A method to improve the efficiency and yield of TOPCon rework wafers

By combining mixed acid cleaning and high-temperature oxidation, the problem of removing impurities from TOPCon rework wafers was solved, achieving integrated repair of the silicon wafer surface and interior, improving the cell efficiency and yield of rework wafers, and reducing costs.

CN123124488APending Publication Date: 2026-11-17TIANJIN ZHONGHUAN PHOTOVOLTAIC TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611307076.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-26
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing TOPCon rework wafer processing technology cannot effectively remove deep-seated metal impurities within the silicon wafer, resulting in severe lattice damage, high silicon dangling bond density, excessive surface recombination, degraded passivation performance, and low efficiency yield of reworked cells.

Method used

A mixed acid cleaning system combined with high-temperature oxidation treatment is adopted. A SiO2 oxide layer is generated by high-temperature oxidation in a pure oxygen atmosphere, which adsorbs and removes heavy metal impurities in the wafer. The surface morphology uniformity is improved by a multi-step texturing process, thus achieving integrated repair of the silicon wafer inside and out.

Benefits of technology

It significantly improves the minority carrier lifetime and cell efficiency of reworked cells, reduces the density of deep-level recombination centers, increases the conversion efficiency and yield of reworked cells, and reduces chemical consumption and modification costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124488A_ABST
    Figure CN123124488A_ABST
Patent Text Reader

Abstract

This invention discloses a method for improving the efficiency and yield of TOPCon rework wafers, comprising the following steps: S1: Cleaning the TOPCon rework wafers in a mixed acid cleaning system to obtain bare silicon rework wafers; S2: Placing the bare silicon rework wafers obtained in step S1 in a boron diffusion tube furnace and performing high-temperature oxidation treatment in a pure oxygen atmosphere to generate a SiO2 oxide layer on the surface of the rework wafers; S3: Removing the SiO2 oxide layer on the surface of the rework wafers obtained in step S2 by acid washing, followed by texturing. This invention achieves integrated repair of rework wafers from the surface to the interior, effectively solving the technical defect of existing processes that cannot remove deep heavy metal impurities within the silicon wafer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of crystalline silicon solar cell manufacturing technology, and in particular relates to a method for improving the efficiency and yield of TOPCon rework wafers. Background Technology

[0002] N-type TOPCon passivated contact solar cells have become the mainstream technology for photovoltaic mass production due to their advantages such as high conversion efficiency, low degradation, and suitability for thin-film production. However, during large-scale mass production, processes such as diffusion, alkaline polishing, edge etching, ALD alumina passivation, and PECVD silicon nitride deposition easily generate a large number of reworked semi-finished wafers. The main defects include residual multilayer dielectric films on the surface, surface dirt, localized contamination, slight leakage, and color differences. These require rework and repair before being put back into production; direct scrapping would result in significant silicon waste and production cost losses.

[0003] Existing publicly available TOPCon rework wafer repair patents and mass production processes generally employ a step-by-step acid-alkali alternating cleaning, layered film peeling, and conventional surface impurity removal technical solution. The core focus is only on removing the film layer and cleaning the surface stains of the silicon wafer: Patent CN121240579A removes single B / PSG, Poly-Si, or oxide layers through a combination of acid washing with different concentrations of HF and alkaline washing; Patent CN119650415A optimizes the acid washing formula to reduce silicon wafer thickness loss; industry patents only target the targeted peeling of single film defects and the scope of protection is limited to surface physical / chemical cleaning repair, without involving the repair of defects inside the silicon wafer.

[0004] The existing TOPCon rework process technology has the following drawbacks: 1. Silicon wafer impurity removal capability issue: In the conventional rework wafer processing flow, only the SiO2, SiNx, and AlOx multilayer dielectric films remaining on the surface of the TOPCon cell rework wafer are removed. Deep metal impurities inside the silicon substrate cannot be removed. Only the surface film layer is cleaned before texturing and subsequent production.

[0005] 2. Rework acid pickling introduces numerous lattice defects and Si dangling bonds: The rework process uses corrosive mixed acids such as HF and HF+HCl to strip polycrystalline silicon, oxide layers, AlOx, and SiNx. The surface crystalline silicon of the silicon wafer is unevenly corroded, generating numerous dislocations, micro-damage, and broken Si-Si bonds, forming high-density silicon dangling bonds. These defects are extremely strong surface carrier recombination centers, directly leading to a significant decrease in minority carrier lifetime in reworked wafers. The recombination rate at the interface of the TOPCon back tunneling oxide layer / polycrystalline silicon passivation structure soars, ultimately resulting in reworked cells having open-circuit voltage (Voc) and conversion efficiency far lower than the original wafers, leading to mass degradation or even scrapping.

[0006] 3. Heavy metal contamination introduced during rework, with internal impurities unable to be effectively removed: Long-term use of the pickling solution precipitates transition metal ions such as Fe, Cu, Ni, and Zn. During the etching and peeling process, these metal ions embed into the silicon surface and may even diffuse into the silicon wafer. Simultaneously, contact between the silicon wafer and the quartz boat and conveyor rollers also introduces metal contamination. Although TOPCon employs a subsequent high-temperature boron diffusion process to remove impurities, the ability to remove deeply diffused metal impurities within the reworked wafer using only boron diffusion and subsequent gettering is limited. Residual impurities can easily lead to poor electroluminescence (EL) performance, increased leakage current, and accelerated light decay in the battery.

