A high-pressure, high-temperature nuclear reactor monitoring and control cable and its manufacturing process
Through the design of multi-layered structures and specific material formulations, the performance deficiencies of cables used in nuclear power plants under high temperature, high pressure, and radiation environments have been solved, achieving a comprehensive improvement in the cables' high temperature resistance, flame retardancy, radiation resistance, and long service life.
Patent Information
- Application Number
- CN202611328314.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-31
- Publication Date
- 2026-11-17
AI Technical Summary
Existing cables used in nuclear power plants have insufficient performance under high temperature, high pressure and radiation environments. In particular, the silicone rubber insulation layer ages quickly and cannot simultaneously meet the requirements of high temperature resistance, flame retardancy, radiation resistance and long service life.
The cable adopts a multi-layer structure design, including a cable core, outer insulation layer, oxygen barrier layer, shielding layer, flame retardant layer, and outer sheath. The outer sheath uses high-temperature resistant silicone rubber material, combined with composite flame retardants, nano zinc oxide, and silane coupling agents, etc. High-temperature resistant composite particles are prepared through a specific process to improve the material performance.
The cable exhibits excellent high-temperature resistance, flame retardancy, and radiation resistance under high-temperature, high-pressure, and radiation environments, extending its service life and meeting the stringent technical requirements of nuclear reactors.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of cable technology, specifically to a high-pressure, high-temperature nuclear reactor monitoring and control cable and its manufacturing process. Background Technology
[0002] Nuclear reactor control cables are a critical component for the safe operation of nuclear power plants, operating long-term in extreme environments such as high temperature, high pressure, strong radiation, and humidity. Third-generation nuclear power plants with large advanced pressurized water reactors have a design lifespan of up to 60 years. Due to nuclear radiation, the associated cables and components cannot be replaced frequently, thus imposing extremely stringent requirements on the cables' high-temperature resistance, radiation resistance, flame retardancy, and long service life. In addition to excellent electrical performance, nuclear-grade cables must simultaneously meet multiple performance indicators, including low smoke, halogen-free, non-toxic, flame retardant, radiation resistant, heat resistant, and fireproof. However, current cables used in nuclear power plants generally suffer from limited functionality, typically employing a combination of fire-resistant silicone rubber insulation, a highly flame-retardant filler layer, and a low-smoke halogen-free outer sheath. While this provides some fire and high-temperature resistance, its radiation shielding effect is minimal. Long-term radiation can easily lead to aging of the silicone rubber insulation, causing a decline in insulation performance and altering the cable's internal properties. Existing fire-resistant and radiation-resistant cables for nuclear power plants, while possessing certain radiation resistance characteristics, have complex structures and manufacturing processes, resulting in high costs.
[0003] As the outermost layer of a cable that directly contacts the external environment, the material properties of the outer sheath play a decisive role in the overall service life and safety of the cable. Currently, the outer sheath materials for nuclear power plant cables mainly use ceramicized fire-resistant silicone rubber, low-smoke halogen-free flame-retardant polyolefins, or phenylene silicone rubber. While silicone rubber possesses certain high-temperature resistance, the long-term operating temperature of conventional silicone rubber typically does not exceed 180°C. In the high-temperature environment of a nuclear reactor (especially under higher temperatures during accident conditions), its thermal stability and thermo-oxidative aging performance are significantly insufficient. Although existing technologies have attempted to improve the high-temperature resistance of silicone rubber by adding inorganic fillers or employing ceramicization techniques, these methods often suffer from problems such as poor filler dispersion, weak interfacial bonding, and poor processing performance. Furthermore, while meeting high-temperature resistance requirements, the outer sheath material must also possess excellent flame retardancy, low-smoke halogen-free characteristics, and good radiation resistance. Existing single-material systems struggle to simultaneously meet these multiple performance demands. Therefore, there is an urgent need to develop an outer sheath material for nuclear reactor monitoring and control cables that combines excellent high-temperature resistance, flame retardancy, radiation resistance, and long service life, in order to overcome the aforementioned deficiencies in existing technologies. Summary of the Invention
[0004] To address the aforementioned technical problems, this invention provides a high-pressure, high-temperature nuclear reactor monitoring and control cable and its manufacturing process.
