A solar cell and its fabrication method, and a photovoltaic module
By stacking a first dielectric layer and a second dielectric layer with different permittivity on the silicon substrate surface of the solar cell, a band barrier is formed, which solves the problem of poor electron and hole separation at the silicon substrate interface and improves photoelectric conversion efficiency.
Patent Information
- Application Number
- CN202611184202.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-05
- Publication Date
- 2026-11-17
AI Technical Summary
Poor electron-hole separation at the silicon substrate interface of solar cells leads to increased carrier recombination, affecting photoelectric conversion efficiency.
A first dielectric layer and a second dielectric layer are stacked on the surface of a silicon substrate. The first dielectric layer is in direct contact with the silicon substrate, and the relative permittivity of the second dielectric layer is higher than that of the first dielectric layer. The two work together to form a better band barrier, which blocks hole diffusion and promotes electron transport.
By creating steep band bends and a high-intensity built-in electric field, hole diffusion is effectively blocked, electron transport is promoted, carrier recombination is reduced, and the photoelectric conversion efficiency of solar cells is improved.
Smart Images

Figure CN123124509A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the technical field of solar cells, and more particularly to a solar cell and its preparation method, and a photovoltaic module. Background Technology
[0002] At the silicon substrate interface of solar cells, poor electron-hole separation easily leads to increased carrier recombination. How to effectively reduce carrier recombination at the silicon substrate interface and improve the photoelectric conversion efficiency of solar cells has become an urgent problem to be solved. Summary of the Invention
[0003] To reduce carrier recombination at the silicon substrate interface and improve the photoelectric conversion efficiency of solar cells, this application provides a solar cell, its fabrication method, and a photovoltaic module.
[0004] In one aspect, this application provides a solar cell.
[0005] The solar cell includes a silicon substrate, on the surface of which a first dielectric layer and a second dielectric layer are stacked. The first dielectric layer is in contact with the surface of the silicon substrate, and the second dielectric layer is located on the side of the first dielectric layer away from the silicon substrate. The first dielectric layer and the second dielectric layer exhibit positive charge characteristics; The relative permittivity of the second dielectric layer is greater than that of the first dielectric layer.
[0006] As an optional implementation, in the embodiments of this application, the fixed positive charge density of the first dielectric layer is greater than the fixed positive charge density of the second dielectric layer.
[0007] As an optional implementation, in the embodiments of this application, the sum of the fixed positive charge density of the first dielectric layer and the fixed positive charge density of the second dielectric layer is 1.5 × 10⁻⁶. 12 cm -2 ~6×10 12 cm -2 .
[0008] As an optional implementation, in the embodiments of this application, the fixed positive charge density of the first dielectric layer is 1×10⁻⁶. 12 cm -2 ~5×10 12 cm -2 The fixed positive charge density of the second dielectric layer is 0.5 × 10⁻⁶. 12 cm -2 ~2×10 12 cm -2 .
[0009] As an optional implementation, in the embodiments of this application, the relative permittivity of the second dielectric layer is 10~25, and / or the relative permittivity of the first dielectric layer is 7~9.
[0010] As an optional implementation, in an embodiment of this application, the interface state density between the material of the first dielectric layer and the silicon substrate is 0.5 × 10⁻⁶. 10 eV -1 ·cm -2 ~8×10 10 eV -1 ·cm -2 The carrier recombination velocity at the interface between the silicon substrate and the first dielectric layer is 15 cm / s to 25 cm / s.
[0011] As an optional implementation, in the embodiments of this application, the sum of the conduction band offset of the first dielectric layer and the conduction band offset of the second dielectric layer is greater than 3.5 eV, and the sum of the valence band offset of the first dielectric layer and the valence band offset of the second dielectric layer is greater than 6 eV.
[0012] As an optional implementation, in the embodiments of this application, the material of the first dielectric layer includes a doped passivation material, the doped passivation material includes a first dopant element and a passivation material, the electronegativity of the first dopant element is greater than or equal to 3, and the passivation material includes one or more combinations of silicon oxide, silicon oxynitride, silicon carbide, and aluminum oxide.
[0013] As an optional implementation, in the embodiments of this application, the content of the first dopant element in the doped passivation material is 0.05 wt%~0.75 wt%; And / or, The first doping element includes at least one of fluorine or chlorine; And / or, The thickness of the first dielectric layer is 1 nm to 5 nm.
[0014] As an optional implementation, in the embodiments of this application, the material of the second dielectric layer includes doped aluminum oxide, wherein the doped aluminum oxide includes a second doping element and aluminum oxide, and the second doping element includes at least one of hafnium or zirconium.
[0015] As an optional implementation, in the embodiments of this application, the content of the second doping element in the doped alumina is 10 wt%~50 wt%; And / or, The thickness of the second dielectric layer is 1 nm to 5 nm.
[0016] As an optional implementation, in the embodiments of this application, the solar cell further includes: a first doped silicon layer disposed on the side of the second dielectric layer away from the silicon substrate, wherein the thickness of the first doped silicon layer is 32 nm to 65 nm.
[0017] As an optional implementation, in the embodiments of this application, the first doped silicon layer includes a first doped silicon sublayer, a silicon oxide layer and a second doped silicon sublayer sequentially stacked on the side of the second dielectric layer away from the silicon substrate; The thickness of the first doped silicon sublayer is 5 nm to 15 nm, the thickness of the silicon oxide layer is 2 nm to 5 nm, and the thickness of the second doped silicon sublayer is 25 nm to 45 nm. The surface doping concentration of the conductive dopant element in the second doped silicon sublayer is greater than that in the first doped silicon sublayer, and the surface doping concentration of the conductive dopant element in the second doped silicon sublayer is 1×10⁻⁶. 19 cm -3 ~9×10 21 cm -3 .
