A method for measuring the thickness of a metal thin film on a diamond substrate
By attaching a composite film layer with patterned openings to a diamond substrate and etching away the metal film, and then measuring the step height using a step detector, the problem of measuring the thickness of the metal film on the diamond substrate in the prior art is solved, and high-precision, low-cost metal film thickness measurement is achieved.
Patent Information
- Application Number
- CN202611345920.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-17
AI Technical Summary
Existing metal thin film detection methods cannot directly measure the thickness of metal thin films on diamond substrates, resulting in the inability to obtain separate metal thin film thickness measurement results.
By bonding a composite film with patterned openings onto a diamond substrate, etching away the metal film in the area to be tested, and then using a step detector to scan and measure the step height to obtain the metal film thickness, the reliance on material optical properties and theoretical models is avoided.
It provides high-precision, intuitive metal thin film thickness measurement results, simplifies the operation process, reduces costs, and is applicable to a variety of metal thin film materials.
Smart Images

Figure CN123111159A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal thin film manufacturing, and in particular to a method for measuring the thickness of metal thin films on diamond substrates. Background Technology
[0002] Metal thin films can be applied to components in many fields. The thickness of the metal thin film directly affects the performance of these components. Therefore, it is necessary to measure the thickness of the metal thin film to ensure that the thickness of the generated metal thin film meets relevant standards.
[0003] There are many existing methods for measuring the thickness of metal thin films, such as using a step detector. However, current technology lacks a process for measuring the thickness of metal thin films directly formed on diamond substrates. If a step detector is used directly, the result is the thickness of the diamond substrate plus the metal thin film as a whole; the thickness of the metal thin film alone cannot be obtained. Therefore, it is necessary to develop a process for measuring the thickness of metal thin films on diamond substrates. Summary of the Invention
[0004] Therefore, a method for measuring the thickness of a metal thin film on a diamond substrate is provided. This method can directly measure the metal thin film on the diamond substrate with high accuracy.
[0005] The specific plan is as follows: A method for measuring the thickness of a metal thin film on a diamond substrate, comprising: S100. A composite film layer with patterned openings is laminated onto a metal thin film on a diamond substrate. The composite film layer includes a stacked UV-resistant adhesive layer and a base film layer, wherein the UV-resistant adhesive layer is in contact with the surface of the metal thin film, and a portion of the metal thin film is exposed through the patterned openings of the composite film layer. This portion is the area to be tested. S200: The metal film in the exposed test area is removed by etching through the patterned opening until the surface of the underlying diamond substrate is exposed. S300: Remove residual corrosion solution and perform cleaning. S400, remove the composite membrane layer. S500: The step height between the area to be tested and the surrounding uncorroded area is measured using a step detector. The step height is the thickness of the metal film.
[0006] In one embodiment, in S100, a pretreatment is first performed on a diamond substrate to form a clean surface, and a metal thin film is deposited on the clean surface by a magnetron sputtering process.
[0007] In one embodiment, the pretreatment in S100 includes cleaning the diamond substrate using a plasma cleaning process.
[0008] In one embodiment, in S100, a laser cutting process is used to form a patterned opening in the composite film layer that penetrates the UV-resistant adhesive layer and the base film layer.
[0009] In one embodiment, in S100, a composite film layer with patterned openings is laminated onto a metal thin film on a diamond substrate using a vacuum lamination process.
[0010] In one embodiment, in S200, a wet etching process is used to remove the metal film from the exposed test area.
[0011] In one embodiment, the wet etching process includes: selecting an etching solution based on the material of the metal film, wherein the etching solution is selected from an acidic etching solution or an alkaline etching solution, controlling the etching temperature to be 25℃-60℃, the etching time to be 30 seconds-300 seconds, and controlling the etching endpoint by an optical endpoint detection method or by a preset time.
[0012] In one embodiment, step S300, removing residual corrosion liquid and cleaning, specifically includes: rinsing the sample surface multiple times (3-5 times recommended) with deionized water to dilute and remove a large amount of acidic or alkaline corrosion liquid. After rinsing with deionized water, acetone can be used for ultrasonic cleaning or soaking, depending on the characteristics of the adhesive layer, to effectively remove residual adhesive layer and organic contaminants. The sample is then placed sequentially into beakers of anhydrous ethanol and deionized water, and ultrasonically cleaned for 5-10 minutes each.
[0013] In one embodiment, S400, removing the composite film layer includes: irradiating the composite film layer with ultraviolet light to reduce the adhesiveness of the ultraviolet anti-adhesive layer, thereby peeling off the composite film layer.
