An electromagnetic shielding composite material based on nacre biomimetic structure, its preparation method and application
By utilizing a biomimetic electromagnetic shielding composite material based on a nacreous layer, and employing a micro-concave-convex nested interlocking structure of conductive and dielectric layers and impedance gradient modulation, the problems of low absorption efficiency and large interface reflection in existing electromagnetic shielding materials over a wide frequency band are solved. This achieves lightweight and structurally integrated electromagnetic shielding effects, making it suitable for high-speed railways and high-performance electronic equipment.
Patent Information
- Application Number
- CN202611619908.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing electromagnetic shielding materials mainly rely on reflection, resulting in low internal absorption efficiency. Multilayer composite materials have discontinuous impedance and large interface reflections, which affect broadband shielding performance and make it difficult to cover electromagnetic interference in complex operating environments such as high-speed trains and bullet trains. Furthermore, the materials are heavy, have poor processability, and limited mechanical properties, which is not conducive to the integration of structural components.
An electromagnetic shielding composite material based on a nacreous biomimetic structure is used. A micro-concave-convex nested interlocking structure is formed by the staggered arrangement of conductive and dielectric layers. The mass concentration of conductive nanomaterials in the conductive layer increases layer by layer, while the concentration of dielectric nanoparticles in the dielectric layer remains constant. By combining impedance gradient modulation and the micro-concave-convex nested interlocking structure, multiple scattering and absorption of electromagnetic waves in the thickness direction can be achieved.
It improves the broadband high-efficiency absorption and low reflection performance of electromagnetic shielding materials, enhances interlayer bonding and mechanical properties, and achieves lightweight and structural integration, making it suitable for electromagnetic shielding of high-speed railways and high-performance electronic equipment.
Smart Images

Figure CN123124322A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electromagnetic shielding materials technology, and in particular relates to an electromagnetic shielding composite material based on a nacreous biomimetic structure, its preparation method, and its application. Background Technology
[0002] In recent years, with the widespread application of high-speed railways, bullet trains, and highly integrated electronic equipment, on-board electronic systems are facing increasingly serious electromagnetic interference (EMI) problems. To ensure stable communication, reliable sensors, and system safety, the research on electromagnetic shielding materials has become an important direction in the field of materials science. Although traditional metallic shielding materials have high shielding effectiveness in the low- to mid-frequency range, they suffer from problems such as heavy weight and high processing difficulty, making it difficult to meet the requirements of lightweight design and complex structural integration in modern trains.
[0003] In recent years, polymer-based composite electromagnetic shielding materials have become a research hotspot. A typical approach involves dispersing conductive fillers such as carbon nanotubes, graphene, carbon fibers, or metal nanosheets within a resin or polymer matrix to form a conductive network, thereby achieving shielding functionality. These homogeneous composite materials exhibit shielding effects within a certain frequency band, but their shielding effectiveness primarily relies on reflection, resulting in low internal absorption loss. Furthermore, the uniform distribution of fillers or uncontrollable interlayer distribution, coupled with a lack of impedance matching in the thickness direction, limits broadband shielding capabilities. Additionally, it is difficult to simultaneously achieve lightweight design, processability, and multifunctional structural integration.
[0004] Biomimetic structural design offers a new approach to solving the aforementioned problems. Patent CN104786615A discloses a shell-like polymer-based electromagnetic shielding material and its preparation method, which forms a composite similar to natural nacre by alternating layers of insulating and conductive layers. While this method improves the shielding effectiveness of the material while maintaining good mechanical properties, its impedance gradient is uncontrollable, making it difficult to achieve gradual attenuation of electromagnetic wave energy in the thickness direction. Furthermore, the conductive layer filler is relatively uniformly distributed or fixed only according to the number of layers, lacking the ability to precisely control the gradient, thus limiting the shielding frequency range and absorption effect. Summary of the Invention
[0005] To address the problems of existing electromagnetic shielding materials that primarily rely on reflection, resulting in low internal absorption efficiency; multilayer composite materials exhibiting impedance discontinuities and high interface reflections, affecting broadband shielding performance; insufficient broadband response capability, making it difficult to cover electromagnetic interference in complex operating environments such as high-speed trains and bullet trains; and material weight, poor processability, and limited mechanical properties, hindering structural integration, this invention provides an electromagnetic shielding composite material based on a nacreous biomimetic structure, its preparation method, and its applications. This invention achieves broadband high-efficiency absorption, low reflection, lightweight design, and structural integration through the synergistic effect of biomimetic nacreous structure design, impedance gradient control, and a micro-concave-convex nested interlocking structure. The prepared nacreous biomimetic electromagnetic shielding composite material can be widely used for electromagnetic shielding in high-speed railways, bullet trains, and high-performance electronic equipment.
[0006] To achieve the above-mentioned objectives, the present invention adopts the following technical solution: In a first aspect, the present invention provides an electromagnetic shielding composite material based on a nacreous biomimetic structure, comprising alternating conductive and dielectric layers, wherein adjacent conductive and dielectric layers form a micro-concave-convex nested interlocking structure; the matrix material in the conductive layer is filled with conductive nanomaterials, and the matrix material in the dielectric layer is filled with dielectric nanomaterials; along the thickness direction of the electromagnetic shielding composite material, the mass concentration of conductive nanomaterials in the spaced conductive layers increases layer by layer, and the mass concentration of dielectric nanoparticles in the spaced dielectric layers is the same.
[0007] Furthermore, in the micro-convex-concave nested interlocking structure, the height of the protrusion is 15-20 μm, the depth of the groove is 15-20 μm, the distance between the highest points of two adjacent protrusions is 80-100 μm, and the distance between the lowest points of two adjacent grooves is 80-100 μm; the height of the protrusion or the depth of the groove is not greater than 1 / 2 of the thickness of the corresponding conductive layer or dielectric layer.
[0008] This invention simulates the interlocking characteristics of natural nacre brick-mud composite by designing a micro-concave-convex nested interlocking structure at each layer interface. The micro-concave-convex nested interlocking interface increases multiple scattering paths, improving the internal absorption loss of electromagnetic waves; at the same time, it enhances the interlayer bonding force and the toughness of the composite material, preventing interlayer slippage or delamination.
[0009] Furthermore, the conductive nanomaterial includes one or both of graphene and carbon nanotubes; the dielectric nanomaterial is selected from titanium dioxide nanoparticles or alumina nanoparticles.
[0010] Graphene or carbon nanotubes, as conductive nanomaterials, can form conductive networks in matrix materials and improve electromagnetic shielding performance through conductive loss, reflection loss, and multiple scattering. Titanium dioxide nanoparticles or alumina nanoparticles, as dielectric nanomaterials, are used to adjust the dielectric constant, improve impedance matching, and enhance electromagnetic wave absorption.
