weft-knitted fabric layer through the connecting yarn.
[0011] In one embodiment of this application, the spacing between adjacent connecting areas is 5-30 mm.
[0012] In one embodiment of this application, one set of the connecting regions is distributed every 2-10 horizontal columns along the longitudinal direction, or arranged in a linear array along the transverse direction, and / or one set of the connecting regions is distributed every 3-15 vertical columns along the transverse direction, or arranged in a linear array along the vertical direction.
[0013] In one embodiment of this application, the distribution density of the clustered organization is 3-8 rows / 10mm in the longitudinal direction and 3-8 columns / 10mm in the transverse direction.
[0014] In one embodiment of this application, the distribution density of the air pores is 4-25 pores / cm², preferably 6-16 pores / cm².
[0015] A second aspect of this application also provides a method for preparing the layered composite fabric as described above, comprising the following steps: S1. A raw fabric comprising a first weft-knitted fabric layer, an intermediate layer, and a second weft-knitted fabric layer is woven using an integrated weaving process; S2. The raw fabric is pre-shaped and post-shaped to obtain the layered composite fabric.
[0016] In one embodiment of this application, in step S2, the predetermined temperature is 150-180°C and the duration is 30-60 seconds.
[0017] A third aspect of this application also provides a textile product comprising the layered composite fabric described above.
[0018] The technical solution provided in this application has at least the following beneficial effects: In this application, a stable layered structure is constructed by setting an intermediate layer between the first and second weft-knitted fabric layers and connecting the three layers together at multiple connection areas. The suspended arcs of adjacent rows of looped fabrics in the intermediate layer are staggered and superimposed along the thickness direction, forming a capillary array that extends throughout the thickness direction. This micron-scale capillary array can drive the wicking of sweat from the skin-contact side without external mechanical pressure, causing it to rapidly migrate to the outer layer of the fabric and evaporate.
[0019] In this application, the first weft-knitted fabric layer, the intermediate layer, and / or the second weft-knitted fabric layer are all covered with breathable holes, and the breathable holes are an integrally formed structure created by the surrounding yarns being pulled together by float yarns. This purely physical weaving method avoids the cutting of yarn fibers by traditional finishing punching processes, reduces burrs and molten hard edges at the edges of the breathable holes, and makes the fabric have excellent softness and comfort when worn against the skin. At the same time, the breathable holes provide macroscopic micro-convection air channels inside the fabric, allowing sweat introduced into the outer layer to quickly vaporize and be expelled, forming a heat dissipation chain of convection, wicking, and evaporation, thereby improving the breathability and heat dissipation of the fabric.
[0020] In this application, the two ends and the middle of the float are firmly fixed to the root of the loop post or the loop of the tucked structure in the corresponding fabric layer, forming a microscopic anchoring structure. This anchoring structure locks the float across the loop base, so that when the fabric is subjected to tensile load, the stress is transmitted along the float to the anchor points of the loop post at both ends and the middle, and then dispersed to the surrounding area through the anchor points, reducing the probability of stress concentration. Therefore, after repeated washing and daily stretching, the yarns at the edges of the vent holes are less likely to slip, reducing the risk of hole enlargement or tearing, and ensuring the dimensional stability and hole shape stability of the fabric after washing.
[0021] In summary, weft-knitted fabrics impart softness and comfort. The capillary array forms a pathway for liquid water transfer, the pores create pathways for air and moisture transfer, and the connecting areas form pathways for load transfer. Sweat can enter the evaporation area through the capillary array, air can contact the evaporation area through the pores, and external forces are dispersed to the surrounding coils through the connecting areas. These three pathways coexist synergistically in space, and combined with weft-knitted fabrics, they achieve a balance of moisture wicking, breathability, heat dissipation, softness and comfort, and dimensional stability. Attached Figure Description
[0022] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application. It is obvious that the drawings described below are merely some embodiments of this application, and those skilled in the art can obtain other drawings based on these drawings without any inventive effort.
[0023] In the attached diagram: Figure 1 A schematic diagram of the structure of a layered composite fabric provided in one embodiment of this application; Figure 2 This is a schematic diagram of the structure of the ring column and ring arc in this application; Figure 3 This is a schematic diagram of the structure of the clustered and looped structures in this application; Figure 4 A schematic diagram of the cluster organization structure in this application; Figure 5 This is a schematic cross-sectional view of the capillary in this application (cut along the fabric thickness direction); Figure 6 This is a top view of the capillary in this application (viewed from above along the fabric thickness direction). Figure 7 This is a schematic diagram of the wicking principle of the capillary tube in this application; Figure 8 A schematic diagram of the structure of a layered composite fabric provided in another embodiment of this application; Figure 9 This is a schematic diagram of the connection between the intermediate layer and the first weft-knitted fabric layer and the second weft-knitted fabric layer according to an embodiment of this application; Figure 10 A schematic diagram illustrating the connection between the intermediate layer and the first and second weft-knitted fabric layers, provided for another embodiment of this application; Figure 11 This is a schematic diagram illustrating the connection between the intermediate layer and the first and second weft-knitted fabric layers, as provided in another embodiment of this application.
[0024] The attached figures are labeled as follows: First weft knitted fabric layer 1, loop column 11, loop arc 12; Intermediate layer 2, coiled structure 21, coil 211, suspension arc 212, looping structure 22, capillary 23, first zone 24, second zone 25; Second weft-knitted fabric layer 3; Connecting yarn 4; 5 vent holes. Detailed Implementation
[0025] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of the embodiments. Based on the embodiments of this application, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of this application.
[0026] In this application, unless otherwise expressly specified and limited, the terms "connection," "fixed," etc., should be interpreted broadly. For example, "fixed" can mean a fixed connection, a detachable connection, or an integral part; it can mean a mechanical connection or an electrical connection; it can mean a direct connection or an indirect connection through an intermediate medium; it can mean the internal communication of two components or the interaction between two components, unless otherwise expressly limited. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances. The term "multiple" means at least two.