[0007] 4. Uneven defect distribution leads to poor consistency of the textured surface in secondary texturing: The silicon atom reactivity varies greatly in the acid pickling damage area. During direct texturing, the anisotropic corrosion rate of the alkaline solution is inconsistent, resulting in problems such as large differences in pyramid size, local over-corrosion pits, color difference across the entire sheet, and high reflectivity. The appearance yield of reworked sheets is low.

[0008] 5. Production line efficiency / yield issues: Due to the large number of high-density silicon dangling bonds generated on the surface of silicon wafers in the traditional process and the introduction of a large number of metal impurities in the rework wafer manufacturing process, the overall efficiency and yield of rework wafers are seriously deviated. The overall efficiency is 0.08%-0.12% lower than the production line, and the overall yield is 5%-10% lower than the production line. The rework wafer yield / efficiency issues urgently need to be improved. Summary of the Invention

[0009] In view of this, the present invention aims to propose a method for improving the efficiency and yield of TOPCon rework wafers, in order to solve at least one of the following technical problems: I. Solve the problems of severe lattice damage, excessive silicon dangling bond density, excessive surface recombination, and deteriorated passivation performance in TOPCon rework wafers after acid washing; 2. Remove heavy metal impurities such as Fe, Cu, and Ni introduced by the chemical solution and mechanical contact during the rework process, both internally and on the surface, reduce the number of deep-level recombination centers, and improve the minority carrier lifetime of the reworked wafer; 3. Utilize the uniform buffering effect of the oxide layer to improve the uniformity of the pyramid textured surface of the reworked sheet during secondary texturing, thereby increasing the yield and efficiency of the reworked battery. Fourth, the boron diffusion tube furnace equipment already in use on the production line can be fully reused without the need for new heat treatment equipment, thus controlling the cost of modification and production capacity consumption.

[0010] To achieve the above objectives, the technical solution of the present invention is implemented as follows: A method for improving the efficiency and yield of TOPCon rework wafers includes the following steps: S1: Place the TOPCon rework wafer in a mixed acid cleaning system for cleaning to obtain the bare silicon rework wafer; S2: Place the bare silicon rework wafer obtained in step S1 in a boron diffusion tube furnace and perform high-temperature oxidation treatment in a pure oxygen atmosphere to generate a SiO2 oxide layer on the surface of the rework wafer. S3: Pickling removes the SiO2 oxide layer on the surface of the reworked sheet obtained in step S2, followed by texturing.

[0011] Furthermore, the cleaning step in step S1 includes the following processes performed in sequence: M1 mixed acid washing process, M2 water washing process, M3 alkaline washing process, M4 water washing process, M5 mixed acid washing process, M6 water washing process, M7 slow lifting process and M8 drying process.

[0012] Furthermore, in the M1 mixed acid washing process, the mixed acid cleaning system is prepared by the following components in volume proportions: 2-4 parts hydrogen peroxide, 17-23 parts hydrofluoric acid, 14-18 parts hydrochloric acid, 50-60 parts pure water, and 4-8 parts catalytic additive. Preferably, the hydrogen peroxide concentration is 32-36 wt%; Preferably, the mass concentration of hydrofluoric acid is 49-50 wt%; Preferably, the hydrochloric acid has a mass concentration of 36-38 wt%. Preferably, the resistivity of pure water is >18 MΩ·cm; The processing time for the M1 mixed pickling process is 1000-1800 seconds, and the temperature is room temperature. And / or, in the M3 alkaline washing process, the alkaline washing solution is prepared according to the following volume ratio: 1-2 parts hydrogen peroxide, 0.5-1.5 parts sodium hydroxide, and 96-98 parts pure water; Preferably, the hydrogen peroxide concentration is 32-36 wt%; Preferably, the mass concentration of sodium hydroxide is 44-46 wt%; Preferably, the resistivity of pure water is >18 MΩ·cm; The processing time for the M3 alkaline washing process is 150-250 seconds, and the temperature is 55-65℃. And / or, in the M5 mixed pickling process, the pickling solution is prepared according to the following volume ratio: 1.5-3 parts hydrofluoric acid, 4.5-6 parts hydrochloric acid and 60-70 parts pure water; Preferably, the mass concentration of hydrofluoric acid is 49-50 wt%; Preferably, the hydrochloric acid has a mass concentration of 36-38 wt%. Preferably, the resistivity of pure water is >18 MΩ·cm; The process conditions for the M5 mixed pickling process are: processing time 150-250s, temperature room temperature.

[0013] Furthermore, the time for the M2 washing process, the M4 washing process, and the M6 ​​washing process is 150-250 seconds, the temperature is room temperature, and the flow rate is 400-1000 L / H; Preferably, the speed of the M7 slow lifting process is 2.0-4.0 mm / s: Preferably, the drying process of M8 takes 700-900 seconds and the temperature is 75-95°C.

[0014] Furthermore, the high-temperature oxidation gettering treatment in step S2 includes the following steps: A1: Raise the temperature inside the furnace tube to the preset preheating temperature and purge with protective gas; A2: Introduce oxygen-containing gas for high-temperature oxidation treatment to generate a SiO2 oxide layer on the surface of the reworked sheet; A3: Stop the flow of oxygen-containing gas and remove the product after cooling under a protective atmosphere.

