A green composite functional fiber for shielding electromagnetic fields and its preparation process
By preparing bio-based core fibers in an aqueous phase, forming an internal conductive network and uniformly depositing magnetic particles, and combining this with phytic acid-doped polypyrrole to form a gradient impedance structure, the problem of uneven distribution of conductive and magnetic components in composite shielding fibers is solved, achieving a balance between efficient electromagnetic shielding and mechanical properties.
Patent Information
- Application Number
- CN202611138994.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-29
- Publication Date
- 2026-11-17
AI Technical Summary
Existing composite shielding fibers suffer from problems such as disordered distribution of conductive and magnetic components, insufficient interfacial bonding, excessive surface reflection, and difficulty in achieving both shielding performance and mechanical properties.
Bio-based core fibers were prepared in an aqueous phase. Sodium alginate, cellulose nanofibers and lignin-derived porous carbon materials were used to form an internal conductive network. Combined with tannic acid adsorption and iron ion coordination, iron oxide particles were uniformly deposited. Phytic acid-doped polypyrrole was used to form a continuous conductive shell. The conductivity and layer thickness were adjusted to form a gradient impedance structure.
It achieves high-efficiency electromagnetic shielding performance, increases the absorption shielding effectiveness ratio, maintains the mechanical properties and stability of the fiber, and reduces the amount of organic solvents used.
Smart Images

Figure CN123108937A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of functional fibers and electromagnetic protection materials, specifically relating to a green composite functional fiber for shielding electromagnetic fields and its preparation process. Background Technology
[0002] With the widespread application of wireless communication equipment, flexible electronic products, wearable sensors, new energy vehicle electronic systems, and high-frequency electrical equipment, complex electromagnetic environments place higher demands on the stable operation of electronic devices and electromagnetic protection for the human body. Compared with traditional electromagnetic shielding materials such as metal plates and metal meshes, fiber and textile materials have the advantages of being lightweight, flexible, easy to process, and suitable for large-area coverage, making them valuable for applications in wearable protection, electronic packaging, and flexible shielding fabrics.
[0003] Existing conductive shielding fibers are typically functionalized using metal coatings, carbon nanomaterials, conductive polymers, or magnetic particles. Metal coatings offer high conductivity and reflective shielding effectiveness, but suffer from drawbacks such as high density, limited bending resistance, easy peeling of the coating, and the generation of metal ion waste liquid during the manufacturing process. While composite fibers made from carbon materials or conductive polymers are lighter, the single conductive network tends to cause strong reflection of incident electromagnetic waves at the material surface, limiting the proportion of electromagnetic waves that penetrate the material and are absorbed and attenuated.
[0004] By combining conductive and magnetic components, conductive losses, interfacial polarization losses, and magnetic losses can be introduced simultaneously. However, existing technologies typically involve directly mixing conductive particles, magnetic particles, and a polymer matrix. This uniform mixing method easily leads to the agglomeration of conductive and magnetic particles, which is not conducive to the formation of a continuous conductive network, nor is it easy to form an impedance structure that gradually changes from the fiber's outer surface to its interior.
[0005] When the surface conductivity of a material is too high, electromagnetic waves are easily reflected strongly at the surface; when the overall conductivity of the material is too low, it is difficult to form effective conductive losses. Therefore, electromagnetic shielding performance depends not only on the content of conductive and magnetic materials, but also on the spatial distribution of each functional component in the fiber cross-sectional direction, interfacial bonding, conductivity levels, and the thickness of each functional layer.
[0006] Sodium alginate and cellulose nanofibers are widely available and can be processed in aqueous phases to form composite fibers with a certain strength. Lignin can be carbonized and activated to produce porous carbon materials. Tannic acid has multiple phenolic hydroxyl groups, which can adsorb onto the surface of bio-based fibers and form coordination with iron ions. Phytic acid contains multiple phosphate groups and can act as a protic acid dopant for polypyrrole, improving the bonding between polypyrrole segments and between polypyrrole and the iron-containing inorganic layer through multi-point ion association.
[0007] However, current technology lacks a composite fiber that can assemble the aforementioned materials in a clearly defined sequence of core, transition, and shell layers, and define the gradient impedance relationship through the synergistic effect of conductivity and thickness. Even with a three-layer structure, if the conductivity or thickness of the outer conductive shell is too high, a strong impedance abrupt change will still occur on the material surface, causing the total shielding effectiveness to mainly come from reflection, rather than achieving a high proportion of absorption shielding effectiveness.
[0008] Therefore, the following issues still need to be addressed: How to enable lignin-derived porous carbon to form a stable internal conductive network in the bio-based core layer during aqueous preparation; How to make the iron oxide particles uniformly fixed on the surface of the core fiber, instead of simply mixing them into the core layer or forming a layer of particles that are easy to fall off; How to improve the conductivity of polypyrrole by using phytic acid, while establishing a verifiable multi-point ion-associated network between polypyrrole segments and between the conductive shell and the magnetic loss transition layer; How to form an effective gradient impedance through the coordinated matching of conductivity and layer thickness, rather than simply forming a three-layer structure with a highly conductive shell; How to achieve high electromagnetic shielding effectiveness while maintaining a high absorption loss ratio, single-fiber mechanical properties, and operational stability. Summary of the Invention
[0009] The purpose of this invention is to provide a green composite functional fiber for electromagnetic shielding and its preparation process, so as to solve the problems of disordered distribution of conductive and magnetic components, insufficient interfacial bonding, excessive surface reflection, and difficulty in balancing shielding performance and mechanical properties in existing composite shielding fibers.
[0010] To achieve the above objectives, the present invention provides the following technical solution: a preparation process for a green composite functional fiber that shields electromagnetic fields, comprising the following steps.
[0011] S1, Preparation of Bio-based Core Fibers Sodium alginate, cellulose nanofibers, and lignin-derived porous carbon materials were added to water, and after dispersion and degassing, a bio-based composite spinning solution was obtained.
[0012] The bio-based composite spinning solution comprises, by weight, the following: 30-45 parts sodium alginate; 35-50 parts of cellulose nanofibers; 8–18 parts of lignin-derived porous carbon material; 1500-3000 parts water.