[0005] The objective of this invention can be achieved through the following technical solutions: A high-pressure, high-temperature nuclear reactor monitoring and control cable comprises, from the inside out, a cable core, an outer insulation layer, an oxygen barrier layer, a shielding layer, a flame-retardant layer, and an outer sheath. The cable core is composed of multiple stranded wires, each wire being a conductor covered with an inner insulation layer. The conductor itself is composed of multiple stranded tinned copper wires. A filler layer is provided between the cable core and the outer insulation layer. This filler layer is made of low-smoke halogen-free flame-retardant polyolefin. The inner insulation layer is made of irradiated cross-linked polyethylene, and the outer insulation layer is made of flame-retardant irradiated cross-linked polyolefin. The oxygen barrier layer is made of ceramicized silicone rubber. The flame-retardant layer is made of fiberglass flame-retardant tape. The shielding layer is woven from tinned copper wires. The outer sheath is made of high-temperature resistant silicone rubber. The high-temperature resistant silicone rubber material comprises the following raw materials in parts by weight: 35-45 parts of methyl vinyl silicone rubber, 5-10 parts of fluorosilicone rubber, 5-8 parts of phenyl silicone rubber, 10-15 parts of high-temperature resistant composite particles, 12-16 parts of composite flame retardant, 3-6 parts of nano zinc oxide, 2-3 parts of silane coupling agent, 2-4 parts of dispersant, and 1.5-2.5 parts of peroxide. Furthermore, the composite flame retardant is composed of magnesium hydroxide, aluminum hydroxide and ammonium polyphosphate, and the mass ratio of the three is 1:1:2; Furthermore, the silane coupling agent is one of long-chain alkylsilanes; Furthermore, the dispersant is a low molecular weight hydroxyl silicone oil with a molecular weight of 300-5000; Furthermore, the peroxide is one of bis(2,5-diphenyl)-2-pentachlor or DCP; The high-temperature resistant composite particles are prepared by the following steps: Step A1: Add hydroxypropyl cellulose to a mixture of ethanol and deionized water and stir until homogeneous. Add hexagonal boron nitride nanosheets (h-BN) and disperse evenly by ultrasonication. Stir for 1 hour, then slowly add tetrabutyl zirconate alcohol solution. After the addition is complete, react at room temperature for 15 hours. Filter, wash, and dry to obtain h-BN@ZrO2 nanomaterials. Furthermore, in step A1, the ratio of hydroxypropyl cellulose, ethanol, deionized water, hexagonal boron nitride nanosheets, and tetrabutyl zirconate alcohol solution is 0.015-0.02 g: 98 mL: 2 mL: 0.1 g: 21.5-21.7 mL; Further, the tetrabutyl zirconate ethanol solution mentioned in step A1 is prepared by mixing and stirring 80% tetrabutyl zirconate in ethanol, and the ratio of tetrabutyl zirconate to ethanol is 1.5-1.7 mL: 20 mL. Step A2: Disperse the h-BN@ZrO2 nanomaterials evenly in ethanol, add silane coupling agent KH570 and stir well, then add deionized water, heat to 45℃ and stir for 5-6 hours, filter, wash and dry to obtain modified h-BN@ZrO2 nanomaterials. Further, the ratio of the amount of h-BN@ZrO2 nanomaterial, ethanol, KH570 and deionized water used in step A2 is 1g:45mL:1-2mL:5mL; Step A3: Stir the organosilicon modifier in toluene to obtain mixture 1; add the modified h-BN@ZrO2 nanomaterials and Karstedt catalyst to toluene, purge with nitrogen and stir for 15 min, while raising the temperature to 80°C, then add mixture 1 dropwise using a constant pressure dropping funnel, finishing the addition within 90 min, then raise the temperature to 100°C and react for 18-24 h, remove the solvent by rotary evaporation, wash with anhydrous ethanol, and dry to obtain high-temperature resistant composite particles; Further, in step A3, the ratio of the modified h-BN@ZrO2 nanomaterial, Karstedt catalyst, toluene, and mixture 1 is 1g:0.01-0.03g:15mL:15mL; Further, in step A3, the ratio of organosilicon modifier to toluene in the mixture 1 is 0.5-1.5g:15mL; Further, the organosilicon modifier described in step A3 is prepared by the following steps: Dimethyldiethoxysilane, trifluoropropanetrimethoxysilane, pentamethyldisiloxane, and the initiator trifluoromethanesulfonic acid were added to a flask and cooled to 0-5°C in an ice-water bath. Under nitrogen protection, deionized water was slowly added dropwise to the flask through a constant-pressure dropping funnel, with the dropping rate controlled to be completed within 30 minutes. The ice-water bath was removed, and the temperature was naturally raised to 25°C. The mixture was stirred for 24 hours. After the reaction was completed, anhydrous sodium bicarbonate was added and stirred for 1 hour, followed by anhydrous sodium sulfate and stirred for 1 hour. The mixture was then filtered, rotary evaporated, and dried to obtain the organosilicon modifier. Furthermore, the ratio of dimethyldiethoxysilane, trifluoropropanetrimethoxysilane, pentamethyldisiloxane and deionized water in the above-mentioned organosilicon modifier is 0.04mol:0.01-0.02mol:0.005-0.01mol:2-4mL; Furthermore, the amounts of initiators trifluoromethanesulfonic acid, anhydrous sodium bicarbonate, and anhydrous sodium sulfate in the above-mentioned organosilicon modifier are 0.1-0.2 wt%, 1-2 wt%, and 15-20 wt% of the total reactants, respectively.
[0006] The manufacturing process of a high-pressure, high-temperature nuclear reactor monitoring and control cable includes the following steps: Step S1: Weigh the raw materials according to the weight parts. Add the high-temperature resistant composite particles, composite flame retardant, nano zinc oxide and silane coupling agent to a high-speed mixer and mix for 10-15 minutes at a speed of 300-500 rpm. Record this as auxiliary material. Mix methyl vinyl silicone rubber, fluorosilicone rubber and phenyl silicone rubber for 5-8 minutes. Then add the auxiliary material and dispersant and mix for 8-12 minutes. Finally add the peroxide and mix for 3-5 minutes. The mixing temperature is ≤40℃. Then sheet, cool and cut to obtain the compound. Step S2: Add the compound obtained in step S1 into an extruder and extrude it at 70-90°C. After extrusion, it passes through the hot air channels of the vulcanization section and the post-vulcanization section for cross-linking vulcanization to obtain the high-temperature resistant silicone rubber material. Further, in step S2, the temperatures of each section of the extruder are set as follows: feeding section 60-70℃, plasticizing section 70-80℃, homogenizing section 80-90℃, and die head 85-95℃; the temperature of the vulcanizing section is 160-190℃, and the time is 25-30 minutes; the temperature of the post-vulcanizing section is 200-230℃, and the time is 8-12 minutes. Step S3: Multiple tinned copper wires are twisted together to form a conductor, which is then covered with polyethylene and cross-linked by electron beam irradiation to form an inner insulation layer, thus forming a wire core; multiple wire cores are then twisted together to form a cable core, which is then covered with flame-retardant polyolefin and cross-linked by electron beam irradiation to form an outer insulation layer; low-smoke halogen-free flame-retardant polyolefin is filled between the cable core and the outer insulation layer to form a filler layer; ceramicized silicone rubber is covered with the outer insulation layer and vulcanized to form an oxygen barrier layer; tinned copper wires are braided around the oxygen barrier layer with a braiding density ≥85% to form a shielding layer; flame-retardant fiberglass tape is wrapped around the shielding layer to form a flame-retardant layer; and the high-temperature resistant silicone rubber material obtained in step S2 is extruded around the flame-retardant layer to form an outer sheath, thus obtaining a high-pressure, high-temperature nuclear reactor monitoring and control cable.