[0015] Further, the heating rate in step A1 is 5~10℃ / min, the preset preheating temperature is 750~820℃, and the temperature is held constant for 180~600s after reaching the preset preheating temperature; the protective gas is nitrogen, and the nitrogen flow rate is 8000~18000sccm. Preferably, the oxygen-containing gas in step A2 is oxygen or dry air, the oxidation temperature is 800~900℃, the isothermal oxidation time is 1200~4800s, and the total film thickness of the generated SiO2 oxide layer is controlled to be 2nm~8nm. Preferably, in step A3, the cooling rate is 3~15℃ / min.

[0016] Further, step S3 includes performing the following steps in sequence: M1 pickling process, M2 water washing process, M3 pre-cleaning process, M4 water washing process, M5 one-step flocking process, M6 water washing process, M7 two-step flocking process, M8 water washing process, M9 alkaline washing process, M10 water washing process, M11 pickling process, M12 water washing process, M13 slow lifting process, and M14 drying process.

[0017] Furthermore, the pickling solution used in the M1 pickling process is prepared according to the following volume ratio: 12-18 parts hydrofluoric acid and 82-88 parts pure water. The mass concentration of hydrofluoric acid is 49-50 wt%; The resistivity of pure water is >18 MΩ·cm; The processing time for the M1 pickling process is 150-250 seconds at room temperature. Preferably, in the M3 pre-cleaning process, the cleaning solution is prepared according to the following volume ratio: 2-6 parts hydrogen peroxide; 0.5-2 parts 44-46 wt% sodium hydroxide; 92-97 parts pure water; The mass concentration of hydrogen peroxide is 32-36 wt%. The mass concentration of sodium hydroxide is 44-46 wt%; The resistivity of pure water is >18 MΩ·cm; The processing time for the M3 pre-cleaning process is 150-250 seconds, and the temperature is 60-75℃. Preferably, in the M5 one-step texturing process, the texturing solution is prepared according to the following volume ratio: 0.5-1.5 parts sodium hydroxide, 0.2-0.6 parts texturing additive, and 98-99.5 parts pure water with a resistivity >18MΩ·cm; The mass concentration of sodium hydroxide is 44-46 wt%; The resistivity of pure water is >18 MΩ·cm; The processing time for the M5 one-step flocking process is 200-350 seconds, and the temperature is 78-85℃.

[0018] Furthermore, in the M7 two-step texturing process, the texturing solution is prepared according to the following volume ratio: 0.1-0.4 parts sodium hydroxide; 0.1-0.3 parts texturing additive; and 99.5-99.9 parts pure water with a resistivity >18MΩ·cm. The mass concentration of sodium hydroxide is 44-46 wt%; The resistivity of pure water is >18 MΩ·cm; The processing time for the M7 two-step flocking process is 60-180 seconds, and the temperature is 55-68℃. Preferably, in the M9 alkaline washing process, the alkaline washing solution is prepared according to the following volume ratio: 2-5 parts hydrogen peroxide, 0.5-1.5 parts sodium hydroxide (NaOH), and 93-98 parts pure water; The mass concentration of hydrogen peroxide is 32-36 wt%. The mass concentration of sodium hydroxide is 44-46 wt%; The resistivity of pure water is >18 MΩ·cm; The processing time for the M9 alkaline washing process is 60-150 seconds, and the temperature is 60-70℃.

[0019] Furthermore, in the M11 pickling process, the pickling solution is prepared according to the following volume ratio: 8-15 parts hydrofluoric acid, 1-4 parts 36-38wt% hydrochloric acid, and 82-90 parts pure water. The mass concentration of hydrofluoric acid is 49-50 wt%; The mass concentration of hydrochloric acid is 36-38 wt%. The resistivity of pure water is >18 MΩ·cm; The M11 pickling process takes 80-180 seconds at room temperature. Preferably, the processing time for the M2, M4, M6, M8, M10, and M12 water washing processes is 150-250 seconds, the temperature is room temperature, and the pure water replenishment flow rate is 400-1000 L / H. Preferably, the processing time of the M13 slow lifting process is 5-30 seconds, and the temperature is 60-85℃; Preferably, the processing time of the M14 drying process is 400-900s, and the temperature is 80-100℃.

[0020] Compared with existing technologies, the method for improving the efficiency and yield of TOPCon rework wafers described in this invention has the following advantages: 1. This application achieves integrated repair of silicon wafers from the surface to the interior, overcoming the fundamental defect of existing technologies that can only clean the surface. This application abandons the single surface cleaning mode of alternating acid / alkali washing and direct texturing in the existing TOPCon rework process. By constructing a new rework system with multi-dielectric film, integrated removal and high-temperature internal gettering purification, and secondary precise impurity removal, while removing multi-layer dielectric films and contaminants on the surface, high-temperature dry oxygen oxidation treatment is used to make heavy metal impurities such as Fe, Cu, and Ni in the rework wafer migrate and accumulate to the surface SiO2 oxide layer and be removed with the oxide layer peeling off. This achieves integrated repair of the rework wafer from the surface to the interior, effectively solving the technical defect that existing processes cannot remove deep heavy metal impurities in the silicon wafer.