[0013] The bio-based composite spinning solution has a solid content of 3.0–7.0 wt% and a viscosity of 3000–12000 mPa·s at 25°C.
[0014] The cellulose nanofibers have an average diameter of 5–50 nm and a length of 0.5–5 μm.
[0015] The bio-based composite spinning solution is extruded into a coagulation bath containing soluble calcium salts for wet spinning, causing calcium ion crosslinking of sodium alginate. After stretching and washing, a bio-based core fiber containing a lignin-derived porous carbon conductive network is obtained.
[0016] Preferably, a spinneret with an inner diameter of 80–300 μm is used, and the bio-based composite spinning solution is extruded into a calcium chloride coagulation bath at a temperature of 15–35 °C at an extrusion speed of 0.2–2.0 mL / min.
[0017] The calcium chloride coagulation bath has a mass concentration of 2-6% and a coagulation time of 2-15 min.
[0018] The solidified fibers were wet-stretched at a stretching ratio of 1.1 to 1.6 to obtain bio-based core fibers with a diameter of 30 to 120 μm.
[0019] Preferred preparation method of lignin-derived porous carbon materials Lignin or lignin sulfonate is mixed with potassium carbonate and heated to 700-900℃ at a heating rate of 2-10℃ / min under inert gas protection, and held at this temperature for 1-3 hours for carbonization and activation.
[0020] The mass ratio of lignin or lignin sulfonate to potassium carbonate is 1:0.5 to 1:1.5.
[0021] The carbonization products were sequentially acid-washed, water-washed, dried, and ground to obtain lignin-derived porous carbon materials with a median particle size D50 of 100–600 nm and a specific surface area of 300–1000 m² / g.
[0022] The porous structure of lignin-derived porous carbon materials is beneficial for increasing the number of interfaces and enabling adjacent porous carbon particles to form an overlapping first conductive network within the bio-based core layer.
[0023] S2. Fabrication of the magnetic loss transition layer The bio-based core fiber is immersed in an aqueous solution of tannic acid with a concentration of 2-12 g / L and a pH of 7.5-9.0 for 10-60 min to allow the tannic acid to be adsorbed onto the surface of the bio-based core fiber.
[0024] The treated bio-based core fibers were placed in an aqueous solution containing ferrous and ferric salts. The molar ratio of ferrous to ferric ions was 1:1.8 to 1:2.2, and the total concentration of ferrous and ferric ions was 0.05 to 0.30 mol / L.
[0025] The pH of the reaction system is adjusted to 9–11 using ammonia or sodium hydroxide aqueous solution, and the reaction is carried out at 50–80℃ for 0.5–2 hours, so that the iron oxide particles nucleate and deposit in situ at the coordination sites provided by tannic acid.
[0026] The average particle size of the formed iron oxide particles is 10–80 nm, and the average thickness of the magnetic loss transition layer is 0.2–1.5 μm.
[0027] Tannic acid adsorbs onto the surface of alginate and cellulose nanofibers, and also anchors the in-situ formed iron oxide particles by coordinating with iron ions through phenolic hydroxyl groups, thereby reducing the possibility of magnetic particles agglomerating and falling off the fiber surface.
[0028] S3, Preparation of continuous conductive shell The fiber with the magnetic loss transition layer is placed in an aqueous reaction solution containing pyrrole monomer and phytic acid.
[0029] The concentration of the pyrrole monomer is 0.05–0.30 mol / L, and the concentration of phytic acid is 0.01–0.08 mol / L.
[0030] In-situ oxidative polymerization is carried out by adding a water-soluble oxidant. The water-soluble oxidant is ammonium persulfate, potassium persulfate, or ferric chloride, and the molar ratio of the water-soluble oxidant to the pyrrole monomer is 0.8:1 to 1.2:1.
[0031] The in-situ oxidative polymerization temperature is 0–10℃, and the reaction time is 2–8 h.
[0032] Phytic acid is first used to dope polypyrrole segments through protonation, thereby increasing the carrier concentration and conductivity of the polypyrrole segments.
[0033] Meanwhile, phytic acid, as a multi-point ion-associative crosslinking agent, has multiple phosphate groups on its molecule that can simultaneously form electrostatic ion pairs with multiple positively charged proton-doped polypyrrole segments, and can also form coordination bonds with Fe ions exposed in the magnetic loss transition layer.
[0034] The aforementioned multi-point electrostatic bonding and coordination bonding form a physical cross-linking network between polypyrrole segments and form multi-point interface connections between the continuous conductive shell and the magnetic loss transition layer.
[0035] The "ionic crosslinking agent" referred to in this invention refers to phytic acid forming the above-mentioned multi-point ionic association and coordination bond through multiple phosphate groups, and is not limited to forming covalent crosslinking bonds.
[0036] The multi-point ion-associative physical cross-linked network can be characterized by the solvent resistance retention rate, surface coverage retention rate, conductivity retention rate, and interfacial peel strength of the continuous conductive shell.
[0037] The average thickness of the phytic acid-doped polypyrrole continuous conductive shell is 0.3–2.0 μm, and its area coverage on the surface of the magnetic loss transition layer is not less than 90%.
[0038] S4, Post-processing Fibers with continuous conductive shells are washed, drawn, and dried to obtain green composite functional fibers that shield electromagnetic fields.
[0039] In steps S1 to S3, water is used as the continuous dispersion medium or reaction medium, and no organic solvents are used.
[0040] The green composite functional fiber prepared by this invention comprises, from the inside out, a bio-based conductive core layer, a tannic acid-iron coordination magnetic loss transition layer, and a phytic acid-doped polypyrrole continuous conductive shell layer.
[0041] The equivalent conductivity of the bio-based conductive core layer is denoted as σ1, the equivalent conductivity of the magnetic loss transition layer is denoted as σ2, and the equivalent conductivity of the continuous conductive shell layer is denoted as σ3.
[0042] The three-layer structure satisfies: σ3>σ1>σ2; σ3 / σ1 ranges from 1.2 to 8.0; σ1 / σ2 ranges from 2 to 50.
