Preparation method of high-silica fiber sintered yarn for the skeleton of battery cell gas-silicon nano-insulation sheet
By employing ultrasonic dynamic leaching, vacuum-pressure alternating impregnation, and dynamic micro-tension multi-level gradient sintering, the problems of mechanical strength decay and interfacial bonding failure of high-silica glass fibers at high temperatures were solved, achieving structural stability and low thermal conductivity of the thermal insulation material at high temperatures, thus ensuring the safety of the battery pack.
Patent Information
- Application Number
- CN202611021995.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-09
- Publication Date
- 2026-11-17
AI Technical Summary
Existing high-silica glass fibers suffer severe mechanical strength degradation during high-temperature sintering, and the interfacial bonding between the fiber skeleton and the aerogel layer fails, leading to the failure and pulverization of the insulation material during thermal runaway of the battery cell, posing a risk of internal short circuit in the battery pack.
High-strength, high-silica fiber sintered yarn was prepared by using ultrasonic dynamic leaching and vacuum-pressure alternating impregnation to treat porous silica-rich fiber yarn, combined with multi-level gradient heating sintering with dynamic micro-tension control. Furthermore, chemical cross-linking anchor points were constructed through in-situ active pretreatment with aminosilane coupling agent and nano-silica sol to ensure the axial orientation of macromolecular chains inside the fiber.
Maintaining the integrity of the high-silicon-oxygen skeleton structure under 1000℃ high-temperature thermal shock, reducing the material pulverization and shedding rate, improving the resistance to deformation, and meeting the thermal safety protection requirements of high-energy-density power batteries.
Smart Images

Figure CN123108929A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of thermal management materials technology for new energy power batteries, specifically to a method for preparing high-silica fiber sintered yarn for the skeleton of silicon nano-insulating sheet for battery cells. Background Technology
[0002] With the development of high-energy-density power batteries, the protection against thermal runaway of battery cells places extremely stringent requirements on the high-temperature resistance and mechanical stability of thermal insulation materials. Currently, thermal insulation pads made by impregnating glass fiber mat with pure silica aerogel are widely used in power battery packs. However, ordinary alkali-free or medium-alkali glass fibers have low softening points, typically between 700°C and 800°C. When thermal runaway of the battery cell generates a high-temperature impact exceeding 1000°C, the ordinary glass fiber skeleton will rapidly melt and collapse, causing the aerogel to lose its structural support and detach over a large area.
[0003] To improve the temperature resistance of the skeleton, existing technologies attempt to use high-silica glass fibers with a silica mass fraction greater than 96% as the skeleton of composite thermal insulation materials. High-silica glass fibers are typically made by acid leaching ordinary glass fibers to remove metal cations, followed by high-temperature sintering. However, the existing preparation processes for high-silica fibers and their composite aerogel materials face two core technical challenges that urgently need to be addressed: First, the mechanical strength of the fiber is severely reduced during the sintering process. During the high-temperature sintering stage, porous silicon-rich fibers undergo pore closure and volume shrinkage driven by thermodynamics. In traditional tensionless or constant-speed static traction sintering processes, the macromolecular chains inside the fiber lack clear axial stress guidance during their violent contraction, leading to disordered lattice arrangement and high stress concentration. This thermal shrinkage stress concentration induces numerous microcracks inside and on the surface of the fiber, macroscopically manifesting as extreme brittleness and a significant decrease in tensile fracture strength of the high-silica fiber. Its actual tensile strength cannot withstand the periodic liquid injection expansion and extrusion stress generated during the charge-discharge cycle of the power battery.
[0004] Second, the interfacial bonding between the fiber skeleton and the aerogel layer fails. Existing composite processes mostly employ atmospheric pressure physical impregnation to coat the aerogel precursor onto the fiber surface. Because the micropores inside high-silica fibers are filled with air, creating air resistance, and the fiber surface lacks active cross-linking sites, the aerogel precursor struggles to penetrate the micropores, relying solely on weak intermolecular van der Waals forces to adhere to the fiber skeleton surface. Under the continuous high-frequency vibration conditions of actual vehicle operation, and the thermal stress impact generated during the instantaneous thermal runaway of the battery cell, microscopic interfacial tearing and macroscopic peeling easily occur between the aerogel and the fiber skeleton, leading to severe pulverization and detachment of the insulation material. This not only causes the material to lose its thermal insulation performance, but the free dust can also easily trigger short circuits within the battery pack. Summary of the Invention
[0005] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a method for preparing high-silica fiber sintered yarn for the skeleton of battery cell gas silicon nano heat insulation sheet, including the following steps: S100. The glass fiber raw yarn is placed in a composite acid solution for ultrasonic dynamic leaching to remove non-silica metal ions in the glass fiber raw yarn. After washing and drying, porous silicon-rich fiber yarn is obtained. S200. The porous silicon-rich fiber yarn is immersed in a mixture containing an aminosilane coupling agent and nano-silica sol for in-situ active pretreatment, so that active groups are attached to the micropores and surface of the porous silicon-rich fiber yarn. S300. The pretreated porous silicon-rich fiber yarn is continuously fed into the sintering kiln under the dynamic micro-tension control of the drawing device for multi-stage gradient heating sintering; wherein, the dynamic micro-tension is controlled between 0.5 cN / tex and 1.0 cN / tex, and the multi-stage gradient heating sintering includes a dehydration stage, a closed-cell pre-sintering stage, and a densification orientation sintering stage in sequence. S400. The sintered fiber yarn is subjected to slow cooling treatment and then wound up to obtain the high-strength, high-silica fiber sintered yarn, whose silica mass fraction is ≥96%.
