Rolled core and its preparation method and lithium-ion battery and its preparation method
By using a combination of composite adhesive and insoluble tape, the stress concentration problem at the R-corner of the wound lithium-ion battery was solved, improving the flexibility and bonding strength of the electrode sheet, and enhancing the cycle life and safety of the battery.
Patent Information
- Application Number
- CN202611513853.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-24
- Publication Date
- 2026-11-17
AI Technical Summary
During the winding of lithium-ion batteries, stress concentration at the R-corner of the electrode leads to problems such as electrode cracking, material loss, and lithium plating. Existing technologies struggle to find a balance between improving flexibility and bonding strength, and existing mitigation methods are either complex or costly.
By using a composite adhesive (polyvinylidene fluoride, polyacrylate copolymer, sodium carboxymethyl cellulose) and applying insoluble tape to the innermost R-corner of the core, the flexibility and bonding strength of the electrode sheet are optimized, and stress concentration is alleviated.
It significantly improves electrode flexibility and bonding strength, reduces the risk of lithium plating, enhances battery cycle life and safety performance, and has a simple process with controllable cost.
Smart Images

Figure CN123120909A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of lithium-ion batteries, and more particularly to a core and a method for preparing the same, and a lithium-ion battery and a method for preparing the same. Background Technology
[0002] Lithium-ion batteries, due to their high energy density, long cycle life, and environmental friendliness, have been widely used in electric vehicles, energy storage systems, and portable electronic devices. The winding process is currently one of the mainstream manufacturing processes for lithium-ion batteries, offering advantages such as high production efficiency and low cost. However, wound batteries present some technical challenges during manufacturing and use, particularly at the innermost R-corner of the core (i.e., the arc transition area where the electrode and current collector meet), where stress concentration is prone to occur, leading to problems such as electrode cracking, material shedding, and lithium plating.
[0003] During the winding process, the electrode experiences significant bending stress at the radius (R-corner). While traditional binders (such as polyvinylidene fluoride, PVDF) offer high bonding strength, their poor flexibility fails to effectively alleviate stress concentration at the R-corner. This problem becomes even more pronounced when electrode thickness is increased to enhance energy density. Furthermore, during charging and discharging, the active material undergoes volume expansion and contraction, further intensifying the stress at the R-corner. This can easily lead to electrode separation from the current collector, causing active material detachment, and consequently, capacity decay and safety issues.
[0004] In existing technologies, increasing the amount of binder or using flexible binders is commonly used to improve electrode flexibility. However, increasing the amount of binder reduces the conductivity of the electrode, affecting the rate performance of the battery; while flexible binders alone can improve flexibility, their bonding strength is insufficient to meet the requirements of high-energy-density batteries. Additionally, some technologies alleviate stress by adding supports at the radius (R-angle) or using gradient porosity designs, but these methods are complex, costly, and have limited effectiveness.
[0005] Therefore, it is desirable to provide an improved winding core and its preparation method, as well as a lithium-ion battery and its preparation method. Summary of the Invention
[0006] The following is an overview of the subject matter described in detail herein. This overview is not intended to limit the scope of protection of this application.
[0007] In one aspect, this application provides a winding core, which is formed by winding an electrode assembly comprising a positive electrode sheet, a negative electrode sheet, and a separator located between the positive electrode sheet and the negative electrode sheet; The positive electrode sheet is prepared from a positive electrode slurry comprising a positive electrode active material, a conductive agent, a solvent, and a first composite binder. The first composite binder comprises, by weight, 80-95 parts of polyvinylidene fluoride, 5-15 parts of polyacrylate copolymer, 2-5 parts of sodium carboxymethyl cellulose, and 2-8 parts of ethylene carbonate. The negative electrode sheet is prepared from a negative electrode slurry comprising a negative electrode active material, a conductive agent, a solvent and a second composite binder. The second composite binder comprises, by weight, 80-95 parts of polyvinylidene fluoride, 5-15 parts of polyacrylate copolymer, 2-5 parts of sodium carboxymethyl cellulose and 2-8 parts of ethylene carbonate. Insoluble adhesive tape is applied to at least one radius corner of at least the innermost layer of the core.