[0011] Furthermore, the matrix material in the conductive layer and the matrix material in the dielectric layer are selected from epoxy resin or polyimide.
[0012] In preparing the electromagnetic shielding composite material, this invention uses a curable polymer material as the matrix material and fills it with conductive nanomaterials or dielectric nanomaterials.
[0013] Furthermore, the thickness of the conductive layer is 80–100 μm; the thickness of the dielectric layer is 80–100 μm.
[0014] The electromagnetic shielding composite material based on a nacre biomimetic structure provided by this invention simulates the "brick-and-mortar" structure of natural nacre. The conductive layer is filled with conductive nanomaterials, and the dielectric layer is filled with dielectric nanomaterials. The thickness, filler content, and micro-interlocking structure of each conductive and dielectric layer can be adjusted according to shielding requirements. A conductive nanomaterial gradient is set along the thickness direction of the electromagnetic shielding composite material, causing a continuous change in impedance. A linear impedance gradient is formed from the incident surface to the exit surface. Through the change in impedance gradient, electromagnetic waves are attenuated layer by layer, improving absorption efficiency and reducing interface reflection.
[0015] Secondly, the present invention provides a method for preparing the electromagnetic shielding composite material based on the nacreous biomimetic structure, comprising the following steps: S1. The conductive nanomaterials are added to the matrix material according to the gradient mass concentration, ultrasonically dispersed, additives are added, and stirred evenly. The first conductive layer mixture, the second conductive layer mixture, the third conductive layer mixture, the fourth conductive layer mixture and the fifth conductive layer mixture are obtained according to the mass concentration from low to high. S2. Add the dielectric nanomaterial to the matrix material, disperse it ultrasonically, add the additives, stir evenly, and obtain a dielectric layer mixture; S3. The first conductive layer mixture prepared in step S1 is used to form a pre-cured first conductive layer through a micro-textured mold or a scraping method, so that its surface forms a micro-uneven morphology; the dielectric layer mixture prepared in step S2 is coated on the first conductive layer to obtain a first dielectric layer; the pre-cured second conductive layer, pre-cured second dielectric layer, pre-cured third conductive layer, pre-cured third dielectric layer, pre-cured fourth conductive layer, pre-cured fourth dielectric layer and pre-cured fifth conductive layer are obtained by coating the pre-cured second conductive layer, pre-cured third conductive layer, pre-cured fourth conductive layer and pre-cured fifth conductive layer in sequence by coating the second conductive layer mixture, the third conductive layer mixture, the fourth conductive layer mixture and the fifth conductive layer mixture prepared in step S1; each pre-cured conductive layer and the adjacent pre-cured dielectric layer form a micro-uneven nested interlocking structure to obtain an interlocked multilayer composite material; S4. The interlocking multilayer composite material prepared in step S3 is pre-cured as a whole to obtain a pre-cured interlocking multilayer composite material; S5. The pre-cured interlocking multilayer composite material prepared in step S4 is hot-pressed and cured to obtain a cured interlocking multilayer composite material. After cooling to room temperature, it is demolded to obtain the electromagnetic shielding composite material based on the nacreous biomimetic structure.
[0016] Further, in steps S1 and S2, the additive is independently selected from interfacial coupling agents or dispersants to improve the uniformity of filler dispersion and interfacial bonding. The dispersant is selected from PVP (polyvinylpyrrolidone), SDBS (sodium dodecylbenzenesulfonate), or nonionic dispersants suitable for carbon-based fillers and inorganic nanoparticles. The dispersant is used to reduce the agglomeration tendency between conductive and dielectric nanomaterials, improve the dispersion stability of the filler in the matrix material, and improve the interfacial bonding between the filler and the matrix material.
[0017] Furthermore, in step S2, the amount of dielectric nanomaterial added remains constant, without a gradient distribution, in order to adjust the dielectric constant and improve impedance matching.
[0018] Further, in step S3, the height of the protrusions in the microtextured mold is 15-20 μm, the depth of the grooves is 15-20 μm, the distance between the highest points of two adjacent protrusions is 80-100 μm, and the distance between the lowest points of two adjacent grooves is 80-100 μm.
[0019] Furthermore, in step S3, the coating method involves using a micro-textured scraper, a toothed scraper, or a microstructure printing roller to coat the surface of the pre-cured first conductive layer, which has not yet fully cured, to form a micro-uneven morphology.
[0020] Further, in step S4, the overall pre-curing temperature is 80℃ and the time is 2 h; in step S5, the hot-press curing temperature is 120~250℃, the pressure is 5 MPa, and the time is 3 h.
[0021] Pre-curing allows the layers to initially bond and fix their shape while maintaining the integrity of the micro-concave-convex interfaces. Hot-press curing then fully cross-links the matrix material, fixing the interlocking interfaces of the micro-concave-convex interfaces and forming a nested interlocking structure. Simultaneously, a continuous impedance gradient structure along the thickness direction is created to ensure uniform bonding of each layer, thereby improving the overall mechanical properties of the electromagnetic shielding composite material.
[0022] Thirdly, the present invention provides an application of the electromagnetic shielding composite material based on the nacreous layer biomimetic structure in electromagnetic shielding of rail transit equipment, communication base stations and high-performance electronic equipment.
[0023] Compared with the prior art, the present invention has the following advantages and technical effects: This invention utilizes impedance gradients and a micro-concave-convex nested interlocking structure for multiple scattering, resulting in sufficient attenuation of electromagnetic waves in the thickness direction and a high absorption ratio. Furthermore, it reduces interlayer reflection and improves shielding efficiency through continuous impedance matching and the micro-concave-convex nested interlocking structure. The micro-concave-convex nested interlocking structure enhances interlayer bonding and toughness, preventing peeling or slippage of the conductive and dielectric layers and improving the mechanical properties of the electromagnetic shielding composite material. The invention employs a combination of resin matrix and nanofillers, resulting in low density and the ability to process complex curved surfaces. This invention is the first to introduce a systematic design of impedance gradient structures and micro-concave-convex nested interlocking structures into biomimetic nacre structure shielding materials, achieving synergistic optimization of absorption, impedance matching, and mechanical properties. Attached Figure Description
[0024] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0025] Figure 1 This is a schematic diagram of the electromagnetic shielding composite material based on a nacreous biomimetic structure, provided in an embodiment of the present invention.