[0018] Secondly, this application provides a method for preparing a solar cell.
[0019] A method for fabricating a solar cell includes the following steps: A first dielectric layer is fabricated on a silicon substrate, such that the first dielectric layer is in contact with the silicon substrate, and the first dielectric layer has a positive charge characteristic. A second dielectric layer is prepared on the side of the first dielectric layer away from the silicon substrate. The second dielectric layer has positive charge characteristics and its relative permittivity is greater than that of the first dielectric layer.
[0020] As an optional implementation, in the embodiments of this application, the material of the first dielectric layer includes a doped passivation material, and the gas source used to prepare the doped passivation material includes a gas source containing a first dopant element and a gas source for depositing passivation material, so as to form the doped passivation material containing the first dopant element, wherein the electronegativity of the first dopant element is greater than or equal to 3, and the first dopant element includes at least one of fluorine or chlorine. The material of the second dielectric layer includes doped alumina. The gas source used to prepare the doped alumina includes a gas source containing a second dopant element and a gas source for depositing alumina, so as to form the doped alumina containing the second dopant element, wherein the second dopant element includes at least one of hafnium or zirconium.
[0021] As an optional implementation, in the embodiments of this application, the gas source containing the first doping element includes one or more combinations of CF4 and CCl4, and the gas source for depositing passivation material includes a first oxygen source, which includes one or more combinations of N2O, H2O, and O2. The gas source containing the second doping element includes one or more combinations of tetraethylmethylamine hafnium and tetraethylmethylamine zirconium, the gas source for depositing alumina includes an aluminum source and a second oxygen source, the aluminum source includes trimethylaluminum, and the second oxygen source includes one or two combinations of H2O and O2.
[0022] As an optional implementation, in the embodiments of this application, the first dielectric layer is prepared by plasma chemical vapor deposition, low-pressure chemical vapor deposition, atomic layer deposition, or plasma-enhanced atomic layer deposition. The method for preparing the first dielectric layer using plasma chemical vapor deposition includes: introducing a gas source containing a first dopant element and a first oxygen source to react, wherein the ratio of the gas flow rate of the gas source containing the first dopant element to the gas flow rate of the first oxygen source is (50 sccm~350 sccm):(4000 sccm~15000 sccm), controlling the reaction temperature at 370℃~470℃, the reaction time at 50 s~120 s, the power at 11000 W~15000 W, and the power frequency at 60 Hz~150 Hz. The second dielectric layer is prepared by atomic layer deposition or plasma-enhanced atomic layer deposition. The method for preparing the second dielectric layer by atomic layer deposition includes: introducing the gas source containing the second dopant element, the second oxygen source, and the aluminum source to carry out a reaction, wherein the gas flow rate ratio of the gas source containing the second dopant element, the second oxygen source, and the aluminum source is (3 sccm~10 sccm):(12 sccm~26 sccm):(15 sccm~40 sccm), controlling the reaction temperature at 175℃~300℃, and the number of reaction cycles is 25~40.
[0023] Thirdly, this application provides a photovoltaic module.
[0024] A photovoltaic module includes a solar cell as described in the first aspect or a solar cell prepared by the method described in the second aspect.
[0025] Compared with the prior art, the beneficial effects of this application are as follows: The solar cell of this application, through the coordinated action of the first and second dielectric layers disposed on the surface of the silicon substrate, can form a better band barrier barrier, blocking hole diffusion and promoting electron transport, thereby better promoting electron and hole separation at the silicon substrate interface, reducing carrier recombination, and effectively improving the photoelectric conversion efficiency of the solar cell.
[0026] Specifically, the first dielectric layer is in direct contact with the silicon substrate surface, forming a fundamental band bend and a fundamental built-in electric field on the silicon substrate surface that blocks holes and promotes electron transport. The second dielectric layer, with its relatively high permittivity, generates a better capacitive coupling effect, inducing a higher equivalent positive charge density at the interface between the first and second dielectric layers, thus further enhancing the fundamental band bend. Therefore, the combination of the first and second dielectric layers creates a relatively steep band bend and constructs a stronger built-in electric field, significantly enhancing the hole diffusion blocking effect. Simultaneously, the combination of the first and second dielectric layers significantly increases the positive charge density, which helps reduce the lateral transport resistance of electrons, promotes electron transport, and effectively reduces carrier recombination. Attached Figure Description
[0027] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0028] Figure 1 This is a schematic diagram of the structure of the first type of solar cell disclosed in the embodiments of this application; Figure 2 This is a schematic diagram of the structure of the second type of solar cell disclosed in the embodiments of this application; Figure 3 This is a schematic diagram of the structure of the first dielectric layer disposed on the silicon substrate as disclosed in the embodiments of this application; Figure 4 This is a schematic diagram of the structure disclosed in this application, in which the second dielectric layer is disposed on the side of the first dielectric layer away from the silicon substrate.
[0029] Icons: 1. Silicon substrate; 2. First dielectric layer; 3. Second dielectric layer; 4. First doped silicon layer; 41. First doped silicon sublayer; 42. Silicon oxide layer; 43. Second doped silicon sublayer; 5. First passivation layer; 6. Second doped silicon layer; 7. Second passivation layer; 8. First electrode; 9. Second electrode. Detailed Implementation
[0030] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, and not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0031] The technical solution of this application will be further described below with reference to the embodiments and accompanying drawings.
[0032] In a first aspect, embodiments of this application provide a solar cell.
[0033] Reference Figure 1 A solar cell includes a silicon substrate 1. A first dielectric layer 2 and a second dielectric layer 3 are stacked on the surface of the silicon substrate 1. The first dielectric layer 2 is in contact with the surface of the silicon substrate 1. The second dielectric layer 3 is located on the side of the first dielectric layer 2 away from the silicon substrate 1.