[0027] In related technologies, perforation methods such as mechanical punching and laser perforation are commonly used to create holes in weft-knitted fabrics. However, the hole-forming process alters the continuous interlocking relationship between the original loops. After the yarn is cut, the force at the edge of the hole cannot continue to be transmitted along the complete loop, making the yarn prone to slippage during washing and stretching. Secondly, the yarn at the hole is cut, resulting in burrs and exposed fibers, which can easily cause skin irritation. Simultaneously, during washing, the cut yarn is easily loosened and slipped under the influence of water flow and friction, causing the holes to gradually enlarge, deform, or even tear after a period of use. Furthermore, traditional punching is affected by factors such as equipment precision, fabric tension, and tool wear, resulting in a hole diameter tolerance typically exceeding ±0.3mm, making it difficult to precisely control the accuracy of the ventilation holes. To achieve breathability, traditional jacquard mesh fabrics often require increased hole size, which reduces the contact area between the fabric and the skin, resulting in a rougher feel.
[0028] In this application, "equivalent diameter" is the diameter obtained by converting a non-circular channel according to an equivalent flow scale.
[0029] In this application, "middle" refers to the area between the two endpoints of the float.
[0030] like Figure 1 As shown, one embodiment of this application provides a layered composite fabric, including a first weft-knitted fabric layer 1, an intermediate layer 2, and a second weft-knitted fabric layer 3. The first weft-knitted fabric layer 1 corresponds to the surface layer, and the second weft-knitted fabric layer 3 corresponds to the bottom layer. Figure 2 As shown, the first weft-knitted fabric layer 1 has loops 11 and loops 12 formed by bending and interlacing yarns, which together form complete loops. The second weft-knitted fabric layer 3 also has loops 11 and loops formed by bending and interlacing yarns. The intermediate layer 2 is located between the first weft-knitted fabric layer 1 and the second weft-knitted fabric layer 3. At multiple connection areas, the intermediate layer 2 is connected to the first weft-knitted fabric layer 1 and the second weft-knitted fabric layer 3, thereby forming a layered composite structure.
[0031] like Figure 1As shown, the first weft-knitted fabric layer 1 can be constructed using a weft-knitted plain knit, 1+1 rib, or 2+2 rib weave, and the second weft-knitted fabric layer 3 can be constructed using a weft-knitted plain knit, 1+1 rib, or satin weave. The first weft-knitted fabric layer 1 can be made of fiber filaments with a fineness of 50-75D. The fiber filaments can be made of polyester or polyamide fibers. For example, the first weft-knitted fabric layer 1 can be formed using knitting equipment with a gauge of E24-E28. Polyester or nylon filaments form a relatively smooth outer surface, which helps reduce pilling and maintain the smoothness of the outer surface. The second weft-knitted fabric layer 3 can be made of moisture-wicking fiber yarn with a fineness of 40-60S. The moisture-wicking fiber yarn can be cotton fiber yarn, modal yarn, bamboo fiber yarn, or a blended yarn formed from at least two of cotton, modal, and bamboo fibers. For example, the second weft-knitted fabric layer 3 can be formed using knitting equipment with a gauge of E24-E28. Moisture-absorbing fiber yarns can absorb moisture from the side that is close to the body and transfer the moisture to the middle layer 2.
[0032] like Figure 3-7 As shown, the intermediate layer 2 has a tucked loop structure 21 and a loop-forming structure 22. The distribution density of the tucked loop structure 21 is 3-8 rows / 10mm in the longitudinal direction and 3-8 columns / 10mm in the transverse direction. The tucked loop structure 21 includes loops 211 and overhangs 212. Specifically, the intermediate layer 2 can adopt a rib tucked loop structure or a double rib tucked loop structure, and adopt a composite circular knitting process of one tucked loop knitting and one loop-forming knitting. The overhangs 212 of the tucked loop structure 21 crosses the corresponding needle position and connects with the loops 211. The height of the tucked loop structure 21 is 1-3 needle lengths, and the length of the overhangs 212 of the tucked loop structure 21 is 0.5-3mm. The overhangs 212 of the tucked loop structure 21 in adjacent rows are staggered and superimposed along the fabric thickness direction, so that the gaps between adjacent overhangs 212 are connected front to back, forming a capillary array that runs through the thickness direction. Specifically, the overhangs 212 of the tucked loop structure 21 are curved and extended in space. After the overhangs 212 of the looped fabric 21 in adjacent rows are misaligned, the local cross-section of the capillary 23 is approximately triangular or elliptical, and this capillary 23 can serve as a channel for sweat to enter and exit. This channel exhibits continuous changes in local convergence and local expansion along the thickness direction, thus forming a "converging-expanding" contraction-expansion flow channel. After sweat enters this channel, it can be conducted to the other side of the fabric along the interconnected tiny gaps. The equivalent diameter of the capillary 23 is 10-300 μm. The capillary pressure difference generated by the capillary 23 can be expressed using the following Young-Laplace capillary pressure formula: ΔP = 2γ·cosθ / r (1); In equation (1), ΔP is the capillary pressure difference, γ is the liquid surface tension, θ is the contact angle between the liquid and the channel wall, and r is the equivalent radius of capillary 23. Under the condition that the liquid properties and contact state are determined, the micron-scale channel can generate capillary suction.
[0033] like Figure 1 As shown, in one embodiment of this application, both the first weft-knitted fabric layer 1 and the intermediate layer 2 are covered with ventilation holes 5. The ventilation holes 5 of the first weft-knitted fabric layer 1 and the intermediate layer 2 correspond to each other in the thickness direction, so that the ventilation holes 5 penetrate through the first weft-knitted fabric layer 1 and the intermediate layer 2. Figure 8 As shown, in another embodiment of this application, both the first weft-knitted fabric layer 1 and the second weft-knitted fabric layer 3 are covered with ventilation holes 5. The ventilation holes 5 are formed by the surrounding yarns being pulled together by floats. When knitting the corresponding hole positions, the predetermined needle does not insert new yarn and does not form new loops 211 (i.e., missing loops), and continuous yarns cross the needle position to form floats. The floats pull on adjacent loops, creating open spaces at the hole positions. In other words, the ventilation holes 5 are formed by the surrounding yarns being pulled together by the floats, i.e., the ventilation holes 5 are formed by the floats hooking the edges. Since the yarns forming the ventilation holes 5 remain continuous, the edges of the ventilation holes 5 do not include broken yarn ends caused by punching or cutting. The two ends and the middle of the floats are fixed to the root of the loop post 11 of the corresponding fabric layer or to the loop 211 of the tuck weave 21. In other words, the two ends and the middle of the floats located on the first weft-knitted fabric layer 1 are fixed to the root of the loop post 11 of the corresponding fabric layer. The floats located on the intermediate layer 2 are fixed at both ends and in the middle to the coils 211 of the loop weave 21. The loop posts 11 and loop arcs 12 form complete coils, thus, in both cases, the floats are fixed at both ends and in the middle to the coils of the corresponding fabric layers. In both cases, a continuous coil-float-coil structure is formed. When the fabric is subjected to transverse or longitudinal stretching, the load borne by the floats can be transferred along the edge of the ventilation holes 5 to adjacent coils, reducing the probability of load concentration on a single cross-section, thereby reducing the risk of hole enlargement during washing or stretching.