[0021] 2. This application significantly repairs lattice damage and saturated silicon dangling bonds, improving minority carrier lifetime. During the rework pickling process, the surface crystalline silicon of the silicon wafer generates numerous dislocations, micro-damage, and broken Si-Si bonds due to uneven corrosion by corrosive mixed acids such as HF and HCl, forming high-density silicon dangling bonds—these defects are extremely strong surface carrier recombination centers. In the high-temperature oxidation gettering step of this invention, through dry oxygen oxidation treatment at 820~880℃, oxygen atoms combine with broken Si-Si bonds to form stable Si-O-Si bonds, resulting in large-area saturated silicon dangling bonds. Simultaneously, the high-temperature annealing effect effectively repairs the lattice distortion and dislocations introduced by pickling, making the surface crystalline structure of the silicon wafer more complete, significantly reducing the surface recombination rate, and greatly improving the minority carrier lifetime of the reworked wafer, providing a physical basis for the recovery of the open-circuit voltage (Voc) of the reworked battery.

[0022] 3. This application efficiently removes heavy metal impurities from the silicon wafer and reduces the density of deep-level recombination centers. During the high-temperature oxidation process, this invention utilizes the physical property that the segregation coefficient of transition metal impurities (Fe, Cu, Ni, Zn, etc.) at the SiO2 / Si interface is much greater than 1. This causes a large number of metal impurities diffused to the silicon wafer surface to migrate and accumulate in the dense SiO2 oxide layer. Subsequently, the oxide layer is completely stripped away in one step using hydrofluoric acid solution, achieving physical removal of the metal impurities. This external gettering mechanism complements the internal gettering effect associated with the high-temperature boron diffusion process in existing TOPCon processes. It effectively solves the common industry problem of metal ions precipitated in the rework pickling bath being embedded in the silicon surface or even diffused into the silicon wafer, making them difficult to remove. This reduces the density of deep-level recombination centers in the PN junction region of the battery and decreases leakage current channels.

[0023] 4. This invention improves the conversion efficiency and mass production yield of reworked cells. Through the synergistic effect of lattice repair and impurity removal, and by using an ultra-thin, uniform SiO2 oxide layer as a corrosion buffer layer, the surface corrosion rate differences caused by acid washing are smoothed out. This results in uniform pyramid morphology after secondary texturing, with no localized over-corrosion pits and no color difference between the two sides. Actual test data shows that after adopting the method of this invention, the conversion efficiency Eta of reworked cells is increased to 26.801%, the rework yield is increased to 95.62%, the rework efficiency decay is significantly reduced from 0.081% to 0.034%, and the low rework yield is significantly reduced from 8.13% to 2.74%, effectively solving the technical pain point of severely low efficiency and yield of reworked cells on the production line.

[0024] 5. This invention significantly reduces chemical consumption and saves material costs. Based on the synergistic effect of composite catalytic additives, this invention achieves high-efficiency etching with low-concentration reagents in the M1 mixed acid washing process. Compared with the traditional HF single-solution segmented cleaning process, the HF consumption is reduced from 3-5L / 10,000 pieces to 1-2L / 10,000 pieces, and the overall reagent consumption is reduced by 30% to 60%, which significantly reduces the material costs of the wet process and has good economic benefits.

[0025] 6. This application fully reuses existing production line equipment without requiring additional investment. The high-temperature oxidation and gettering step of this invention fully reuses the boron diffusion tube furnace equipment already in use on the TOPCon mass production line. The oxidation and gettering process can be completed during the intervals of the boron diffusion process or during idle periods of the equipment, without the need for any additional heat treatment equipment. This effectively controls the cost of process modification and mass production capacity consumption, and has good feasibility for industrialization and promotion.

[0026] 7. The present invention features a streamlined process flow, a wide operating window, and is suitable for large-scale mass production. It integrates the multi-step, segmented acid-base alternating cleaning process in conventional rework processes into an integrated mixed acid cleaning process, shortening the total rework cleaning time. At the same time, the process parameters of each process are set with a wide adjustable range, which has low dependence on equipment accuracy and operating accuracy. It is easy to quickly introduce and stably operate in existing mass production lines and has excellent mass production adaptability. Attached Figure Description

[0027] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an undue limitation of the invention. In the drawings: Figure 1 This is a schematic diagram of a rework process to improve the efficiency and yield of TOPCon reworked wafers, as proposed in this invention. Figure 2 This is a schematic diagram of a process proposed in this invention to improve the efficiency and yield of TOPCon rework wafers. Detailed Implementation

[0028] It should be noted that, unless otherwise specified, the embodiments and features described in the present invention can be combined with each other.

[0029] The present invention will now be described in detail with reference to the accompanying drawings and embodiments.

[0030] Unless otherwise specified, all chemical reagents used in this invention are conventional electronic-grade (EL-grade) or UP-grade (ultra-pure-grade) reagents in the art. The TOPCon cell rework wafers used are semi-finished silicon wafers that do not meet the appearance or electrical performance specifications produced during the diffusion, alkaline polishing, edge etching, ALD alumina passivation, and PECVD silicon nitride deposition processes of N-type monocrystalline silicon TOPCon cells.