[0008] In this application, the term "R-angle" generally refers to the arc-shaped transition area at the junction of the electrode and the current collector. In this application, insoluble adhesive tape can be applied to the R-angle locations at the innermost or penultimate layer (the location of the highest electrode stress) and / or the penultimate layer of the core. Each core has 1-4 R-angle locations where insoluble adhesive tape can be applied. Figure 1 (Three locations are shown).
[0009] In this application, the term "insoluble tape" refers to a tape in which neither the base film material nor the adhesive material reacts with the components of the electrolyte (such as the electrolyte commonly used in lithium-ion batteries). In other words, the insoluble tape will not dissolve in the electrolyte, or the electrolyte will not enter the tape and cause adverse physical or chemical changes such as expansion.
[0010] The electrolyte applicable to this application may include any conventional electrolyte used in lithium-ion batteries, which may include solvents, lithium salts, and additives. For example, the main components of the solvent may be EC, EMC, or DMC, with a solvent ratio of 3:4:3; the lithium salt may include LiPF6 with a solute concentration of 1.0~1.2 mol / L; the additives may be VC at a content of 2~4 wt%; FEC at a content of 1~2 wt%, etc.
[0011] In one exemplary embodiment, the mass of the first composite binder accounts for 0.5%-1% of the total mass of the positive electrode slurry, and the mass of the second composite binder accounts for 0.1%-0.5% of the total mass of the negative electrode slurry.
[0012] In one exemplary embodiment, the first composite adhesive and the second composite adhesive may be the same or different.
[0013] In one exemplary embodiment, the polyacrylate copolymer is a butyl acrylate-methyl acrylate copolymer or an ethyl acrylate-methyl methacrylate copolymer; and / or, The insoluble tape includes a base film and an adhesive coated on the surface of the base film.
[0014] In one exemplary embodiment, the positive electrode active material is at least one selected from lithium iron phosphate, nickel-cobalt-manganese ternary materials, and lithium cobalt oxide; and / or, The conductive agent is at least one of conductive carbon black, graphene, and carbon nanotubes; and / or, The solvent is selected from at least one of N-methylpyrrolidone, water, and N,N-dimethylformamide; and / or, The base film is selected from at least one of polyethylene, polypropylene, poly(m-phenylene isophthalamide), polyethylene terephthalate, polyimide, and composite materials comprising ethylene carbonate and polyvinylidene fluoride; and / or, The adhesive is selected from either acrylates or silicones.
[0015] In one exemplary embodiment, the base film comprises 90-97 parts by weight of ethylene carbonate and 3-10 parts by weight of polyvinylidene fluoride.
[0016] In an exemplary embodiment, the negative electrode active material is at least one of graphite, silicon-carbon composite material, and lithium titanate; the conductive agent is at least one of conductive carbon black, graphene, and carbon nanotubes; and the solvent is selected from at least one of N-methylpyrrolidone, water, and N,N-dimethylformamide.
[0017] In one exemplary embodiment, the thickness of the positive electrode is 120µm-183µm; and / or, The thickness of the negative electrode sheet is 136µm-145µm; and / or, The thickness of the insoluble adhesive tape is 10μm-50μm; and / or, The thickness of the diaphragm is 3μm-50μm; and / or, The diaphragm is selected from at least one of polyethylene, polypropylene, polyvinylidene fluoride, polyimide membrane, polyamide membrane, and composite membrane of polypropylene and polyethylene.
[0018] On the other hand, this application provides a method for preparing a core, the method comprising the following steps: S1: The positive electrode active material, conductive agent, solvent and first composite binder are mixed to form a positive electrode slurry, and the positive electrode slurry is coated on the positive electrode current collector, dried and rolled to obtain a positive electrode sheet; S2: Mix the negative electrode active material, conductive agent, solvent and second composite binder to form a negative electrode slurry, and coat the negative electrode slurry onto the negative electrode current collector, dry and roll to obtain a negative electrode sheet; S3: Stack the positive electrode sheet, the separator, and the negative electrode sheet in sequence, apply insoluble adhesive tape to at least one R-corner of at least the innermost layer of the core to be formed, and then wind it to obtain the core.