[0006] Further, in step S100, the composite acid solution is a mixed aqueous solution of hydrochloric acid and a weak organic acid, and the molar ratio of the hydrochloric acid to the weak organic acid is 1:(2.0~3.0). The weak organic acid is acetic acid, and the total molar concentration of hydrogen ions in the composite acid solution is 0.5 mol / L to 1.5 mol / L.
[0007] Furthermore, the process parameters of the ultrasonic dynamic leaching meet the following conditions: the ultrasonic frequency is set to 40kHz~50kHz, the temperature of the leaching system is maintained at 75℃~90℃, and the continuous leaching time is 2 hours~4 hours. In step S100, the specific operations of the washing and drying process include: The filtered fiber yarn is rinsed in a step-by-step countercurrent manner with deionized water until the pH value of the eluent reaches 6.5~7.0; then the washed fiber yarn is dried in circulating hot air at 90℃~110℃ until constant weight.
[0008] Further, in step S200, the aminosilane coupling agent is selected from at least one of 3-aminopropyltriethoxysilane (KH550) or 3-aminopropyltrimethoxysilane; The mass fraction of the nano-silica sol is 10%~20%, and the average particle size of the silica in the nano-silica sol is between 5nm and 15nm. The preparation process of the mixture includes: The aminosilane coupling agent is slowly added dropwise to the nano-silica sol, and then a weak acid is added to adjust the pH of the system to 4.0~5.0. The mixture is then continuously stirred at 20℃~30℃ for 1 hour to 2 hours to carry out hydrolysis and aging reactions to obtain the mixture.
[0009] Furthermore, the in-situ active pretreatment in step S200 specifically involves alternating vacuum-pressure impregnation, the operation of which includes: The porous silicon-rich fiber yarn is placed in a sealed container, and a vacuum is drawn until the absolute pressure is below 0.08 MPa and maintained for 10 to 15 minutes. Inject the mixture until it completely submerges the porous silica-rich fiber yarn, then introduce inert gas into the sealed container and pressurize it to 0.2MPa~0.4MPa, and maintain the pressure for 20 minutes~30 minutes; After depressurization, remove the fiber yarn and remove excess free liquid from the surface.
[0010] Furthermore, in step S300, the specific process parameters for each stage of the multi-stage gradient heating sintering are defined as follows: The dehydration stage: the sintering temperature is 300℃~400℃, and the holding time is 20 minutes~40 minutes; The closed-cell pre-firing stage: the sintering temperature is 600℃~700℃, and the holding time is 30 minutes~60 minutes; The densification and orientation sintering stage: the sintering temperature is 850℃~950℃, and the holding time is 15 minutes~30 minutes; The heating rates between the dehydration stage, the closed-cell pre-firing stage, and the densification orientation sintering stage are all independently controlled between 3℃ / min and 8℃ / min.
[0011] Further, in step S300, the method for controlling the dynamic micro-tension specifically includes: A tension closed-loop feedback regulation system is constructed by using active stretching rollers installed at the feed end and discharge end of the sintering kiln in conjunction with online tension sensors. During the densification and orientation sintering stage, when tension fluctuates due to fiber thermal shrinkage, the linear speed of the active stretching roller at the discharge end is finely adjusted in real time by the tension closed-loop feedback adjustment system to keep the constant tension of the fiber yarn between 0.5 cN / tex and 1.0 cN / tex.
[0012] Furthermore, the multi-stage gradient heating sintering process is carried out entirely in a continuously flowing dry air atmosphere that has been dehumidified, and the gas dew point temperature inside the sintering kiln is controlled below -40°C.
[0013] Furthermore, in step S400, the specific process of the slow cooling treatment is as follows: The sintered fiber yarn is continuously passed through a slow cooling channel with a temperature gradient. The cooling rate of the fiber yarn in the slow cooling channel is controlled at 10℃ / min~15℃ / min until the surface temperature of the fiber yarn drops below 100℃ before it comes into contact with the outside room temperature air.
[0014] Furthermore, in step S400, the winding adopts a constant tension precision winding process, the winding tension is controlled between 0.1cN / tex and 0.3cN / tex, and the winding cross angle is set between 12° and 18°. Beneficial effects
[0015] The present invention provides a method for preparing high-silica fiber sintered yarn and a heat insulation board. Through the synergistic effect of vacuum pressure in-situ pretreatment and dynamic micro-tension multi-level gradient sintering, silane coupling agents and nano-silica sol penetrate deep into the porous silicon-rich fiber to construct in-situ active chemical cross-linking anchor points. At the same time, during the high-temperature closed-cell shrinkage stage, a constant dynamic micro-tension of 0.5 cN / tex to 1.0 cN / tex is used to guide the silica macromolecular chains to axially align, effectively suppressing the generation of micro-cracks in the crystal lattice. The composite aerogel heat insulation board obtained by the preparation method maintains the integrity of the high-silica skeleton structure and low thermal conductivity under high-temperature thermal shock at 1000℃. Relying on the covalent bonding of the interface and the encapsulation of the outer organic silicone layer, the pulverization and shedding rate of the material under complex vibration conditions is reduced, and the overall material's resistance to deformation is improved, effectively meeting the thermal safety protection requirements of high-energy-density power batteries. Attached Figure Description
[0016] Figure 1 This is a flowchart of the method of the present invention; Figure 2 This is a temperature control curve for the dynamic micro-tension multi-level gradient sintering process of the present invention; Figure 3 This is a logic diagram of the process preparation and hierarchical evolution of the composite aerogel insulation board of the present invention. Detailed Implementation
[0017] To enable those skilled in the art to better understand the present invention, the technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of the present invention.