[0026] Figure 2 This is a schematic diagram of the micro-concave-convex nested interlocking structure in the electromagnetic shielding composite material based on the biomimetic structure of nacre provided in an embodiment of the present invention; wherein, 1 is a conductive layer; 1-1 is a first conductive layer; 1-2 is a second conductive layer; 1-3 is a third conductive layer; 1-4 is a fourth conductive layer; 1-5 is a fifth conductive layer; 2 is a dielectric layer; and 3 is a micro-textured mold forming interface. Detailed Implementation
[0027] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as a limitation of the present invention, but rather as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0028] It should be understood that the terminology used in this invention is merely for describing particular embodiments and is not intended to limit the invention. Furthermore, with respect to numerical ranges in this invention, it should be understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Every smaller range between any stated value or intermediate value within a stated range, and any other stated value or intermediate value within said range, is also included in this invention. The upper and lower limits of these smaller ranges may be independently included or excluded from the range.
[0029] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art. While only preferred methods and materials have been described herein, any methods and materials similar or equivalent to those described herein may be used in the implementation or testing of this invention. All references to this specification are incorporated by way of citation to disclose and describe methods and / or materials associated with those references. In the event of any conflict with any incorporated reference, the content of this specification shall prevail.
[0030] Various modifications and variations can be made to the specific embodiments described in this specification without departing from the scope or spirit of the invention, as will be apparent to those skilled in the art. Other embodiments derived from this specification will also be apparent to those skilled in the art. This specification and embodiments are merely exemplary.
[0031] The terms “include,” “including,” “have,” “contain,” etc., used in this article are all open-ended terms, meaning that they include but are not limited to.
[0032] This invention provides an electromagnetic shielding composite material based on a nacreous biomimetic structure, comprising alternating conductive and dielectric layers, with adjacent conductive and dielectric layers forming a micro-convex nested interlocking structure; the matrix material of the conductive layers is filled with conductive nanomaterials, and the matrix material of the dielectric layers is filled with dielectric nanomaterials; along the thickness direction of the electromagnetic shielding composite material, the mass concentration of conductive nanomaterials in the spaced conductive layers increases layer by layer, and the mass concentration of dielectric nanoparticles in the spaced dielectric layers is the same.
[0033] Figure 1 This is a schematic diagram of the electromagnetic shielding composite material based on a pearl layer biomimetic structure provided in an embodiment of the present invention; Figure 2 This is a schematic diagram of the micro-concave-convex nested interlocking structure in the electromagnetic shielding composite material based on the nacreous layer biomimetic structure provided in the embodiments of the present invention; Wherein, 1 is the conductive layer; 1-1 is the first conductive layer; 1-2 is the second conductive layer; 1-3 is the third conductive layer; 1-4 is the fourth conductive layer; 1-5 is the fifth conductive layer; 2 is the dielectric layer; and 3 is the microtextured mold forming interface.
[0034] In some preferred embodiments of the present invention, the height of the protrusion in the micro-convex-concave nested interlocking structure is 15-20 μm, the depth of the groove is 15-20 μm, the distance between the highest points of two adjacent protrusions is 80-100 μm, and the distance between the lowest points of two adjacent grooves is 80-100 μm; the height of the protrusion or the depth of the groove is not greater than 1 / 2 of the thickness of the corresponding conductive layer or dielectric layer.
[0035] In some preferred embodiments of the present invention, the conductive nanomaterial includes one or both of graphene and carbon nanotubes; the dielectric nanomaterial is selected from titanium dioxide nanoparticles or alumina nanoparticles.
[0036] In some preferred embodiments of the present invention, the matrix material in the conductive layer and the matrix material in the dielectric layer are selected from epoxy resin or polyimide.
[0037] In some preferred embodiments of the present invention, the thickness of the conductive layer is 80-100 μm; the thickness of the dielectric layer is 80-100 μm.
[0038] This invention provides a method for preparing an electromagnetic shielding composite material based on a nacreous biomimetic structure, comprising the following steps: Step 1: Prepare conductive layer mixture: Prepare mixtures of matrix material and conductive nanomaterial according to the designed ratio, add additives to ensure uniform dispersion of filler, and obtain conductive layer mixtures with mass concentrations from low to high. Step 2: Prepare dielectric layer mixture: Prepare a mixture of matrix material and dielectric nanomaterial according to the designed ratio, add additives to ensure uniform dispersion of filler, and obtain dielectric layer mixture; Step 3, Layered Coating and Micro-interlocking: Each layer of the mixture is sequentially coated or poured into the mold to form a conductive / dielectric interleaved structure; a micro-interlocking structure is formed between each layer, and the microstructure is controlled by micro-textured molds or scraping techniques; Step 4, Overall Pre-curing: After the lamination is completed, overall pre-curing is performed to allow the layers to bond initially; then hot-press curing is performed to fix the micro-concave-convex interface and impedance gradient structure. Step 5, Post-processing: After cooling and demolding, the material undergoes surface polishing, cutting, or further functionalization. The final product is an electromagnetic shielding composite material based on a nacreous layer biomimetic structure, featuring a continuous impedance gradient in the thickness direction and multi-interface micro-concave-convex nesting and interlocking.
[0039] In some preferred embodiments of the present invention, when using a micro-textured mold, micro-protrusions and grooves are pre-processed on the mold surface. The micro-textured mold is one with micro-protrusions and grooves pre-processed on its surface. The height of the protrusions is 15–20 μm, the depth of the grooves is 15–20 μm, the distance between the highest points of two adjacent protrusions is 80–100 μm, and the distance between the lowest points of two adjacent grooves is 80–100 μm. After the conductive layer mixture or dielectric layer mixture is applied, the mixture fills the grooves and covers the protrusion areas under the action of the mold texture. After pre-curing, a micro-protrusion-concave morphology corresponding to the mold texture is formed on the layer surface. When the next layer of mixture is applied, its material enters the recessed areas of the previous layer surface and covers the adjacent protrusion structures, thereby forming a micro-protrusion-concave nested interlocking structure between the conductive layer and the dielectric layer, realizing interlayer physical interlocking.
[0040] In some preferred embodiments of the present invention, when using a scraping technique, a micro-textured scraper, a toothed scraper, or a microstructured printing roller is used to scrape and shape the surface of the layer that is not yet fully cured. By adjusting the scraper texture shape, scraping speed, scraping pressure, and the viscosity of the mixture, regular or quasi-regular microgrooves, microprotrusions, and micro-depressions are formed on the layer surface. Subsequently, the next layer of mixture is applied, so that the next layer of material fills the micro-depressions on the surface of the previous layer and covers the micro-protrusions. After overall pre-curing and hot-press curing, a stable nested and interlocking micro-protrusion structure is formed.