[0007] The beneficial effects of this invention are: The nuclear reactor monitoring and control cable provided by this invention has a structural design that fully considers the multiple performance requirements under the special environment of a nuclear power plant. From the inside out, the cable comprises a cable core, a filler layer, an outer insulation layer, an oxygen barrier layer, a shielding layer, a flame-retardant layer, and an outer sheath. The filler layer, located between the cable core and the outer insulation layer, is used to fix the cable core and buffer external stress. The synergistic configuration of the oxygen barrier layer and the flame-retardant layer effectively improves the cable's safety and integrity under fire conditions. The shielding layer resists external electromagnetic interference, ensuring the stability of signal transmission. The outer sheath, as the outermost layer directly in contact with the external environment, is made of the high-temperature resistant silicone rubber material unique to this invention, playing a crucial protective role in the overall performance of the cable. Through the above structural optimization, this cable not only possesses excellent high-pressure and high-temperature resistance but also good flame retardancy, a long service life, and superior radiation resistance, fully meeting the stringent technical requirements for monitoring and control cables used in nuclear reactors.
[0008] In this invention, the high-temperature resistant silicone rubber material used in the outer sheath embodies the concept of multi-component synergistic reinforcement in its component design. This material uses methyl vinyl silicone rubber, fluorosilicone rubber, and phenyl silicone rubber as the rubber matrix, and is formulated with high-temperature resistant composite particles, composite flame retardants, nano-zinc oxide, silane coupling agents, dispersants, and peroxides, among other additives, through processes such as mixing and vulcanization. Methyl vinyl silicone rubber, as the base compound, imparts excellent high and low temperature resistance and electrical insulation to the material; the introduction of fluorosilicone rubber significantly improves the material's oil and solvent resistance; and phenyl silicone rubber further enhances the material's low-temperature resistance, radiation resistance, and high-temperature mechanical properties. The combined use of these three rubbers achieves complementary and optimized performance, providing a fundamental guarantee for the long-term stable operation of the outer sheath material in the extreme environment of a nuclear reactor.
[0009] In this invention, the high-temperature resistant composite particles are the core functional component for improving the high-temperature resistance of silicone rubber materials. The preparation method involves: using h-BN as a substrate, generating zirconium dioxide nanoparticles on its surface through in-situ synthesis; subsequently, surface modification is performed using a silane coupling agent; and finally, an organosilicon modifier is grafted to form composite particles with a core-shell structure. This structural design endows the composite particles with multiple functions, significantly improving their dispersibility and interfacial compatibility in the silicone rubber matrix.
[0010] As the core substrate, h-BN possesses an excellent layered structure and extremely high thermal conductivity. When uniformly dispersed within the silicone rubber matrix, it forms a physical barrier, effectively hindering the diffusion of oxygen molecules and delaying the thermo-oxidative aging process of the material. Furthermore, the high thermal conductivity of h-BN rapidly conducts and diffuses locally accumulated heat, preventing heat concentration that could lead to premature thermal degradation of the matrix. Simultaneously, as a stable rigid framework, h-BN helps improve the overall structural integrity of the composite material under high-temperature conditions.
[0011] The introduction of ZrO2 can significantly improve the thermal stability and char formation rate of silicone rubber composites. The char layer formed at high temperatures can effectively isolate heat and oxygen, inhibiting further degradation inside the material. On the other hand, ZrO2 can also form a good interfacial interaction with the silicone rubber matrix. In-situ growth of ZrO2 on the h-BN surface can increase surface roughness and active sites. This not only enhances the binding force with subsequent organosilicon modifiers, but also provides more physical crosslinking points for the silicone rubber macromolecular chains, further restricting the movement of molecular chains at high temperatures, thereby improving the thermomechanical properties of the material.
[0012] To further optimize the interfacial compatibility between the composite particles and the silicone rubber matrix, this invention pretreats the BN@ZrO2 core-shell structure with a silane coupling agent, followed by grafting an organosilicon modifier. The main chain of this modifier is an organosilicon segment, chemically similar to the polysiloxane main chain of the silicone rubber matrix. Following the principle of "like dissolves like," it significantly improves the dispersion of the composite particles in the matrix and enhances interfacial bonding. This good interfacial compatibility effectively reduces phonon scattering at the interface, lowers the interfacial thermal resistance, and allows the enhanced thermal conductivity of the composite particles to be fully realized. Simultaneously, the fluorinated groups introduced into the side chains of the organosilicon modifier possess low surface energy and chemical inertness, forming a dense hydrophobic and oleophobic protective layer on the surface of the composite particles and even the final material. This protective layer effectively resists the attack of corrosive media such as oxygen and water vapor at high temperatures. Especially in the temperature range below 350°C, it effectively inhibits the main thermal degradation mechanism of silicone rubber side chains due to oxidation, thereby significantly extending the service life of the material in high-temperature environments. Detailed Implementation
[0013] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0014] Example 1: High-temperature resistant composite particles were prepared by the following steps: Step A1: Add 0.015g of hydroxypropyl cellulose to a mixture of 98mL of ethanol and 2mL of deionized water and stir until homogeneous. Add 0.1g of hexagonal boron nitride nanosheets and disperse evenly by ultrasonication. Stir for 1h, then slowly add 21.5mL of tetrabutyl zirconate alcohol solution. After the addition is complete, react at room temperature for 15h. Filter, wash, and dry to obtain h-BN@ZrO2 nanomaterials. The tetrabutyl zirconate alcohol solution is prepared by mixing and stirring 80% tetrabutyl zirconate in ethanol, and the ratio of tetrabutyl zirconate to ethanol is 1.5mL:20mL. Step A2: Disperse 1g of h-BN@ZrO2 nanomaterial evenly in 45mL of ethanol, add 1mL of silane coupling agent KH570 and stir well, then add 5mL of deionized water, heat to 45℃ and stir for 5h, filter, wash and dry to obtain modified h-BN@ZrO2 nanomaterial. Preferably, the ZrO2 synthesized in situ on the h-BN surface is a high-performance heat-resistant ceramic filler. The in-situ synthesis method ensures that the ZrO2 particles can be uniformly and firmly attached to the h-BN surface, avoiding the agglomeration problem caused by traditional physical mixing.
