A method for preparing a wet strength agent with low organochlorine content and the wet strength agent itself.
By combining neutral high-temperature hydrolysis and specific adsorption purification processes, the problem of the difficulty in reducing organochlorine content in existing technologies has been solved, enabling the preparation of low organochlorine wet strength agents that meet food-grade standards while maintaining high wet strength performance, and are environmentally friendly and pollution-free.
Patent Information
- Application Number
- CN202611345803.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies cannot reduce the organic chlorine content in paper products to <2 mg/kg without significantly sacrificing wet strength performance, and traditional methods have environmental risks or performance loss problems.
A combined process of neutral high-temperature hydrolysis and specific adsorption purification was adopted. Hydrolysis was carried out under controlled conditions of pH value of 6.8~7.2, temperature of 88~92℃ and appropriate dilution. Then, β-cyclodextrin-grafted modified montmorillonite was used as an adsorbent to remove free ECH, DCP and MCPD. Finally, a wet strength agent with low organochlorine content was obtained by plate and frame filter press and vacuum concentration.
It achieves a reduction of organochlorine content to <2 mg/kg, meeting food-grade standards, with a wet strength retention rate of up to 92%~96%, and is green and environmentally friendly with no secondary pollution, making it suitable for upgrading existing production lines.
Abstract
Description
Technical Field
[0001] This invention relates to the field of papermaking technology, specifically to a method for preparing a wet strength agent with low organochlorine content and the wet strength agent itself. Background Technology
[0002] With increasingly stringent global environmental regulations, especially the EU No. 10 / 2011 Food Contact Materials Regulation and the US FDA 21 CFR 176.170's strict restrictions on organochlorine compounds (AOX) and certain halogenated compounds (DCP, MCPD) in paper products, the paper industry has an increasingly urgent need for wet strength agents with ultra-low organochlorine content.
[0003] There are three main sources of organochlorine in PAE resin:
[0004] Free ECH: Epichlorohydrin that has not fully reacted during synthesis;
[0005] Small molecule haloalcohols: DCP and MCPD (strong carcinogens) generated by ECH hydrolysis.
[0006] Bound chlorine: Chlorohydrin groups (—CH(OH)—CH2Cl) covalently bonded to the polymer side chain.
[0007] The existing technical solutions for reducing organochlorine compounds and their limitations are as follows:
[0008] Extended reaction time method: This method consumes free ECH and chlorohydrin groups by extending the holding time. However, this method easily leads to excessive cross-linking or ring-opening hydrolysis of nitrogen-containing heterocyclic butaneonium ions, resulting in a 20% to 30% decrease in wet strength properties. Furthermore, bound chlorine cannot be completely eliminated, and organochlorine remains at a level of 10 to 20 mg / kg.
[0009] Activated carbon adsorption method: Powdered activated carbon is used to adsorb small molecules such as DCP. However, activated carbon also has significant physical adsorption on PAE cation exchange resin (loss rate of about 15%~20%), and filtration is difficult, making it unsuitable for continuous industrial production.
[0010] Solvent extraction: Organic chlorine compounds are extracted using organic solvents such as ethyl acetate. While this method is effective at removing chlorine (down to <5 mg / kg), it carries the risk of solvent residue, increases production costs and poses fire hazards, and does not conform to the principles of green chemistry.
[0011] Post-treatment after alkaline hydrolysis: There are reports of using strong base (pH>10) and high temperature hydrolysis to dechlorinate, but strong alkaline conditions will cause irreversible ring opening of nitrogen heterocyclic butaneonium ions, and wet strong activity will be almost completely lost.
[0012] Therefore, developing a green process to stabilize primary organochlorines to <2 mg / kg without significantly sacrificing wet strength performance remains a technical challenge for the industry. Summary of the Invention
[0013] This invention provides a method for preparing a wet strength agent with low organochlorine content, thereby reducing the organochlorine content.