[0019] On the other hand, this application provides a wound lithium-ion battery, including the above-described core or a core prepared by the above-described method.
[0020] On the other hand, this application provides a method for preparing a wound lithium-ion battery, the method comprising assembling the above-mentioned core or a core prepared by the above method into a housing, injecting electrolyte, and encapsulating, thereby obtaining the wound lithium-ion battery.
[0021] On the other hand, this application provides a battery module including a plurality of the above-described wound lithium-ion batteries or a plurality of wound lithium-ion batteries prepared by the above-described method.
[0022] Compared with the prior art, this application has the following beneficial effects: 1. Significantly Improved Electrode Flexibility: By introducing polyacrylate copolymers and sodium carboxymethyl cellulose, the flexibility of the electrode is significantly improved, reducing the risk of breakage during winding. Polyacrylate copolymers have a low glass transition temperature, effectively improving the bending performance of the electrode; sodium carboxymethyl cellulose, as a thickener and flexibility agent, further enhances the mechanical properties of the electrode.
[0023] 2. Good Adhesion Strength: Polyvinylidene fluoride (PVDF) serves as the main binder, ensuring the adhesion strength of the electrode sheets and preventing the active material from detaching. The addition of ethylene carbonate improves the compatibility between the binder and the electrolyte, enabling the formation of a stable interfacial film during charge and discharge, thus enhancing the battery's cycle performance.
[0024] 3. Effective relief of R-corner stress: Insoluble tape is set at at least the innermost R-corner of the core, which reserves space for the volume expansion of the electrode during charging and discharging, effectively relieving stress concentration at the R-corner and preventing the electrode from cracking and falling off.
[0025] 4. Significantly reduced lithium plating risk: By optimizing the binder formulation and applying insoluble tape, the flexibility and interface stability of the electrode at the R-corner are improved, reducing the risk of lithium plating caused by uneven current density distribution and improving the safety performance of the battery.
[0026] 5. Simple process and controllable cost: The composite adhesive and insoluble tape application process used in this application are compatible with existing production lines, requiring no additional complex equipment. The process is simple, the cost is controllable, and it is easy to industrialize.
[0027] 6. Significantly improved cycle life: By improving the stress distribution and interface stability at the R-corner, the cycle life of the battery is significantly improved.
[0028] Other features and advantages of this application will be set forth in the following description, and will be apparent in part from the description, or may be learned by practicing the application. Other advantages of this application can be realized and obtained by means of the solutions described in the description and the accompanying drawings. Attached Figure Description
[0029] The accompanying drawings are used to provide an understanding of the technical solutions of this application and constitute a part of the specification. They are used together with the embodiments of this application to explain the technical solutions of this application and do not constitute a limitation on the technical solutions of this application.
[0030] Figure 1 A schematic diagram showing the application position of the insoluble adhesive tape used for the core in Embodiment 1 of this application is shown. Detailed Implementation
[0031] To make the objectives, technical solutions, and advantages of this application clearer, the embodiments of this application are described in detail below. It should be noted that, unless otherwise specified, the embodiments and features described in these embodiments can be arbitrarily combined with each other.
[0032] Unless otherwise specified, all materials used in the following examples and comparative examples are commercially available.
[0033] Example 1 Preparation of composite adhesive: Take 90 kg of polyvinylidene fluoride (PVDF), 8 kg of butyl acrylate-methyl acrylate copolymer (which can be purchased from BASF, such as Acronal A110), 3 kg of sodium carboxymethyl cellulose (CMC), and 5 kg of ethylene carbonate (EC) by weight, mix them evenly to obtain the composite adhesive.
[0034] Preparation of positive electrode slurry: Take 920 kg of lithium iron phosphate positive electrode active material (which can be purchased from Guoxuan High-Tech Co., Ltd.), 15 kg of conductive carbon black, 5 kg of carbon nanotubes, 20 kg of composite binder prepared in Example 1, and 1200 kg of N-methylpyrrolidone (NMP), and add them sequentially to a mixing tank. Stir for 2 hours at a revolution speed of 25 rpm / min and a rotation speed of 3000 rpm / min. Pass the mixture through a 100-mesh sieve to obtain the positive electrode slurry.