[0015] Step A3: Mix 0.5g of organosilicon modifier in 15mL of toluene to obtain mixture 1; add 1g of modified h-BN@ZrO2 nanomaterial and 0.01g of Karstedt catalyst to 15mL of toluene, purge with nitrogen and stir for 15min, while raising the temperature to 80℃, then add 15mL of mixture 1 dropwise using a constant pressure dropping funnel, stopping the addition within 90min, then raise the temperature to 100℃ and react for 18h, remove the solvent by rotary evaporation, wash with anhydrous ethanol, and dry to obtain high-temperature resistant composite particles; Preferably, the organosilicon modifier in step A3 is prepared by the following steps: 0.04 mol of dimethyldiethoxysilane, 0.01 mol of trifluoropropanetrimethoxysilane, 0.005 mol of pentamethyldisiloxane, and the initiator trifluoromethanesulfonic acid were added to a flask and cooled to 0-5°C in an ice-water bath. Under nitrogen protection, 2 mL of deionized water was slowly added dropwise to the flask through a constant-pressure dropping funnel, with the dropping rate controlled to be completed within 30 minutes. The ice-water bath was removed, and the temperature was naturally raised to 25°C. The mixture was stirred for 24 hours. After the reaction was completed, anhydrous sodium bicarbonate was added and stirred for 1 hour, followed by anhydrous sodium sulfate and stirred for 1 hour. The mixture was then filtered, rotary evaporated, and dried to obtain the organosilicon modifier. The amounts of the initiator trifluoromethanesulfonic acid, anhydrous sodium bicarbonate, and anhydrous sodium sulfate were 0.1 wt%, 1 wt%, and 15 wt% of the total reactants, respectively.
[0016] Example 2: High-temperature resistant composite particles were prepared by the following steps: Step A1: Add 0.018g of hydroxypropyl cellulose to a mixture of 98mL of ethanol and 2mL of deionized water and stir until homogeneous. Add 0.1g of hexagonal boron nitride nanosheets and disperse evenly by ultrasonication. Stir for 1h, then slowly add 21.6mL of tetrabutyl zirconate alcohol solution. After the addition is complete, react at room temperature for 15h. Filter, wash, and dry to obtain h-BN@ZrO2 nanomaterials. The tetrabutyl zirconate alcohol solution is prepared by mixing and stirring 80% tetrabutyl zirconate in ethanol, and the ratio of tetrabutyl zirconate to ethanol is 1.6mL:20mL. Step A2: Disperse 1g of h-BN@ZrO2 nanomaterials evenly in 45mL of ethanol, add 1.5mL of silane coupling agent KH570 and stir well, then add 5mL of deionized water, heat to 45℃ and stir for 5.5h, filter, wash and dry to obtain modified h-BN@ZrO2 nanomaterials. Step A3: Mix 1 g of organosilicon modifier in 15 mL of toluene to obtain mixture 1; add 1 g of modified h-BN@ZrO2 nanomaterial and 0.02 g of Karstedt catalyst to 15 mL of toluene, purge with nitrogen and stir for 15 min, while raising the temperature to 80 °C, then add 15 mL of mixture 1 dropwise using a constant pressure dropping funnel, stopping the addition within 90 min, then raise the temperature to 100 °C and react for 21 h, remove the solvent by rotary evaporation, wash with anhydrous ethanol, and dry to obtain high-temperature resistant composite particles; Preferably, the organosilicon modifier in step A3 is prepared by the following steps: 0.04 mol of dimethyldiethoxysilane, 0.05 mol of trifluoropropanetrimethoxysilane, 0.0075 mol of pentamethyldisiloxane, and the initiator trifluoromethanesulfonic acid were added to a flask and cooled to 0-5°C in an ice-water bath. Under nitrogen protection, 3 mL of deionized water was slowly added dropwise to the flask through a constant-pressure dropping funnel, with the dropping rate controlled to be completed within 30 minutes. The ice-water bath was removed, and the temperature was naturally raised to 25°C. The mixture was stirred for 24 hours. After the reaction was completed, anhydrous sodium bicarbonate was added and stirred for 1 hour, followed by anhydrous sodium sulfate and stirred for 1 hour. The mixture was then filtered, rotary evaporated, and dried to obtain the organosilicon modifier. The amounts of the initiator trifluoromethanesulfonic acid, anhydrous sodium bicarbonate, and anhydrous sodium sulfate were 0.15 wt%, 1.5 wt%, and 18 wt% of the total reactants, respectively.