[0034] The above structure forms a coordinated heat and mass transfer path. Sweat absorbed by the second weft-knitted fabric layer 3 enters the capillaries 23 and is conducted along the thickness direction to the vicinity of the first weft-knitted fabric layer 1. The vents 5 allow outside air to contact the intermediate layer 2, promoting the evaporation of moisture conducted to the outside. This creates a heat dissipation path that continuously coordinates air convection, capillary conduction, and surface evaporation.
[0035] Compared to weaving followed by mechanical punching or laser perforation, this application eliminates the need to cut the yarn at the edge of the pores during the pore-forming process, thus reducing the risk of broken yarn edges or molten hard edges. For example, under 5x magnification, no burrs or fiber ends formed by cut yarns are observed at the edge of the ventilation hole 5, which helps maintain a soft feel against the skin.
[0036] In this application, air vents 5 are formed by the surrounding yarns being drawn together by floats, and a capillary array is formed by the suspended arcs 212 of the staggered overlapping loop structure 21. Multiple connecting areas maintain interlayer connectivity. The air vents 5 facilitate air convection and moisture evaporation, the capillary array facilitates liquid conduction in the thickness direction, and the connecting areas provide interlayer support and stress dispersion. The combination of these three structures within the same weft-knitted fabric helps to balance breathability and heat dissipation, moisture wicking, dimensional stability after washing, and softness and comfort.
[0037] like Figure 1 As shown, the distribution density of the air pores 5 is 4-25 pores / cm². 2 Preferably 6-16 per cm 2 The ventilation holes 5 can be arranged in a square, rhomboid, hexagonal, or rhythmic checkerboard pattern. Different arrays ensure that the ventilation holes 5 are distributed among the fabric's solid loops 211. During the weaving process, the ventilation holes 5 avoid connecting areas, creating spatial complementarity between the ventilation hole array and the interlayer support array. The ventilation holes 5 create localized air gaps between the fabric and the skin. When the skin and fabric move relative to each other, or when the fabric recovers from pressure, air can exchange between the ventilation holes 5 and the air gaps. The diameter of the ventilation holes 5 is 0.8-4.0 mm. The shape of the ventilation holes 5 can be rhomboid, elliptical, or approximately circular.
[0038] like Figure 1 As shown, a connecting area is distributed every 2-10 transverse rows along the longitudinal direction, or a group of connecting areas arranged in a linear array along the transverse direction. A connecting area is set every 3-15 longitudinal rows along the transverse direction, or a group of connecting areas arranged in a linear array along the longitudinal direction. The longitudinal and transverse array arrangement creates a three-dimensional lattice stress dispersion network for the connecting areas. Under tension or compression, the load can be gradually transferred through the connecting areas on adjacent transverse and longitudinal rows, reducing the probability of a single vent hole 5 edge or a single yarn bearing a concentrated load. The spacing between adjacent connecting areas is 5-30mm. During knitting, the positions of the vent holes 5 and the needle positions of the connecting areas are staggered. The needle positions corresponding to the connecting areas maintain a looping or tucking action, while the needle positions corresponding to the vent holes 5 perform a skipped loop action, thus forming an avoidance zone. The equivalent diameter of the connecting area is 1-5mm. The connecting area connects the first weft-knitted fabric layer 1, the intermediate layer 2, and the second weft-knitted fabric layer 3 in the thickness direction, and provides recovery support after the fabric is compressed. When the connecting area is subjected to normal pressure, the suspension arc 212 or connecting yarn 4 in the connecting area undergoes elastic bending. When the pressure decreases, the suspension arc 212 or connecting yarn 4 releases its elastic deformation, allowing the first weft-knitted fabric layer 1 and the second weft-knitted fabric layer 3 to restore their spacing. When the fabric is subjected to tangential load, multiple connecting areas can jointly restrict the relative movement between layers and transfer the load to the surrounding coils.
[0039] like Figure 9As shown, in one embodiment of this application, the connecting area is formed by alternating connections of tufted weave 21 and looped weave 22. Exemplarily, between the upper needle plate and lower needle cylinder of a double-sided circular knitting machine, tufted weave 21 and looped weave 22 are knitted alternately in a 1:1 or 1:2 ratio, so that adjacent layers of fabric are interconnected by the overhanging arc 212 of the tufted weave 21 and the looping arc 12 of the weft-knitted fabric, forming an integrated three-dimensional sandwich structure. Specifically, at each connecting area, the overhanging arc 212 of the tufted weave 21 of the middle layer 2 is interconnected with the looping arc 12 of the first weft-knitted fabric layer 1 and the second weft-knitted fabric layer 3, thereby connecting the three layers into one.
[0040] like Figure 10 As shown, as an alternative implementation, the connecting area is formed using connecting yarn 4. Specifically, at each connecting area, the connecting yarn 4 shuttles back and forth between the first weft-knitted fabric layer 1, the intermediate layer 2, and the second weft-knitted fabric layer 3, and connects with the loops of the three fabric layers respectively. The path of the connecting yarn 4 can be zigzag-shaped, corresponding to the connecting paths of the tuck weave 21, the loop-forming weave 22, and the tuck weave 21 in sequence. The connecting yarn 4 can be made of polyester low-elasticity yarn with a fineness of 75-150D, or it can be made of spandex core-spun yarn. The input end of the connecting yarn 4 supplies yarn to the knitting area through an independent yarn feeding path. After the connection is completed, the connecting area formed is removed from the machine together with the first weft-knitted fabric layer 1, the intermediate layer 2, and the second weft-knitted fabric layer 3 to form a composite fabric.