[0014] The present invention adopts the following technical solution:
[0015] A method for preparing a wet strength agent with low organochlorine content includes the following steps:
[0016] (1) Polycondensation and crosslinking
[0017] Polycondensation: Adipic acid and diethylenetriamine are added to a reaction vessel in a preset ratio and melt-polymerized to obtain polyamide polyamine;
[0018] Dissolving: Cool to 85~90℃, add deionized water to adjust the solid content to 19%~21%, and adjust the pH to 4.5~5.5 with dilute sulfuric acid;
[0019] Crosslinking: Cool down to 60~65℃, add ECH dropwise over 2~2.5h, heat up to 75~80℃ and keep the temperature for reaction, take a sample every 15min to measure the viscosity until the viscosity of the Forecast cup reaches 50~70 seconds;
[0020] (2) High-temperature selective hydrolysis
[0021] Solid content adjustment: After the crosslinking reaction reaches the target viscosity, deionized water is added to the reactor to adjust the solid content of the system to 15%~18%;
[0022] pH adjustment: Use a 5% dilute NaOH solution to fine-tune the pH of the system to a neutral range of 6.8~7.2;
[0023] Heating hydrolysis: The system temperature is raised to 88℃~92℃ and stirred at this temperature for 2.5~3.5 hours. During this period, samples are taken every 30 minutes to determine the content of free ECH, DCP, MCPD and resin viscosity.
[0024] (3) Specific adsorption purification
[0025] Cooling: Cool the hydrolyzed system to 45℃~50℃;
[0026] Add adsorbent: Add composite adsorbent;
[0027] Adsorption time: Stir slowly for 1 to 1.5 hours to ensure adsorption equilibrium;
[0028] (4) Separation and concentration
[0029] The adsorbent residue is separated and removed, and the filtrate is placed in a vacuum concentration tank to evaporate excess water, thereby increasing the solid content back to 19%~21%.
[0030] Add formic acid to adjust the pH to 3.0-3.5, add preservatives, and filter out the material.
[0031] As a preferred embodiment, in step (1), polycondensation is performed by adding adipic acid and diethylenetriamine to a reaction vessel at a molar ratio of 1:1.05~1.10 and performing melt polycondensation at 160~175℃ for 3.5~4h, with an acid value ≤5, to obtain polyamide polyamine.
[0032] Preferably, in step (1), the ratio of ECH:diethylenetriamine unit is 1.3~1.5:1.
[0033] Preferably, the amount of the composite adsorbent added is 0.8% to 1.2% of the dry weight of the resin.
[0034] Preferably, the composite adsorbent is β-cyclodextrin-grafted modified montmorillonite.
[0035] Preferably, the preparation method of the composite adsorbent includes:
[0036] Sodium-based montmorillonite was grafted with β-cyclodextrin under acidic conditions, so that cyclodextrin molecules were linked to the interlayer and surface of montmorillonite through ester or ether bonds.
[0037] Preferably, in step (4), the adsorbent residue is separated and removed using a plate and frame filter press or a disc centrifuge with a filter cloth pore size ≤ 5 μm.
[0038] Preferably, in step (4), the filtrate is placed in a vacuum concentrator and the excess water is evaporated under the conditions of temperature ≤45℃ and vacuum degree -0.085~-0.095MPa, so that the solid content is increased back to 19%~21%.
[0039] Preferably, the amount of preservative added is 0.05% to 0.1%.
[0040] This invention provides a wet strength agent with low organochlorine content prepared by the preparation method described above.
[0041] Compared with the prior art, the present invention has the following beneficial effects:
[0042] (1) Primary organochlorine content < 2 mg / kg, meeting food-grade standards: After dual purification through "hydrolysis + adsorption", the primary organochlorine content of the product of this invention can be stably maintained at 1.2~1.8 mg / kg. Free ECH was not detected (detection limit 0.001%), and the total content of DCP+MCPD was < 0.3 mg / kg. It fully meets the most stringent food contact paper requirements of EU 10 / 2011 and US FDA, and can be directly used for high-end paper products such as napkins, coffee filters, and tea bags.
[0043] (2) Extremely high wet strength retention: By precisely controlling the hydrolysis conditions (neutral pH, ≤92℃), this invention achieves selective removal of harmful chlorohydrin groups, while the retention rate of active nitrogen heterocyclic butaneonium ions can reach 88%~93%. According to papermaking application tests, compared with traditional high-chlorine products (organic chlorine ~34 mg / kg), the wet strength retention rate of the paper produced by this invention reaches 92%~96%, that is, sacrificing minimal performance for huge environmental advantages.