[0014] In one embodiment, the recess is located at one end of the metal film and is surrounded by the remaining metal film, and the number of the patterned openings is one or more.
[0015] The beneficial effects of this application are as follows: This method can directly measure metal thin films on diamond substrates. It uses a profilometer for mechanical contact scanning to directly measure the physical height difference of the steps, without relying on any theoretical models or material parameters (such as refractive index) for conversion. This method provides an intuitive, traceable absolute thickness value with high measurement accuracy. The measurement results are unaffected by the reflectivity, absorptivity, or transparency of the metal thin film. Whether it is highly reflective gold or silver, or other highly absorptive metals, accurate measurements can be made without relying on the material's optical properties. By bonding a composite film layer with patterned openings to define the corrosion area, this method is simpler, lower in cost, and easier to operate than traditional photolithography processes. The sample preparation method is also simple and convenient. The measurement directly obtains the surface profile curve, making the step height immediately apparent, and the data analysis and interpretation are very intuitive. Attached Figure Description
[0016] Figure 1 This is a schematic diagram of the fabrication of a metal thin film on a diamond substrate according to an embodiment of this application.
[0017] Figure 2 This is a schematic diagram of a composite film layer with a patterned opening, representing an embodiment of this application.
[0018] Figure 3 This is a schematic diagram illustrating the bonding of a composite film layer to a metal thin film according to an embodiment of this application.
[0019] Figure 4 This is a schematic diagram of the metal film in the area to be tested after etching, according to an embodiment of this application.
[0020] Figure 5 This is a schematic diagram of the composite film layer after being peeled off, according to an embodiment of this application.
[0021] Figure 6 This is a schematic diagram illustrating the detection of the pit depth H by a probe of a step detector according to an embodiment of this application. The pit depth H is equal to the thickness of the metal film.
[0022] Figure 7 This is a flowchart illustrating a method for measuring the thickness of a metal thin film on a diamond substrate, as described in an embodiment of this application.
[0023] in: 1. Diamond substrate; 2. Metal thin film; 3. Composite film layer; 31. Patterned opening; 4. Probe. Detailed Implementation
[0024] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Many specific details are set forth in the following description to provide a thorough understanding of the present invention. However, the present invention can be practiced in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0025] like Figures 1 to 7 As shown, embodiments of this application provide a method for measuring the thickness of a metal thin film on a diamond substrate, the method comprising the following steps: S100. A composite film layer 3 with patterned openings 31 is bonded onto a metal thin film 2 on a diamond substrate 1. The number of patterned openings 31 is one or more. The composite film layer 3 includes a stacked UV-resistant adhesive layer and a base film layer, wherein the UV-resistant adhesive layer is in contact with the surface of the metal thin film 2, and a portion of the metal thin film 2 is exposed through the patterned openings 31 of the composite film layer 3. This portion is the area to be tested, such as... Figures 1 to 3 As shown.
[0026] S200, the exposed metal film 2 of the test area is removed by etching through the patterned opening 31 until the surface of the underlying diamond substrate 1 is exposed, such as... Figure 4 As shown.
[0027] S300: Remove residual liquid after corrosion and perform cleaning.
[0028] S400, Remove composite membrane layer 3, such as Figure 5 As shown.
[0029] S500. A step height is measured between the tested area and the surrounding uncorroded area using a step detector. This step height is the thickness of the metal film 2. Figure 6 As shown, in actual measurement, it is the measurement of Figure 6 The depth H of the pit is equal to the thickness of the metal film 2.
[0030] In one embodiment, in S100, a pretreatment is first performed on the diamond substrate 1 to form a clean surface, and a metal thin film 2 is deposited on the clean surface by a magnetron sputtering process.
[0031] Specifically, the aforementioned metal thin film 2 can be a copper thin film with a thickness of 100 nm.
[0032] In one embodiment, in S100, the pretreatment includes cleaning the diamond substrate 1 using a plasma cleaning process.
[0033] Specifically, in the above-mentioned plasma cleaning process, the processing gas is selected from oxygen, argon or a combination thereof, the processing power is 100W-500W, and the processing time is 30 seconds-180 seconds.
[0034] In one embodiment, in S100, a laser cutting process is used to form a patterned opening 31 in the composite film layer 3 that penetrates the UV anti-adhesion layer and the base film layer.