[0043] The average thickness of the continuous conductive shell is denoted as t3, and the average thickness of the magnetic loss transition layer is denoted as t2. The ratio of t3 to t2 is 1:0.3 to 1:2.
[0044] In a preferred embodiment of the present invention: σ3 / σ1 is 2.0 to 2.5; σ1 / σ2 is 15 to 30; The ratio of t3 to t2 is 1:0.5 to 1:1.5.
[0045] When the three parameters are all within the above-mentioned preferred range, the absorption shielding effectiveness (SEA) of the fiber fabric in the 8.2–12.4 GHz frequency band accounts for more than 70% of the total shielding effectiveness (SET).
[0046] The parameter range does not imply that higher conductivity or greater thickness of the continuous conductive shell is always more advantageous. When σ3 / σ1 exceeds 8.0, or when t3∶t2 exceeds the shell relative thickness corresponding to 1∶0.3, a large impedance abrupt change is easily formed between the outer layer and the internal structure, which significantly improves the reflection shielding effectiveness SER, while the absorption shielding effectiveness SEA as a proportion of the total shielding effectiveness SET decreases.
[0047] The equivalent conductivity was characterized using an independent simulated membrane.
[0048] The bio-based conductive core layer simulated membrane was prepared using the same proportion of solid raw materials as the bio-based conductive core layer and was cross-linked with calcium chloride.
[0049] The magnetic loss transition layer simulation film uses the same ratio of tannic acid, ferrous salt, and ferric salt as the magnetic loss transition layer, reacts in situ on a polytetrafluoroethylene plate, and is then peeled off after drying.
[0050] The continuous conductive shell simulation film uses the same ratio of pyrrole, phytic acid and oxidant as the continuous conductive shell, and is polymerized in situ on a polytetrafluoroethylene plate, then washed, dried and peeled off.
[0051] After each simulated membrane was conditioned for 24 hours at 25±2℃ and 65±4% relative humidity, its volumetric conductivity was measured.
[0052] The difference in conductivity among the three layers creates a continuous conductive loss path in the outer layer. The middle low-conductivity magnetic loss layer reduces the impedance abrupt change between the high-conductivity outer layer and the inner core layer, and introduces magnetic loss and interface polarization. The internal porous carbon conductive network further generates conductive loss and multiple reflections.
[0053] Based on 100% dry weight of green composite functional fibers, the preferred composition includes: Calcium ion crosslinked alginate and cellulose nanofibers: 55-61%; Lignin-derived porous carbon materials: 9-13%; The magnetic loss transition layer, comprising 11–16% of the structure of ferric oxide and tannic acid-iron coordination, is composed of iron oxide. Phytic acid-doped polypyrrole continuous conductive shell 16-20%.
[0054] The sum of the contents of each component is 100%.
[0055] Within the aforementioned composition range, by adjusting the relative contents of the bio-based matrix, porous carbon, iron oxide, and polypyrrole, the mechanical properties, electrical conductivity, shielding effectiveness, and absorption shielding effectiveness ratio of the single fiber can be adjusted.
[0056] Compared with the prior art, the present invention provides a green composite functional fiber for shielding electromagnetic fields and its preparation process, which has the following beneficial effects: using alginate and cellulose nanofibers to form a bio-based load-bearing skeleton, and lignin-derived porous carbon forming a first conductive network inside the core layer, it can maintain the spinnability and mechanical properties of the fiber while reducing the amount of petrochemical polymers used.
[0057] This invention induces in-situ nucleation of iron oxide on the surface of the core fiber through tannic acid surface adsorption and iron ion coordination, so that the magnetic particles are concentrated between the conductive core layer and the conductive shell layer, avoiding the disorderly agglomeration of magnetic particles inside the core layer.
[0058] Phytic acid combines the effects of protic acid doping and multi-point ion-associative crosslinking in polypyrrole, which can improve the conductivity of polypyrrole and enhance the bonding between polypyrrole segments and between the continuous conductive shell and the magnetic loss transition layer.
[0059] The multi-point ion pairs formed by phytic acid polyphosphate groups and the coordination effect of Fe enable the continuous conductive shell to maintain a high quality retention rate, coverage rate and conductivity retention rate after being soaked in N-methylpyrrolidone, and improve the peel strength between the conductive shell and the magnetic loss transition layer.
[0060] This invention forms a graded gradient impedance structure in the fiber cross-section direction by making σ3 > σ1 > σ2 and controlling σ3 / σ1, σ1 / σ2, and t3∶t2. Compared with abrupt impedance structures that only have a highly conductive thick shell, this structure can reduce SER and improve SEA and SEA / SET while maintaining a high SET.
[0061] This invention employs an internal porous carbon conductive network and an external polypyrrole conductive shell to form a dual conductive network. Even if local cracks appear in the outer layer, the internal conductive network can still maintain a certain level of conductivity and electromagnetic shielding.
[0062] The main spinning, magnetic layer construction, and polypyrrole polymerization processes of this invention are all carried out in an aqueous phase without the use of organic solvents, thus reducing the need for organic solvent recovery and volatile organic compound treatment. Attached Figure Description
[0063] Figure 1 This is a SEM comparison image of the three-layer structure of the green composite functional fiber cross-section in Example 4 and Comparative Example 6 of the present invention; Figure 2 This is a comparison image of in-situ nucleation SEM and Fe element surface distribution in the Fe3O4 magnetic loss transition layer of Example 4 and Comparative Example 2. Figure 3 This is a SEM comparison image of the continuous conductive shell morphology of phytic acid-doped polypyrrole in Example 4 and Comparative Example 4 of the present invention. Figure 4 This is a high-magnification SEM comparison image of the thickness of the continuous conductive shell and the gradient structure cross-section of Example 4 and Comparative Example 7 of the present invention. Detailed Implementation
[0064] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0065] Please see Figures 1-4This invention provides a technical solution for a green composite functional fiber for shielding electromagnetic fields and its preparation process: Unless otherwise specified, all percentages are mass percentages; the water is deionized water; the conductivity test temperature is 25±2℃; the examples and comparative examples all use the same batch of sodium alginate, cellulose nanofibers, tannic acid, phytic acid, pyrrole and iron salts.