[0017] Example 3: High-temperature resistant composite particles were prepared by the following steps: Step A1: Add 0.02g of hydroxypropyl cellulose to a mixture of 98mL of ethanol and 2mL of deionized water and stir until homogeneous. Add 0.1g of hexagonal boron nitride nanosheets and disperse evenly by ultrasonication. Stir for 1h, then slowly add 21.7mL of tetrabutyl zirconate alcohol solution. After the addition is complete, react at room temperature for 15h. Filter, wash, and dry to obtain h-BN@ZrO2 nanomaterials. The tetrabutyl zirconate alcohol solution is prepared by mixing and stirring 80% tetrabutyl zirconate in ethanol, and the ratio of tetrabutyl zirconate to ethanol is 1.7mL:20mL. Step A2: Disperse 1g of h-BN@ZrO2 nanomaterial evenly in 45mL of ethanol, add 2mL of silane coupling agent KH570 and stir well, then add 5mL of deionized water, heat to 45℃ and stir for 6h, filter, wash and dry to obtain modified h-BN@ZrO2 nanomaterial. Step A3: Mix 1.5g of organosilicon modifier in 15mL of toluene to obtain mixture 1; add 1g of modified h-BN@ZrO2 nanomaterial and 0.03g of Karstedt catalyst to 15mL of toluene, purge with nitrogen and stir for 15min, while raising the temperature to 80℃, then add 15mL of mixture 1 dropwise using a constant pressure dropping funnel, stopping the addition within 90min, then raise the temperature to 100℃ and react for 24h, remove the solvent by rotary evaporation, wash with anhydrous ethanol, and dry to obtain high-temperature resistant composite particles; Preferably, the organosilicon modifier in step A3 is prepared by the following steps: 0.04 mol of dimethyldiethoxysilane, 0.02 mol of trifluoropropanetrimethoxysilane, 0.01 mol of pentamethyldisiloxane, and the initiator trifluoromethanesulfonic acid were added to a flask and cooled to 0-5°C in an ice-water bath. Under nitrogen protection, 4 mL of deionized water was slowly added dropwise to the flask through a constant-pressure dropping funnel, with the dropping rate controlled to be completed within 30 minutes. The ice-water bath was removed, and the temperature was naturally raised to 25°C. The mixture was stirred for 24 hours. After the reaction was completed, anhydrous sodium bicarbonate was added and stirred for 1 hour, followed by anhydrous sodium sulfate and stirred for 1 hour. The mixture was then filtered, rotary evaporated, and dried to obtain the organosilicon modifier. The amounts of the initiator trifluoromethanesulfonic acid, anhydrous sodium bicarbonate, and anhydrous sodium sulfate were 0.2 wt%, 2 wt%, and 20 wt% of the total reactants, respectively.
[0018] Example 4: A manufacturing process for a high-pressure, high-temperature nuclear reactor monitoring and control cable includes the following steps: Step S1: Weigh the raw materials according to the weight parts. Add 10 parts of the high-temperature resistant composite particles prepared in Example 1, 12 parts of the composite flame retardant, 3 parts of nano zinc oxide and 2 parts of silane coupling agent to a high-speed mixer and mix at 300 rpm for 10 min. This is recorded as the auxiliary material. Mix 35 parts of methyl vinyl silicone rubber, 5 parts of fluorosilicone rubber and 5 parts of phenyl silicone rubber for 5 min. Then add the auxiliary material and 2 parts of dispersant and mix for 8 min. Finally, add 1.5 parts of peroxide and mix for 3 min. The mixing temperature is ≤40℃. Then sheet, cool and cut to obtain the compound. Preferably, the composite flame retardant is composed of magnesium hydroxide, aluminum hydroxide, and ammonium polyphosphate, and the mass ratio of the three is 1:1:2; the silane coupling agent is dodecyltrimethoxysilane; the dispersant is low molecular weight hydroxyl silicone oil with a molecular weight of 300-5000; and the peroxide is bis(2,5-diphenyl)propionate (PSP). Step S2: Add the compound obtained in step S1 into an extruder and extrude it at 70°C. After extrusion, it passes through the hot air channels of the vulcanization section and the post-vulcanization section for cross-linking vulcanization to obtain the high-temperature resistant silicone rubber material. Preferably, the temperatures of each section of the extruder in step S2 are set as follows: feeding section 60-70℃, plasticizing section 70-80℃, homogenizing section 80-90℃, and die head 85-95℃; the temperature of the vulcanizing section is 165℃ and the time is 22 minutes; the temperature of the post-vulcanizing section is 200℃ and the time is 8 minutes. Step S3: Multiple tinned copper wires are twisted together to form a conductor, which is then covered with polyethylene and cross-linked by electron beam irradiation to form an inner insulation layer, thus forming a wire core; multiple wire cores are then twisted together to form a cable core, which is then covered with flame-retardant polyolefin and cross-linked by electron beam irradiation to form an outer insulation layer; low-smoke halogen-free flame-retardant polyolefin is filled between the cable core and the outer insulation layer to form a filler layer; ceramicized silicone rubber is covered with the outer insulation layer and vulcanized to form an oxygen barrier layer; tinned copper wires are braided around the oxygen barrier layer with a braiding density ≥85% to form a shielding layer; flame-retardant fiberglass tape is wrapped around the shielding layer to form a flame-retardant layer; and the high-temperature resistant silicone rubber material obtained in step S2 is extruded around the flame-retardant layer to form an outer sheath, thus obtaining a high-pressure, high-temperature nuclear reactor monitoring and control cable.