[0041] like Figure 11As shown, as an alternative implementation, the connecting area is formed by localized clustered point connections. Specifically, along the direction from the center to the edge of the vent 5, the intermediate layer 2 is divided into a first region 24 and a second region 25. The first region 24 is a reinforced area located around the vent 5, and the second region 25 is a regular area outside the first region 24. The distribution density of the clustered structure 21 in the first region 24 is greater than that in the second region 25. The first region 24 is a region 1-3 mm from the edge of the vent 5, preferably 1.5-2 mm from the edge of the vent 5. The distribution density of the clustered structure 21 in the first region 24 is 6-8 rows / 10 mm longitudinally and 6-8 columns / 10 mm laterally, while the distribution density of the clustered structure 21 in the second region 25 is 3-5 rows / 10 mm longitudinally and 3-5 columns / 10 mm laterally. The loops 212 of the tucked weave 21 in the first zone 24 are interlocked with the loops 12 of the first weft-knitted fabric layer 1 and the second weft-knitted fabric layer 3, forming a local connection at the connecting area. The loops 212 of the higher-density tucked weave 21 constitute a reinforced area around the ventilation hole 5, allowing the tensile load on the ventilation hole 5 to be distributed to the surrounding more loops 211. The second zone 25 maintains a lower distribution density to preserve softness and airflow space. Alternatively, at all connecting areas in the first zone 24, the intermediate layer 2 is connected to the first weft-knitted fabric layer 1 and the second weft-knitted fabric layer 3 via connecting yarns 4. In other words, all connecting areas are located in the first zone 24, meaning the intermediate layer 2 is only connected to the first weft-knitted fabric layer 1 and the second weft-knitted fabric layer 3 in the first zone 24.
[0042] In actual production, any one of the three connection methods can be selected according to the product weight, elastic support and hole reinforcement requirements. The connection methods can also be combined if there is no weaving conflict.
[0043] In this application, a stable layered structure is constructed by setting an intermediate layer 2 between the first weft-knitted fabric layer 1 and the second weft-knitted fabric layer 3, and connecting the three layers together at multiple connection areas. In the intermediate layer 2, the overhanging arcs 212 of adjacent horizontal rows of looped weaves 21 are staggered and superimposed along the thickness direction, forming a capillary array that extends throughout the thickness direction. This micron-scale capillary array can drive the wicking of sweat on the skin-contact side without external mechanical pressure, causing it to rapidly migrate to the outer layer of the fabric and evaporate.
[0044] In this application, the first weft-knitted fabric layer 1, the intermediate layer 2, and / or the second weft-knitted fabric layer 3 are all covered with ventilation holes 5, and the ventilation holes 5 are an integrally formed structure created by pulling the surrounding yarns together with float yarns. This purely physical weaving method avoids the cutting of yarn fibers by traditional finishing punching processes, reduces burrs and molten hard edges at the ventilation hole edges, and makes the fabric have good softness and comfort when worn against the skin. At the same time, the ventilation holes 5 provide macroscopic convection channels for the interior of the fabric, allowing sweat introduced into the outer layer to quickly vaporize and be discharged, forming a heat dissipation link of convection, wicking, and evaporation, thereby improving the breathability and heat dissipation of the fabric.
[0045] In this application, the floats at both ends and the middle are firmly fixed to the roots of the loop posts 11 or the loops 211 of the tucked weave 21 of the corresponding fabric layer, forming a microscopic anchoring structure. This anchoring structure locks the floats across the loop base, so that when the fabric is subjected to tensile loads, the stress is transmitted along the floats to the anchor points of the loop posts at both ends and the middle, or the loops, and then dispersed to the surrounding area through the anchor points, reducing the probability of stress concentration. Therefore, after repeated washing and daily stretching, the yarns at the edges of the vent holes are less likely to slip, reducing the risk of hole enlargement or tearing, and ensuring the dimensional stability and hole shape stability of the fabric after washing.
[0046] In summary, weft-knitted fabrics impart softness and comfort. The capillary array forms a pathway for liquid water transfer, the pores create pathways for air and moisture transfer, and the connecting areas form pathways for load transfer. Sweat can enter the evaporation area through the capillary array, air can contact the evaporation area through the pores, and external forces are dispersed to the surrounding coils through the connecting areas. These three pathways coexist synergistically in space, and combined with weft-knitted fabrics, they achieve a balance of moisture wicking, breathability, heat dissipation, softness and comfort, and dimensional stability.
[0047] Another embodiment of this application provides a method for preparing a layered composite fabric, comprising: S1. A raw fabric consisting of a first weft knitted fabric layer 1, an intermediate layer 2, and a second weft knitted fabric layer 3 is woven using an integrated knitting process; S2. The raw fabric is pre-shaped and post-shaped to obtain a layered composite fabric.
[0048] In this application, during the integrated knitting process, yarns for the first weft knitted fabric layer 1, the intermediate layer 2, the second weft knitted fabric layer 3, and connecting yarn 4 (if necessary) are respectively loaded onto bobbins and fed into corresponding yarn feeding paths. Multiple yarn feeding paths are used for compound knitting involving loop formation, loop gathering, and loop gaps. The first weft knitted fabric layer 1 is formed using yarn, the second weft knitted fabric layer 3 is formed using yarn, and the intermediate layer 2 is formed by alternating loop gathering and loop formation using yarn. When the integrated knitting reaches the needle position corresponding to the ventilation hole 5, the CNC system changes the loop formation command at the predetermined position to a floating yarn command. The corresponding needle retains the old loop 211 without inserting new yarn, and the yarn crosses the needle position to form a loop gap floating yarn edge (i.e., the floating yarn pulls the surrounding yarn to form the ventilation hole 5). Adjacent needle positions perform a tucking action (for the middle layer 2, a tucking action is performed) or a loop forming action (for the first weft knitted fabric layer 1 and / or the second weft knitted fabric layer 3, a loop forming action is performed), so that the two ends and the middle of the float are fixed to the root of the loop post 11 of the corresponding fabric layer or the loop 211 of the tucking organization 21.