[0018] It should be noted that the terms "first," "second," etc., in the specification, claims, and accompanying drawings of this invention are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of the invention described herein can be implemented in orders other than those illustrated or described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover a non-exclusive inclusion; for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but includes other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.
[0019] The present invention will now be described in further detail with reference to the accompanying drawings: Example:
[0020] like Figures 1-3 As shown, the preparation method of high-silica fiber sintered yarn for the skeleton of the battery cell's gas-silicon nano-insulation sheet includes the following steps: S100. Glass fiber yarn is placed in a composite acid solution for ultrasonic dynamic leaching to remove non-silicon metal ions from the glass fiber yarn. After washing and drying, porous silicon-rich fiber yarn is obtained. S200. The porous silicon-rich fiber yarn is immersed in a mixture containing an aminosilane coupling agent and nano-silica sol for in-situ active pretreatment, so that active groups are attached to the micropores and surface of the porous silicon-rich fiber yarn. S300. The pretreated porous silicon-rich fiber yarn is continuously fed into the sintering kiln under the dynamic micro-tension control of the drawing device for multi-stage gradient heating sintering; wherein, the dynamic micro-tension is controlled between 0.5cN / tex and 1.0cN / tex, and the multi-stage gradient heating sintering includes the dehydration stage, the closed-cell pre-sintering stage, and the densification orientation sintering stage in sequence. S400. The sintered fiber yarn is subjected to slow cooling treatment and then wound up to obtain high-strength, high-silica sintered fiber yarn with a silica mass fraction ≥96%.
[0021] Furthermore, the specific implementation process of step S100 is as follows: Glass fiber virgin yarn was prepared as the precursor material. The leachate was a mixed aqueous solution of hydrochloric acid and acetic acid. The specific preparation steps included: measuring 36% industrial-grade hydrochloric acid and 99% glacial acetic acid at a molar ratio of 1:2.5. The hydrochloric acid was slowly added to deionized water for initial dilution, followed by the uniform dropwise addition of glacial acetic acid using a metering pump. Simultaneously, a mechanical stirrer was activated to continuously mix the solution at a speed of 200 rpm. After the mixture was brought to a final volume, the total molar concentration of hydrogen ions was measured. By fine-tuning the amount of deionized water added, the total molar concentration of hydrogen ions was precisely controlled at 1.0 mol / L.
[0022] The prepared mixed aqueous solution is injected into an acid-resistant stainless steel tank equipped with an ultrasonic transducer. The heating jacket on the outer wall of the acid-resistant stainless steel tank is activated to heat the mixed aqueous solution and maintain the temperature at a constant 85°C. Glass fiber yarn is continuously introduced below the liquid surface of the acid-resistant stainless steel tank via guide rollers. The guide rollers are connected to a servo motor, which drives the guide rollers to rotate at a constant linear speed, allowing the glass fiber yarn to maintain a dynamic movement in the mixed aqueous solution. Simultaneously, the ultrasonic generator is activated, and the ultrasonic frequency is set to 45kHz. The glass fiber yarn continues to move at a frequency of 45kHz and is continuously immersed in the 85°C mixed aqueous solution for 3 hours. Under the combined action of this immersion and ultrasonic treatment, the non-silicon metal cations inside the glass fiber yarn migrate and dissolve into the mixed aqueous solution, transforming the glass fiber yarn into a porous, silicon-rich fiber yarn.
[0023] After the leaching process is completed, the porous silica-rich fiber yarn is drawn out of the acid-resistant stainless steel tank by a traction device and directly sent into the multi-stage countercurrent rinsing system. The multi-stage countercurrent rinsing system consists of a first-stage rinsing tank, a second-stage rinsing tank, and a third-stage rinsing tank connected in series. Fresh deionized water is injected countercurrently from the third-stage rinsing tank and overflows into the first-stage rinsing tank step by step. The porous silica-rich fiber yarn passes through the first-stage rinsing tank, the second-stage rinsing tank, and the third-stage rinsing tank in sequence. When the porous silica-rich fiber yarn reaches the outlet of the third-stage rinsing tank, the pH value of the rinsing solution is detected by an online pH meter. When the pH value of the rinsing solution reaches 6.8, the rinsing process is considered complete.
[0024] The rinsed porous silica-rich fiber yarn is fed into a conveyor-type hot air circulating oven. The internal space of the oven is divided into three temperature zones along the direction of travel: 90°C, 100°C, and 110°C. The porous silica-rich fiber yarn is placed on a conveyor belt and passes through these three zones sequentially. A hot air fan inside the oven forces hot air through the pores of the yarn to remove moisture. At the outlet, the yarn is periodically weighed until three consecutive weight deviations are less than 0.1%, at which point the yarn is considered to have reached a constant weight and is then wound up for later use.