[0035] Preparation of negative electrode slurry: Take 950 kg of artificial graphite negative electrode active material, 10 kg of conductive carbon black, 50 kg of composite binder prepared in Example 1, and an appropriate amount of deionized water. Stir for 1.5 hours at a revolution speed of 20 rpm / min and a rotation speed of 2500 rpm / min. Pass through a 100-mesh sieve to obtain negative electrode slurry.
[0036] Preparation of insoluble tape: By weight, take 95 kg of ethylene carbonate and 5 kg of polyvinylidene fluoride, mix them evenly, heat and melt them at 80°C, coat them into a film with a thickness of 30 μm, and obtain a base film after cooling and solidification; coat the surface of the base film with an acrylic adhesive to obtain an insoluble tape with a thickness of 40 µm.
[0037] Fabrication of wound lithium-ion batteries: S1: The prepared positive electrode slurry is coated onto an aluminum foil current collector, dried at 120℃, and rolled until the compaction density is 3.2 g / cm³. 3 A positive electrode sheet with a thickness of 180µm was obtained.
[0038] S2: The prepared negative electrode slurry is coated onto a copper foil current collector, dried at 100℃, and rolled until the compaction density is 1.6 g / cm³. 3 The negative electrode sheet with a thickness of 140µm was obtained.
[0039] S3: Stack the positive electrode sheet, separator (using polyethylene separator), and negative electrode sheet in sequence, at the three innermost R-corners of the core to be formed (e.g., ...). Figure 1 (Illustratively shown) Apply insoluble adhesive tape, then wind it. The initial winding tension is 450g, decreasing by 8g per turn, with a minimum tension of 200g, to obtain the core.
[0040] S4: Assemble the core into the aluminum shell, inject electrolyte (1M LiPF6 / EC+DMC+EMC, volume ratio 1:1:1), encapsulate, bake at 105℃ for 48 hours, and perform formation, aging, and capacity testing to obtain a lithium-ion battery.
[0041] Comparative Example 1 The difference from Example 1 is that conventional PVDF binders are used in both the positive and negative electrode slurries (without the addition of polyacrylate copolymers, sodium carboxymethyl cellulose (CMC) and ethylene carbonate (EC), and insoluble tape is not applied during winding).
[0042] Comparative Example 2 The difference from Example 1 is that conventional PVDF binder is used in both the positive and negative electrode slurries, but insoluble tape is applied during winding.
[0043] Comparative Example 3 The difference from Example 1 is that the composite binder prepared in Example 1 is used in both the positive and negative electrode slurries, but insoluble tape is not applied during winding.
[0044] Performance testing The performance of the lithium-ion batteries prepared in Example 1 and Comparative Examples 1-3 was tested, and the results are shown in Table 1 below.
[0045] Table 1 As can be seen from the results in Table 1, the lithium-ion battery prepared in Example 1 of this application is significantly superior to the comparative examples in terms of electrode flexibility, electrode integrity at the R-corner, initial charge-discharge efficiency, cycle performance, and safety. Comparative Example 1, due to the lack of composite adhesive and bonding process, exhibits poor performance across all indicators. Comparative Example 2, although coated with insoluble tape, still suffers from a high electrode cracking rate at the R-corner due to insufficient adhesive flexibility. Comparative Example 3, while employing a composite adhesive, fails to completely resolve the stress concentration problem at the R-corner due to the absence of insoluble tape, resulting in slightly lower cycle performance than Example 1.
[0046] Therefore, this application effectively solves the stress concentration problem at the R-corner of wound lithium-ion batteries by optimizing the binder formulation and winding process, significantly improving the cycle life and safety performance of the batteries, and has important application value.
[0047] Although embodiments of this application have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting this application. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of this application.