[0035] Specifically, in the above laser cutting process, the laser wavelength is selected from 355nm, and the cutting depth penetrates the ultraviolet anti-adhesion layer and the base film layer, but does not penetrate the protective film layer (release film, which is connected to the ultraviolet anti-adhesion layer. In use, the release film is separated from the ultraviolet anti-adhesion layer, and then the ultraviolet anti-adhesion layer is brought into contact with the surface of the metal film 2).
[0036] In one embodiment, in S100, a composite film layer 3 with patterned openings 31 is bonded to a metal film 2 on a diamond substrate 1 using a vacuum lamination process.
[0037] Specifically, in the above-mentioned vacuum lamination process, the lamination temperature is 40℃, the lamination pressure is 0.2MPa-0.6MPa, and the vacuum degree is less than 10Pa, in order to eliminate air bubbles between the composite film layer 3 and the metal thin film 2 to be tested.
[0038] In one embodiment, in S200, a wet etching process is used to remove the metal film 2 exposed in the test area.
[0039] Specifically, the wet etching process includes: selecting an etching solution based on the material of the metal film 2, the etching solution being selected from acidic or alkaline etching solutions, controlling the etching temperature to be 25℃-60℃, the etching time to be 30 seconds-300 seconds, and controlling the etching endpoint by optical endpoint detection method or by a preset time.
[0040] In one embodiment, step S300, removing residual corrosion liquid and cleaning, specifically includes: rinsing the sample surface multiple times (3-5 times recommended) with deionized water to dilute and remove a large amount of acidic or alkaline corrosion liquid. After rinsing with deionized water, acetone can be used for ultrasonic cleaning or soaking, depending on the characteristics of the adhesive layer, to effectively remove residual adhesive layer and organic contaminants. Then, the sample is sequentially placed in beakers of anhydrous ethanol and deionized water, and ultrasonically cleaned for 5-10 minutes each.
[0041] In one embodiment, in step S400, removing the composite film layer 3 includes: subjecting the composite film layer 3 to ultraviolet irradiation to reduce the adhesiveness of the ultraviolet anti-adhesive layer, thereby peeling off the composite film layer 3.
[0042] In one embodiment, the recess is located at one end of the metal film 2 and is surrounded by the remaining metal film 2. This configuration allows the probe 4 to enter the recess via the metal film 2 regardless of the direction of movement, facilitating the measurement of the recess depth H.
[0043] Implementation method 1: A method for measuring the thickness of a metal thin film on a diamond substrate, the method comprising the following steps: S100. The diamond substrate 1 is cleaned using a plasma cleaning process to form a clean surface. In the above plasma cleaning process, the processing gas is selected from oxygen, argon, or a combination thereof, the processing power is 100W, and the processing time is 180 seconds.
[0044] A copper thin film 2 is deposited on a clean surface using magnetron sputtering. A composite film layer 3 with a patterned opening 31 is then bonded onto the copper thin film 2 on a diamond substrate 1 using a vacuum lamination process. The number of patterned openings 31 is one. In this vacuum lamination process, the lamination temperature is 40°C, the lamination pressure is 0.2 MPa-0.6 MPa, and the vacuum level is below 10 Pa to eliminate air bubbles between the composite film layer 3 and the copper thin film 2 under test.
[0045] Specifically, a laser cutting process is used to form a patterned opening 31 in the composite film layer 3 that penetrates both the UV-resistant adhesive layer and the base film layer. In the laser cutting process, the laser wavelength is selected from 355nm, and the cutting depth penetrates both the UV-resistant adhesive layer and the base film layer.
[0046] The composite film layer 3 comprises a stacked ultraviolet anti-adhesion layer and a base film layer. The ultraviolet anti-adhesion layer is in contact with the surface of the metal thin film 2, and a portion of the metal thin film 2 is exposed through the patterned opening 31 of the composite film layer 3. This portion is the area to be tested. Figures 1 to 3 As shown.
[0047] S200. Using a wet etching process, the exposed metal film 2 of the test area is removed through the patterned opening 31 until the surface of the underlying diamond substrate 1 is exposed. Figure 4 As shown. The wet etching process includes: selecting an etching solution based on the material of the metal film 2, the etching solution being selected from acidic or alkaline etching solutions, controlling the etching temperature at 25°C, the etching time at 300 seconds, and controlling the etching endpoint by optical endpoint detection method or by a preset time.
[0048] S300: Remove residual liquid after corrosion and perform cleaning.