[0044] (3) Green and environmentally friendly, with no secondary pollution: This invention does not involve organic solvents throughout the process. The hydrolysis byproducts are glycerol and sodium chloride (both non-toxic and harmless substances). The adsorbent is a natural mineral grafted modified material that can be incinerated or landfilled. The AOX content in the wastewater is reduced by more than 80% compared to traditional processes, significantly reducing the burden of wastewater treatment.
[0045] (4) Wide process window, suitable for upgrading existing production lines: This invention only requires adding an adsorbent feeding device and a plate and frame filter press to the existing PAE reactor to complete the production line upgrade. The hydrolysis step can be carried out using the original reactor, and the equipment investment is relatively small. Detailed Implementation
[0046] The present invention will be further described in detail below with reference to specific embodiments, but the scope of protection of the present invention is not limited thereto.
[0047] Example 1
[0048] (a) Conventional polycondensation and crosslinking
[0049] 1. Polycondensation: Adipic acid and diethylenetriamine are added to a reaction vessel at a molar ratio of 1:1.05~1.10 and melt-condensed at 160~175℃ for 3.5~4h. The acid value is ≤5, and polyamide-polyamine is obtained.
[0050] 2. Dissolving: Cool to 85~90℃, add deionized water to adjust the solid content to 19%~21%, and adjust the pH to 4.5~5.5 with dilute sulfuric acid.
[0051] 3. Crosslinking: Cool to 60-65℃, add ECH (ECH : diethylenetriamine units = 1.3-1.5 : 1) dropwise over 2-2.5 hours, then heat to 75-80℃ and maintain the temperature for reaction. Take a sample every 15 minutes to measure the viscosity until the viscosity of the Forecast-4 cup reaches 50-70 seconds.
[0052] (ii) High-temperature selective hydrolysis
[0053] This step is one of the core innovations of this invention, and its essential difference from the prior art lies in the precise control of the reaction medium conditions.
[0054] 1. Procedure: Once the crosslinking reaction reaches the target viscosity, do not add an acidic terminator. Add deionized water to the reactor to adjust the solid content of the system to 15%~18% (appropriate dilution is beneficial for uniform hydrolysis).
[0055] 2. pH adjustment: Use dilute NaOH solution (5% concentration) to fine-tune the pH of the system to a neutral range of 6.8~7.2.
[0056] 3. Heating hydrolysis: Raise the system temperature to 88℃~92℃ and maintain this temperature with stirring for 2.5~3.5 hours. During this period, take samples every 30 minutes to determine the content of free ECH, DCP, MCPD and resin viscosity.
[0057] 4. Mechanism Explanation: Under these specific conditions (neutral, 88-92℃, moderate dilution), two competing reactions occur in the system:
[0058] (1) Favorable reaction (target): The unstable β-chlorohydrin group (—CH(OH)—CH2Cl) on the polymer chain undergoes hydrolysis, and the chlorine atom is replaced by a hydroxyl group to generate a glycerol group structure (—CH(OH)—CH2OH), releasing Cl⁻ ions. This reaction is a nucleophilic substitution (SN2) mechanism. Neutral conditions favor the hydroxyl group (—OH) as a nucleophile to attack, and avoid the ring-opening of nitrogen-containing heterocyclic butanetonium caused by strong bases.
[0059] (2) Reactions requiring control (side reactions): Azacyclobutaneonium ions may also undergo ring-opening hydrolysis at high temperatures. However, studies have shown that under conditions of pH 6.8~7.2 and temperature ≤92℃, the ring-opening rate constant of azacyclobutaneonium ions is only 1 / 5~1 / 8 of that of chlorohydrin hydrolysis. That is, this invention achieves selective removal of "harmful chlorine" (chlorohydrin) while protecting "beneficial active groups" (azacyclobutaneonium).
[0060] (3) At the same time, free ECH and DCP / MCPD are rapidly hydrolyzed into glycerol and chloride under these conditions, eliminating toxicity at the source.
[0061] 5. Control indicators: Sampling and testing requirements after hydrolysis:
[0062] (1) Free ECH ≤ 0.005%;
[0063] (2) Total content of DCP + MCPD ≤ 0.5 mg / kg;
[0064] (3) The viscosity should not increase by more than 15% compared to before hydrolysis (if the viscosity increases too quickly, it indicates that the cross-linking is excessive, which can be controlled by shortening the hydrolysis time).