Claims
1. A core, characterized in that, The core is formed by winding an electrode assembly consisting of a positive electrode sheet, a negative electrode sheet, and a separator located between the positive electrode sheet and the negative electrode sheet; The positive electrode sheet is prepared from a positive electrode slurry comprising a positive electrode active material, a conductive agent, a solvent, and a first composite binder. The first composite binder comprises, by weight, 80-95 parts of polyvinylidene fluoride, 5-15 parts of polyacrylate copolymer, 2-5 parts of sodium carboxymethyl cellulose, and 2-8 parts of ethylene carbonate. The negative electrode sheet is prepared from a negative electrode slurry comprising a negative electrode active material, a conductive agent, a solvent and a second composite binder. The second composite binder comprises, by weight, 80-95 parts of polyvinylidene fluoride, 5-15 parts of polyacrylate copolymer, 2-5 parts of sodium carboxymethyl cellulose and 2-8 parts of ethylene carbonate. Insoluble adhesive tape is applied to at least one radius corner of at least the innermost layer of the core.
2. The core of claim 1, wherein The first composite binder accounts for 0.5%-1% of the total mass of the positive electrode slurry, and the second composite binder accounts for 0.1%-0.5% of the total mass of the negative electrode slurry; and / or, The first composite adhesive may be the same as or different from the second composite adhesive.
3. The core of claim 1, wherein The polyacrylate copolymer is a butyl acrylate-methyl acrylate copolymer or an ethyl acrylate-methyl methacrylate copolymer; and / or, The insoluble tape includes a base film and an adhesive coated on the surface of the base film.
4. The core of claim 1, wherein The positive electrode active material is at least one of lithium iron phosphate, nickel-cobalt-manganese ternary materials, and lithium cobalt oxide; and / or, The conductive agent is at least one of conductive carbon black, graphene, and carbon nanotubes; and / or, The solvent is selected from at least one of N-methylpyrrolidone, water, and N,N-dimethylformamide; and / or, The base film is selected from at least one of polyethylene, polypropylene, poly(m-phenylene isophthalamide), polyethylene terephthalate, polyimide, and composite materials comprising ethylene carbonate and polyvinylidene fluoride; and / or, The adhesive is selected from either acrylates or silicones.
5. The core of claim 1 wherein, The negative electrode active material is at least one of graphite, silicon-carbon composite material, and lithium titanate; and / or, The conductive agent is at least one of conductive carbon black, graphene, and carbon nanotubes; and / or, The solvent is selected from at least one of N-methylpyrrolidone, water, and N,N-dimethylformamide.
6. The core according to any one of claims 1-5, characterized in that The thickness of the positive electrode sheet is 120µm-183µm; and / or, The thickness of the negative electrode sheet is 136µm-145µm; and / or, The thickness of the insoluble adhesive tape is 10μm-50μm; and / or, The thickness of the diaphragm is 3μm-50μm; and / or, The diaphragm is selected from at least one of polyethylene, polypropylene, polyvinylidene fluoride, polyimide membrane, polyamide membrane, and composite membrane of polypropylene and polyethylene.
7. A method of making a roll core, characterized by, The method includes the following steps: S1: The positive electrode active material, conductive agent, solvent and first composite binder are mixed to form a positive electrode slurry, and the positive electrode slurry is coated on the positive electrode current collector, dried and rolled to obtain a positive electrode sheet; S2: Mix the negative electrode active material, conductive agent, solvent and second composite binder to form a negative electrode slurry, and coat the negative electrode slurry onto the negative electrode current collector, dry and roll to obtain a negative electrode sheet; S3: Stack the positive electrode sheet, the separator, and the negative electrode sheet in sequence, apply insoluble adhesive tape to at least one R-corner of at least the innermost layer of the core to be formed, and then wind it to obtain the core.
8. A wound lithium-ion battery, characterized by The core includes any one of claims 1 to 6 or the core prepared by the method of claim 7.
9. A method of manufacturing a wound lithium-ion battery, characterized by, The method includes assembling the core according to any one of claims 1 to 6 or the core prepared by the method according to claim 7 into a housing, injecting electrolyte, and encapsulating to obtain the wound lithium-ion battery.
10. A battery module, characterized by This includes multiple wound lithium-ion batteries as described in claim 8 or multiple wound lithium-ion batteries prepared by the method described in claim 9.