[0019] Example 5: A manufacturing process for a high-pressure, high-temperature nuclear reactor monitoring and control cable includes the following steps: Step S1: Weigh the raw materials according to the weight parts. Add 12 parts of the high-temperature resistant composite particles prepared in Example 2, 14 parts of the composite flame retardant, 4.5 parts of nano zinc oxide and 2.5 parts of silane coupling agent to a high-speed mixer and mix at 400 rpm for 12 min. This is recorded as the auxiliary material. Mix 40 parts of methyl vinyl silicone rubber, 7.5 parts of fluorosilicone rubber and 6.5 parts of phenyl silicone rubber for 7 min. Then add the auxiliary material and 3 parts of dispersant and mix for 10 min. Finally, add 2 parts of peroxide and mix for 4 min. The mixing temperature is ≤40℃. Then sheet, cool and cut to obtain the compound. Preferably, the composite flame retardant is composed of magnesium hydroxide, aluminum hydroxide, and ammonium polyphosphate, and the mass ratio of the three is 1:1:2; the silane coupling agent is hexadecyltrimethoxysilane; the dispersant is low molecular weight hydroxyl silicone oil with a molecular weight of 300-5000; and the peroxide is DCP. Step S2: Add the compound obtained in step S1 into an extruder and extrude it at 80°C. After extrusion, it passes through the hot air channels of the vulcanization section and the post-vulcanization section for cross-linking vulcanization to obtain the high-temperature resistant silicone rubber material. Preferably, the temperatures of each section of the extruder in step S2 are set as follows: feeding section 60-70℃, plasticizing section 70-80℃, homogenizing section 80-90℃, and die head 85-95℃; the temperature of the vulcanizing section is 170℃ and the time is 25min; the temperature of the post-vulcanizing section is 220℃ and the time is 10min. Step S3: Multiple tinned copper wires are twisted together to form a conductor, which is then covered with polyethylene and cross-linked by electron beam irradiation to form an inner insulation layer, thus forming a wire core; multiple wire cores are then twisted together to form a cable core, which is then covered with flame-retardant polyolefin and cross-linked by electron beam irradiation to form an outer insulation layer; low-smoke halogen-free flame-retardant polyolefin is filled between the cable core and the outer insulation layer to form a filler layer; ceramicized silicone rubber is covered with the outer insulation layer and vulcanized to form an oxygen barrier layer; tinned copper wires are braided around the oxygen barrier layer with a braiding density ≥85% to form a shielding layer; flame-retardant fiberglass tape is wrapped around the shielding layer to form a flame-retardant layer; and the high-temperature resistant silicone rubber material obtained in step S2 is extruded around the flame-retardant layer to form an outer sheath, thus obtaining a high-pressure, high-temperature nuclear reactor monitoring and control cable.
[0020] Example 6: A manufacturing process for a high-pressure, high-temperature nuclear reactor monitoring and control cable includes the following steps: Step S1: Weigh the raw materials according to the weight parts. Add 15 parts of the high-temperature resistant composite particles prepared in Example 3, 16 parts of the composite flame retardant, 6 parts of nano zinc oxide and 3 parts of silane coupling agent to a high-speed mixer and mix at 500 rpm for 15 min. This is recorded as the auxiliary material. Mix 45 parts of methyl vinyl silicone rubber, 10 parts of fluorosilicone rubber and 8 parts of phenyl silicone rubber for 8 min. Then add the auxiliary material and 4 parts of dispersant and mix for 12 min. Finally, add 2.5 parts of peroxide and mix for 5 min. The mixing temperature is ≤40℃. Then sheet, cool and cut to obtain the compound. Preferably, the composite flame retardant is composed of magnesium hydroxide, aluminum hydroxide, and ammonium polyphosphate, and the mass ratio of the three is 1:1:2; the silane coupling agent is octadecyltriethoxysilane; the dispersant is low molecular weight hydroxyl silicone oil with a molecular weight of 300-5000; and the peroxide is bis(2,5-diphenyl)propionate (PSP). Step S2: Add the compound obtained in step S1 into an extruder and extrude it at 90°C. After extrusion, it passes through the hot air channels of the vulcanization section and the post-vulcanization section for cross-linking vulcanization to obtain the high-temperature resistant silicone rubber material. Preferably, the temperatures of each section of the extruder in step S2 are set as follows: feeding section 60-70℃, plasticizing section 70-80℃, homogenizing section 80-90℃, and die head 85-95℃; the temperature of the vulcanizing section is 180℃ and the time is 28min; the temperature of the post-vulcanizing section is 230℃ and the time is 12min. Step S3: Multiple tinned copper wires are twisted together to form a conductor, which is then covered with polyethylene and cross-linked by electron beam irradiation to form an inner insulation layer, thus forming a wire core; multiple wire cores are then twisted together to form a cable core, which is then covered with flame-retardant polyolefin and cross-linked by electron beam irradiation to form an outer insulation layer; low-smoke halogen-free flame-retardant polyolefin is filled between the cable core and the outer insulation layer to form a filler layer; ceramicized silicone rubber is covered with the outer insulation layer and vulcanized to form an oxygen barrier layer; tinned copper wires are braided around the oxygen barrier layer with a braiding density ≥85% to form a shielding layer; flame-retardant fiberglass tape is wrapped around the shielding layer to form a flame-retardant layer; and the high-temperature resistant silicone rubber material obtained in step S2 is extruded around the flame-retardant layer to form an outer sheath, thus obtaining a high-pressure, high-temperature nuclear reactor monitoring and control cable.
[0021] Comparative Example 1: This comparative example is a measurement and control cable. The difference between this example and Example 6 is that h-BN is used instead of the high-temperature resistant composite particles prepared in Example 3. All other aspects are the same.
[0022] Comparative Example 2: This comparative example is a measurement and control cable. The difference between this example and Example 6 is that ZrO2 is used instead of the high-temperature resistant composite particles prepared in Example 3. All other aspects are the same.
[0023] Comparative Example 3: This comparative example is a measurement and control cable. The difference between this example and Example 6 is that the high-temperature resistant composite particles prepared in Example 3 were not added. All other aspects are the same.