[0034] The first dielectric layer 2 and the second dielectric layer 3 have positive charge characteristics.
[0035] The relative permittivity of the second dielectric layer 3 is greater than that of the first dielectric layer 2.
[0036] In solar cells, when holes diffuse from a silicon substrate to a metal electrode, they must first overcome a potential barrier at the valence band peak (Ev) of the silicon substrate to transition to the dielectric layer located on the back side of the silicon substrate. This barrier height is called the "valence band offset (ΔEv)," which is the difference between the Ev of the silicon substrate and the Ev of the dielectric layer. A larger ΔEv value means a greater barrier to overcome for a hole to transition from the silicon substrate to the dielectric layer, making it more difficult and thus more conducive to blocking hole diffusion. Furthermore, the high built-in electric field strength on the silicon substrate surface is beneficial for blocking holes and promoting electron-hole separation at the silicon substrate interface, effectively reducing carrier recombination.
[0037] This application, through the coordinated action of the first dielectric layer 2 and the second dielectric layer 3 disposed on the surface of the silicon substrate 1, can promote the separation of electrons and holes at the interface of the silicon substrate 1 while enhancing electron transport capability and reducing carrier recombination, thereby effectively improving the photoelectric conversion efficiency of the solar cell.
[0038] Specifically, the first dielectric layer 2 directly contacts the surface of the silicon substrate 1. The fixed positive charge provided by the first dielectric layer 2 can act directly on the surface of the silicon substrate 1 with minimal loss, generating a certain valence band shift and forming a better basic band bending and a basic built-in electric field. Based on this, a second dielectric layer 3, with a relatively higher permittivity than the first dielectric layer 2, is stacked on the side of the first dielectric layer 2 away from the silicon substrate 1, which enhances the capacitive coupling effect. Furthermore, due to the positive charge characteristics of the second dielectric layer 3, it effectively avoids the generation of a reverse electric field between the second dielectric layer 3 and the first dielectric layer 2. Under the amplification effect of the capacitive coupling with a high relative permittivity, the charge effect can be superimposed in the same direction, thereby inducing a higher equivalent positive charge density at the interface between the first dielectric layer 2 and the second dielectric layer 3. This significantly increases the valence band shift between the silicon substrate 1 and the first dielectric layer 2, raising the hole transition barrier.
[0039] With the first dielectric layer 2 and the second dielectric layer 3 working together, a steep bandgap can be formed and a strong built-in electric field can be constructed, effectively improving the hole blocking effect. This confines holes within the silicon substrate 1 or allows them to diffuse to the other side of the silicon substrate 1. Furthermore, the combination of the first dielectric layer 2 and the second dielectric layer 3 significantly increases the fixed positive charge density, which helps reduce the lateral electron transport resistance and improve electron transport performance. This effectively suppresses carrier recombination at the interface of the silicon substrate 1, thereby improving the electrical performance of the solar cell.
[0040] If the second dielectric layer 3 has negative charge characteristics, the reverse electric field generated by the second dielectric layer 3 will weaken the band bending formed by the first dielectric layer 2 on the surface of the silicon substrate 1, thereby having a negative effect on blocking hole diffusion.
[0041] The first dielectric layer 2 of this application is in direct contact with the surface of the silicon substrate 1, and is made of a material with a relatively low permittivity. This is because if a dielectric layer with a higher relative permittivity (such as the second dielectric layer 3) is directly disposed on the surface of the silicon substrate 1, a large number of unsaturated "dangling bonds" and structural defects are easily generated at the interface due to lattice mismatch and poor chemical bond matching, thereby introducing a high density of interface defect states, which in turn leads to an increase in carrier recombination. Using the first dielectric layer 2 with a low relative permittivity as the direct contact layer of the silicon substrate 1 can effectively reduce the interface defect states on the surface of the silicon substrate 1.
[0042] Furthermore, ensuring direct contact between the first dielectric layer 2 (with a fixed positive charge density higher than the second dielectric layer 3) and the silicon substrate 1 is crucial for achieving optimal electron and hole separation. If other dielectric layers (such as the second dielectric layer 3) are inserted between the first dielectric layer 2 and the silicon substrate 1, the electric field generated by the first dielectric layer 2 will be severely attenuated and shielded when it passes through other dielectric layers to the surface of the silicon substrate 1. This ultimately leads to poor performance of the built-in electric field, significantly deteriorating the selective electron transport and hole blocking effects.
[0043] It should be noted that fixed positive charge refers to the net positive charge that exists within the dielectric layer (such as silicon oxide, silicon nitride, aluminum oxide, etc.) or near the interface between the dielectric layer and the silicon substrate, and whose position is fixed and cannot move under normal device operating conditions. Fixed positive charge density is a way of quantifying fixed positive charge using the area density method, with units of cm⁻¹. -2 Specifically, it refers to the net amount of positive charge contained in a unit area. The magnitude of a fixed positive charge density can be obtained through capacitance-voltage (CV) testing.
[0044] In some embodiments, the fixed positive charge density of the first dielectric layer 2 is greater than the fixed positive charge density of the second dielectric layer 3.
[0045] The first dielectric layer 2 is directly disposed on the silicon substrate 1 and has a large fixed positive charge density. This allows the fixed positive charge of the first dielectric layer 2 to act directly on the surface of the silicon substrate 1 with less loss, giving full play to the advantage that the fixed positive charge density of the first dielectric layer 2 is higher than that of the second dielectric layer 3, forming a stronger built-in electric field, thereby further promoting electron transport and blocking hole transition.