[0066] Preparation parameters of lignin-derived porous carbon materials.
[0067] Table 1. Preparation parameters of lignin-derived porous carbon materials
[0068] Example 1 contains the low-value end of the lignin-derived porous carbon preparation parameters, Example 2 is located in the middle region, Example 3 contains the high-value end, and Examples 4 to 6 are used to verify the feasibility of different cross combinations.
[0069] Preparation parameters of bio-based core fibers Table 2 Composition of Bio-based Composite Spinning Solution
[0070] Table 3 Wet spinning parameters
[0071] Parameters of magnetic loss transition layer and continuous conductive shell Table 4 Fabrication parameters of the magnetic loss transition layer
[0072] Table 5 Parameters for the fabrication of continuous conductive shells
[0073] Examples 5 and 6 cover the endpoints of ranges where t3∶t2 is 1∶2 and 1∶0.3, respectively.
[0074] Example 1 Sodium lignosulfonate and potassium carbonate were mixed at a mass ratio of 1:0.5, and the mixture was heated to 700℃ at a rate of 2℃ / min under nitrogen protection and held at that temperature for 1 hour. After cooling, the mixture was washed with 1 mol / L hydrochloric acid aqueous solution, then washed with water until neutral, dried, and ground to obtain a lignin-derived porous carbon material with a D50 of 100 nm and a specific surface area of 300 m² / g.
[0075] 30 parts sodium alginate, 35 parts cellulose nanofibers and 8 parts lignin-derived porous carbon material were added to 2360 parts water, dispersed at high speed for 30 min, ultrasonically dispersed for 20 min, and degassed under vacuum to obtain a spinning solution with a solid content of 3.0 wt%.
[0076] Using a spinneret with an inner diameter of 80 μm, the fiber was extruded into a 2% calcium chloride aqueous solution at 15 °C at a rate of 0.2 mL / min, coagulated for 2 min, wet-stretched at 1.6 times, and washed with water to obtain a bio-based core fiber with a diameter of approximately 30 μm.
[0077] The core fibers were immersed in a 2 g / L tannic acid aqueous solution with a pH of 7.5 for 10 min, and then placed in a solution with a total iron ion concentration of 0.05 mol / L and Fe²⁺. + With Fe³ + In an aqueous solution with a molar ratio of 1:1.8, the pH was adjusted to 9, and the reaction was carried out at 50°C for 0.5 h to form a magnetic loss transition layer with a thickness of about 0.20 μm.
[0078] The fiber was placed in an aqueous solution with a pyrrole concentration of 0.05 mol / L and a phytic acid concentration of 0.01 mol / L. Ammonium persulfate was added at 0°C with a molar ratio of ammonium persulfate to pyrrole of 0.8:1. The reaction was carried out for 8 hours to form a continuous conductive shell with a thickness of about 0.30 μm.
[0079] The fibers were washed, stretched, and dried to obtain the green composite functional fiber of Example 1.
[0080] Example 2 Example 2 was prepared according to the same basic process as Example 1, except that the lignin-derived porous carbon material, bio-based composite spinning solution, wet spinning, magnetic loss transition layer and continuous conductive shell were prepared using the parameters of Example 2 in Tables 1 to 5.
[0081] Example 3 Example 3 was prepared according to the same basic process as Example 1, except that the parameters of Example 3 in Tables 1 to 5 were used.
[0082] Example 4 Sodium lignosulfonate and potassium carbonate were mixed at a mass ratio of 1:1 and heated to 800℃ at a rate of 5℃ / min under nitrogen protection, and held at that temperature for 2 hours. After acid washing, water washing, drying and grinding, a lignin-derived porous carbon material with a D50 of 250nm and a specific surface area of 720m² / g was obtained.
[0083] 40 parts sodium alginate, 45 parts cellulose nanofibers and 15 parts lignin-derived porous carbon material were added to 2100 parts water, dispersed, ultrasonicated and degassed under vacuum to obtain a bio-based composite spinning solution with a solid content of 4.5 wt% and a viscosity of 7200 mPa·s.
[0084] Using a spinneret with an inner diameter of 180 μm, the fiber was extruded into a 4% calcium chloride aqueous solution at 25 °C at a rate of 1.0 mL / min, solidified for 8 min, and then wet-stretched at a ratio of 1.3 to obtain a bio-based core fiber with a diameter of approximately 80 μm.
[0085] The core fibers were treated in a 6 g / L tannic acid aqueous solution (pH 8.0) for 30 min. Subsequently, they were placed in a solution with a total iron ion concentration of 0.16 mol / L and Fe²⁺. + With Fe³ + In an aqueous solution with a molar ratio of 1:2, the pH was adjusted to 10, and the reaction was carried out at 65°C for 1 hour to form a magnetic loss transition layer with a thickness of about 0.80 μm.
[0086] The fiber was placed in an aqueous solution with a pyrrole concentration of 0.15 mol / L and a phytic acid concentration of 0.03 mol / L. Ammonium persulfate with an equimolar amount of pyrrole was added at 5°C, and the reaction was carried out for 4 hours to form a continuous conductive shell with a thickness of about 1.00 μm and a coverage of about 96.5%.
[0087] The fibers were washed, stretched to 1.05 times their original length, and dried at 60°C to obtain the green composite functional fiber of Example 4.
[0088] Example 5 Example 5 was prepared according to the same basic process as Example 1, using the parameters of Example 5 in Tables 1 to 5.
[0089] Example 6 Example 6 was prepared according to the same basic process as Example 1, using the parameters of Example 6 in Tables 1 to 5.
[0090] Fiber dry weight composition Table 6. Fiber dry weight composition of Examples 1-6
[0091] Comparative Example 1 differs only in that lignin-derived porous carbon materials are not added to the bio-based composite spinning solution; all other conditions are the same as in Example 4.