[0049] In one embodiment of this application, 1-3 adjacent needles are arranged in a single row containing a missing loop to perform a floating yarn action. A row containing a missing loop is inserted every 2-6 rows of loops. The number of missing loops in a single row accounts for 5%-40% of the total number of needles in that row, and can be controlled within 10%-25%. In both the transverse and longitudinal directions, the knitting program can cycle according to a rhythm of 1-3 missing loops and 4-10 loops. This allows for control of the hole type, hole diameter, and the distribution density of the ventilation holes 5 during the knitting stage. The integrated knitting process simultaneously forms the first weft-knitted fabric layer 1, the intermediate layer 2, the second weft-knitted fabric layer 3, the connecting area, and the ventilation holes 5, resulting in a raw fabric containing the above three layers after knitting. This process eliminates the need for additional mechanical punching, laser perforation, or other steps, reducing damage to the continuous yarn skeleton caused by secondary processing.
[0050] In one embodiment of this application, the pre-setting temperature is 150-180°C, and the duration is 30-60 seconds. The post-setting temperature is 120-180°C, and the duration is 10-30 seconds. Dyeing or printing can be performed as needed, with the dyeing or printing process occurring between the pre-setting and post-setting processes. The dyeing temperature is 90-120°C, the liquor ratio is 1:10-20, and the duration is 30-60 minutes.
[0051] Another embodiment of this application provides a textile product comprising the above-described layered composite fabric, or a layered composite fabric prepared according to the above-described preparation method. The textile product can be a bed sheet, pillowcase, summer quilt, sofa cover, or cushion, or it can be clothing. The layered composite fabric can constitute the entire fabric area of the textile product, or it can constitute localized areas requiring moisture wicking and breathability.
[0052] In summary, the first weft-knitted fabric layer 1, the intermediate layer 2, and the second weft-knitted fabric layer 3 constitute a layered composite skeleton. The capillary array provides a liquid conduction path in the thickness direction, and the vent holes 5 provide an air exchange path. By fixing the two ends and the middle of the floats forming the vent holes 5 to the root of the corresponding fabric layer's loop post 11 or the loop 211 of the tuck weave 21, the continuity of the edges of the vent holes 5 can be maintained. The connecting areas and corresponding avoidance areas maintain interlayer support. All structures work together within the same knitting system, which is beneficial for balancing moisture wicking, breathability and heat dissipation, soft touch, and dimensional stability after washing.
[0053] Furthermore, the use of terms such as "first" and "second" in this application is for descriptive purposes only and should not be construed as indicating or implying their relative importance or implicitly specifying the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of those features. Additionally, the term "and / or" in this application merely describes the relationship between related objects, indicating that three relationships may exist. For example, A and / or B can represent: A existing alone, A and B existing simultaneously, or B existing alone. Furthermore, the technical solutions of the various embodiments can be combined with each other, but this must be based on the ability of those skilled in the art to implement them. When the combination of technical solutions is contradictory or impossible to implement, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection claimed in this application.
[0054] In this application, the testing procedure for the equivalent diameter of the capillary is as follows: a thin cross-sectional slice (thickness 5-10 μm) is cut along the thickness direction of the fabric, photographed under an optical microscope (200x magnification), and the cross-sectional area A of the capillary is obtained by analyzing the image using image analysis software, according to the formula " "To calculate the equivalent diameter, five cross-sectional thin-slice samples at different locations were taken for each type of fabric for measurement. Five capillaries were taken from each cross-sectional thin-slice for testing, and the arithmetic mean was taken as the test result." In this application, the air permeability was tested in accordance with GB / T 5453-2025 "Textiles - Determination of air permeability of fabrics"; In this application, the wicking height (longitudinal) and wicking height (lateral) are tested in accordance with GB / T 21655.1-2023 Part 1: Single Combination Test Method; In this application, the instantaneous cooling sensation upon contact was tested in accordance with GB / T 35263-2017 Test and evaluation of instantaneous cooling sensation performance of textiles upon contact; In this application, the thickness retention rate after washing (50 times) is determined by continuously washing the fabric 50 times using program 4N of a type A washing machine according to GB / T 8629-2017 "Test Procedures for Household Washing and Drying of Textiles". Before washing, the thickness of the fabric at five different locations is tested according to GB / T 3820-1997 "Determination of Thickness of Textiles and Textile Products", and the average value is taken as the initial thickness T0. After washing, the thickness T1 is measured using the same method. The thickness retention rate after washing (50 times) is calculated according to the formula "Thickness retention rate after washing (50 times) = T1 / T0 × 100%". In this application, the bursting strength was tested in accordance with GB / T 19976-2005 Determination of bursting strength of textiles by steel ball method; In this application, the softness test procedure is as follows: the bending stiffness B (μN) is measured using a KES-FB2 fabric bending stiffness tester. m² / m), sample size 20cm×20cm, bending direction along the longitudinal direction, tested after 24h conditioning under standard atmosphere (GB / T 6529, 20℃±2℃, 65%±4% RH), each fabric was tested in parallel 3 times, and the arithmetic mean was taken as the test result; softness is expressed by bending stiffness B value, the smaller the bending stiffness B value, the softer the fabric. In this application, the testing steps for the missing ring aperture (i.e., the aperture of the vent) are as follows: the maximum inscribed diameter of the vent is measured using a stereomicroscope under a standard light source; 10 vents at different locations are randomly selected from each sample for measurement, and the arithmetic mean is taken as the test result. In this application, the test procedure for the rate of change in the diameter of the missing loops after washing (50 times) is as follows: Wash continuously for 50 times using program 4N of a type A washing machine according to GB / T 8629-2017 "Test Procedures for Household Washing and Drying of Textiles"; before washing, measure the diameter of 10 vents located at different positions using the above-mentioned method for measuring the diameter of the missing loops (the arithmetic mean is not taken here), and record it as d0; after washing, measure the diameter of the above 10 vents in the same way, and record it as d1; according to the formula "Rate of change in the diameter of the missing loops after washing (50 times) = (d1 / d0)", the measurement is performed on the vents. The change rate of the missing pore diameter after washing (50 times) is calculated by “d0) / d0×100%”. The maximum value of the change rate of the pore diameter of the 10 vents is taken as the test result. In this application, the air permeability of the missing pores (i.e., the air permeability of the vents) is tested in accordance with GB / T 5453-2025 "Textiles - Determination of Air Permeability of Fabrics". A test area (covering one or more vents) is selected directly above the vents, and the airflow rate is tested at a pressure difference of 100 Pa. The results are expressed in cm⁻¹. 3 / (s cm 2The result indicates that the air permeability of each fabric at five different locations with missing loops was tested, and the arithmetic mean was taken as the test result.