[0049] S400, Remove composite film layer 3, specifically including irradiating composite film layer 3 with ultraviolet light to reduce the adhesiveness of the ultraviolet anti-adhesive layer, thereby peeling off composite film layer 3, such as... Figure 5 As shown.
[0050] S500. A step height is measured between the tested area and the surrounding uncorroded area using a step detector. This step height is the thickness of the metal film 2. Figure 6 As shown, in actual measurement, it is the measurement of Figure 6 The depth H of the pit is equal to the thickness of the metal film 2.
[0051] Implementation Method 2: A method for measuring the thickness of a metal thin film on a diamond substrate, the method comprising the following steps: S100. The diamond substrate 1 is cleaned using a plasma cleaning process to form a clean surface. In the above plasma cleaning process, the processing gas is selected from oxygen, argon, or a combination thereof, the processing power is 300W, and the processing time is 80 seconds.
[0052] A copper thin film 2 is deposited on a clean surface using magnetron sputtering. A composite film layer 3 with patterned openings 31 is then bonded onto the copper thin film 2 on a diamond substrate 1 using a vacuum lamination process. The number of patterned openings 31 is two. In this vacuum lamination process, the lamination temperature is 40°C, the lamination pressure is 0.2 MPa-0.6 MPa, and the vacuum level is below 10 Pa to eliminate air bubbles between the composite film layer 3 and the copper thin film 2 under test.
[0053] Specifically, a patterned opening 31 penetrating the UV-resistant adhesive layer and the base film layer is formed in the composite film layer 3 using a laser cutting process. In the laser cutting process, the laser wavelength is selected from 355nm, and the cutting depth penetrates the UV-resistant adhesive layer and the base film layer.
[0054] The composite film layer 3 comprises a stacked ultraviolet anti-adhesion layer and a base film layer. The ultraviolet anti-adhesion layer is in contact with the surface of the metal thin film 2, and a portion of the metal thin film 2 is exposed through the patterned opening 31 of the composite film layer 3. This portion is the area to be tested. Figures 1 to 3 As shown.
[0055] S200. Using a wet etching process, the exposed metal film 2 of the test area is removed through the patterned opening 31 until the surface of the underlying diamond substrate 1 is exposed. Figure 4 As shown. The wet etching process includes: selecting an etching solution based on the material of the metal film 2, the etching solution being selected from acidic or alkaline etching solutions, controlling the etching temperature at 45°C, the etching time at 120 seconds, and controlling the etching endpoint by optical endpoint detection method or by a preset time.
[0056] S300: Remove residual liquid after corrosion and perform cleaning.
[0057] S400, Remove composite film layer 3, specifically including irradiating composite film layer 3 with ultraviolet light to reduce the adhesiveness of the ultraviolet anti-adhesive layer, thereby peeling off composite film layer 3, such as... Figure 5 As shown.
[0058] S500. A step height is measured between the tested area and the surrounding uncorroded area using a step detector. This step height is the thickness of the metal film 2. Figure 6 As shown, in actual measurement, it is the measurement of Figure 6 The depth H of the pit is equal to the thickness of the metal film 2.
[0059] Implementation Method 3: A method for measuring the thickness of a metal thin film on a diamond substrate, the method comprising the following steps: S100. The diamond substrate 1 is cleaned using a plasma cleaning process to form a clean surface. In the above plasma cleaning process, the processing gas is selected from oxygen, argon, or a combination thereof, the processing power is 500W, and the processing time is 30 seconds.
[0060] A copper thin film 2 is deposited on a clean surface using magnetron sputtering. A composite film layer 3 with a patterned opening 31 is then bonded onto the copper thin film 2 on a diamond substrate 1 using a vacuum lamination process. The number of patterned openings 31 is one. In this vacuum lamination process, the lamination temperature is 40°C, the lamination pressure is 0.2 MPa-0.6 MPa, and the vacuum level is below 10 Pa to eliminate air bubbles between the composite film layer 3 and the copper thin film 2 under test.
[0061] Specifically, a patterned opening 31 penetrating the UV-resistant adhesive layer and the base film layer is formed in the composite film layer 3 using a laser cutting process. In the laser cutting process, the laser wavelength is selected from 355nm, and the cutting depth penetrates the UV-resistant adhesive layer and the base film layer.
[0062] The composite film layer 3 comprises a stacked ultraviolet anti-adhesion layer and a base film layer. The ultraviolet anti-adhesion layer is in contact with the surface of the metal thin film 2, and a portion of the metal thin film 2 is exposed through the patterned opening 31 of the composite film layer 3. This portion is the area to be tested. Figures 1 to 3 As shown.