[0092] Comparative Example 2 differs only in that the tannic acid aqueous solution treatment step is omitted, and the bio-based core fiber is directly placed in an aqueous solution of ferrous and ferric salts for iron oxide deposition. All other conditions are the same as in Example 4.
[0093] Comparative Example 3 differs only in that the same mass of iron oxide particles as in Example 4 is directly added to the bio-based composite spinning solution, and no independent magnetic loss transition layer is set on the surface of the core fiber. All other conditions are the same as in Example 4.
[0094] Comparative Example 4 differs only in that hydrochloric acid of equal proton equivalent is used instead of phytic acid as the polypyrrole dopant, while the pyrrole concentration, oxidant dosage, polymerization temperature, and polymerization time are the same as in Example 4.
[0095] Comparative Example 5 differs only in that it does not undergo in-situ polymerization of pyrrole and does not form a continuous conductive shell; all other conditions are the same as in Example 4.
[0096] Comparative Example 6 Comparative Example 6 uses the same dry weight composition as Example 4, consisting of alginate, cellulose nanofibers, porous carbon, iron oxide, and polypyrrole. However, the porous carbon, iron oxide, and pre-prepared phytic acid-doped polypyrrole particles are mixed into the spinning solution in a single step for wet spinning, thus avoiding the formation of a core-transition-shell structure. Except for the spatial assembly method of the functional components, the other conditions are the same as in Example 4.
[0097] Comparative Example 7 Comparative Example 7 is based on Example 4, except that the concentration of pyrrole monomer in step S3 is increased from 0.15 mol / L to 0.50 mol / L, while the phytic acid concentration, the molar ratio of ammonium persulfate to pyrrole, the polymerization temperature and the polymerization time remain unchanged.
[0098] The continuous conductive shell prepared in Comparative Example 7 had an average thickness of 3.60 μm, an equivalent conductivity σ3 of 160 S / cm, an equivalent conductivity σ1 of 18.0 S / cm for the bio-based conductive core, and an equivalent conductivity σ2 of 0.60 S / cm for the magnetic loss transition layer.
[0099] In Comparative Example 7, σ3 / σ1 is 8.89 and t3∶t2 is 1∶0.22, both of which exceed the scope of this invention.
[0100] Although Comparative Example 7 still has a core-transition-shell structure and the electrical conductivity values are still in the order of σ3 > σ1 > σ2, the conductivity and thickness of the outer conductive shell are too high relative to the internal structure, resulting in a sudden impedance structure caused by a high-conductivity thick shell.
[0101] Performance testing 1. Specific surface area testing of porous carbon The specific surface area of lignin-derived porous carbon materials was determined using the nitrogen adsorption BET method according to GB / T 19587—2017. This standard is currently the prevailing standard.
[0102] 2. Fiber cross-section and layer thickness testing The fiber was placed in liquid nitrogen and fractured brittlely. After gold sputtering, the cross-section was observed using a scanning electron microscope.
[0103] No fewer than 10 fibers are randomly selected from each group, and no fewer than 10 measurements are taken at each fiber along the circumference. The arithmetic mean of the core diameter, transition layer thickness, and shell thickness is calculated respectively.
[0104] The coverage of the conductive shell was analyzed using binarized SEM images of the fiber surface. At least 20 fields of view were randomly selected for each group, and the coverage was defined as the ratio of the surface projection area covered by polypyrrole to the total surface projection area.
[0105] 3. Testing of equivalent conductivity of layered structures and conductivity of single fibers The resistivity tests of each individual simulated membrane and single composite fiber were conducted in accordance with GB / T 12703.4—2010, using a four-probe test fixture adapted to the sample size. GB / T 12703.4—2010 is currently the prevailing standard.
[0106] The ends of each fiber were fixed with conductive silver paste, and the effective test length was 20 mm. The fiber cross-sectional area was calculated based on the average diameter measured by SEM.
[0107] The conductivity of a single fiber is calculated using the following formula: σ = L / (R×A).
[0108] Where σ is the conductivity, L is the effective test length, R is the measured resistance, and A is the fiber cross-sectional area.
[0109] Each test group should contain no fewer than 10 fibers, and the results should be the arithmetic mean.
[0110] 4. Single fiber tensile property test The tensile properties of a single green composite functional fiber are tested according to GB / T 14344—2022 using a single-fiber clamp. This standard is currently the prevailing standard.
[0111] The sample was conditioned for 24 hours at a temperature of 20±2℃ and a relative humidity of 65±4%.
[0112] The clamping distance is 20 mm, and the tensile speed is 10 mm / min. Each test group consists of no less than 20 fibers. After removing the specimens that break abnormally at the clamps, the arithmetic mean of the tensile strength and elongation at break is calculated.
[0113] 5. Preparation of Fiber Fabrics Plain weave fabrics were made using the same weaving density for the fibers of each embodiment and comparative example.
[0114] By adjusting the warp and weft densities, the fabric surface density is made to be 120±3g / m², and the thickness is 0.45±0.02mm.
[0115] The fabric's unit area mass is determined according to GB / T 4669—2008, which is currently the prevailing standard.
[0116] 6. Electromagnetic shielding performance test The electromagnetic shielding performance of planar fabric materials was tested using a vector network analyzer and a coaxial fixture, following the method described in ASTM D4935-18. ASTM D4935-18 is still listed in the current standard catalog.
[0117] The test frequency band is 8.2 to 12.4 GHz.
[0118] Calculate reflectivity R, transmittance T, and absorptivity A based on the scattering parameters: R = |S 11 |²; T = |S 21 |²; A = 1 - R - T.
[0119] The total electromagnetic shielding effectiveness (SET) is calculated using the following formula: SET = -10lgT.
[0120] The reflection shielding effectiveness SER is calculated according to the following formula: SER = -10lg(1-R).
[0121] The absorption and shielding effectiveness (SEA) is calculated using the following formula: SEA=-10lg[T / (1-R)].
[0122] The contribution ratio of absorption and shielding effectiveness is calculated as SEA / SET×100%.
[0123] For each tissue sample, at least five samples should be tested, and the average value within the 8.2–12.4 GHz frequency band should be taken.