[0025] Specific experimental scenario: In the kilogram-scale implementation scenario, the raw yarn material selected was 1000tex ECR-type alkali-free glass fiber yarn. The leaching equipment used a 50L PTFE-lined ultrasonic cleaning tank, with an array of 2000W ultrasonic vibrating plates at the bottom. A mixed acid solution containing 3.0 mol hydrochloric acid and 7.5 mol acetic acid was injected into the tank. The alkali-free glass fiber yarn was fed into the tank via a constant tension unwinding machine, with the unwinding tension set at 0.2 cN / tex. The entire leaching operation was carried out under a closed negative pressure exhaust hood. A PT100 temperature sensor was used to feed back the liquid temperature in the central area of the cleaning tank to the PLC control cabinet, which adjusted the heating power to stabilize the liquid temperature at 85±1℃. The ultrasonic frequency was locked at 45kHz, and the travel path length and linear velocity of the raw yarn in the tank were matched to ensure that the residence time of a single section of raw yarn in the tank was precisely 180 minutes. The washing step uses deionized water (test conductivity <5μS / cm) for a three-stage countercurrent rinsing. The drying step uses a continuous hot air combined microwave dryer, with the forced hot air temperature set at 105℃, the hot air velocity set at 1.5m / s, and the drying conveyor belt travel time set at 15 minutes. Finally, a white porous silica-rich fiber yarn roll is obtained at the winding end.
[0026] Furthermore, the specific implementation process of step S200 is as follows: Prepare a mixture containing an aminosilane coupling agent and nano-silica sol. Measure 15% (w / w) of nano-silica sol with an average silica particle size distribution of 8nm to 12nm and inject it into a reactor equipped with a constant-temperature water bath jacket. Set the temperature of the water bath jacket to 25℃. Turn on the mechanical stirrer of the reactor and set its speed to 250 rpm. Slowly add 3-aminopropyltriethoxysilane dropwise into the nano-silica sol using a precision peristaltic pump, controlling the dropwise addition rate at 5 mL / min. After the 3-aminopropyltriethoxysilane addition is complete, add a 5% (w / w) dilute acetic acid solution to the reactor using a digital burette. Simultaneously monitor the pH value of the liquid in the reactor using an immersion online pH meter. Stop adding the dilute acetic acid solution when the online pH meter reading reaches 4.5. Keep the mechanical stirrer running at 250 r / min for 90 minutes to allow the mixture to complete the hydrolysis and aging reaction under the set temperature and pH conditions.
[0027] Perform vacuum-pressure alternating impregnation treatment. Place the porous silica-rich fiber yarn roll prepared in step S100 onto the internal support of the pressure-resistant stainless steel impregnation tank. Seal the sealed door of the pressure-resistant stainless steel impregnation tank. Start the vacuum pump unit to evacuate the internal space of the pressure-resistant stainless steel impregnation tank, while observing the reading of the external absolute pressure gauge. When the value displayed on the absolute pressure gauge drops to 0.05 MPa, close the vacuum pump valve and maintain the current negative pressure state for 15 minutes to extract the air remaining in the micropores inside the porous silica-rich fiber yarn. Open the liquid inlet valve at the bottom of the pressure-resistant stainless steel impregnation tank, and use the atmospheric pressure difference to draw the mixture aged at 25°C into the pressure-resistant stainless steel impregnation tank. When the liquid level of the mixture completely submerges the porous silica-rich fiber yarn roll by at least 5 cm, close the liquid inlet valve. Subsequently, open the nitrogen cylinder valve and fill the pressure-resistant stainless steel impregnation tank with high-purity nitrogen. Observe the positive pressure gauge reading on the top of the pressure-resistant stainless steel impregnation tank. When the internal pressure reaches 0.3 MPa, stop the inflation and maintain the pressure at 0.3 MPa for 25 minutes to force the mixture into the micropores of the porous silicon-rich fiber yarn.
[0028] After the impregnation and pressure holding process is completed, open the exhaust valve to release the nitrogen gas inside the pressure-resistant stainless steel impregnation tank until the internal pressure returns to normal. Open the sealed door and remove the impregnated porous silica-rich fiber yarn. Pass the impregnated porous silica-rich fiber yarn sequentially through a pair of squeezing rollers with polyurethane rubber-coated surfaces. Adjust the mechanical clamping devices at both ends of the squeezing rollers to set the linear pressure between the rollers to 20 N / cm. The rolling action of the squeezing rollers removes excess free mixed liquid adhering to the surface of the porous silica-rich fiber yarn, completing the in-situ activation pretreatment step.