[0031] Example 1 This embodiment provides a method for improving the efficiency and yield of TOPCon rework wafers, specifically including the following steps: S1: Mixed acid cleaning to obtain bare silicon rework wafers Reworked wafers that do not meet appearance or electrical performance specifications from various processes in the TOPCon battery production line (diffusion, alkaline polishing, edge etching, ALD alumina passivation, PECVD silicon nitride deposition, etc.) are collected, placed in cleaning baskets, and sent to an automatic rework cleaning machine for cleaning. The cleaning process includes the following steps in sequence: M1 mixed acid washing, M2 water washing, M3 alkaline washing, M4 water washing, M5 mixed acid washing, M6 water washing, M7 slow lifting, and M8 drying. The process parameters for each step are as follows: M1 Mixed Acid Washing Process: Prepare the mixed acid cleaning system according to the following volume ratios: 3 parts 32wt% hydrogen peroxide, 20 parts 49wt% hydrofluoric acid, 16 parts 36wt% hydrochloric acid, 55 parts pure water with resistivity >18MΩ·cm, and 6 parts catalytic additive. The catalytic additive is Topband BR110V02.

[0032] The processing time was 1400 seconds, and the temperature was room temperature (25±3℃).

[0033] M2 water washing process: Use pure water with resistivity >18MΩ·cm for overflow cleaning, processing time 200s, temperature room temperature, replenishment flow rate 600L / h.

[0034] M3 Alkaline Washing Process: Prepare the alkaline washing solution according to the following volume ratios: 1.5 parts of 32wt% hydrogen peroxide, 1 part of 45wt% sodium hydroxide, and 97.5 parts of pure water with a resistivity >18MΩ·cm. Processing time: 200s, temperature: 60℃.

[0035] M4 washing process: Same as M2 washing process.

[0036] M5 mixed pickling process: Prepare the pickling solution according to the following volume ratios: 2 parts 49wt% hydrofluoric acid, 5 parts 36wt% hydrochloric acid, and 93 parts pure water with resistivity >18MΩ·cm. Processing time: 200s, temperature: room temperature.

[0037] M6 washing process: Same as M2 washing process.

[0038] M7 slow lifting process: The slow lifting speed is set to 3mm / s, the processing time is 20s, and the temperature is 55℃.

[0039] M8 drying process: processing time 800s, temperature 90℃.

[0040] After the above cleaning, the multilayer dielectric film (SiNx, AlOx, SiO2, etc.) and surface dirt on the surface of the rework wafer are completely removed, and a bare silicon rework wafer is obtained.

[0041] S2: High-temperature oxidation and gettering treatment The bare silicon rework wafer obtained in step S1 is placed in a boron diffusion tube furnace (model: CTCO, tube diameter φ300mm) for high-temperature oxidation gettering treatment, specifically including: A1 preheating stage: The temperature is increased from room temperature to 780℃ at a rate of 8℃ / min, while high-purity nitrogen (99.999% purity) is introduced as a protective gas at a flow rate of 12000 sccm. The temperature is maintained for 300s to stabilize the temperature field inside the furnace and eliminate temperature differences in the silicon wafers.

[0042] A2 Dry Oxygen Oxidation Stage: The temperature is raised to the oxidation temperature of 850℃, nitrogen gas is stopped, and high-purity oxygen (99.999% purity) is introduced at a flow rate of 10000 sccm. The furnace pressure is maintained at 700 mbar, and the isothermal oxidation treatment time is 2400 s. Through this high-temperature dry oxygen oxidation, a dense SiO2 oxide layer with a thickness of 3.5 nm (measured by ellipsometry) is formed on the surface of the rework wafer. During this process, oxygen atoms combine with silicon dangling bonds generated by acid pickling damage to form stable Si-O-Si bonds, saturated dangling bonds; at the same time, heavy metal impurities such as Fe, Cu, and Ni adsorbed in the silicon wafer and on its surface migrate in large quantities and accumulate in this oxide layer due to their high segregation coefficient at the Si / SiO2 interface.

[0043] A3 Cooling and Unloading Stage: Stop the oxygen supply, switch to high-purity nitrogen (flow rate 15000 sccm) to purge the furnace tube for 10 minutes, and cool down to below 750℃ at a rate of 8℃ / min. After breaking the vacuum, remove the quartz boat to complete the oxidation and impurity removal process.

[0044] S3: Oxide layer pickling removal and secondary texturing The reworked sheet with a SiO2 oxide layer obtained in step S2 is fed into a texturing and cleaning machine, where it undergoes the following processes sequentially: M1 acid washing, M2 water washing, M3 pre-cleaning, M4 water washing, M5 one-step texturing, M6 water washing, M7 two-step texturing, M8 water washing, M9 alkaline washing, M10 water washing, M11 acid washing, M12 water washing, M13 slow lifting, and M14 drying. The process parameters for each process are as follows: M1 pickling process: Prepare the pickling solution by volume ratio: 15 parts 49wt% hydrofluoric acid and 85 parts pure water with resistivity >18MΩ·cm. Processing time: 220s, temperature: room temperature. This step is used to completely remove the SiO2 oxide layer containing metallic impurities generated in step S2.

[0045] M2 washing process: Same as M2 washing process in S1.

[0046] M3 Pre-cleaning Process: Prepare the cleaning solution according to the following volume ratios: 4 parts 32wt% hydrogen peroxide, 1 part 45wt% sodium hydroxide, and 95 parts pure water with a resistivity >18MΩ·cm. Processing time: 220s, temperature: 68℃.