[0046] In some embodiments, the sum of the fixed positive charge density of the first dielectric layer 2 and the fixed positive charge density of the second dielectric layer 3 is 1.5 × 10⁻⁶. 12 cm -2 ~6×10 12 cm -2 When the sum of the fixed positive charge density of the first dielectric layer 2 and the fixed positive charge density of the second dielectric layer 3 is within the aforementioned range, a more suitable band bend can be formed, better blocking holes and improving electron tunneling performance. For example, the sum of the fixed positive charge density of the first dielectric layer 2 and the fixed positive charge density of the second dielectric layer 3 can be 1.5 × 10⁻⁶. 12 cm -2 3×10 12 cm -2 4.5×10 12 cm -2 6×10 12 cm -2 wait.
[0047] When the sum of the fixed positive charge densities of the two layers is too low, the resulting bandgap is too gentle, resulting in poor hole blocking ability and high contact resistance, which is not conducive to further improving the photoelectric conversion efficiency of the battery. When the sum of the fixed positive charge densities of the two layers is too high, the resulting bandgap is too steep, leading to increased interface tunneling leakage, excessively high hole barrier, increased contact resistance instead of decreased contact resistance, reduced minority carrier lifetime, and even increased stress on the first dielectric layer 2 and the second dielectric layer 3, resulting in compromised stability.
[0048] In some embodiments, the fixed positive charge density of the first dielectric layer 2 is 1×10⁻⁶. 12 cm -2 ~5×10 12 cm -2 The fixed positive charge density of the second dielectric layer 3 is 0.5 × 10⁻⁶. 12 cm -2 ~2×10 12 cm -2 When the fixed positive charge density of the first dielectric layer 2 is within the above-mentioned range, the hole-blocking effect of the first dielectric layer 2 and the contact resistance between the first dielectric layer 2 and the silicon substrate 1 can be better balanced. When the fixed positive charge density of the first dielectric layer 2 is less than 1×10⁻⁶, the hole-blocking effect of the first dielectric layer 2 and the contact resistance between the first dielectric layer 2 and the silicon substrate 1 can be better balanced. 12 cm -2 The blocking effect on holes is poor. When the fixed positive charge density of the first dielectric layer 2 is higher than 5 × 10⁻⁶, the effect is not good. 12 cm -2 This can easily lead to an increase in leakage current and an increase in the contact resistance between the first dielectric layer 2 and the silicon substrate 1. When the fixed positive charge density of the second dielectric layer 3 is within the aforementioned range, it can effectively enhance band bending. If the fixed positive charge of the first dielectric layer 2 and the second dielectric layer 3 is too large, it is not conducive to reducing leakage current; if it is too small, it is not conducive to enhancing the band bending effect, ultimately limiting further improvement in the photoelectric conversion efficiency of the solar cell.
[0049] For example, the fixed positive charge density of the first dielectric layer 2 can be 1×10⁻⁶. 12 cm -2 2×10 12 cm -2 3×10 12 cm -2 4×10 12 cm -2 5×10 12 cm -2 The fixed positive charge density of the second dielectric layer 3 can be 0.5 × 10⁻⁶. 12 cm -2 1×10 12 cm -2 1.5×10 12 cm -2 2×10 12 cm -2 wait.
[0050] In some embodiments, the relative permittivity of the second dielectric layer 3 is 10~25. Controlling the relative permittivity of the second dielectric layer 3 within this range can better enhance capacitive coupling while maintaining the band gap of the second dielectric layer 3 within a suitable range. This avoids the problem of an excessively narrow band gap leading to a decrease in the tunneling barrier and an exponential increase in direct tunneling and defect-assisted tunneling currents. When the relative permittivity of the second dielectric layer 3 is too high, it means that its material band gap is too narrow, resulting in an excessively low tunneling barrier for holes, leading to a significant increase in tunneling and defect-assisted tunneling currents, which is detrimental to reducing leakage current. When the relative permittivity of the second dielectric layer 3 is too low, the enhancement effect of capacitive coupling is limited, which is not conducive to improving the attraction effect of the second dielectric layer 3 for electrons.
[0051] For example, the relative permittivity of the second dielectric layer 3 is 10, 13, 15, 20, 25, etc.
[0052] In some embodiments, the relative permittivity of the first dielectric layer 2 is 7 to 9. A relative permittivity within this range is beneficial for reducing the introduction of interface defect states on the silicon substrate 1 and improving the interface quality of the silicon substrate 1. Exemplarily, the relative permittivity of the first dielectric layer 2 is 7, 8, 9, etc. The relative permittivity can be obtained by capacitance-voltage (CV) testing. If the relative permittivity of the first dielectric layer 2 is too high, it is not conducive to forming a good interface contact between the first dielectric layer 2 and the silicon substrate 1, and it is not conducive to reducing interface defect states on the silicon substrate 1. If the relative permittivity of the first dielectric layer 2 is too low, it is not conducive to reducing the tunneling leakage current at the interface of the silicon substrate 1.
[0053] In one specific embodiment, the interface state density between the material of the first dielectric layer 2 and the silicon substrate 1 is 0.5 × 10⁻⁶. 10 eV -1 ·cm -2 ~8×10 10 eV -1 ·cm -2 The carrier recombination velocity at the interface between the silicon substrate 1 and the first dielectric layer 2 is 15 cm / s to 25 cm / s. The first dielectric layer 2 is in direct contact with the surface of the silicon substrate 1, which can better reduce the interface state density of the silicon substrate, effectively passivate interface defects of the silicon substrate 1, improve the interface quality of the silicon substrate 1, and reduce carrier recombination. When the interface state density of the silicon substrate 1 is too high, carrier recombination at the interface of the silicon substrate 1 becomes more likely, and a higher carrier recombination velocity is observed.