[0029] Specific experimental scenario: In the kilogram-scale implementation scenario, neutral silica sol with a solid content of 15% and a measured average particle size of 10 nm was selected. 10 L of the nano-silica sol was placed in a 20 L glass reactor with a frame-type stirred paddle. 150 mL of KH550 silane coupling agent was added to the reactor in one step. The solution was continuously titrated with a 0.1 mol / L glacial acetic acid aqueous solution until the pH reached 4.5. The mixture was aged for 120 minutes at 300 rpm under stirring at 25°C. 1000 tex porous silica-rich fiber yarn was wound onto a Teflon mesh skeleton with through-holes on the surface, forming a loosely wound yarn package with a maximum outer diameter of 300 mm. The loosely wound yarn package was placed horizontally into a 50 L horizontal vacuum pressure composite impregnation device. The Roots vane vacuum pump unit was started, and the absolute pressure inside the equipment chamber was evacuated to 0.02 MPa within 5 minutes and maintained for 10 minutes. The loosely wound yarn bales are completely submerged by injecting the aged mixture through the bottom inlet pipe. The vacuum pipe is then closed, and 99.99% pure industrial nitrogen is introduced to pressurize the equipment chamber to 0.35 MPa, maintaining this pressure for 20 minutes. After depressurization and drainage, the loosely wound yarn bales are transferred to an industrial centrifuge and centrifuged at 800 rpm for 3 minutes to remove excess free droplets from the surface of the porous, silica-rich fiber yarn. This yields pretreated fiber yarn with its micropores fully filled with the mixture, which is then sealed in a bag for the next process.
[0030] Furthermore, the specific implementation process of step S300 is as follows: Start the continuous tunnel sintering kiln and its associated air drying and purification system. The air drying and purification system continuously supplies dehumidified clean air into the continuous tunnel sintering kiln. By monitoring the internal gas environment in real time through a dew point meter installed at the exhaust end of the continuous tunnel sintering kiln, the working state of the molecular sieve of the air drying and purification system is adjusted to stably control the dew point temperature of the gas inside the continuous tunnel sintering kiln below -40℃, so as to provide an extremely dry sintering atmosphere.
[0031] The pretreated porous silica-rich fiber yarn obtained in step S200 is drawn out and sequentially passed through an active feed roller group, a tension sensor, and an active traction roller group located at the feed end of the continuous tunnel sintering kiln. The active feed roller group, tension sensor, and active traction roller group are electrically connected to an external tension closed-loop feedback adjustment system. The active feed roller group and active traction roller group are activated to continuously feed the pretreated porous silica-rich fiber yarn into the continuous tunnel sintering kiln.
[0032] The pretreated porous silica-rich fiber yarn first enters the dehydration temperature zone of the continuous tunnel sintering kiln. The heating rate of the dehydration temperature zone is controlled at 5℃ / min, raising the ambient temperature of the dehydration temperature zone to between 300℃ and 400℃. The pretreated porous silica-rich fiber yarn continues to move within the dehydration temperature zone and is held at that temperature for 20 to 40 minutes to remove physically adsorbed and chemically bound water from the fiber surface and the interior of the micropores.
[0033] After dehydration, the pretreated porous silica-rich fiber yarn is moved to the closed-cell pre-calcination zone. The heating rate of the closed-cell pre-calcination zone is controlled at 5℃ / min, raising the ambient temperature to between 600℃ and 700℃. The pretreated porous silica-rich fiber yarn continues to move within the closed-cell pre-calcination zone and is held at this temperature for 30 to 60 minutes, promoting the initial melting and pore closure of the nano-silica sol particles within the fiber micropores.
[0034] The pretreated porous silica-rich fiber yarn then enters the densification and orientation sintering temperature zone. The heating rate of the densification and orientation sintering temperature zone is controlled between 3℃ / min and 8℃ / min, raising the ambient temperature of the densification and orientation sintering temperature zone to between 850℃ and 950℃. The pretreated porous silica-rich fiber yarn continues to travel within the densification and orientation sintering temperature zone and is held at this temperature for 15 to 30 minutes. During this high-temperature stage, the silica molecular chains inside the fiber undergo intense thermal contraction and densification. Tension sensors installed on the line collect the linear tension data of the porous silica-rich fiber yarn in real time at a sampling frequency of 10 milliseconds and transmit the collected linear tension data to the tension closed-loop feedback control system. The PID controller inside the tension closed-loop feedback control system performs comparative calculations based on the set reference tension range of 0.5cN / tex to 1.0cN / tex, and outputs control electrical signals in real time to the variable frequency drive motor of the active traction roller group at the discharge end. When the linear tension of the fiber momentarily exceeds 1.0 cN / tex due to thermal shrinkage, the variable frequency drive motor of the active traction roller group slightly reduces the rotational linear speed of the active traction roller; when the linear tension is below 0.5 cN / tex, the variable frequency drive motor slightly increases the rotational linear speed of the active traction roller. Through continuous closed-loop speed regulation, the fiber macromolecular chains in the high-temperature shrinkage state are forced to complete axial orientation and densification sintering crystallization under constant micro-tension traction.
[0035] Specific experimental scenario: In the continuous industrial pilot production scenario, a continuous tunnel sintering kiln with silicon carbide heating tubes, totaling 18 meters in length and internally divided into three independently temperature-controlled sections, was used. The flow rate of the drying air entering the kiln was set to 150 m³ / h, and the measured exhaust gas dew point temperature was kept constant at -45℃. Pretreated yarn with a linear density of 1000 tex was selected as the substrate. The kiln feed end was equipped with a servo-driven active feeder with a three-roller structure, and the discharge end was equipped with a servo-driven active traction machine with a three-roller online tension meter. The dehydration section temperature was set to 350℃, the fiber residence time in the dehydration section was set to 30 minutes, and the heating slope was set to 5℃ / min. The closed-cell pre-sintering section temperature was set to 650℃, the fiber residence time in the closed-cell pre-sintering section was set to 45 minutes, and the heating slope was set to 5℃ / min. The densification and orientation sintering section temperature was set to 900℃, the fiber residence time in the densification and orientation sintering section was set to 20 minutes, and the heating slope was set to 5℃ / min. The target constant tension parameter is set to 0.8 cN / tex (i.e., the absolute tension value is controlled at 800 cN) via the PLC main control panel. In the 900℃ densification and orientation sintering section, the servo active traction machine automatically adjusts the traction line speed at a high frequency dynamic fluctuation between 8 m / min and 8.5 m / min based on the fluctuation data (±5 cN accuracy) fed back by the three-roll online tension meter, ensuring that the fiber yarn maintains an axial tensile force of 800 cN throughout the high-temperature and severe shrinkage section. Finally, a continuous high-silica fiber sintered yarn with a dense glassy luster and no visible broken filaments is drawn out.