[0041] Through the aforementioned layered coating and micro-convex nested interlocking interface forming process, a continuous micro-convex nested interlocking structure is formed between each conductive layer and dielectric layer. This micro-convex nested interlocking structure, on the one hand, increases the multiple scattering and propagation paths of electromagnetic waves within the material, improving electromagnetic wave absorption loss; on the other hand, it enhances the interlayer mechanical interlocking effect, improving the interlayer bonding force of the composite material and reducing the risk of interlayer slippage, peeling, or delamination.
[0042] This invention also provides an application of the aforementioned electromagnetic shielding composite material based on a nacreous biomimetic structure in electromagnetic shielding of rail transit equipment, communication base stations, and high-performance electronic equipment.
[0043] Example 1: A method for preparing an electromagnetic shielding composite material based on a nacreous biomimetic structure This embodiment aims to verify the feasibility of nacre biomimetic structures, impedance gradients, and micro-concave-convex nested interlocking structures in resin-based composite materials; and to evaluate the expected effects of CNT gradient filling and micro-concave-convex nested interlocking interfaces on broadband electromagnetic shielding absorption, interface reflection, and material toughness. The specific preparation method is as follows: S1. Preparation of conductive layer mixture: CNTs were added to E-51 (bisphenol A type epoxy resin) at mass concentrations of 2 wt%, 4 wt%, 6 wt%, 8 wt%, and 10 wt%, respectively, and ultrasonically treated for 30 min to uniformly disperse the CNTs and break up the agglomerates. Then, 1 wt% of KH-550 (γ-aminopropyltriethoxysilane) was added and stirred evenly to enhance the interfacial bonding between CNTs and E-51, resulting in five sets of conductive layer mixtures, which were named first conductive layer mixture, second conductive layer mixture, third conductive layer mixture, fourth conductive layer mixture, and fifth conductive layer mixture, respectively. S2. Preparation of dielectric layer mixture: Add titanium dioxide nanoparticles with a particle size of 20 nm to E-51 at a mass concentration of 5 wt%, and ultrasonically disperse for 20 min to ensure uniform distribution of titanium dioxide nanoparticles. Add 1 wt% KH-550 and stir evenly to enhance the interfacial bonding between titanium dioxide nanoparticles and E-51 to form dielectric layer mixture. S3. Layered Coating and Micro-Antenna Interlocking: In this embodiment, the height of the protrusions in the micro-textured mold is 20 μm, the depth of the grooves is 20 μm, the distance between the highest points of two adjacent protrusions is 100 μm, and the distance between the lowest points of two adjacent grooves is 100 μm. The first conductive layer mixture prepared in step S1 is poured into the micro-textured mold, with a thickness controlled at 100 μm. Under the action of the micro-textured mold, the first conductive layer mixture fills the grooves and covers the protrusion areas. After pre-curing at 60°C for 30 min, a pre-cured first conductive layer is obtained, and its surface forms a micro-antenna morphology corresponding to the micro-textured mold. The dielectric layer mixture prepared in step S2 is coated on the pre-cured first conductive layer, with a thickness controlled at 100 μm. After pre-curing at 60°C for 30 min, the dielectric layer mixture forms a corresponding micro-antenna morphology on the surface of the pre-cured first conductive layer, resulting in a pre-cured first dielectric layer. Layers are coated layer by layer according to the above method, and each layer is pre-cured at 60°C for 30 min after coating. The following layers were obtained: a pre-cured second conductive layer (obtained by coating the second conductive layer mixture prepared in step S1), a pre-cured second dielectric layer (obtained by coating the dielectric layer mixture prepared in step S2), a pre-cured third conductive layer (obtained by coating the third conductive layer mixture prepared in step S1), a pre-cured third dielectric layer (obtained by coating the dielectric layer mixture prepared in step S2), a pre-cured fourth conductive layer (obtained by coating the fourth conductive layer mixture prepared in step S1), a pre-cured fourth dielectric layer (obtained by coating the dielectric layer mixture prepared in step S2), and a pre-cured fifth conductive layer (obtained by coating the fifth conductive layer mixture prepared in step S1). Each layer had a thickness of 100 μm. Each pre-cured conductive layer and the adjacent pre-cured dielectric layer formed a micro-concave-convex nested interlocking structure to achieve interlayer physical interlocking. This resulted in an interlocked multilayer composite material in which the CNT mass concentration increased layer by layer along the material thickness direction from the incident surface to the exit surface, while the titanium dioxide nanoparticle content in the dielectric layer remained unchanged. S4. Overall pre-curing: The interlocking multilayer composite material prepared in step S3 is placed in an oven and pre-cured at 80°C for 2 hours to obtain the pre-cured interlocking multilayer composite material. S5. Hot pressing curing: The pre-cured interlocking multilayer composite material prepared in step S4 is placed in a hot press, the temperature is set to 120℃, the pressure is 5 MPa, and it is cured for 3 h to obtain the cured interlocking multilayer composite material. S6. Cooling and post-processing: The cured interlocking multilayer composite material prepared in step S5 is naturally cooled to room temperature, demolded, and an electromagnetic shielding composite material based on a nacreous biomimetic structure is obtained.