[0047] M4 washing process: Same as M2 washing process.

[0048] M5 One-Step Texturing Process: The texturing solution is prepared according to the following volume ratios: 1 part 45wt% sodium hydroxide, 0.4 parts texturing additive, and 98.6 parts pure water with a resistivity >18MΩ·cm (in this embodiment, the texturing additive is a polyethyleneimine-polyethylene glycol composite with a mass ratio of 3:1, used to promote uniform pyramid nucleation). Processing time: 280s, temperature: 82℃.

[0049] M6 washing process: Same as M2 washing process.

[0050] M7 Two-Step Texturing Process: Prepare the texturing solution according to the following volume ratios: 0.2 parts 45wt% sodium hydroxide, 0.15 parts texturing additive, and 99.65 parts pure water with a resistivity >18MΩ·cm (texturing additive is the same as in step M5). The texturing additives for the first and second steps are different. The first-step texturing additive can be TS57V12, while the second-step texturing additive can be TS7BV12. Processing time: 110 seconds; temperature: 60℃.

[0051] M8 washing process: Same as M2 washing process.

[0052] M9 Alkaline Washing Process: Prepare the alkaline washing solution according to the following volume ratios: 3 parts 32wt% hydrogen peroxide, 1 part 45wt% sodium hydroxide, and 96 parts pure water with a resistivity >18MΩ·cm. Processing time: 100s, temperature: 65℃.

[0053] M10 washing process: Same as M2 washing process.

[0054] M11 pickling process: Prepare the pickling solution according to the following volume ratios: 10 parts 49wt% hydrofluoric acid, 2 parts 36wt% hydrochloric acid, and 88 parts pure water with a resistivity >18MΩ·cm. Processing time: 120s, temperature: room temperature.

[0055] M12 washing process: Same as M2 washing process.

[0056] M13 slow lifting process: slow lifting speed 3mm / s, processing time 10s, temperature 75℃.

[0057] M14 drying process: processing time 600s, temperature 95℃.

[0058] After the above steps, the repaired TOPCon rework wafer is obtained and can be reused in subsequent battery manufacturing processes (such as boron diffusion, SE laser doping, ALD passivation, etc.).

[0059] Comparative Example 1 To verify the beneficial effects of the technical solution of this invention, this comparative example provides a conventional rework method for TOPCon rework sheets. This method is a process commonly used in the industry, which involves alternating acid and alkali cleaning to remove the film and then directly texturing. Specifically, it includes the following steps: S1: Rework film is removed by alternating acid and alkali cleaning. Semi-finished reworked cells (with appearance and electrical performance defects consistent with the examples) generated from various processes of the same batch of TOPCon batteries were collected and placed in a cleaning basket, then sent to a rework cleaning machine for multi-step acid-alkali alternating cleaning to remove residual multilayer dielectric films (SiNx, AlOx, SiO2, Poly-Si, etc.) and surface contaminants. The cleaning process sequentially includes M1 acid washing, M2 water washing, M3 alkaline washing, M4 water washing, M5 alkaline cleaning, M6 water washing, M7 acid washing, M8 water washing, M9 slow lifting, and M10 drying. The process parameters for each process are as follows: M1 pickling process: Prepare the pickling solution according to the following volume ratios: 130L of 49wt% hydrofluoric acid (EL grade) and 320L of pure water with a resistivity >18MΩ·cm (volume ratio approximately HF:pure water = 1:2.46). Processing time: 800s, temperature: room temperature (25±3℃). This step is used for the initial stripping of the surface oxide layer and silicon nitride layer.

[0060] M2 water washing process: Use pure water with resistivity >18MΩ·cm for overflow cleaning, processing time 200s, temperature room temperature, replenishment flow rate 600L / h.

[0061] M3 Alkaline Washing Process: Prepare the alkaline washing solution according to the following volume ratios: 8L of 45wt% sodium hydroxide (EL grade) and 528L of pure water with a resistivity >18MΩ·cm (volume ratio approximately NaOH:pure water = 1:66). Processing time: 300s; temperature: 65℃. This step is used to remove the polycrystalline silicon layer and part of the oxide layer.

[0062] M4 washing process: Same as M2 washing process.

[0063] M5 Alkaline Cleaning Process: Prepare the alkaline cleaning solution according to the following volume ratios: 6L of 32wt% hydrogen peroxide, 3L of 45wt% sodium hydroxide, and 528L of pure water with a resistivity >18MΩ·cm. Processing time: 200s, temperature: 60℃. This step is used to further remove organic contaminants and residual membrane layers.

[0064] M6 washing process: Same as M2 washing process.

[0065] M7 Pickling Process: Prepare the pickling solution according to the following volume ratios: 95L of 49wt% hydrofluoric acid, 25L of 36wt% hydrochloric acid, and 297L of pure water with a resistivity >18MΩ·cm (volume ratio approximately HF:HCl:pure water = 1:0.26:3.13). Processing time: 200s, temperature: room temperature. This step is used to neutralize residual alkaline solution from the preceding process and remove metal ion contaminants.

[0066] M8 washing process: Same as M2 washing process.

[0067] M9 slow lifting process: slow lifting speed 3mm / s, processing time 20s, temperature 55℃.

[0068] M10 drying process: processing time 800s, temperature 90℃.