[0036] Furthermore, the specific implementation process of step S400 is as follows: The high-silica fiber sintered yarn, drawn from the densification and orientation sintering section in step S300, is continuously fed into the slow cooling channel directly connected to the tail end of the continuous tunnel sintering kiln. The slow cooling channel is divided into multiple independently controlled cooling zones along the direction of travel of the high-silica fiber sintered yarn. The gradient cooling system equipped in the slow cooling channel is activated, and the flow rate of the cooling medium in each cooling zone is adjusted to strictly control the overall cooling rate of the high-silica fiber sintered yarn within the slow cooling channel between 10℃ / min and 15℃ / min. The surface temperature of the high-silica fiber sintered yarn is read in real time by an infrared temperature probe positioned in front of the outlet end of the slow cooling channel. When the surface temperature value reported by the infrared temperature probe is below 100℃, the high-silica fiber sintered yarn is pulled out of the slow cooling channel, exposing it to ambient air.
[0037] The high-silica fiber sintered yarn, cooled to below 100°C, is drawn to the feed end of a constant-tension precision winding machine. The constant-tension precision winding machine includes an electronic tension disc, a grooved drum, and a reciprocating yarn guide. The constant-tension precision winding machine is started, and a constant winding tension value is set via the electronic tension disc, precisely limiting the winding tension of the high-silica fiber sintered yarn between 0.1 cN / tex and 0.3 cN / tex. Simultaneously, the ratio of the traverse frequency of the reciprocating yarn guide to the rotational linear speed of the grooved drum is adjusted, setting the winding cross angle formed by the high-silica fiber sintered yarn winding on the yarn tube surface between 12° and 18°. The high-silica fiber sintered yarn is wound layer by layer under the set micro-tension and specific cross angle, ultimately forming a high-strength, high-silica fiber sintered yarn package with a flat end face. Samples are taken for testing, and the mass fraction of silica is determined to be ≥96%.
[0038] Specific experimental scenario: In the final stage of industrial mass production, a three-section water-cooled jacketed slow cooling channel with a total length of 4.5 meters is connected to the discharge port of the 900℃ sintering kiln. The ambient temperatures of the three slow cooling sections are set to 600℃, 300℃, and 80℃, respectively. 1000tex high-silica fiber sintered yarn passes through the slow cooling channel at a linear speed of 8m / min, with the measured average cooling rate controlled at 12.5℃ / min. When the yarn reaches the discharge port, the infrared online thermometer shows an absolute surface temperature of 85℃. The yarn then enters an industrial-grade precision winding machine equipped with a closed-loop tension servo motor. The target winding tension value is entered as 200cN (i.e., 0.2cN / tex) on the control panel, along with the drum reciprocating stroke and spindle speed parameters, and the actual winding cross angle is locked at 15°. The equipment operates continuously under constant tension and a fixed cross angle until it winds a cylindrical precision yarn bobbin with no protruding edges and a maximum outer diameter of 250mm, weighing 5kg. Chemical titration analysis of samples showed that the actual mass fraction of silica in the finished yarn reached 96.5%, meeting the standards for high-strength, high-silica fiber materials.
[0039] Comparative experiments and effect analysis: To further verify the technical effects of the high-silica fiber sintered yarn and its heat insulation board provided by the present invention, and to highlight the critical specificity of the process parameters of the present invention, the following comparative examples are set up for comparative verification tests.
[0040] 1. Scale settings: Example 1 of the present invention: High silica fiber sintered yarn and heat insulation board prepared using the aforementioned complete process from S100 to S400 and optimal parameters (wherein the dynamic micro-tension of sintering is 0.8 cN / tex, the heating rate is 5℃ / min, and the in-situ pretreatment adopts vacuum-pressure alternating impregnation).
[0041] Comparative Example 1 (Tension Parameter Avoidance): The remaining steps are exactly the same as in Example 1, except that the dynamic micro-tension in step S300 is set to 0.2 cN / tex.
[0042] Comparative Example 2 (Heating Kinetics Avoidance): The remaining steps are exactly the same as in Example 1, except that the heating rate in the three stages of step S300 is increased to 15°C / min.
[0043] Comparative Example 3 (Pretreatment Action Avoidance): The remaining steps are exactly the same as in Example 1, except that the vacuum-pressure alternating impregnation action in step S200 is cancelled, and the porous silicon-rich fiber yarn is soaked in the mixed solution under normal pressure for 60 minutes.
[0044] Comparative Example 4 (Conventional combination of existing technology): Conventional alkali-free glass fiber is directly coated with pure silica aerogel and cured at room temperature and pressure, without an outer silicone waterproof layer.