[0055] Example 1 This embodiment provides a layered composite fabric, the preparation process of which is as follows: S1. The surface layer yarn is made of 100% polyester filament with a fineness of 75D / 72F (where 72F indicates that the total number of single filaments of polyester filament is 72, and 75D indicates that the fineness of polyester filament is 75D). The bottom layer yarn is made of cotton-modal blended yarn with a fineness of 40S (in which the mass ratio of cotton fiber to modal fiber in the blended yarn is 60:40). The middle layer yarn is made of 100% polyester yarn with a fineness of 100D / 72F (this yarn is a special yarn for tuck-in). The connecting yarn is made of spandex core-spun yarn (this spandex core-spun yarn has a fineness of 150D polyester as the core yarn and a fineness of 40D spandex as the cover yarn, with a mass ratio of core yarn to cover yarn of 80:20). The yarn is woven in an integrated manner using a double-sided circular knitting machine (machine size E28, bobbin diameter of 30 inches, number of passes 90F). The integrated knitting process parameters are as follows: During the surface layer knitting process, a 1+1 rib knitting structure is formed using a single loop-forming system. During the intermediate layer 2 knitting process, a composite circular knitting process using a single loop-forming system and a single loop-forming system is used to form a rib structure, resulting in an intermediate layer with loop-forming structure 21 and loop-forming structure 22. The height of loop-forming structure 21 is 2 stitch lengths, and the length of the overhang arc 212 of loop-forming structure 21 is 1.2mm. During the bottom layer knitting process, a 1+1 rib structure is formed using a single loop-forming system. During the knitting of connecting yarn 4, a connecting area is set every 5 rows and 7 columns, with a spacing of 5mm (vertical) × 7mm (horizontal) between adjacent connecting areas. The connecting area is a circular area with a diameter of 2mm. The distribution density of loop-forming structure 21 is: 5 rows / 10mm vertically and 5 columns / 10mm horizontally. During the knitting of both the surface layer and intermediate layer 2, missing loop knitting is performed to form ventilation holes 5 that penetrate the surface layer and intermediate layer 2. The missing loop stitch instructions are as follows: The missing loop row cycle is 1 missing loop inserted every 3 rows. The number of missing loop stitches is 1 per row, with a missing loop ratio of 14.3%. The missing loop and loop formation cycle rhythm is alternating between 1 missing loop and 6 loops. Middle layer 2 missing loop anchoring: A tuck stitch 21 is placed one stitch adjacent to the missing loop stitch position, thus fixing both ends and the middle of the float yarn to the loop 211 of the tuck stitch 21, forming a ventilation hole edge structure of loop 211-float yarn-loop 211. Top layer missing loop anchoring: A loop is placed one stitch adjacent to the missing loop stitch position, thus fixing both ends and the middle of the float yarn to the root of the loop post 11, forming a ventilation hole 5 edge structure of loop-float yarn-loop. Missing loop hole placement: Missing loop holes avoid the stitch positions in the connecting area. The formed air pores 5 have a pore diameter of 1.8 mm, the pore shape of the air pores 5 is approximately rhomboid, the distribution density of the air pores 5 is 9 pores / cm², and the air pores 5 are arranged in a checkerboard pattern. The woven fabric has a weight of 215 g / m² and a thickness of 2.4 mm. The fabric structure of the raw fabric is as follows: Along the longitudinal direction (the longitudinal direction is the Wales direction): the top layer has a 1+1 rib knit; the middle layer 2 has a rib knit loop knit (every 5 rows there is a set of rib knit loop loop suspension arcs 212, the suspension arcs 212 are staggered and superimposed between adjacent needle beds to form capillaries 23); the bottom layer has a 1+1 rib knit, and the connecting yarn 4 connects the middle layer 2 with the top layer and the bottom layer in a "Z" shape; the float yarn at the missing loop row (one missing loop is inserted every 3 rows) forms a continuous hook-edge ventilation hole 5 between the top layer and the middle layer 2; the spacing between adjacent connecting areas is 5mm×7mm.
[0056] Along the transverse (courses direction) section: the connecting areas are evenly distributed with 7 longitudinal rows at intervals; the distribution of missing ring holes is as follows: 1 missing ring and 6 complete rings are rhythmically and evenly distributed, and the missing ring holes avoid the connecting areas.
[0057] S2. Pre-shape the raw fabric at 160℃ for 45 seconds; The pre-shaped fabric was placed in a dye bath at 100℃ with a liquor ratio of 1:15 for 60 minutes. The dye bath was prepared by deionized water and reactive dye Reactive Red 3BS (CI Reactive Red 195), and the mass ratio of reactive dye Reactive Red 3BS (CI Reactive Red 195) to the fabric was 2:100. The raw fabric is removed from the dyeing solution and set at 150°C for 20 seconds to obtain a layered composite fabric.
[0058] The equivalent diameter of capillary 23, air permeability, wicking height (longitudinal), wicking height (transverse), instantaneous cooling sensation upon contact, thickness retention rate after washing (50 times), bursting strength, softness, pore diameter (i.e., the diameter of the air pore), pore diameter change rate after washing (50 times), and air permeability of pore holes (i.e., the air permeability of the air pore) in the fabric prepared in this embodiment were tested and compared with commercially available plain weave fabrics. The results are shown in Table 1.