[0065] (III) Specific adsorption purification
[0066] After high-temperature hydrolysis, the residual organochlorine in the system was reduced to a low level (approximately 3-5 mg / kg). To further achieve the target of <2 mg / kg, physical adsorption purification was introduced.
[0067] 1. Procedure: Cool the hydrolyzed system to 45℃~50℃.
[0068] 2. Adding Adsorbent: Add a composite adsorbent at a concentration of 0.8%~1.2% of the resin's oven-dry weight. This adsorbent is β-cyclodextrin-grafted modified montmorillonite. The preparation method is briefly described as follows: Sodium-based montmorillonite is grafted with β-cyclodextrin under acidic conditions, causing cyclodextrin molecules to be linked to the montmorillonite layers and surface via ester or ether bonds.
[0069] 3. Adsorption principle:
[0070] (1) β-cyclodextrin has a hydrophilic outer wall and a hydrophobic cavity, which can recognize and encapsulate small molecule halogenated compounds such as DCP and MCPD, and can specifically capture these linear organochlorine molecules.
[0071] (2) Montmorillonite has a layered silicate structure and a negatively charged surface, which can adsorb free small molecule impurities in cationic PAE resin. At the same time, its interlayer domain can accommodate organochlorine complexes encapsulated by cyclodextrin.
[0072] (3) The key point is that the adsorbent has a very low adsorption rate (<3% loss) on the high molecular weight PAE cationic resin itself because the macromolecules cannot enter the cyclodextrin cavity, and the surface of montmorillonite is more hydrophilic after grafting cyclodextrin, which weakens the electrostatic adsorption of PAE macromolecules.
[0073] 4. Adsorption time: Stir slowly for 1 to 1.5 hours to ensure adsorption equilibrium.
[0074] (iv) Separation and Concentration
[0075] 1. Use a plate and frame filter press (filter cloth pore size ≤ 5μm) or a disc centrifuge to separate and remove the adsorbent residue.
[0076] 2. Place the filtrate in a vacuum concentrator and evaporate excess water under conditions of temperature ≤45℃ and vacuum degree -0.085~-0.095MPa to increase the solid content from ~15% back to 19%~21%.
[0077] 3. Add formic acid to adjust the pH to 3.0~3.5, add an appropriate amount of preservative (0.05%~0.1%), and filter out the material.
[0078] This invention has the following key features:
[0079] Key Point 1: Precise combination of conditions for "neutral high-temperature hydrolysis":
[0080] Temperature: 88~92℃ (below this temperature, hydrolysis efficiency is insufficient; above this temperature, nitrogen-containing heterocyclic butanes begin to undergo significant ring-opening deactivation).
[0081] pH: 6.8~7.2 (below this pH, the hydrolysis rate is too slow; above this pH, the cationic active groups are damaged).
[0082] Time: 2.5~3.5 hours;
[0083] Solid content: 15%~18% (hydrolysis stage).
[0084] Key Point 2: Using β-cyclodextrin-grafted modified montmorillonite as a specific adsorbent, selective adsorption of small molecule organochlorines such as DCP and MCPD is achieved, while there is almost no loss of PAE macromolecular resin.
[0085] Key Point 3: The order of the "hydrolysis + adsorption" series process cannot be reversed. Hydrolysis must be performed first to convert the bound chlorohydrin into a soluble small molecule halogen, and then adsorption removal can be carried out; if adsorption is performed first, the bound chlorine will still remain on the polymer chain, and the standard cannot be met.
[0086] The wet strength agent prepared in this embodiment has the following characteristics:
[0087] (1) Primary organochlorine content < 2 mg / kg, meeting food-grade standards: After dual purification through "hydrolysis + adsorption", the primary organochlorine content of the product of this invention can be stably maintained at 1.2~1.8 mg / kg. Free ECH was not detected (detection limit 0.001%), and the total content of DCP+MCPD was < 0.3 mg / kg. It fully meets the most stringent food contact paper requirements of EU 10 / 2011 and US FDA, and can be directly used for high-end paper products such as napkins, coffee filters, and tea bags.
[0088] (2) Extremely high wet strength retention: By precisely controlling the hydrolysis conditions (neutral pH, ≤92℃), this invention achieves selective removal of harmful chlorohydrin groups, while the retention rate of active nitrogen heterocyclic butaneonium ions can reach 88%~93%. According to papermaking application tests, compared with traditional high-chlorine products (organic chlorine ~34 mg / kg), the wet strength retention rate of the paper produced by this invention reaches 92%~96%, that is, sacrificing minimal performance for huge environmental advantages.