[0044] Example 2: A method for preparing an electromagnetic shielding composite material based on a nacreous biomimetic structure. This embodiment aims to verify the feasibility of constructing a thickness-direction impedance gradient and a micro-interlocking nested structure with interlocking micro-concave and convex features using highly conductive graphene in a polyimide matrix; to evaluate the broadband absorption capability and high-temperature stability of the electromagnetic shielding composite material; and to provide a lightweight, high-temperature resistant material solution. The specific preparation method is as follows: S1. Preparation of conductive layer mixture: Graphene was added to a polyimide precursor solution with a solid content of 15 wt% at concentrations of 3 wt%, 6 wt%, 9 wt%, 12 wt%, and 15 wt%, respectively. The polyimide precursor solution was prepared by dissolving polyamic acid, which is formed by the condensation polymerization of pyromellitic dianhydride and 4,4′-diaminodiphenyl ether, in N,N-dimethylacetamide (the same below). The mixture was ultrasonically treated for 30 min to ensure uniform dispersion of graphene and break up agglomerates. 1 wt% KH-550 was added and stirred evenly to obtain five sets of conductive layer mixtures, which were named first conductive layer mixture, second conductive layer mixture, third conductive layer mixture, fourth conductive layer mixture, and fifth conductive layer mixture, respectively. S2. Preparation of dielectric layer mixture: Alumina nanoparticles with a particle size of 30 nm are added to the polyimide precursor solution at a concentration of 5 wt%, and ultrasonically dispersed for 20 min to ensure uniform distribution of alumina nanoparticles. 1 wt% KH-550 is added and stirred evenly to form dielectric layer mixture. S3. Layered Coating and Micro-Antenna Interlocking: In this embodiment, the height of the protrusions in the micro-textured mold is 15 μm, the depth of the grooves is 15 μm, the distance between the highest points of two adjacent protrusions is 80 μm, and the distance between the lowest points of two adjacent grooves is 80 μm. The first conductive layer mixture prepared in step S1 is poured into the micro-textured mold, with a thickness controlled at 80 μm. Under the action of the micro-textured mold, the first conductive layer mixture fills the grooves and covers the protrusion areas. After pre-curing at 60°C for 30 min, a pre-cured first conductive layer is obtained, and its surface forms a micro-antenna morphology corresponding to the micro-textured mold. The dielectric layer mixture prepared in step S2 is coated on the pre-cured first conductive layer, with a thickness controlled at 80 μm. After pre-curing at 60°C for 30 min, the dielectric layer mixture forms a corresponding micro-antenna morphology on the surface of the pre-cured first conductive layer, resulting in a pre-cured first dielectric layer. Layers are coated layer by layer according to the above method, and each layer is pre-cured at 60°C for 30 min after coating. The process yields a pre-cured second conductive layer (obtained by coating the second conductive layer mixture prepared in step S1), a pre-cured second dielectric layer (obtained by coating the dielectric layer mixture prepared in step S2), a pre-cured third conductive layer (obtained by coating the third conductive layer mixture prepared in step S1), a pre-cured third dielectric layer (obtained by coating the dielectric layer mixture prepared in step S2), a pre-cured fourth conductive layer (obtained by coating the fourth conductive layer mixture prepared in step S1), a pre-cured fourth dielectric layer (obtained by coating the dielectric layer mixture prepared in step S2), and a pre-cured fifth conductive layer (obtained by coating the fifth conductive layer mixture prepared in step S1). Each layer has a thickness of 80 μm. Each pre-cured conductive layer and the adjacent pre-cured dielectric layer form a micro-concave-convex nested interlocking structure, resulting in an interlocked multilayer composite material in which the graphene mass concentration increases layer by layer along the material thickness direction from the incident surface to the exit surface, while the alumina nanoparticle content in the dielectric layer remains unchanged. S4. Overall pre-curing: The interlocking multilayer composite material prepared in step S3 is placed in an oven and pre-cured at 80°C for 2 hours to obtain the pre-cured interlocking multilayer composite material. S5. Hot pressing curing: The pre-cured interlocking multilayer composite material prepared in step S4 is placed in a hot press, the temperature is set to 250℃, the pressure is 5 MPa, and it is cured for 3 h to obtain the cured interlocking multilayer composite material. S6. Cooling and post-processing: The cured interlocking multilayer composite material prepared in step S5 is naturally cooled to room temperature, demolded, and an electromagnetic shielding composite material based on a nacreous biomimetic structure is obtained.
[0045] Example 3: A method for preparing an electromagnetic shielding composite material based on a nacreous biomimetic structure. This embodiment aims to verify the feasibility of achieving broadband high absorption in electromagnetic shielding composite materials through multi-filler synergy, impedance gradient, and micro-concave-convex nested interlocking structures. It also explores the contribution of the gradient distribution of CNT and graphene composite fillers to absorption efficiency and interlayer bonding strength. In this embodiment, considering that CNT and graphene can synergistically construct a conductive network after composite use, to avoid excessively high total conductive filler content leading to increased resin viscosity and filler agglomeration, the CNT content is set to 4–8 wt%; the graphene content is set to 1–5 wt%. CNT and graphene together form a composite conductive filler gradient, improving the broadband absorption and shielding performance of the electromagnetic shielding composite material. The specific preparation method is as follows: S1. Preparation of conductive layer mixture: CNT and graphene are added to five parts of E-51 according to the designed mass fraction, wherein the CNT content is 4 wt%, 5 wt%, 6 wt%, 7 wt% and 8 wt%, and the graphene content is 1 wt%, 2 wt%, 3 wt%, 4 wt% and 5 wt%, respectively. CNT and graphene together form a composite conductive filler gradient to form a conductive network and impedance gradient with continuous increase in thickness. The mixture is ultrasonically treated for 30 min to fully disperse CNT and graphene and break up agglomerates. 1 wt% sodium dodecylbenzenesulfonate is added as a dispersant, and stirring is continued for 30 min to obtain five sets of conductive layer mixtures, which are named first conductive layer mixture, second conductive layer mixture, third conductive layer mixture, fourth conductive layer mixture and fifth conductive layer mixture, respectively. S2. Preparation of dielectric layer mixture: Add titanium dioxide nanoparticles with a particle size of 20 nm to bisphenol A type epoxy resin at a mass concentration of 3 wt%, and sonicate for 20 min to make the titanium dioxide nanoparticles uniformly distributed. Add 1 wt% sodium dodecylbenzenesulfonate as a dispersant and continue stirring for 30 min to obtain dielectric layer mixture. S3. Layered Coating and Micro-protrusion Interlocking: In this embodiment, a scraping technique is used to prepare the micro-protrusion morphology. The first conductive layer mixture prepared in step S1 is coated onto a polytetrafluoroethylene release film substrate with a thickness controlled at 100 μm. It is pre-cured at 60°C for 20 min to form an incompletely cured first conductive layer with a still malleable surface. A scraper with microtextured texture is used to scrape the mixture, forming a micro-protrusion morphology. The height of the protrusions is 20 μm, the depth of the grooves is 20 μm, the distance between the highest points of two adjacent protrusions is 100 μm, and the distance between the lowest points of two adjacent grooves is 100 μm. The dielectric layer mixture prepared in step S2 is coated onto the pre-cured first conductive layer with a thickness controlled at 100 μm. After pre-curing at 60°C for 20 min, the dielectric layer mixture forms a corresponding micro-protrusion morphology on the surface of the pre-cured first conductive layer, obtaining the pre-cured first dielectric layer. This process of layered coating and pre-curing (60°C, 20 min) is repeated. The following layers were obtained: a pre-cured second conductive layer (obtained by coating the second conductive layer mixture prepared in step S1), a pre-cured second dielectric layer (obtained by coating the dielectric layer mixture prepared in step S2), a pre-cured third conductive layer (obtained by coating the third conductive layer mixture prepared in step S1), a pre-cured third dielectric layer (obtained by coating the dielectric layer mixture prepared in step S2), a pre-cured fourth conductive layer (obtained by coating the fourth conductive layer mixture prepared in step S1), a pre-cured fourth dielectric layer (obtained by coating the dielectric layer mixture prepared in step S2), and a pre-cured fifth conductive layer (obtained by coating the fifth conductive layer mixture prepared in step S1). Each layer had a thickness of 100 μm. Each pre-cured conductive layer and the adjacent pre-cured dielectric layer formed a micro-concave-convex nested interlocking structure, resulting in an interlocked multilayer composite material in which the mass concentration of CNTs and graphene gradually increased from the incident surface to the exit surface along the thickness direction of the material, while the content of titanium dioxide nanoparticles in the dielectric layer remained unchanged. S4. Overall pre-curing: The interlocking multilayer composite material prepared in step S3 is placed in an oven and pre-cured at 80°C for 2 hours to obtain the pre-cured interlocking multilayer composite material. S5 Hot-press curing: The pre-cured interlocking multilayer composite material prepared in step S4 is placed in a hot press, the temperature is set to 120℃, the pressure is 5 MPa, and it is cured for 3 h to obtain the cured interlocking multilayer composite material. S6. Cooling and post-processing: The cured interlocking multilayer composite material prepared in step S5 is naturally cooled to room temperature, demolded, and an electromagnetic shielding composite material based on a nacreous biomimetic structure is obtained.