[0069] After the above cleaning process, the dielectric film on the surface of the rework wafer is removed, and a bare silicon wafer is obtained.

[0070] S2: Direct secondary texturing (without high-temperature oxidation and impurity removal treatment) The bare silicon rework wafer obtained in step S1 is directly fed into a texturing and cleaning machine for secondary texturing. The texturing process includes conventional pre-cleaning, one or two-step alkaline texturing, post-cleaning, acid washing, slow lifting, and drying. The specific process parameters are the same as those of conventional texturing processes in the field (consistent with the subsequent texturing parameters in step S3 of the embodiment, except for the oxide layer acid washing M1 step), and will not be described again here. This comparative example does not include any high-temperature oxidation gettering treatment steps.

[0071] Performance Testing and Comparison The reworked wafers repaired in this comparative example were made into finished batteries using the same post-processing steps as the example (boron diffusion, SE laser doping, ALD alumina passivation, PECVD silicon nitride deposition, screen printing sintering, etc.). The batteries were then compared with the example group and the normal production wafers from the same batch in terms of electrical performance (testing equipment: Halm-IV tester, standard test conditions: AM1.5G, 25℃). The results are shown in Table 1. Comparative Example 2 The difference from Example 1 is that the high-temperature oxidation and gettering treatment in step S2 is not performed.

[0072] Comparative Example 3 The difference from Example 1 is that the mixed acid cleaning system in step S1 M1 mixed acid washing process is 23 parts of 49wt% hydrofluoric acid, 16 parts of 36wt% hydrochloric acid, 55 parts of pure water with resistivity >18MΩ·cm, and 6 parts of catalytic additive.

[0073] Comparative Example 4 The difference from Example 1 is that the production line is used for segmented cleaning and film removal + high-temperature oxidation and impurity removal + oxide layer removal + texturing.

[0074] Comparative Example 5 The difference from Example 1 is that in step S2, the A2 dry oxygen oxidation stage is heated to an oxidation temperature of 700°C.

[0075] Comparative Example 6 The difference from Example 1 is that in step S2, the A2 dry oxygen oxidation stage is heated to an oxidation temperature of 1000°C. The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for improving the efficiency and yield of TOPCon rework wafers, characterized in that: Includes the following steps: S1: Place the TOPCon rework wafer in a mixed acid cleaning system for cleaning to obtain the bare silicon rework wafer; S2: Place the bare silicon rework wafer obtained in step S1 in a boron diffusion tube furnace and perform high-temperature oxidation treatment in a pure oxygen atmosphere to generate a SiO2 oxide layer on the surface of the rework wafer. S3: Pickling removes the SiO2 oxide layer on the surface of the reworked sheet obtained in step S2, followed by texturing.

2. The method for improving the efficiency and yield of TOPCon rework wafers according to claim 1, characterized in that: The cleaning process in step S1 includes the following steps performed in sequence: M1 mixed acid washing, M2 water washing, M3 alkaline washing, M4 water washing, M5 mixed acid washing, M6 water washing, M7 slow lifting, and M8 drying.

3. The method for improving the efficiency and yield of TOPCon rework wafers according to claim 2, characterized in that: In the M1 mixed acid washing process, the mixed acid cleaning system is prepared by the following components in volume proportions: 2-4 parts hydrogen peroxide, 17-23 parts hydrofluoric acid, 14-18 parts hydrochloric acid, 50-60 parts pure water, and 4-8 parts catalytic additive. Preferably, the hydrogen peroxide concentration is 32-36 wt%; Preferably, the mass concentration of hydrofluoric acid is 49-50 wt%; Preferably, the hydrochloric acid has a mass concentration of 36-38 wt%. Preferably, the resistivity of pure water is >18 MΩ·cm; The processing time for the M1 mixed pickling process is 1000-1800 seconds, and the temperature is room temperature. And / or, in the M3 alkaline washing process, the alkaline washing solution is prepared according to the following volume ratio: 1-2 parts hydrogen peroxide, 0.5-1.5 parts sodium hydroxide, and 96-98 parts pure water; Preferably, the hydrogen peroxide concentration is 32-36 wt%; Preferably, the mass concentration of sodium hydroxide is 44-46 wt%; Preferably, the resistivity of pure water is >18 MΩ·cm; The processing time for the M3 alkaline washing process is 150-250 seconds, and the temperature is 55-65℃. And / or, in the M5 mixed pickling process, the pickling solution is prepared according to the following volume ratio: 1.5-3 parts hydrofluoric acid, 4.5-6 parts hydrochloric acid and 60-70 parts pure water; Preferably, the mass concentration of hydrofluoric acid is 49-50 wt%; Preferably, the hydrochloric acid has a mass concentration of 36-38 wt%. Preferably, the resistivity of pure water is >18 MΩ·cm; The process conditions for the M5 mixed pickling process are: processing time 150-250s, temperature room temperature.

4. The method for improving the efficiency and yield of TOPCon rework wafers according to claim 2, characterized in that: The time for the M2, M4, and M6 water washing processes is 150-250 seconds, the temperature is room temperature, and the flow rate is 400-1000 L / H. Preferably, the speed of the M7 slow lifting process is 2.0-4.0 mm / s: Preferably, the drying process of M8 takes 700-900 seconds and the temperature is 75-95°C.