[0124] 7. Washing stability test Fabric washing and treatment shall be carried out in accordance with GB / T 8629—2017. This standard is currently the prevailing standard.
[0125] After 10 washes, the average total electromagnetic shielding effectiveness of the fabric was retested, and the ratio of the SET after washing to the SET before washing was used as the shielding effectiveness retention rate.
[0126] 8. Solvent stability test of N-methylpyrrolidone Following the evaluation criteria for liquid chemical reagent immersion in GB / T 11547—2008, N-methylpyrrolidone immersion tests were conducted on Example 4 and Comparative Example 4. GB / T 11547—2008 is currently the prevailing standard.
[0127] Each group weighs out a fiber bundle with an initial dry weight of 100±2mg, denoted as m0.
[0128] The fiber bundle was placed in 20 mL of N-methylpyrrolidone and soaked at 25±2 °C for 24 h, while shaking at 60 r / min.
[0129] After soaking, it was washed three times with anhydrous ethanol and dried to constant weight under vacuum at 60℃, which was recorded as m1.
[0130] The shell mass retention rate is calculated as m1 / m0×100%.
[0131] The shell area coverage was re-determined using SEM, and the fiber bundle conductivity was tested. The ratio of conductivity after immersion to conductivity before immersion was defined as the conductivity retention rate.
[0132] 9. Continuous conductive shell interface peel strength test Using the same raw material ratio and processing conditions as the corresponding fibers, a magnetic loss transition layer and a continuous conductive shell were sequentially prepared on the surface of a flexible alginate-cellulose nanofiber membrane to obtain a simulated layered membrane.
[0133] A high-strength polyester backing is bonded to the surface of the continuous conductive shell, and a peeling start end is reserved.
[0134] Referencing GB / T 2790—1995, the interfacial peel strength between the continuous conductive shell and the magnetic loss transition layer is determined using a 180° peel method. GB / T 2790—1995 is currently the prevailing standard.
[0135] The sample width is 25 mm, the peeling speed is 100 mm / min, and each group of tests shall have no less than 5 samples. The average peeling force in the stable peeling range shall be taken and converted into peeling strength per unit width.
[0136] This test is used for a relative comparison between Example 4 and Comparative Example 4, and does not directly equate the peel strength of the simulated layered membrane to the absolute interfacial strength of a single cylindrical fiber.
[0137] Test Results Table 7. Test results of the three-layer structure and conductivity.
[0138] Table 8 Draft data on single-fiber performance and electromagnetic shielding performance of the embodiments
[0139] Table 9. Relationship between gradient impedance parameters and the proportion of absorption shielding contribution.
[0140] As shown in Table 9, Examples 2 and 4 simultaneously satisfy σ3 / σ1 = 2.0 to 2.5, σ1 / σ2 = 15 to 30, and t3:t2 = 1:0.5 to 1:1.5, with SEA / SET reaching 71.2% and 77.2%, respectively.
[0141] Example 1 has a small conductivity gradient and insufficient conductivity loss capability; Example 3 has σ1 / σ2 reaching 50, indicating a large conductivity difference between the core layer and the transition layer; Example 5 has a relatively thick magnetic loss transition layer; Example 6 has a relatively thick continuous conductive shell. Although the above examples all satisfy the basic scope of the claims, their SEA / SET is lower than that of Examples 2 and 4 within the preferred window.
[0142] Table 10 Draft data of test results for Example 4 and comparative examples
[0143] Table 11 Macroscopic verification results of phytic acid multi-point ion association
[0144] Test Result Analysis As can be seen from Examples 1 to 6, within the range of composition, process, conductivity and layer thickness defined by the present invention, green composite functional fibers with a core-transition-shell structure can be prepared.
[0145] Example 1 has a high proportion of bio-based matrix and a low content of conductive components. It has high tensile strength and elongation at break, and its electrical conductivity and electromagnetic shielding effectiveness are in the low value range of the present invention.
[0146] Example 3 has a high content of porous carbon and polypyrrole, and its single fiber conductivity and total electromagnetic shielding effectiveness are high, but its tensile strength and elongation at break are close to the low value range of the present invention.
[0147] In Examples 2 and 4, σ3 / σ1, σ1 / σ2, and t3∶t2 are all within the preferred gradient window, and the SEA / SET of both examples reaches more than 70%.
[0148] Example 4 achieves a suitable conductivity and layer thickness match between the conductive core layer, the magnetic loss transition layer, and the continuous conductive shell layer, with an average total shielding effectiveness of 49.1 dB, an SEA of 37.9 dB, and an SEA / SET ratio of 77.2%.
[0149] As can be seen from Example 4 and Comparative Example 1, without the addition of lignin-derived porous carbon material, the single fiber conductivity decreased from 34.2 S / cm to 9.5 S / cm, and the SET decreased from 49.1 dB to 32.8 dB, indicating that the internal porous carbon conductive network is an important component in forming dual conductive pathways and improving electromagnetic shielding effectiveness.
[0150] As can be seen from Example 4 and Comparative Example 2, after omitting the tannic acid pretreatment, it is difficult for iron oxide to form a uniform and continuous anchoring layer on the surface of the core fiber. The coverage of the polypyrrole shell layer decreased from 96.5% to 58.4%, and the shielding effectiveness retention rate decreased from 93.5% to 68.7% after 10 washes.
[0151] As can be seen from Example 4 and Comparative Example 3, when iron oxide is directly mixed into the core layer, although the material contains the same mass of magnetic components, it cannot form an independent magnetic loss transition layer between the two conductive networks, and its SET and SEA are significantly reduced.
[0152] As can be seen from Example 4 and Comparative Example 4, after replacing phytic acid with hydrochloric acid, polypyrrole still has a high conductivity, but the tensile strength, SEA / SET and washing stability are significantly reduced.
[0153] As shown in Table 11, the mass retention rate, shell coverage rate and conductivity retention rate of Example 4 after NMP immersion are significantly higher than those of Comparative Example 4; the simulated layered membrane interface peel strength of Example 4 is 1.82 N / cm, which is about 2.46 times that of Comparative Example 4.