[0063] S200. Using a wet etching process, the exposed metal film 2 of the test area is removed through the patterned opening 31 until the surface of the underlying diamond substrate 1 is exposed. Figure 4As shown. The wet etching process includes: selecting an etching solution based on the material of the metal film 2, the etching solution being selected from acidic or alkaline etching solutions, controlling the etching temperature at 60°C, the etching time at 30 seconds, and controlling the etching endpoint by optical endpoint detection method or by a preset time.
[0064] S300: Remove residual liquid after corrosion and perform cleaning.
[0065] S400, Remove composite film layer 3, specifically including irradiating composite film layer 3 with ultraviolet light to reduce the adhesiveness of the ultraviolet anti-adhesive layer, thereby peeling off composite film layer 3, such as... Figure 5 As shown.
[0066] S500. A step height is measured between the tested area and the surrounding uncorroded area using a step detector. This step height is the thickness of the metal film 2. Figure 6 As shown, in actual measurement, it is the measurement of Figure 6 The depth H of the pit is equal to the thickness of the metal film 2.
[0067] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0068] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. A method for measuring the thickness of a metal thin film on a diamond substrate, characterized in that, include: S100. A composite film layer with patterned openings is laminated onto a metal thin film on a diamond substrate. The composite film layer includes a stacked UV-resistant adhesive layer and a base film layer, wherein the UV-resistant adhesive layer is in contact with the surface of the metal thin film, and a portion of the metal thin film is exposed through the patterned openings of the composite film layer. This portion is the area to be tested. S200: The metal film in the exposed test area is removed by etching through the patterned opening until the surface of the underlying diamond substrate is exposed, resulting in a pit in the test area relative to the surrounding area. S300: Remove residual corrosion solution and perform cleaning. S400, remove the composite membrane layer. S500: The step height between the area to be tested and the surrounding uncorroded area is measured using a step detector. The step height is the thickness of the metal film.
2. The method for measuring the thickness of a metal thin film on a diamond substrate according to claim 1, characterized in that, In step S100, a pretreatment is first performed on a diamond substrate to form a clean surface, and a metal thin film is deposited on the clean surface by magnetron sputtering.
3. The method for measuring the thickness of a metal thin film on a diamond substrate according to claim 2, characterized in that, In step S100, the pretreatment includes cleaning the diamond substrate using a plasma cleaning process.
4. The method for measuring the thickness of a metal thin film on a diamond substrate according to claim 1, characterized in that, In S100, a laser cutting process is used to form a patterned opening in the composite film layer that penetrates the UV-resistant adhesive layer and the base film layer.
5. The method for measuring the thickness of a metal thin film on a diamond substrate according to claim 1, characterized in that, In S100, a composite film layer with patterned openings is bonded onto a metal thin film on a diamond substrate using a vacuum lamination process.
6. The method for measuring the thickness of a metal thin film on a diamond substrate according to claim 1, characterized in that, In step S200, a wet etching process is used to remove the metal film from the exposed test area.
7. The method for measuring the thickness of a metal thin film on a diamond substrate according to claim 6, characterized in that, The wet etching process includes: selecting an etching solution based on the material of the metal film, the etching solution being selected from acidic or alkaline etching solutions, controlling the etching temperature to be 25℃-60℃, the etching time to be 30 seconds-300 seconds, and controlling the etching endpoint by optical endpoint detection method or by preset time.
8. The method for measuring the thickness of a metal thin film on a diamond substrate according to claim 1, characterized in that, In S300, the removal of residual corrosion liquid and cleaning specifically includes: rinsing multiple times with deionized water to dilute and remove acidic or alkaline corrosion liquid; after rinsing with deionized water, ultrasonic cleaning or soaking with acetone to remove residual adhesive layer and organic contaminants; and then sequentially placing the solution into beakers of anhydrous ethanol and deionized water for ultrasonic cleaning for 5-10 minutes each.
9. The method for measuring the thickness of a metal thin film on a diamond substrate according to claim 1, characterized in that, In step S400, removing the composite film layer includes: irradiating the composite film layer with ultraviolet light to reduce the adhesiveness of the ultraviolet anti-adhesion layer, thereby peeling off the composite film layer.
10. The method for measuring the thickness of a metal thin film on a diamond substrate according to claim 1, characterized in that, The recess is located at one end of the metal film and is surrounded by the remaining metal film, and the number of the pattern openings is one or more.