5. The method for improving the efficiency and yield of TOPCon rework wafers according to claim 1, characterized in that: The high-temperature oxidation gettering process described in step S2 includes the following steps: A1: Raise the temperature inside the furnace tube to the preset preheating temperature and purge with protective gas; A2: Introduce oxygen-containing gas for high-temperature oxidation treatment to generate a SiO2 oxide layer on the surface of the reworked sheet; A3: Stop the flow of oxygen-containing gas and remove the product after cooling under a protective atmosphere.

6. The method for improving the efficiency and yield of TOPCon rework wafers according to claim 5, characterized in that: The heating rate in step A1 is 5~10℃ / min, the preset preheating temperature is 750~820℃, and the temperature is held constant for 180~600s after reaching the preset preheating temperature; the protective gas is nitrogen, and the nitrogen flow rate is 8000~18000sccm. Preferably, the oxygen-containing gas in step A2 is oxygen or dry air, the oxidation temperature is 800~900℃, the isothermal oxidation time is 1200~4800s, and the total film thickness of the generated SiO2 oxide layer is controlled to be 2nm~8nm. Preferably, in step A3, the cooling rate is 3~15℃ / min.

7. The method for improving the efficiency and yield of TOPCon rework wafers according to claim 1, characterized in that: Step S3 includes the following steps performed in sequence: M1 pickling process, M2 water washing process, M3 pre-cleaning process, M4 water washing process, M5 one-step flocking process, M6 water washing process, M7 two-step flocking process, M8 water washing process, M9 alkaline washing process, M10 water washing process, M11 pickling process, M12 water washing process, M13 slow lifting process, and M14 drying process.

8. A method for improving the efficiency and yield of TOPCon rework wafers according to claim 7, characterized in that: The pickling solution used in the M1 pickling process is prepared according to the following volume ratio: 12-18 parts hydrofluoric acid and 82-88 parts pure water. The mass concentration of hydrofluoric acid is 49-50 wt%; The resistivity of pure water is >18 MΩ·cm; The processing time for the M1 pickling process is 150-250 seconds at room temperature. Preferably, in the M3 pre-cleaning process, the cleaning solution is prepared according to the following volume ratio: 2-6 parts hydrogen peroxide; 0.5-2 parts 44-46 wt% sodium hydroxide; 92-97 parts pure water; The mass concentration of hydrogen peroxide is 32-36 wt%. The mass concentration of sodium hydroxide is 44-46 wt%; The resistivity of pure water is >18 MΩ·cm; The processing time for the M3 pre-cleaning process is 150-250 seconds, and the temperature is 60-75℃. Preferably, in the M5 one-step texturing process, the texturing solution is prepared according to the following volume ratio: 0.5-1.5 parts sodium hydroxide, 0.2-0.6 parts texturing additive, and 98-99.5 parts pure water with a resistivity >18MΩ·cm; The mass concentration of sodium hydroxide is 44-46 wt%; The resistivity of pure water is >18 MΩ·cm; The M5 one-step flocking process takes 200-350 seconds and is carried out at a temperature of 78-85℃.

9. A method for improving the efficiency and yield of TOPCon rework wafers according to claim 7, characterized in that: In the M7 two-step texturing process, the texturing solution is prepared according to the following volume ratio: 0.1-0.4 parts sodium hydroxide; 0.1-0.3 parts texturing additive; and 99.5-99.9 parts pure water with a resistivity >18MΩ·cm. The mass concentration of sodium hydroxide is 44-46 wt%; The resistivity of pure water is >18 MΩ·cm; The processing time for the M7 two-step flocking process is 60-180 seconds, and the temperature is 55-68℃. Preferably, in the M9 alkaline washing process, the alkaline washing solution is prepared according to the following volume ratio: 2-5 parts hydrogen peroxide, 0.5-1.5 parts sodium hydroxide (NaOH), and 93-98 parts pure water; The mass concentration of hydrogen peroxide is 32-36 wt%. The mass concentration of sodium hydroxide is 44-46 wt%; The resistivity of pure water is >18 MΩ·cm; The processing time for the M9 alkaline washing process is 60-150 seconds, and the temperature is 60-70℃.

10. A method for improving the efficiency and yield of TOPCon rework wafers according to claim 7, characterized in that: In the M11 pickling process, the pickling solution is prepared according to the following volume ratio: 8-15 parts hydrofluoric acid, 1-4 parts 36-38 wt% hydrochloric acid, and 82-90 parts pure water. The mass concentration of hydrofluoric acid is 49-50 wt%; The mass concentration of hydrochloric acid is 36-38 wt%; The resistivity of pure water is >18 MΩ·cm; The M11 pickling process takes 80-180 seconds at room temperature. Preferably, the processing time for the M2, M4, M6, M8, M10, and M12 water washing processes is 150-250 seconds, the temperature is room temperature, and the pure water replenishment flow rate is 400-1000 L / H. Preferably, the processing time of the M13 slow lifting process is 5-30 seconds, and the temperature is 60-85℃; Preferably, the processing time of the M14 drying process is 400-900s, and the temperature is 80-100℃.

Citation Information

Patent Citations

  • Efficient cleaning method for crystalline silicon solar cell reworked piece

    CN119650415A

  • Processing method suitable for PE route TOPCon crystalline silicon battery rework piece

    CN121240579A