[0054] For example, the interface state density of the first dielectric layer 2 material can be 0.5 × 10⁻⁶ with that of the silicon substrate 1. 10 eV -1 ·cm -2 3×10 10 eV -1·cm -2 5×10 10 eV -1 ·cm -2 8×10 10 eV -1 ·cm -2 wait.
[0055] In some embodiments, the interface state density between the material of the second dielectric layer 3 and the silicon substrate 1 is 5.5 × 10⁻⁶. 11 eV -1 ·cm -2 ~9×10 12 eV -1 ·cm -2 Because the second dielectric layer 3 is made of a material with a high relative permittivity, if this material is in direct contact with the surface of the silicon substrate 1, it is prone to generating a large number of unsaturated "dangling bonds" and structural defects at the interface due to lattice mismatch and poor chemical bond matching, resulting in a high interface state density at the interface. For example, the interface state density between the second dielectric layer 3 and the silicon substrate 1 can be 5.5 × 10⁻⁶. 11 eV -1 ·cm -2 6.5×10 11 eV -1 ·cm -2 7.5×10 11 eV -1 ·cm -2 8.5×10 11 eV -1 ·cm -2 9×10 12 eV -1 ·cm -2 wait.
[0056] It should be noted that the interface density of states can be measured by the high-frequency-quasi-static CV combined method (i.e., the combination of high-frequency CV and quasi-static CV (or low-frequency CV)).
[0057] The interface state density on the surface of silicon substrate 1 is mainly affected by the first dielectric layer 2, which is in direct contact with it. The second dielectric layer 3 enhances field passivation through capacitive coupling, and the two work together to reduce interfacial carrier recombination on silicon substrate 1. If the order of the two is reversed, so that the second dielectric layer 3 with a high relative permittivity is in direct contact with silicon substrate 1, the interface passivation effect is easily weakened and carrier recombination is increased.
[0058] In some embodiments, the sum of the conduction band offset of the first dielectric layer 2 and the conduction band offset of the second dielectric layer 3 is greater than 3.5 eV. The sum of the valence band offset of the first dielectric layer 2 and the valence band offset of the second dielectric layer 3 is greater than 6 eV.
[0059] When the conduction band offset of the first dielectric layer 2 and the conduction band offset of the second dielectric layer 3, as well as the valence band offset of the first dielectric layer 2 and the valence band offset of the second dielectric layer 3, are respectively set within the aforementioned ranges, holes can be better blocked, and electron tunneling into subsequent functional layers can be efficiently promoted. For example, the sum of the conduction band offsets of the first dielectric layer 2 and the second dielectric layer 3 can be 4 eV, 5 eV, or 6 eV, and the sum of the valence band offsets of the first dielectric layer 2 and the second dielectric layer 3 can be 7 eV, 8 eV, or 9 eV, etc. When the sum of the conduction band offsets of the first dielectric layer 2 and the second dielectric layer 3, or the sum of the valence band offsets of the first dielectric layer 2 and the second dielectric layer 3, is too low, it is not conducive to forming a steeper band bend, resulting in a limited improvement in the hole blocking barrier. When the sum of the conduction band offset of the first dielectric layer 2 and the conduction band offset of the second dielectric layer 3, or the sum of the valence band offset of the first dielectric layer 2 and the valence band offset of the second dielectric layer 3, is too high, it is easy to cause an increase in interface tunneling leakage due to the energy band being too steep.
[0060] In one specific embodiment, the conduction band offset of the first dielectric layer 2 is greater than 2 eV, and the valence band offset of the first dielectric layer 2 is greater than 4 eV. The conduction band offset of the second dielectric layer 3 is greater than 1.5 eV, and the valence band offset of the second dielectric layer 3 is greater than 2 eV. Exemplarily, the conduction band offset of the first dielectric layer 2 can be 3 eV, 4 eV, 5 eV, etc., and the valence band offset of the first dielectric layer 2 can be 5 eV, 6 eV, 7 eV, etc.
[0061] In one specific embodiment, the conduction band offset of the second dielectric layer 3 is greater than 1.5 eV, and the valence band offset of the second dielectric layer 3 is greater than 2 eV. The conduction band offset of the second dielectric layer 3 can be 2 eV, 3 eV, 4 eV, etc., and the valence band offset of the second dielectric layer 3 can be 3 eV, 4 eV, 5 eV, etc.
[0062] It should be noted that the conduction band shift and valence band shift can be obtained by combining X-ray photoelectron spectroscopy (XPS) with reflected electron energy loss spectroscopy (REELS).
[0063] In some embodiments, the material of the first dielectric layer 2 includes a doped passivation material, which comprises a first dopant element and the passivation material. The electronegativity of the first dopant element is greater than or equal to 3. The passivation material includes one or more combinations of silicon oxide, silicon oxynitride, silicon carbide, and aluminum oxide.
[0064] Since silicon has an electronegativity of approximately 1.90, and the electronegativity of the first dopant is greater than or equal to 3, the first dopant can form a strong polar chemical bond with the silicon substrate 1. This strong polar chemical bond helps to generate a stable and relatively strong interfacial dipole layer at the interface between the silicon substrate 1 and the first dielectric layer 2. The presence of this interfacial dipole layer can introduce a fixed potential transition barrier at the interface, thereby significantly increasing the valence band shift of the first dielectric layer 2. This significantly increases the energy barrier that holes need to overcome for transitions, thus achieving more effective separation of holes and electrons. When the electronegativity of the first dopant is less than 3, the difference in electronegativity between the first dopant and silicon is small, which is not conducive to improving the separation effect of electrons and holes. For example, the electronegativity of the first dopant can be 3.1, 3.3, 3.5, 3.8, 4, etc.