[0059] Table 1 Test Results of Example 1
[0060] Note: -- indicates not tested. The improvement is based on the corresponding indicators of commercially available plain weave fabrics. The improvement is the test result of the corresponding indicators in Example 1.
[0061] Example 2 This embodiment provides a layered composite fabric, the preparation process of which is as follows: S1. Using 100% polyester filament with a fineness of 50D / 36F as the surface layer yarn, cotton-modal-bamboo fiber blended yarn with a fineness of 60S (in which the mass ratio of cotton fiber, modal fiber and bamboo fiber is 50:30:20) as the bottom layer yarn, 100% polyester yarn with a fineness of 75D / 72F (this yarn is a special yarn for tuck loops) as the middle layer yarn, and spandex core-spun yarn (this spandex core-spun yarn has a fineness of 100D polyester as the core yarn and a fineness of 30D spandex as the covering yarn, with a mass ratio of core yarn to covering yarn of 70:30) as the connecting yarn 4, the entire process is integrated using a computerized flat knitting machine (machine size E24, needle bed width of 100 inches). The integrated knitting process parameters are as follows: The surface layer is knitted to form a weft-knit plain knit structure. The middle layer 2 is knitted to form a double rib knit structure, which has a knit structure 21 and a loop structure 22. The height of the knit structure 21 is 1 stitch length, and the length of the overhang arc 212 of the knit structure 21 is 0.8 mm. The bottom layer is knitted to form a weft-knit plain knit structure. During the knitting process of the connecting yarn 4, the connection is only made at the connection area of the reinforcement area (the reinforcement area is a ring-shaped area 2 mm away from the edge of the vent hole 5, which is the first area 24). The spacing between adjacent connection areas is 6 mm × 6 mm, and the connection area is a circular area with a diameter of 3 mm. The distribution density of the knit structure 21 in the reinforcement area is: 8 rows / 10 mm in the longitudinal direction and 8 columns / 10 mm in the transverse direction. The distribution density of the knit structure in the second area 25 is 5 rows / 10 mm in the longitudinal direction and 5 columns / 10 mm in the transverse direction. During the knitting of both the top layer and the middle layer 2, missing loops are used to form ventilation holes 5 that penetrate both the top layer and the middle layer 2. The missing loop stitch instructions are as follows: the missing loop row cycle is 1 missing loop inserted every 2 rows. The number of missing loop stitches is 1 missing loop stitch per row; the missing loop ratio is 20%. The rhythm of missing loops and loop formation is: 1 missing loop stitch and 4 loop formation stitches are regularly distributed. Intermediate layer 2 missing loop anchoring: a tuck stitch 21 is set on the stitch adjacent to the missing loop stitch position, thereby fixing both ends and the middle of the float yarn to the loop 211 of the tuck stitch 211, forming a ventilation hole edge structure of loop 211-float yarn-loop 211. Top layer missing loop anchoring: a loop 211 is set on the stitch adjacent to the missing loop stitch position, thereby fixing both ends and the middle of the float yarn to the root of the loop post 11, forming a ventilation hole edge structure of loop-float yarn-loop 5. Missing loop hole placement: the missing loop hole position avoids the stitch position where the connecting area is located. The formed air pores 5 have a pore diameter of 2.2 mm, the pore shape of the air pores 5 is approximately rhomboid, the distribution density of the air pores 5 is 16 pores / cm², and the air pores 5 are arranged in a rhomboid array. The weight of the woven fabric is 182 g / m² and the thickness is 1.9 mm. S2. Pre-shape the raw fabric at 170℃ for 40 seconds; The pre-shaped fabric was placed in a dye bath at 90°C with a liquor ratio of 1:12 for 50 minutes. The dye bath was prepared by deionized water and low-reactivity dye CI Reactive Blue 19 (anthraquinone structure), and the mass ratio of low-reactivity dye CI Reactive Blue 19 (anthraquinone structure) to the fabric was 2.5:100. The raw fabric is removed from the dyeing solution and set at 140°C for 25 seconds to obtain a layered composite fabric.
[0062] The equivalent diameter of capillaries, air permeability, wicking height (longitudinal), wicking height (transverse), instantaneous cooling sensation upon contact, thickness retention after washing (50 times), bursting strength, softness, pore diameter (i.e., the diameter of the pores), pore diameter change rate after washing (50 times), and pore ventilation (i.e., the ventilation capacity of the pores) of the fabric prepared in this embodiment were tested and compared with commercially available plain weave fabrics. The results are shown in Table 2.
[0063] Table 2 Test Results of Example 2
[0064] Note: -- indicates not tested. The improvement is based on the corresponding indicators of commercially available plain weave fabrics. The improvement is the test result of the corresponding indicators in Example 2.
[0065] As shown in Tables 1 and 2, compared with Example 1, the air permeability and wicking height of Example 2 are significantly improved. This result indicates that, in this application, by increasing the distribution density of the tuck stitch 21, the breathability, heat dissipation, and moisture wicking properties of the fabric can be further improved.
[0066] Comparative Example 1 The difference between this comparative example and Example 1 is that: the intermediate layer 2 is not woven, the connecting yarn 4 is not used to connect the surface layer and the bottom layer, and the ventilation holes 5 are not formed by loop weaving.
[0067] Comparative Example 2 The difference between this comparative example and Example 1 is that the top layer, middle layer 2 and bottom layer are not connected by connecting yarn 4, and the ventilation holes 5 are not formed by loop weaving.
[0068] Comparative Example 3 The difference between this comparative example and Example 1 is that: no missing loop stitch position is set, that is, the ventilation hole 5 is not formed by missing loop knitting.
[0069] Comparative Example 4 The difference between this comparative example and Example 1 is that during the knitting of the surface layer and intermediate layer, the missing loop stitches are arranged adjacently (two consecutive stitches perform a missing loop). Specifically, during the knitting of the surface layer, no loop is set between adjacent missing loop stitches; only loop arcs are knitted. Thus, only the two ends of the float yarn are fixed to the root of the loop post 11, and the middle part of the float yarn is not fixed to the root of the loop post 11. During the knitting of the intermediate layer, no tufting structure 21 is set between adjacent missing loop stitches. Thus, only the two ends of the float yarn are fixed to the loop 211 of the tufting structure 21, and the middle part of the float yarn is not fixed to the loop 211 of the tufting structure 21. Therefore, no anchoring structure is formed during the knitting of the surface layer and intermediate layer.