[0154] The above results indicate that the role of phytic acid is not limited to ordinary proton acid doping. Multiple phosphate groups on the phytic acid molecule form electrostatic ion pairs with multiple proton-doped polypyrrole segments and coordinate with Fe ions in the magnetic loss transition layer, forming a multi-point physical cross-linking network between polypyrrole segments and between the continuous conductive shell and the magnetic loss transition layer.
[0155] As shown in Example 4 and Comparative Example 5, when a continuous polypyrrole conductive shell is not formed, the single-fiber conductivity and overall shielding effectiveness are significantly reduced. Although the SEA / SET ratio is still relatively high, the absolute SEA and SET are insufficient.
[0156] As can be seen from Example 4 and Comparative Example 6, when the total content of each functional component is basically the same, the SET is only 40.1dB and the SEA / SET is 56.6% when porous carbon, iron oxide and polypyrrole are uniformly mixed into the core layer, which is significantly lower than that in Example 4, indicating that the layered structure is not a simple superposition of components.
[0157] As can be seen from Example 4 and Comparative Example 7, Comparative Example 7 significantly increased the conductivity and thickness of the outer polypyrrole shell by increasing the pyrrole concentration alone. Its SET reached 52.6 dB, slightly higher than that of Example 4, but the SER increased from 11.2 dB to 27.0 dB, and the SEA / SET decreased from 77.2% to 48.7%.
[0158] Comparative Example 7 shows that although increasing the outer layer conductivity and shell thickness can improve the overall shielding effectiveness, the shielding mechanism is mainly transformed into surface reflection, and the high absorption contribution ratio pursued by this invention cannot be obtained.
[0159] Both Example 4 and Comparative Example 7 have a core-transition-shell structure. The main difference between them lies in whether the conductivity and thickness of the outer conductive shell match the internal structure. Therefore, Comparative Example 7 further demonstrates that the technical effect of the present invention does not solely originate from the three-layer structure itself, but rather from the synergistic effect of the conductivity gradient and layer thickness ratio of the three-layer structure.
[0160] Based on the embodiments and comparative examples, the technical effects of the present invention derive from the following synergistic relationships: Lignin-derived porous carbon constructs the first conductive network inside the bio-based core layer; Tannic acid induces in-situ nucleation of iron oxide through surface adsorption and iron ion coordination, forming a continuous magnetic loss transition layer; Phytic acid acts as both a protic acid dopant and a multi-point ion-associated crosslinking agent for polypyrrole, forming a stable second conductive network. The three-layer structure satisfies σ3>σ1>σ2, and forms a graded rather than abrupt gradient impedance through the matching of σ3 / σ1, σ1 / σ2 and t3∶t2; When electromagnetic waves enter the fiber, they undergo sequential conductive loss, interface polarization loss, magnetic loss, and multiple reflection loss.
Claims
1. A preparation process for a green composite functional fiber that shields electromagnetic fields, characterized in that, Includes the following steps: S1. Sodium alginate, cellulose nanofibers and lignin-derived porous carbon materials are added to water, and after dispersion and degassing, a bio-based composite spinning solution is obtained. The bio-based composite spinning solution is extruded into a coagulation bath containing soluble calcium salts for wet spinning, so that sodium alginate undergoes ionic cross-linking. After stretching and washing, a bio-based core fiber containing a lignin-derived porous carbon conductive network is obtained. S2. The bio-based core fiber is immersed in an aqueous solution of tannic acid, allowing the tannic acid to be adsorbed onto the surface of the bio-based core fiber. Subsequently, the bio-based core fiber adsorbed with tannic acid is placed in an aqueous solution containing ferrous and ferric ions. The pH of the aqueous solution is adjusted to 9-11, and the reaction is carried out at 50-80°C, so that the iron oxide particles are nucleated and deposited in situ at the coordination sites provided by the tannic acid, forming a tannic acid-iron coordination magnetic loss transition layer on the surface of the bio-based core fiber. S3. The fiber with the magnetic loss transition layer is placed in an aqueous reaction solution containing pyrrole monomer and phytic acid. A water-soluble oxidant is added for in-situ oxidative polymerization, so that the polypyrrole with phytic acid as a dopant and ionic crosslinking agent forms a continuous conductive shell on the surface of the magnetic loss transition layer. The phytic acid improves the conductivity of polypyrrole by proton acid doping of the polypyrrole segments, and forms multi-point ionic association and interfacial bonding between the polypyrrole segments and between the polypyrrole and the magnetic loss transition layer through its polyphosphate groups. S4. The fiber with the continuous conductive shell is washed, stretched and dried to obtain a green composite functional fiber that shields electromagnetic fields. The green composite functional fiber comprises, from the inside out, a bio-based conductive core layer, a tannic acid-iron coordination magnetic loss transition layer, and a phytic acid-doped polypyrrole continuous conductive shell layer. The lignin-derived porous carbon conductive network and the phytate-doped polypyrrole continuous conductive shell form internal conductive pathways and surface conductive pathways, respectively. The iron oxide particles in the magnetic loss transition layer provide magnetic loss. The bio-based conductive core, magnetic loss transition layer and continuous conductive shell form a hierarchical gradient impedance structure through the difference in conductivity and layer thickness.
2. The preparation process of the green composite functional fiber for shielding electromagnetic fields according to claim 1, characterized in that, In step S1, the bio-based composite spinning solution comprises, by weight, the following: 30-45 parts sodium alginate; 35-50 parts of cellulose nanofibers; 8–18 parts of lignin-derived porous carbon material; 1500-3000 parts water; The bio-based composite spinning solution has a solid content of 3.0–7.0 wt% and a viscosity of 3000–12000 mPa·s at 25°C. The cellulose nanofibers have an average diameter of 5–50 nm and a length of 0.5–5 μm.