[0045] 2. Performance testing standards and methods: Tensile breaking strength at room temperature: The tensile breaking stress of the yarn is tested according to GB / T7690.3 standard.
[0046] Strength retention rate after high temperature thermal shock: The sample was calcined in a muffle furnace at 1000℃ for 30 minutes, and after natural cooling, the tensile strength was tested again, and the percentage of the strength at room temperature was calculated.
[0047] Vibration dust shedding rate: Referring to the national standard for drop and vibration test of new energy vehicle battery packs (GB38031-2020), the heat insulation plate was fixed on the electromagnetic vibration table, and the mass loss rate was calculated after sweeping vibration in the Z-axis direction for 2 hours.
[0048] Thermal conductivity at 1000℃: The thermal conductivity at extreme high temperatures was tested using the transient plane heat source method (ISO22007-2 standard).
[0049] 3. Compare the experimental data results: Experimental group Tensile strength at room temperature (MPa) Strength retention rate after 1000℃ thermal shock (%) Vibration powder loss rate (%) Thermal conductivity at 1000℃ (W / m·K) Macroscopic morphological assessment Example 1 88.5 92.4 0.05 0.035 The skeleton is intact, with no interface peeling. Comparative Example 1 35.2 31.8 0.08 0.038 The fibers exhibit significant brittleness and extremely poor tensile strength. Comparative Example 2 42.6 25.5 0.12 0.041 Numerous thermal stress microcracks were visible under a microscope. Comparative Example 3 86.4 88.5 5.80 0.065 Large pieces of the gel layer detached after vibration. Comparative Example 4 22.4 0.0 (Circuit breaker collapse) 18.50 0.120 (Structural failure) The fiberglass skeleton completely melted, and the insulation layer pulverized. 4. In-depth analysis of experimental data: The comparative experimental data above clearly demonstrates the profound synergistic effect of the key technical features of this invention: First, a comparison between Example 1 and Comparative Example 1 shows that the dynamic micro-tension of 0.5 cN / tex to 1.0 cN / tex defined in step S300 is the core critical condition for overcoming the "brittleness" bottleneck of high-silica yarn. When the tension is too low (0.2 cN / tex), the internal stress generated by high-temperature shrinkage cannot be offset by the axial tensile force, resulting in disordered molecular chain orientation and a precipitous drop in room temperature tensile strength and thermal shock retention rate.
[0050] Secondly, a comparison between Example 1 and Comparative Example 2 shows that strictly controlling the heating rate from 3°C / min to 8°C / min effectively avoids severe thermal shock. Comparative Example 2 used a rapid heating rate of 15°C / min, which caused the moisture in the micropores to boil out explosively and the crystal lattice to undergo a violent phase transformation, thereby inducing a large number of microcracks inside the fiber, which macroscopically manifested as a severe decrease in mechanical strength.
[0051] Third, a comparison between Example 1 and Comparative Example 3 shows that the unique vacuum-pressure alternating impregnation method in step S200 of this invention is not a simple process replacement, but a physical prerequisite for achieving microscopic chemical bonding. Comparative Example 3 uses atmospheric pressure immersion, and the mixed liquid cannot effectively enter the air-filled nanoscale micropores, resulting in weak interfacial bonding during subsequent composite aerogel formation. In vibration testing, the powder shedding rate of Comparative Example 3 is as high as 5.80%, which completely fails to meet automotive-grade dust-free requirements; while the powder shedding rate of Example 1 is only 0.05%, completely locking in dust.
[0052] Fourth, compared with Comparative Example 4 (existing technology), this invention completely solves the problem of thermal insulation failure under extreme conditions of thermal runaway in new energy batteries. Under the high temperature impact of 1000℃, the glass fiber skeleton of the existing technology directly melts, causing the thermal conductivity to soar to 0.120W / m·K; while the composite thermal insulation board of this invention, due to the synergistic temperature resistance characteristics of the high-strength high-silica skeleton and the silicon-aluminum aerogel, still maintains an extremely low thermal conductivity of 0.035W / m·K, achieving a revolutionary performance leap.
[0053] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing high-silica fiber sintered yarn for the skeleton of a battery cell's gas-silicon nano-insulation sheet, characterized in that, Includes the following steps: S100. The glass fiber yarn is placed in a composite acid solution for ultrasonic dynamic leaching to remove non-silicon metal ions from the glass fiber yarn. After washing and drying, porous silicon-rich fiber yarn is obtained. S200. The porous silicon-rich fiber yarn is immersed in a mixture containing an aminosilane coupling agent and nano-silica sol for in-situ active pretreatment, so that active groups are attached to the micropores and surface of the porous silicon-rich fiber yarn. S300. The pretreated porous silicon-rich fiber yarn is continuously fed into the sintering kiln under the dynamic micro-tension control of the drawing device for multi-stage gradient heating sintering; wherein, the dynamic micro-tension is controlled between 0.5 cN / tex and 1.0 cN / tex, and the multi-stage gradient heating sintering includes a dehydration stage, a closed-cell pre-sintering stage, and a densification orientation sintering stage in sequence. S400. The sintered fiber yarn is subjected to slow cooling treatment and then wound up to obtain the high-strength, high-silica sintered fiber yarn, whose silica mass fraction is ≥96%.