[0065] Passivation materials such as silicon oxide, silicon oxynitride, silicon carbide, and aluminum oxide not only possess good passivation capabilities for interface defects, but also, when combined with a highly electronegative first dopant element, can significantly alter the charge distribution within the film layer, enhancing the fixed positive charge density of the doped passivation material. Taking aluminum oxide as an example, pure aluminum oxide typically exhibits high fixed negative charge characteristics. However, when highly electronegative fluorine is incorporated into aluminum oxide, the charge polarity of the film layer reverses, transforming it into a film layer with high fixed positive charge density, thus meeting the positive charge characteristics requirements of the first dielectric layer 2 in this application.
[0066] In some embodiments, the content of the first dopant element in the passivation material is 0.05 wt% to 0.75 wt%. Controlling the content of the first dopant element within this range can significantly increase the fixed positive charge density of the passivation material, enhance its attraction to electrons, and increase the valence band shift. When the first dopant element is excessively doped, phase separation easily occurs in the first dielectric layer 2, which is detrimental to the structural stability of the first dielectric layer 2 or leads to a decrease in insulation performance. When the doping amount of the first dopant element is too low, it is not conducive to increasing the fixed positive charge density of the first dielectric layer 2.
[0067] For example, in the doped passivation material, the content of the first dopant element can be 0.05 wt%, 0.2 wt%, 0.5 wt%, 0.75 wt%, etc. The content of the first dopant element in the doped passivation material can be measured using a time-of-flight secondary ion mass spectrometer (TOF-SIMS).
[0068] For example, the first doping element includes at least one of fluorine or chlorine. Fluorine has an electronegativity of 3.98, and chlorine has an electronegativity of 3.16, both of which can well meet the requirements of the above-mentioned strong polar bonding. Furthermore, the first dielectric layer 2 doped with fluorine or chlorine has the advantages of low interface defect density and low interface recombination rate, resulting in better surface passivation effect on the silicon substrate 1.
[0069] In some embodiments, the thickness of the first dielectric layer 2 is 1 nm to 5 nm. This thickness allows the first dielectric layer 2 to form an effective hole-blocking barrier due to its high fixed positive charge density. Furthermore, the relatively thin thickness of the first dielectric layer 2 allows electrons to pass through it into subsequent film layers, avoiding obstruction of electron transport or increased series resistance caused by excessive thickness. For example, the thickness of the first dielectric layer 2 can be 1 nm, 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, 4.5 nm, 5 nm, etc.
[0070] In some embodiments, the material of the second dielectric layer 3 includes doped alumina, which comprises a second dopant element and alumina. The second dopant element includes at least one of hafnium or zirconium. By introducing hafnium or zirconium into the alumina, the relative permittivity of the doped alumina can be effectively increased, thereby better utilizing the capacitive coupling amplification effect of the second dielectric layer 3.
[0071] In some embodiments, the content of the second dopant element in the doped alumina is 10 wt% to 50 wt%. This content of hafnium or zirconium can form a good solid solution or composite structure with the alumina matrix, effectively improving the relative permittivity. When the content of hafnium or zirconium is too low, the gain in relative permittivity of the doped alumina is not significant. Conversely, when the content of hafnium or zirconium is too high, it can easily damage the original interfacial properties of the alumina, which is detrimental to further improving the photoelectric conversion efficiency of the solar cell. For example, the content of the second dopant element in the doped alumina can be 10 wt%, 20 wt%, 35 wt%, 50 wt%, etc. The doping amount of the second dopant element in the alumina can be measured using time-of-flight secondary ion mass spectrometry (TOF-SIMS).
[0072] In some embodiments, the thickness of the second dielectric layer 3 is 1 nm to 5 nm. Similar to the first dielectric layer 2, the second dielectric layer 3 also maintains a relatively thin thickness to facilitate electron passage through the double dielectric layer, while working with the first dielectric layer 2 to effectively block holes. Exemplarily, the thickness of the second dielectric layer 3 is 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, etc. If the thickness of the second dielectric layer 3 is too high, it is not conducive to electron passage through the second dielectric layer. If the thickness of the second dielectric layer 3 is too low, it is not conducive to achieving the capacitive coupling enhancement effect, nor to enhancing the hole blocking effect.
[0073] Reference Figure 1In some embodiments, the solar cell further includes a first doped silicon layer 4, which is disposed on the side of the second dielectric layer 3 facing away from the silicon substrate 1. The thickness of the first doped silicon layer 4 is 32 nm to 65 nm. Traditionally, the thickness of the first doped silicon layer 4 is typically set above 100 nm. This thickness of the first doped silicon layer 4 has a certain blocking effect on holes, but the optical parasitic absorption is also relatively large. By thinning the thickness of the first doped silicon layer 4 to between 32 nm and 65 nm, the optical parasitic absorption can be significantly reduced. However, the hole blocking ability of this thickness of the first doped silicon layer 4 is relatively limited, the carrier recombination loss is large, and after the thickness of the first doped silicon layer 4 is reduced, electron transport is hindered, and the lateral transport resistance increases linearly. In this embodiment, the combination of the first dielectric layer 2 and the second dielectric layer 3 disposed between the silicon substrate 1 and the first doped silicon layer 4 can perform the main hole blocking function while promoting electron transport. This allows for excellent hole blocking performance, reducing carrier recombination losses and lowering the lateral transport resistance of electrons, even when the thickness of the first doped silicon layer 4 is set to a relatively thin range of 32 nm to 65 nm. For example, the thickness of the first doped silicon layer 4 can be 32 nm, 40 nm, 50 nm, 65 nm, etc. If the thickness of the first doped silicon layer 4 is too high, it is not conducive to further reducing optical parasitic absorption. If the thickness of the first doped silicon layer 4 is too low, it is not conducive to increasing the surface doping concentration of conductive dopants in the first doped silicon layer 4, and thus not conducive to reducing the contact resistance of the first doped silicon layer 4.