3. The preparation process of the green composite functional fiber for shielding electromagnetic fields according to claim 1, characterized in that, The lignin-derived porous carbon material was prepared by the following method: Lignin or lignin sulfonate is mixed with potassium carbonate and heated to 700-900°C at a heating rate of 2-10°C / min under inert gas protection, and held at that temperature for 1-3 hours for carbonization and activation. The mass ratio of lignin or lignin sulfonate to potassium carbonate is 1:0.5 to 1:1.5; The carbonization products were sequentially acid-washed, water-washed, dried, and ground to obtain lignin-derived porous carbon materials with a median particle size D50 of 100–600 nm and a specific surface area of 300–1000 m² / g.
4. The preparation process of the green composite functional fiber for shielding electromagnetic fields according to claim 1, characterized in that, Step S1 specifically includes: The bio-based composite spinning solution was extruded into a coagulation bath at a temperature of 15–35°C using a spinneret with an inner diameter of 80–300 μm and an extrusion speed of 0.2–2.0 mL / min. The coagulation bath is a calcium chloride aqueous solution with a mass concentration of 2-6%, and the coagulation time is 2-15 min; The solidified fibers were wet-stretched at a stretch ratio of 1.1 to 1.6 and washed with deionized water to obtain bio-based core fibers with a diameter of 30 to 120 μm.
5. The preparation process of the green composite functional fiber for shielding electromagnetic fields according to claim 1, characterized in that, Step S2 specifically includes: The bio-based core fiber was immersed in an aqueous solution of tannic acid with a concentration of 2-12 g / L and a pH of 7.5-9.0 for 10-60 min. The treated bio-based core fiber was placed in an aqueous solution containing ferrous salt and ferric salt, wherein the molar ratio of ferrous ions to ferric ions was 1:1.8 to 1:2.2, and the total concentration of ferrous ions and ferric ions was 0.05 to 0.30 mol / L. The pH of the reaction system was adjusted to 9–11 using ammonia or sodium hydroxide aqueous solution, and the reaction was carried out at 50–80℃ for 0.5–2 hours. The average particle size of the formed iron oxide particles is 10–80 nm, and the average thickness of the tannic acid-iron coordination magnetic loss transition layer is 0.2–1.5 μm.
6. The preparation process of the green composite functional fiber for shielding electromagnetic fields according to claim 1, characterized in that, In step S3: The concentration of the pyrrole monomer in the aqueous reaction solution is 0.05–0.30 mol / L; The concentration of phytic acid in the aqueous reaction solution is 0.01–0.08 mol / L; The water-soluble oxidant is ammonium persulfate, potassium persulfate, or ferric chloride, and the molar ratio of the water-soluble oxidant to the pyrrole monomer is 0.8:1 to 1.2:
1. The in-situ oxidative polymerization is carried out at a temperature of 0–10°C for a reaction time of 2–8 h. The average thickness of the formed phytic acid-doped polypyrrole continuous conductive shell is 0.3 to 2.0 μm, and the area coverage of the continuous conductive shell on the surface of the magnetic loss transition layer is not less than 90%.
7. The preparation process of the green composite functional fiber for shielding electromagnetic fields according to claim 1, characterized in that: The iron oxide particles in the magnetic loss transition layer are fixed to the surface of the bio-based core fiber through the coordination structure formed by the phenolic hydroxyl groups of tannic acid and iron ions. The phytic acid-doped polypyrrole continuous conductive shell and the magnetic loss transition layer are bonded together by hydrogen bonding, electrostatic interaction, iron ion coordination and multi-point ion association formed by phytic acid polyphosphate groups. The lignin-derived porous carbon material overlaps with each other inside the bio-based core fiber to form a first conductive network, and the phytic acid-doped polypyrrole continuous conductive shell forms a second conductive network. The iron oxide particles are distributed between the first and second conductive networks, causing electromagnetic waves entering the fiber to generate conductive losses, dipole polarization losses, interface polarization losses, magnetic losses, and multiple reflection losses.
8. The preparation process of the green composite functional fiber for shielding electromagnetic fields according to claim 1, characterized in that, The resulting green composite functional fiber forms a graded impedance structure by controlling the conductivity and thickness of the three-layer structure: The equivalent conductivity of the bio-based conductive core layer is σ1, the equivalent conductivity of the tannic acid-iron coordination magnetic loss transition layer is σ2, and the equivalent conductivity of the phytic acid-doped polypyrrole continuous conductive shell layer is σ3, and satisfies: σ3>σ1>σ2; σ3 / σ1 ranges from 1.2 to 8.0, and σ1 / σ2 ranges from 2 to 50; The average thickness of the continuous conductive shell is t3, the average thickness of the magnetic loss transition layer is t2, and the ratio of t3 to t2 is 1:0.3 to 1:
2. The equivalent conductivity σ1, σ2 and σ3 are characterized by the volume conductivity of independent films prepared using the same raw material composition and processing conditions as the corresponding layers, measured at 25±2℃. Through the synergy of the conductivity levels and thickness ratios, electromagnetic waves undergo impedance changes and multi-interface attenuation between the continuous conductive shell, the magnetic loss transition layer, and the bio-based conductive core layer.
9. A green composite functional fiber for shielding electromagnetic fields, characterized in that, include: A bio-based conductive core layer comprising calcium ion-crosslinked alginate, cellulose nanofibers, and lignin-derived porous carbon material dispersed between the alginate and cellulose nanofibers. A magnetic loss transition layer is coated on the outside of the bio-based conductive core layer. The magnetic loss transition layer includes a tannic acid-iron coordination structure and iron oxide particles fixed by the tannic acid-iron coordination structure. A continuous conductive shell covering the magnetic loss transition layer, the continuous conductive shell comprising polypyrrole with phytic acid as a dopant and ionic crosslinking agent; The diameter of the bio-based conductive core layer is 30–120 μm, the average thickness of the magnetic loss transition layer is 0.2–1.5 μm, and the average thickness of the continuous conductive shell layer is 0.3–2.0 μm. The average particle size of the iron oxide particles is 10-80 nm, and the area coverage of the continuous conductive shell on the surface of the magnetic loss transition layer is not less than 90%. The equivalent conductivity of the bio-based conductive core layer, the magnetic loss transition layer, and the continuous conductive shell layer are σ1, σ2, and σ3, respectively, and satisfy σ3 > σ1 > σ2.