[0024] The measurement and control cables prepared in Examples 4-6 and Comparative Examples 1-3 were subjected to performance tests: High-temperature resistance test: The measurement and control cables prepared in Examples 4-6 and Comparative Examples 1-3 were subjected to a heat aging test according to GB / T2951.12-2008 standard. After being kept at 250℃ for 168h, the samples were taken out and their tensile strength retention rate and elongation at break retention rate were tested according to GB / T 528-2009. After cooling to room temperature, the tensile strength retention rate X (80%≤X<90% is qualified, 90%≤X<95% is good, ≥95% is excellent) and elongation at break retention rate (70%≤X<80% is qualified, 80%≤X<90% is good, ≥90% is excellent) and elongation at break retention rate were tested. The appearance of the samples after the test was observed to see if they cracked or powdered. Long life performance testing: Referring to IEEE Std 383 "Qualification of Class 1E cables for nuclear power plants", the samples were subjected to aging tests at 135℃, 150℃, 165℃ and 180℃ respectively (refer to GB / T 2951.12-2008). At each temperature point, the samples were periodically removed and their elongation at break was tested according to GB / T 528-2009 standard until the retention rate dropped to 50% of the initial value. This was taken as the end point of the life and the service life was estimated. Flame retardant performance test: The flame retardant performance of vertically installed bundled cables was tested in accordance with GB / T 18380.33-2022. After the test, the cables in the examples and comparative examples all belong to flame retardant Class A. Nuclear radiation resistance and high voltage resistance performance tests: The nuclear radiation resistance and high voltage resistance performance of control cables are tested according to GB / T 22577-2025. For the nuclear radiation resistance test, the sample cable is irradiated with 250kGy of gamma rays. After the irradiation, the sample is taken out and allowed to recover in a standard laboratory environment for 16 hours. During and after the irradiation, the cable sample is observed to have no cracking, pulverization, or obvious deformation. For the high voltage resistance test, the irradiated and aged cable sample is kept in a bent state (the bending diameter is about 40 times the outer diameter of the cable). The sample is immersed in water and a high AC voltage (3.15kV / mm) is applied directly to it. If it does not break down for 5 minutes, it is considered qualified.
[0025] The test results are shown in Table 1: Table 1: Performance Test Results
[0026] As can be seen from Table 1, the measurement and control cable prepared by this invention not only has excellent high temperature resistance, high pressure resistance and radiation resistance, but also excellent flame retardant properties and a long service life.
[0027] The above content is merely an example and illustration of the concept of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described or use similar methods to replace them, as long as they do not deviate from the scope defined by the inventive concept, they should all fall within the protection scope of the present invention.
Claims
1. A high-pressure, high-temperature nuclear reactor monitoring and control cable, characterized in that, From the inside out, it includes the cable core, outer insulation layer, oxygen barrier layer, shielding layer, flame retardant layer, and outer sheath. The cable core is composed of multiple stranded wires, each wire being a conductor covered with an inner insulation layer. The conductor itself is composed of multiple stranded tinned copper wires. A filler layer is provided between the cable core and the outer insulation layer. This filler layer is made of low-smoke halogen-free flame-retardant polyolefin. The inner insulation layer is made of irradiated cross-linked polyethylene, and the outer insulation layer is made of flame-retardant irradiated cross-linked polyolefin. The oxygen barrier layer is made of ceramicized silicone rubber. The flame-retardant layer is made of fiberglass flame-retardant tape. The shielding layer is woven from tinned copper wires. The outer sheath is made of high-temperature resistant silicone rubber. The high-temperature resistant silicone rubber material comprises the following raw materials in parts by weight: 35-45 parts of methyl vinyl silicone rubber, 5-10 parts of fluorosilicone rubber, 5-8 parts of phenyl silicone rubber, 10-15 parts of high-temperature resistant composite particles, 12-16 parts of composite flame retardant, 3-6 parts of nano zinc oxide, 2-3 parts of silane coupling agent, 2-4 parts of dispersant, and 1.5-2.5 parts of peroxide. The high-temperature resistant composite particles are prepared by modifying h-BN@ZrO2 nanomaterials with an organosilicon modifier; the modified h-BN@ZrO2 nanomaterials are prepared by loading ZrO2 onto the surface of h-BN and then modifying it with KH570; the organosilicon modifier is prepared by reacting dimethyldiethoxysilane, trifluoropropanetrimethoxysilane and pentamethyldisiloxane.
2. The high-pressure, high-temperature nuclear reactor monitoring and control cable according to claim 1, characterized in that, The high-temperature resistant composite particles are prepared by the following steps: Step A1: Add hydroxypropyl cellulose to a mixture of ethanol and deionized water and stir until homogeneous. Add h-BN and disperse evenly by ultrasonication. Stir for 1 hour, then slowly add tetrabutyl zirconate solution. After the addition is complete, react at room temperature for 15 hours. Filter, wash, and dry to obtain h-BN@ZrO2 nanomaterials. Step A2: Disperse the h-BN@ZrO2 nanomaterials evenly in ethanol, add silane coupling agent KH570 and stir well, then add deionized water, heat to 45℃ and stir for 5-6 hours, filter, wash and dry to obtain modified h-BN@ZrO2 nanomaterials. Step A3: Stir the organosilicon modifier in toluene to obtain mixture 1; add the modified h-BN@ZrO2 nanomaterials and Karstedt catalyst to toluene, purge with nitrogen and stir for 15 min, while simultaneously raising the temperature to 80°C, then add mixture 1 dropwise using a constant pressure dropping funnel, stopping the addition within 90 min, then raise the temperature to 100°C and react for 18-24 h, remove the solvent by rotary evaporation, wash with anhydrous ethanol, and dry to obtain high-temperature resistant composite particles.