[0074] Reference Figure 2 In some embodiments, the first doped silicon layer 4 includes a first doped silicon sublayer 41, a silicon oxide layer 42, and a second doped silicon sublayer 43 sequentially stacked on the side of the second dielectric layer 3 facing away from the silicon substrate 1. The thickness of the first doped silicon sublayer 41 is 5 nm to 15 nm. The thickness of the silicon oxide layer 42 is 2 nm to 5 nm. The thickness of the second doped silicon sublayer 43 is 25 nm to 45 nm. The surface doping concentration of the conductive dopant element in the second doped silicon sublayer 43 is greater than that in the first doped silicon sublayer 41. The surface doping concentration of the conductive dopant element in the second doped silicon sublayer 43 is 1 × 10⁻⁶. 19 cm -3 ~9×10 21 cm -3 .
[0075] By providing a silicon oxide layer 42 of a specific thickness between the first doped silicon sublayer 41 and the second doped silicon sublayer 43, the silicon oxide layer 42 can block the diffusion of conductive dopants toward the silicon substrate 1, thereby promoting the enrichment of conductive dopants on the surface of the second doped silicon sublayer 43 and increasing the surface doping concentration of conductive dopants in the second doped silicon sublayer 43 to 1×10⁻⁶.19 cm -3 ~9×10 21 cm -3 This arrangement helps reduce the contact resistance between the second doped silicon sublayer 43 and the first electrode 8, thereby improving carrier transport performance. For example, the thickness of the first doped silicon sublayer 41 can be 5 nm, 8 nm, 12 nm, 15 nm, etc. The thickness of the silicon oxide layer 42 can be 2 nm, 3.5 nm, 5 nm, etc. The thickness of the second doped silicon sublayer 43 can be 25 nm, 30 nm, 35 nm, 40 nm, 45 nm, etc. The surface doping concentration of the conductive dopant element in the second doped silicon sublayer 43 can be 1 × 10⁻⁶. 19 cm -3 5×10 19 cm -3 7×10 19 cm -3 9×10 21 cm -3 wait.
[0076] It should be noted that the surface doping concentration of conductive doping elements in the first doped silicon sublayer 41 and the second doped silicon sublayer 43 can be obtained by secondary ion mass spectrometry (SIMS), or by electrochemical capacitance-voltage (ECV) testing.
[0077] In some embodiments, the silicon substrate 1 is an N-type silicon substrate 1, and the first dielectric layer 2 and the second dielectric layer 3 are disposed on the back surface side of the silicon substrate 1.
[0078] When collecting electrons on the back surface of the N-type silicon substrate 1, it is necessary to block the diffusion of holes to improve the electron collection effect. When the first dielectric layer 2 and the second dielectric layer 3 of this application are disposed on the back surface of the N-type silicon substrate 1 in a specific order, a high-strength band barrier barrier can be formed, which has an excellent blocking effect on the diffusion of holes and can also enhance electron transport, thereby more effectively ensuring the efficient and selective extraction of electrons.
[0079] In some embodiments, the side of the first doped silicon layer 4 facing away from the silicon substrate 1 also includes a first passivation layer 5.
[0080] In some embodiments, the light-receiving side of the silicon substrate 1 further includes a second doped silicon layer 6 and a second passivation layer 7 stacked sequentially. One of the first doped silicon layer 4 and the second doped silicon layer 6 is an N-type doped layer, and the other is a P-type doped layer. The solar cell also includes a first electrode 8 and a second electrode 9. The first electrode 8 passes through the first passivation layer 5 and forms an ohmic contact with the first doped silicon layer 4. The second electrode 9 passes through the second passivation layer 7 and forms an ohmic contact with the second doped silicon layer 6.
[0081] The conductive dopant element is either an N-type or a P-type conductive dopant element. The N-type conductive dopant element can be phosphorus, arsenic, etc., and the P-type conductive dopant element can be boron, gallium, etc. For example, the materials of the first doped silicon sublayer 41 and the second doped silicon sublayer 43 may specifically include doped polycrystalline silicon, doped amorphous silicon, or doped microcrystalline silicon, etc. For example, the first doped silicon sublayer 41 can be a first doped polycrystalline silicon sublayer, a first doped amorphous silicon sublayer, or a first doped microcrystalline silicon sublayer, and the second doped silicon sublayer 43 can be a second doped polycrystalline silicon sublayer, a second doped amorphous silicon sublayer, or a second doped microcrystalline silicon sublayer.
[0082] The silicon oxide layer 42 located between the first doped silicon sublayer 41 and the second doped silicon sublayer 43 can be a doped silicon oxide layer. The doped silicon oxide layer has the same conductive dopant element as the first doped silicon sublayer 41 and the second doped silicon sublayer 43. For example, when the conductive dopant element of the first doped silicon sublayer 41 and the second doped silicon sublayer 43 is phosphorus, the conductive dopant element of the doped silicon oxide layer is also phosphorus.
[0083] The materials of the first passivation layer 5 and the second passivation layer 7 independently include one or more combinations of silicon oxide, silicon oxynitride, silicon nitride, and aluminum oxide. For example, the first passivation layer 5 includes a silicon oxynitride layer and a silicon nitride layer sequentially stacked on the side of the first doped silicon layer 4 facing away from the silicon substrate 1. The second passivation layer 7 includes an aluminum oxide layer, a silicon oxynitride layer, and a silicon nitride layer sequentially stacked on the side of the second doped silicon layer 6 facing away from the silicon substrate 1.
[0084] Secondly, embodiments of this application provide a method for preparing a solar cell.