[0089] (3) Green and environmentally friendly, with no secondary pollution: This invention does not involve organic solvents throughout the process. The hydrolysis byproducts are glycerol and sodium chloride (both non-toxic and harmless substances). The adsorbent is a natural mineral grafted modified material that can be incinerated or landfilled. The AOX content in the wastewater is reduced by more than 80% compared to traditional processes, significantly reducing the burden of wastewater treatment.
Claims
1. A method for preparing a wet strength agent with low organochlorine content, characterized in that, Includes the following steps: (1) Polycondensation and crosslinking Polycondensation: Adipic acid and diethylenetriamine are added to a reaction vessel in a preset ratio and melt-polymerized to obtain polyamide polyamine; Dissolving: Cool to 85~90℃, add deionized water to adjust the solid content to 19%~21%, and adjust the pH to 4.5~5.5 with dilute sulfuric acid; Crosslinking: Cool down to 60~65℃, add ECH dropwise over 2~2.5h, heat up to 75~80℃ and keep the temperature for reaction, take a sample every 15min to measure the viscosity until the viscosity of the Forecast cup reaches 50~70 seconds; (2) High-temperature selective hydrolysis Solid content adjustment: After the crosslinking reaction reaches the target viscosity, deionized water is added to the reactor to adjust the solid content of the system to 15%~18%; pH adjustment: Use a 5% dilute NaOH solution to fine-tune the pH of the system to a neutral range of 6.8~7.2; Heating hydrolysis: The system temperature is raised to 88℃~92℃ and stirred at this temperature for 2.5~3.5 hours. During this period, samples are taken every 30 minutes to determine the content of free ECH, DCP, MCPD and resin viscosity. (3) Specific adsorption purification Cooling: Cool the hydrolyzed system to 45℃~50℃; Add adsorbent: Add composite adsorbent; Adsorption time: Stir slowly for 1 to 1.5 hours to ensure adsorption equilibrium; (4) Separation and concentration The adsorbent residue is separated and removed, and the filtrate is placed in a vacuum concentration tank to evaporate excess water, thereby increasing the solid content back to 19%~21%. Add formic acid to adjust the pH to 3.0-3.5, add preservatives, and filter out the material.
2. The method for preparing a low-organochlorine content wet strength agent according to claim 1, characterized in that, In step (1), polycondensation: adipic acid and diethylenetriamine are added to the reactor at a molar ratio of 1:1.05~1.10 and melt-condensed at 160~175℃ for 3.5~4h. The acid value is ≤5, and polyamide polyamine is obtained.
3. The method for preparing a low-organochlorine content wet strength agent according to claim 1, characterized in that, In step (1), ECH: diethylenetriamine unit = 1.3~1.5:
1.
4. The method for preparing a low-organochlorine content wet strength agent according to claim 1, characterized in that, The amount of the composite adsorbent added is 0.8% to 1.2% of the dry weight of the resin.
5. The method for preparing a low-organochlorine content wet strength agent according to claim 1, characterized in that, The composite adsorbent is β-cyclodextrin-grafted modified montmorillonite.
6. The method for preparing a low-organochlorine content wet strength agent according to claim 1, characterized in that, The preparation method of the composite adsorbent includes: Sodium-based montmorillonite was grafted with β-cyclodextrin under acidic conditions, so that cyclodextrin molecules were linked to the interlayer and surface of montmorillonite through ester or ether bonds.
7. The method for preparing a low-organochlorine content wet strength agent according to claim 1, characterized in that, In step (4), the adsorbent residue is separated and removed using a plate and frame filter press or a disc centrifuge with a filter cloth pore size ≤5μm.
8. The method for preparing a low-organochlorine content wet strength agent according to claim 1, characterized in that, In step (4), the filtrate is placed in a vacuum concentrator and the excess water is evaporated under the conditions of temperature ≤45℃ and vacuum degree -0.085~-0.095MPa, so that the solid content is increased back to 19%~21%.
9. The method for preparing a low-organochlorine content wet strength agent according to claim 1, characterized in that, The amount of the preservative added is 0.05% to 0.1%.
10. A wet strength agent with low organochlorine content prepared by the preparation method according to any one of claims 1 to 9.