[0070] The air permeability, wicking height (longitudinal direction), and thickness retention after washing (50 times) of Comparative Examples 1-3 were tested, and the change rate of missing loop pore size after washing (50 times) of Comparative Example 4 was tested. The results were compared with the fabric of Example 1, and the results are shown in Table 3.
[0071] Table 3 Test results of Example 1 and Comparative Examples 1-4
[0072] As shown in Table 3, the wicking height (longitudinal direction) of Comparative Example 2 is increased by 108% compared to Comparative Example 1. This result indicates that in this application, the capillary array formed by the overlapping and staggered suspension arcs of adjacent horizontal loop structures along the thickness direction can significantly improve the moisture absorption and wicking properties of the fabric.
[0073] As shown in Table 3, the thickness retention rate (50 times) of Comparative Example 3 after washing was improved by 21% compared to Comparative Example 2. This result indicates that in this application, connecting the intermediate layer with the first weft-knitted fabric layer and the second weft-knitted fabric layer at multiple connection areas can improve the dimensional stability of the fabric.
[0074] As shown in Table 3, compared with Comparative Example 3, the air permeability of Example 1 was increased by 62%, and the change rate of missing loop pore size after washing (50 times) was significantly reduced. These results indicate that in this application, by using float yarn to pull the surrounding yarns to form air pores, the air permeability of the fabric can be effectively improved while maintaining pore shape stability.
[0075] As shown in Table 3, the rate of change in the missing loop diameter after washing (50 times) of Comparative Example 4 is significantly improved compared to Example 1. This result indicates that, in this application, by fixing both ends and the middle of the float to the root of the loop post of the corresponding fabric layer or to the loop of the tucked structure, an anchoring structure can be formed, thereby improving the hole stability of the fabric.
[0076] The above embodiments are merely illustrative of the principles and effects of this application and are not intended to limit this application. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of this application. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in this application should still be covered by the claims of this application.
Claims
1. A layered composite fabric, characterized in that, include: The first weft-knitted fabric layer and the second weft-knitted fabric layer, both of which have loops and loops; An intermediate layer, located between the first weft-knitted fabric layer and the second weft-knitted fabric layer, is connected to the first weft-knitted fabric layer and the second weft-knitted fabric layer at multiple connection areas; The intermediate layer has a coiled structure and a looped structure. The coiled structure includes coils and suspended arcs. The suspended arcs of adjacent rows of the coiled structure are staggered and superimposed along the thickness direction to form a capillary array that runs through the thickness direction. The first weft-knitted fabric layer, the intermediate layer, and / or the second weft-knitted fabric layer are all covered with ventilation holes. The ventilation holes are formed by pulling the surrounding yarns together with floats. The two ends and the middle of the floats are fixed to the root of the loop post of the corresponding fabric layer or the loop of the tucked structure. If adjacent fabric layers are covered with the ventilation holes, the ventilation holes penetrate the adjacent corresponding fabric layers.
2. The layered composite fabric as described in claim 1, characterized in that, The layered composite fabric meets at least one of the following requirements (1)-(3): (1) The equivalent diameter of the capillary is 10-300 μm; (2) The pore diameter of the vent is 0.8-4.0 mm; (3) The equivalent diameter of the connecting area is 1-5 mm.
3. The layered composite fabric as described in claim 1 or 2, characterized in that, The layered composite fabric satisfies at least one of the following (4)-(6): (1) At all the connection areas, the looped arc of the intermediate layer is connected to the looped arc of the first weft knitted fabric layer and the second weft knitted fabric layer, thus connecting the intermediate layer with the first weft knitted fabric layer and the second weft knitted fabric layer. (2) At all the said connecting areas, the intermediate layer is connected to the first weft-knitted fabric layer and the second weft-knitted fabric layer by connecting yarn; (3) Along the direction from the center to the edge of the ventilation hole, the intermediate layer is divided into a first area and a second area. The distribution density of the tucked structure in the first area is greater than that in the second area. At all the connecting areas, the hanging arc of the tucked structure in the first area is connected to the loop arc of the first weft-knitted fabric layer and the second weft-knitted fabric layer, connecting the intermediate layer with the first weft-knitted fabric layer and the second weft-knitted fabric layer. Alternatively, at all the connecting areas in the first area, the intermediate layer is connected to the first weft-knitted fabric layer and the second weft-knitted fabric layer through the connecting yarn.
4. The layered composite fabric as described in claim 3, characterized in that, The spacing between adjacent connecting areas is 5-30mm.
5. The layered composite fabric as described in claim 3, characterized in that, One set of the connecting regions is distributed every 2-10 rows along the longitudinal direction, or arranged in a linear array along the transverse direction; and / or, one set of the connecting regions is distributed every 3-15 columns along the transverse direction, or arranged in a linear array along the vertical direction.
6. The layered composite fabric as described in claim 1, characterized in that, The distribution density of the clustered structure is 3-8 rows / 10mm in the longitudinal direction and 3-8 columns / 10mm in the transverse direction.
7. The layered composite fabric as described in claim 1 or 2, characterized in that, The distribution density of the air pores is 4-25 pores / cm².
8. The method for preparing the layered composite fabric according to any one of claims 1-7, characterized in that, Includes the following steps: S1. A raw fabric comprising a first weft-knitted fabric layer, an intermediate layer, and a second weft-knitted fabric layer is woven using an integrated weaving process; S2. The raw fabric is pre-shaped and post-shaped to obtain the layered composite fabric.
9. The method for preparing the layered composite fabric as described in claim 8, characterized in that, In step S2, the predetermined temperature is 150-180℃ and the duration is 30-60s.
10. A textile product, characterized in that, The textile includes the layered composite fabric as described in any one of claims 1-7 or the layered composite fabric prepared according to the method as described in claim 8 or 9.