[0046] Comparative Example 1 Same as Example 1, except that the mass concentration of CNTs is the same in each conductive layer and the mass concentration of titanium dioxide nanoparticles is the same in each dielectric layer. The specific preparation method is as follows: S1. Preparation of conductive layer mixture: Add CNTs to E-51 at a concentration of 5 wt%, sonicate for 30 min to uniformly disperse and break up agglomerates, add 1 wt% KH-550, stir evenly to obtain conductive layer mixture; S2. Preparation of dielectric layer mixture: Same as in Example 1; S3. Layered Coating and Micro-texture Interlocking: The micro-texture mold used in this comparative example is the same as in Example 1; the conductive layer mixture prepared in step S1 is poured into the micro-texture mold, with a thickness controlled at 100 μm. Under the action of the micro-texture mold, the conductive layer mixture fills the grooves and covers the raised areas. After pre-curing at 60°C for 30 min, a pre-cured first conductive layer is obtained, and its surface forms a micro-texture morphology corresponding to the micro-texture mold; the dielectric layer mixture prepared in step S2 is coated on the pre-cured first conductive layer, with a thickness controlled at 100 μm. After pre-curing at 60°C for 30 min, the dielectric layer mixture forms a corresponding micro-texture morphology on the surface of the pre-cured first conductive layer, obtaining a pre-cured first dielectric layer; the above method is followed to coat layer by layer, and each layer is pre-cured at 60°C for 30 min after coating, resulting in a pre-cured second conductive layer, a pre-cured second dielectric layer, a pre-cured third conductive layer, a pre-cured third dielectric layer, a pre-cured fourth conductive layer, a pre-cured fourth dielectric layer, and a pre-cured fifth conductive layer, each with a thickness of 100 μm. μm, each pre-cured conductive layer and the adjacent pre-cured dielectric layer form a micro-concave-convex nested interlocking structure to achieve interlayer physical interlocking. The mass concentration of CNTs in each conductive layer is 5 wt%, and the mass concentration of titanium dioxide nanoparticles in each dielectric layer is 5 wt%, forming an interlocking multilayer composite material. S4. Overall pre-curing: Same as in Example 1; S5. Hot pressing curing: Same as in Example 1; S6. Cooling and post-processing: Same as in Example 1, to prepare electromagnetic shielding composite material.
[0047] Comparative Example 2 Same as Example 1, except that the micro-interlocking nested structure is removed, and the surfaces of each layer remain flat. The specific preparation method is as follows: S1. Preparation of conductive layer mixture: Same as in Example 1; S2. Preparation of dielectric layer mixture: Same as in Example 1; S3. Layer Coating: Pour the first conductive layer mixture prepared in step S1 into a mold with a flat bottom, controlling the thickness to 100 μm, and pre-cur it at 60℃ for 30 min to obtain a pre-cured first conductive layer; coat the dielectric layer mixture prepared in step S2 onto the pre-cured first conductive layer, controlling the thickness to 100 μm, and pre-cur it at 60℃ for 30 min to obtain a pre-cured first dielectric layer; coat layer by layer according to the above method, and pre-cur each layer at 60℃ for 30 min after coating. The following processes were performed to obtain a pre-cured second conductive layer (obtained by coating the second conductive layer mixture prepared in step S1), a pre-cured second dielectric layer (obtained by coating the dielectric layer mixture prepared in step S2), a pre-cured third conductive layer (obtained by coating the third conductive layer mixture prepared in step S1), a pre-cured third dielectric layer (obtained by coating the dielectric layer mixture prepared in step S2), a pre-cured fourth conductive layer (obtained by coating the fourth conductive layer mixture prepared in step S1), a pre-cured fourth dielectric layer (obtained by coating the dielectric layer mixture prepared in step S2), and a pre-cured fifth conductive layer (obtained by coating the fifth conductive layer mixture prepared in step S1). The thickness of each layer was 100 μm. The interfaces between each pre-cured conductive layer and the adjacent pre-cured dielectric layer remained flat. This resulted in a multilayer composite material in which the CNT mass concentration increased layer by layer along the thickness direction of the material from the incident surface to the exit surface, while the content of titanium dioxide nanoparticles in the dielectric layer remained unchanged. S4. Overall pre-curing: Same as in Example 1; S5 hot-press curing: Same as Example 1; S6. Cooling and post-processing: Same as in Example 1, to prepare electromagnetic shielding composite material.
[0048] Performance testing The electromagnetic shielding composite materials based on the nacreous layer biomimetic structure prepared in Examples 1-3 and the electromagnetic shielding composite materials prepared in Comparative Examples 1-2 were subjected to broadband electromagnetic shielding performance, absorption efficiency, density and interlayer shear strength tests to evaluate their electromagnetic shielding effect, lightweight characteristics and interlayer bonding performance.
[0049] 1. Broadband electromagnetic shielding effectiveness and absorption efficiency test The electromagnetic shielding composite materials based on the nacreous layer biomimetic structure prepared in Examples 1-3 and the electromagnetic shielding composite materials prepared in Comparative Examples 1-2 were cut into standard specimens that matched the test fixtures. The surface of the specimens was polished to ensure that the upper and lower surfaces were flat and the thickness was uniform, so as to avoid the influence of edge burrs on the electromagnetic parameter test. Before the test, the thickness of the specimens was measured using a vernier caliper or a micrometer, and the average value at different positions was recorded.