3. The high-pressure, high-temperature nuclear reactor monitoring and control cable according to claim 2, characterized in that, In step A1, the ratio of hydroxypropyl cellulose, ethanol, deionized water, hexagonal boron nitride nanosheets, and tetrabutyl zirconate alcohol solution is 0.015-0.02 g: 98 mL: 2 mL: 0.1 g: 21.5-21.7 mL; the tetrabutyl zirconate ethanol solution is prepared by mixing and stirring 80% tetrabutyl zirconate in ethanol, and the ratio of tetrabutyl zirconate to ethanol is 1.5-1.7 mL: 20 mL.
4. The high-pressure, high-temperature nuclear reactor monitoring and control cable according to claim 2, characterized in that, The ratio of h-BN@ZrO2 nanomaterial, ethanol, KH570 and deionized water used in step A2 is 1g:45mL:1-2mL:5mL.
5. The high-pressure, high-temperature nuclear reactor monitoring and control cable according to claim 2, characterized in that, In step A3, the ratio of the modified h-BN@ZrO2 nanomaterial, Karstedt catalyst, toluene, and mixture 1 is 1g:0.01-0.03g:15mL:15mL, and the ratio of the organosilicon modifier to toluene in mixture 1 is 0.5-1.5g:15mL.
6. The high-pressure, high-temperature nuclear reactor monitoring and control cable according to claim 2, characterized in that, The organosilicon modifier mentioned in step A3 is prepared by the following steps: Dimethyldiethoxysilane, trifluoropropanetrimethoxysilane, pentamethyldisiloxane and initiator trifluoromethanesulfonic acid were added to a flask and cooled to 0-5°C in an ice-water bath. Under nitrogen protection, deionized water was slowly added dropwise to the flask through a constant pressure dropping funnel, and the dropping rate was controlled to be completed within 30 minutes. Remove the ice-water bath and allow the temperature to rise naturally to 25°C. Stir the reaction for 24 hours. After the reaction is complete, add anhydrous sodium bicarbonate and stir for 1 hour, then add anhydrous sodium sulfate and stir for 1 hour. Filter, rotary evaporate, and dry to obtain the organosilicon modifier.
7. The high-pressure, high-temperature nuclear reactor monitoring and control cable according to claim 6, characterized in that, The ratio of dimethyldiethoxysilane, trifluoropropanetrimethoxysilane, pentamethyldisiloxane, and deionized water in the organosilicon modifier is 0.04 mol: 0.01-0.02 mol: 0.005-0.01 mol: 2-4 mL. The amounts of the initiators trifluoromethanesulfonic acid, anhydrous sodium bicarbonate, and anhydrous sodium sulfate are 0.1-0.2 wt%, 1-2 wt%, and 15-20 wt% of the total reactants, respectively.
8. The high-pressure, high-temperature nuclear reactor monitoring and control cable according to claim 1, characterized in that, The composite flame retardant is composed of magnesium hydroxide, aluminum hydroxide and ammonium polyphosphate, and the mass ratio of the three is 1:1:2; the silane coupling agent is one of long-chain alkyl silanes; the dispersant is low molecular weight hydroxyl silicone oil with a molecular weight of 300-5000; the peroxide is one of bis(2,5-diphenyl)-DCP or DCP.
9. A manufacturing process for the high-pressure, high-temperature nuclear reactor monitoring and control cable according to any one of claims 1-8, characterized in that, Includes the following steps: Step S1: Weigh the raw materials according to the weight parts. Add the high-temperature resistant composite particles, composite flame retardant, nano zinc oxide and silane coupling agent to a high-speed mixer and mix for 10-15 minutes at a speed of 300-500 rpm. Record this as auxiliary material. Mix methyl vinyl silicone rubber, fluorosilicone rubber and phenyl silicone rubber for 5-8 minutes. Then add the auxiliary material and dispersant and mix for 8-12 minutes. Finally add the peroxide and mix for 3-5 minutes. The mixing temperature is ≤40℃. Then sheet, cool and cut to obtain the compound. Step S2: Add the compound obtained in step S1 into an extruder and extrude it at 70-90°C. After extrusion, it passes through the hot air channels of the vulcanization section and the post-vulcanization section for cross-linking vulcanization to obtain the high-temperature resistant silicone rubber material. Step S3: Multiple tinned copper wires are twisted together to form a conductor, which is then covered with polyethylene and cross-linked by electron beam irradiation to form an inner insulation layer, thus forming a wire core; multiple wire cores are then twisted together to form a cable core, which is then covered with flame-retardant polyolefin and cross-linked by electron beam irradiation to form an outer insulation layer; low-smoke halogen-free flame-retardant polyolefin is filled between the cable core and the outer insulation layer to form a filler layer; ceramicized silicone rubber is covered with the outer insulation layer and vulcanized to form an oxygen barrier layer; tinned copper wires are braided around the oxygen barrier layer with a braiding density ≥85% to form a shielding layer; flame-retardant fiberglass tape is wrapped around the shielding layer to form a flame-retardant layer; and the high-temperature resistant silicone rubber material obtained in step S2 is extruded around the flame-retardant layer to form an outer sheath, thus obtaining a high-pressure, high-temperature nuclear reactor monitoring and control cable.
10. The manufacturing process of a high-pressure, high-temperature nuclear reactor monitoring and control cable according to claim 9, characterized in that, In step S2, the temperatures of each section of the extruder are set as follows: feeding section 60-70℃, plasticizing section 70-80℃, homogenizing section 80-90℃, and die head 85-95℃; the temperature of the vulcanizing section is 160-190℃, and the time is 20-30 min; the temperature of the post-vulcanizing section is 200-230℃, and the time is 8-12 min.