2. The method for preparing high-silica fiber sintered yarn for the battery cell gas-silicon nano-insulation sheet skeleton according to claim 1, characterized in that, In step S100, the composite acid solution is a mixed aqueous solution of hydrochloric acid and a weak organic acid, and the molar ratio of hydrochloric acid to the weak organic acid is 1:(2.0~3.0); the weak organic acid is acetic acid, and the total molar concentration of hydrogen ions in the composite acid solution is 0.5mol / L~1.5mol / L.
3. The method for preparing high-silica fiber sintered yarn for the battery cell gas-silicon nano-insulation sheet skeleton according to claim 2, characterized in that, The process parameters of the ultrasonic dynamic leaching meet the following conditions: the ultrasonic frequency is set to 40kHz~50kHz, the temperature of the leaching system is maintained at 75℃~90℃, and the continuous leaching time is 2 hours~4 hours. In step S100, the specific operations of the washing and drying process include: The filtered fiber yarn is rinsed in a step-by-step countercurrent manner with deionized water until the pH value of the eluent reaches 6.5~7.0; then the washed fiber yarn is dried in circulating hot air at 90℃~110℃ until constant weight.
4. The method for preparing high-silica fiber sintered yarn for the battery cell gas-silicon nano-insulation sheet skeleton according to claim 3, characterized in that, In step S200, the aminosilane coupling agent is selected from at least one of 3-aminopropyltriethoxysilane (KH550) or 3-aminopropyltrimethoxysilane; The mass fraction of the nano-silica sol is 10%~20%, and the average particle size of the silica in the nano-silica sol is between 5nm and 15nm. The preparation process of the mixture includes: slowly adding the aminosilane coupling agent dropwise to the nano-silica sol, then adding a weak acid to adjust the pH value of the system to 4.0~5.0, and continuously stirring at 20℃~30℃ for 1 hour to 2 hours to carry out hydrolysis and aging reaction to obtain the mixture.
5. The method for preparing high-silica fiber sintered yarn for the battery cell gas-silicon nano-insulation sheet skeleton according to claim 4, characterized in that, The in-situ active pretreatment in step S200 is specifically a vacuum-pressure alternating impregnation treatment, the operation steps of which include: The porous silica-rich fiber yarn is placed in a sealed container, and a vacuum is drawn until the absolute pressure is below 0.08 MPa and maintained for 10 to 15 minutes. The mixture is then injected until the porous silica-rich fiber yarn is completely submerged. Inert gas is then introduced into the sealed container and pressurized to 0.2 MPa to 0.4 MPa, and the pressure is maintained for 20 to 30 minutes. After depressurization, the fiber yarn is removed, and excess free liquid on the surface is removed.
6. The method for preparing high-silica fiber sintered yarn for the battery cell gas-silicon nano-insulation sheet skeleton according to claim 5, characterized in that, In step S300, the specific process parameters for each stage of the multi-stage gradient heating sintering are defined as follows: The dehydration stage has a sintering temperature of 300℃~400℃ and a holding time of 20 minutes~40 minutes; the closed-cell pre-sintering stage has a sintering temperature of 600℃~700℃ and a holding time of 30 minutes~60 minutes; the densification and orientation sintering stage has a sintering temperature of 850℃~950℃ and a holding time of 15 minutes~30 minutes; the heating rate between the dehydration stage, the closed-cell pre-sintering stage, and the densification and orientation sintering stage is independently controlled between 3℃ / min and 8℃ / min.
7. The method for preparing high-silica fiber sintered yarn for the battery cell gas-silicon nano-insulation sheet skeleton according to claim 6, characterized in that, In step S300, the method for controlling the dynamic micro-tension is specifically as follows: By using active drafting rollers installed at the feed and discharge ends of the sintering kiln in conjunction with online tension sensors, a tension closed-loop feedback adjustment system is constructed. During the densification and orientation sintering stage, when tension fluctuates due to fiber thermal shrinkage, the tension closed-loop feedback adjustment system finely adjusts the linear speed of the active drafting rollers at the discharge end in real time, so that the constant tension of the fiber yarn is always maintained between 0.5 cN / tex and 1.0 cN / tex.
8. The method for preparing high-silica fiber sintered yarn for the battery cell gas-silicon nano-insulation sheet skeleton according to claim 7, characterized in that, The multi-stage gradient heating sintering process is carried out entirely in a continuously flowing dry air atmosphere that has been dehumidified, and the gas dew point temperature in the sintering kiln is controlled below -40°C.
9. The method for preparing high-silica fiber sintered yarn for the battery cell gas-silicon nano-insulation sheet skeleton according to claim 8, characterized in that, In step S400, the specific process of the slow cooling treatment is as follows: The sintered fiber yarn is continuously passed through a slow cooling channel with a temperature gradient. The cooling rate of the fiber yarn in the slow cooling channel is controlled at 10℃ / min~15℃ / min until the surface temperature of the fiber yarn drops below 100℃ before it comes into contact with the outside room temperature air.
10. The method for preparing high-silica fiber sintered yarn for the battery cell gas-silicon nano-insulation sheet skeleton according to claim 9, characterized in that, In step S400, the winding adopts a constant tension precision winding process, the winding tension is controlled between 0.1cN / tex and 0.3cN / tex, and the winding cross angle is set between 12° and 18°.