[0050] Broadband electromagnetic shielding effectiveness was tested using a vector network analyzer in the 1–18 GHz frequency band. During testing, the sample was placed in a coaxial fixture, and the scattering parameters, including the reflection parameter S, were measured at different frequencies. 11 and transmission parameter S 21 Before testing, the vector network analyzer was calibrated to eliminate the influence of cables, connectors, and fixtures on the test results. Subsequently, continuous scanning was performed in the 1–18 GHz range to obtain data on the reflection, transmission, and shielding performance of the samples over a wide frequency range. Specifically, when testing the electromagnetic shielding composite materials based on the nacreous layer biomimetic structure prepared in Examples 1-3 and the electromagnetic shielding composite material prepared in Comparative Example 2, the electromagnetic wave incident surface was the first conductive layer of each electromagnetic shielding composite material. When testing the electromagnetic shielding composite material prepared in Comparative Example 1, the electromagnetic wave incident surface was not limited.
[0051] EMI SE (Electromagnetic Interference Shielding Effectiveness) is calculated based on the transmission coefficient: ; Among them, SE T Total electromagnetic shielding effectiveness, measured in dB; S 21 These are the transmission parameters measured by a vector network analyzer.
[0052] Based on the S obtained from the test 11 and S 21 The reflection coefficient can be further calculated. R Transmission coefficient T and absorption coefficient A : ; ; ; in, R This indicates the proportion of incident electromagnetic waves reflected by the material surface. T Indicates the proportion of materials, A This represents the proportion of material absorbed and lost after entering the material's interior. To evaluate the absorption-dominant shielding characteristics of the material, the effective absorption ratio is further calculated: ; in, A eff This indicates the proportion of electromagnetic waves that are absorbed and consumed when they enter the material.
[0053] The test results are shown in Table 1.
[0054] 2. Density test Density testing was used to evaluate the lightweight characteristics of the composite materials. The electromagnetic shielding composite materials based on the nacreous layer biomimetic structure prepared in Examples 1-3 and the electromagnetic shielding composite materials prepared in Comparative Examples 1-2 were cut into regular block-shaped samples. Edge burrs were removed, and the surfaces were smoothed. The mass of the samples was weighed using an electronic balance with an accuracy of not less than 0.001 g. The length, width, and thickness of the samples were measured using vernier calipers or a micrometer, with at least three measurements taken in each direction and the average value calculated. The sample volume was then calculated. The measurement results are shown in Table 1, and the sample density was calculated using the following formula: ; Where ρ is the sample density, in g / cm³. 3 m is the sample mass in grams; V is the sample volume in centimeters. 3 .
[0055] 3. Interlaminar shear strength test Interlaminar shear strength was used to evaluate the interfacial bonding performance between adjacent conductive and dielectric layers in the electromagnetic shielding composite materials based on the nacreous layer biomimetic structure prepared in Examples 1-3 and the electromagnetic shielding composite materials prepared in Comparative Examples 1-2. Before testing, the above composite materials were cut into short beam specimens, ensuring that the specimen edges were flat and free of obvious gaps or delamination defects.
[0056] Interlaminar shear properties were assessed using a universal testing machine with a three-point bending short beam shear test. During the test, the specimen was placed on a three-point bending fixture, and the span was adjusted to ensure the span-to-thickness ratio met the interlaminar shear test requirements. The loading head was positioned at the center of the specimen, and a constant loading rate was applied downwards. The load values at which interlaminar shear failure occurred or the maximum load was recorded. At least five parallel specimens were tested for each group of samples, and the average value was taken as the final result. The test results are shown in Table 1. The interlaminar shear strength was calculated using the following formula: ; Where τ is the interlaminar shear strength in MPa; p is the maximum load at which the specimen fails in N; b is the specimen width in mm; and h is the specimen thickness in mm.
[0057] Table 1. Test results of Examples 1-3 and Comparative Examples 1-2
[0058] Table 1 shows that in Comparative Example 1, the mass concentration of conductive nanomaterials added to each conductive layer is the same, and the mass concentration of dielectric nanomaterials added to each dielectric layer is the same. The uniform distribution of fillers reduces the impedance gradient in the thickness direction, resulting in an average electromagnetic shielding effectiveness of 42 dB and an absorption ratio of only 65%. The broadband absorption efficiency is slightly lower, but the interlayer toughness is still maintained. In Comparative Example 2, during the preparation of the electromagnetic shielding composite material, the removal of the micro-concave-convex nested interlocking structure reduces the number of multiple scattering paths, leading to a decrease in absorption efficiency. The average electromagnetic shielding effectiveness is 40 dB, and the absorption ratio is 60%. At the same time, the interlayer bonding force is weakened, and the interlayer shear strength is only 3 MPa.
[0059] The electromagnetic shielding composite materials based on the nacreous layer biomimetic structure prepared in Examples 1 and 2 have average electromagnetic shielding efficiencies of 45 dB and 50 dB in the 1–18 GHz frequency band, respectively, absorption ratios of 70% and 75%, and densities of 1.18 g / cm³. 3 and 1.32 g / cm 3 The interlaminar shear strengths were 5 MPa and 6 MPa, respectively, demonstrating that compared to Comparative Examples 1 and 2, setting a thickness-direction impedance gradient and a micro-concave-convex nested interlocking structure can synergistically improve broadband absorption efficiency and reduce interface reflection. The micro-concave-convex nested interlocking structure enhances interlaminar bonding while maintaining the lightweight nature and good interlaminar toughness of the composite material. The electromagnetic shielding composite material based on the nacreous layer biomimetic structure prepared in Example 1 has a significantly lower density than commonly used aluminum-based, steel-based, or copper-based metal shielding materials, indicating that this composite material has a good lightweight advantage while maintaining high electromagnetic shielding effectiveness. It is suitable for shielding internal structural components of high-speed trains and EMUs, lightweight electronic cabin partitions, sensor protective covers, and protection of onboard communication and radar modules with high broadband absorption requirements.
[0060] The electromagnetic shielding composite material based on the nacreous layer biomimetic structure prepared in Example 3 has an average electromagnetic shielding effectiveness of 52 dB in the 1–18 GHz frequency band, an absorption ratio of 80%, and a density of 1.22 g / cm³. 3 The interlaminar shear strength is 6 MPa, demonstrating that the synergistic effect of multiple fillers, impedance gradient, and micro-concave-convex nested interlocking structure in the conductive layer further improves the broadband absorption efficiency. The composite material is lightweight and has good structural integration. This electromagnetic shielding composite material can be used for electronic shielding inside high-speed trains, EMUs, and high-frequency communication cabins, as well as for the protection of radar / communication modules with high broadband absorption requirements.
[0061] Furthermore, this invention also changed the electromagnetic wave incident surface to the fifth conductive layer of the composite material, and re-measured the broadband electromagnetic shielding effectiveness and absorption efficiency of the electromagnetic shielding composite material based on the nacreous layer biomimetic structure prepared in Example 1. The average electromagnetic shielding effectiveness was 43 dB, and the effective absorption rate was 68%, which proved that the reverse impedance gradient caused the impedance matching on the incident side to decrease, the reflection to increase, and the absorption efficiency to decrease.
[0062] 4. High-temperature resistance test The present invention conducts high-temperature performance tests on the electromagnetic shielding composite material based on the nacreous layer biomimetic structure prepared in Example 2. The test method is as follows: the sample is placed in a 200℃ oven and kept at a temperature of 2 h, and then cooled to room temperature. The average electromagnetic shielding effectiveness and interlayer shear strength before and after the heat preservation are tested to evaluate the material's shielding performance retention and interlayer interface bonding stability under high temperature environment. The test results are as follows: Before heat preservation at 200℃: the average electromagnetic shielding effectiveness is 50dB, and the interlaminar shear strength is 6MPa; after heat preservation at 200℃: the average electromagnetic shielding effectiveness is 48dB, and the interlaminar shear strength is 5.5MPa; the average electromagnetic shielding effectiveness retention rate after heat preservation at 200℃ is 96%, and the interlaminar shear strength retention rate is 92%. This proves that in the preparation of electromagnetic shielding composite material in Example 2, due to the good heat resistance of the polyimide matrix and the enhanced interlaminar interlocking structure of the micro-concave-convex nested interlocking structure, the material still maintains good shielding performance and interface bonding performance after high-temperature treatment. This electromagnetic shielding composite material can be applied to electronic shielding components, cabin communication modules, radar radomes, sensor protection, and shielding materials for lightweight and complex curved surface structure components in high-temperature environments inside high-speed trains or aircraft cabins.
[0063] The above are merely preferred embodiments of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. An electromagnetic shielding composite material based on a nacreous biomimetic structure, characterized in that, It consists of staggered conductive and dielectric layers, with adjacent conductive and dielectric layers forming a micro-concave-convex nested interlocking structure; the matrix material in the conductive layer is filled with conductive nanomaterials, and the matrix material in the dielectric layer is filled with dielectric nanomaterials; along the thickness direction of the electromagnetic shielding composite material, the mass concentration of conductive nanomaterials in the spaced conductive layers increases layer by layer, and the mass concentration of dielectric nanoparticles in the spaced dielectric layers is the same.
2. The electromagnetic shielding composite material based on a nacreous biomimetic structure according to claim 1, characterized in that, In the micro-convex-concave nested interlocking structure, the height of the protrusion is 15-20 μm, the depth of the groove is 15-20 μm, the distance between the highest points of two adjacent protrusions is 80-100 μm, and the distance between the lowest points of two adjacent grooves is 80-100 μm; the height of the protrusion or the depth of the groove is not greater than 1 / 2 of the thickness of the corresponding conductive layer or dielectric layer.
3. The electromagnetic shielding composite material based on a nacreous biomimetic structure according to claim 1, characterized in that, The conductive nanomaterial includes one or both of graphene and carbon nanotubes; the dielectric nanomaterial is selected from titanium dioxide nanoparticles or alumina nanoparticles.
4. The electromagnetic shielding composite material based on a nacreous biomimetic structure according to claim 1, characterized in that, The matrix material in the conductive layer and the matrix material in the dielectric layer are both selected from epoxy resin or polyimide.
5. The electromagnetic shielding composite material based on a nacreous biomimetic structure according to claim 1, characterized in that, The thickness of the conductive layer is 80–100 μm; the thickness of the dielectric layer is 80–100 μm.
6. A method for preparing an electromagnetic shielding composite material based on a nacreous biomimetic structure as described in any one of claims 1 to 5, characterized in that, Includes the following steps: S1. The conductive nanomaterials are added to the matrix material according to the gradient mass concentration, ultrasonically dispersed, additives are added, and stirred evenly. The first conductive layer mixture, the second conductive layer mixture, the third conductive layer mixture, the fourth conductive layer mixture and the fifth conductive layer mixture are obtained according to the mass concentration from low to high. S2. Add the dielectric nanomaterial to the matrix material, disperse it ultrasonically, add the additives, stir evenly, and obtain a dielectric layer mixture; S3. The first conductive layer mixture prepared in step S1 is used to form a pre-cured first conductive layer through a micro-textured mold or a scraping method, so that its surface forms a micro-uneven morphology; the dielectric layer mixture prepared in step S2 is coated on the first conductive layer to obtain a first dielectric layer; the pre-cured second conductive layer, pre-cured second dielectric layer, pre-cured third conductive layer, pre-cured third dielectric layer, pre-cured fourth conductive layer, pre-cured fourth dielectric layer and pre-cured fifth conductive layer are obtained by coating the pre-cured second conductive layer, pre-cured third conductive layer, pre-cured fourth conductive layer and pre-cured fifth conductive layer in sequence by coating the second conductive layer mixture, the third conductive layer mixture, the fourth conductive layer mixture and the fifth conductive layer mixture prepared in step S1; each pre-cured conductive layer and the adjacent pre-cured dielectric layer form a micro-uneven nested interlocking structure to obtain an interlocked multilayer composite material; S4. The interlocking multilayer composite material prepared in step S3 is pre-cured as a whole to obtain a pre-cured interlocking multilayer composite material; S5. The pre-cured interlocking multilayer composite material prepared in step S4 is hot-pressed and cured to obtain a cured interlocking multilayer composite material. After cooling to room temperature, it is demolded to obtain the electromagnetic shielding composite material based on the nacreous biomimetic structure.
7. The preparation method according to claim 6, characterized in that, In step S3, the height of the protrusions in the microtextured mold is 15-20 μm, the depth of the grooves is 15-20 μm, the distance between the highest points of two adjacent protrusions is 80-100 μm, and the distance between the lowest points of two adjacent grooves is 80-100 μm.
8. The preparation method according to claim 6, characterized in that, In step S3, the coating method involves using a micro-textured scraper, a toothed scraper, or a microstructure printing roller to coat the surface of the pre-cured first conductive layer, which has not yet fully cured, to form a micro-uneven morphology.
9. The preparation method according to claim 6, characterized in that, In step S4, the overall pre-curing temperature is 80℃ and the time is 2h; in step S5, the hot-press curing temperature is 120~250℃, the pressure is 5 MPa, and the time is 3h.
10. The application of the electromagnetic shielding composite material based on the nacreous layer biomimetic structure as described in any one of claims 1 to 5 in electromagnetic shielding of rail transit equipment, communication base stations and high-performance electronic equipment.
Citation Information
Patent Citations
Nacre-like structure polymer based electromagnetic shielding material and preparation method thereof
CN104786615A