[0085] A method for fabricating a solar cell, referring to... Figures 3 to 4 This includes the following steps: A first dielectric layer 2 is fabricated on a silicon substrate 1, and the first dielectric layer 2 is brought into contact with the silicon substrate 1 to obtain the following: Figure 3 The structure shown has a first dielectric layer 2 that exhibits positive charge characteristics.
[0086] A second dielectric layer 3 is fabricated on the side of the first dielectric layer 2 facing away from the silicon substrate 1, resulting in the following... Figure 4 The structure is shown. The second dielectric layer 3 exhibits positive charge characteristics. The relative permittivity of the second dielectric layer 3 is greater than that of the first dielectric layer 2.
[0087] By sequentially fabricating the first dielectric layer 2 and the second dielectric layer 3 on the surface of the silicon substrate 1, the combination of the first dielectric layer 2 and the second dielectric layer 3 can be used to block hole diffusion while promoting electron transport, thereby improving the separation effect of holes and electrons, reducing carrier recombination, and improving the electron collection effect.
[0088] In some embodiments, the material of the first dielectric layer 2 includes a doped passivation material. The gas source used to prepare the doped passivation material includes a gas source containing a first dopant element and a gas source for depositing the passivation material, to form a doped passivation material containing the first dopant element. The electronegativity of the first dopant element is greater than 3; exemplarily, the first dopant element includes at least one of fluorine or chlorine. Using a gas source containing a first dopant element and a gas source for depositing the passivation material to prepare the first dielectric layer 2 facilitates uniform in-situ doping of the first dopant element during the film formation process.
[0089] The material of the second dielectric layer 3 includes doped alumina. The gas source used to prepare the doped alumina includes a gas source containing the second dopant element and a gas source for depositing alumina, to form doped alumina containing the second dopant element. Exemplarily, the second dopant element includes at least one of hafnium or zirconium. By using a gas source containing the second dopant element and a gas source for depositing alumina as raw materials for preparing the second dielectric layer 3, it is beneficial to achieve uniform doping of the second dopant element, forming a second dielectric layer 3 with better uniformity of second dopant element distribution, thereby improving the quality of the second dielectric layer 3.
[0090] In some embodiments, the gas source containing the first dopant element includes one or more combinations of CF4 and CCl4, and the gas source for depositing the passivation material includes a first oxygen source, which includes one or more combinations of N2O, H2O, and O2. Using CF4 or CCl4 as the gas source containing the first dopant element can effectively introduce fluorine or chlorine into the first dielectric layer 2. Using N2O, H2O, O2, etc. as the first oxygen source can oxidize the interface of the silicon substrate 1 and form a silicon oxide component. When the gas source containing the first dopant element and the gas source for depositing the passivation material are combined, fluorine-doped silicon oxide or chlorine-doped silicon oxide can be formed.
[0091] In some embodiments, the gas source containing the second dopant element includes one or more combinations of tetraethylmethylamine hafnium and tetraethylmethylamine zirconium. The gas source for depositing alumina includes an aluminum source and a second oxygen source. The aluminum source includes trimethylaluminum. The second oxygen source includes one or more combinations of H2O and O2. Tetraethylmethylamine hafnium or tetraethylmethylamine zirconium has excellent volatility, and using tetraethylmethylamine hafnium or tetraethylmethylamine zirconium as the gas source containing the second dopant element can effectively introduce hafnium or zirconium into the second dielectric layer 3. Using trimethylaluminum as the aluminum source and H2O, O2, etc. as the second oxygen source can form an alumina component. When the gas source containing the second dopant element and the gas source for depositing alumina are combined, hafnium-doped alumina or zirconium-doped alumina can be formed.
[0092] In some embodiments, the first dielectric layer 2 is prepared using plasma-enhanced chemical vapor deposition (PECVD), low-pressure chemical vapor deposition (LPCVD), atomic layer deposition (ALD), or plasma-enhanced ALD. Specifically, the method for preparing the first dielectric layer 2 using PECVD includes: introducing a gas source containing a first dopant element and a first oxygen source for reaction, wherein the ratio of the gas flow rate of the gas source containing the first dopant element to the gas flow rate of the first oxygen source is (50 sccm~350 sccm):(4000 sccm~15000 sccm), controlling the reaction temperature at 370℃~470℃, the reaction time at 50 s~120 s, the power at 11000 W~15000 W, and the power frequency at 60 Hz~150 Hz. By combining these parameters, a first dielectric layer 2 of excellent quality can be deposited. For example, the gas flow rate of the gas source containing the first doped element can be 50 sccm, 100 sccm, 200 sccm, 300 sccm, 350 sccm, etc., the gas flow rate of the first oxygen source can be 4000 sccm, 8000 sccm, 12000 sccm, 15000 sccm, etc., the reaction temperature for preparing the first dielectric layer 2 can be 370℃, 420℃, 470℃, etc., the reaction time can be 50 s, 80 s, 100 s, 120 s, etc., the power can be 11000 W, 13000 W, 15000 W, etc., and the power supply frequency can be 60 Hz, 80 Hz, 120 Hz, 150 Hz, etc.
[0093] The second dielectric layer 3 is prepared using atomic layer deposition (ALD) or plasma-enhanced atomic layer deposition (PELD). The ALD method involves introducing a gas source containing a second dopant element, a second oxygen source, and an aluminum source for reaction. The flow rate ratio of the gas source containing the second dopant element to the second oxygen source and the aluminum source is (3 sccm~10 sccm):(12 sccm~26 sccm):(15 sccm~40 sccm). The reaction temperature is controlled at 175℃~300℃, and the number of reaction cycles is 25~40. By combining these parameters, a high-quality second dielectric layer 3 can be deposited. For example, the gas flow rate of the gas source containing the second doped element can be 3 sccm, 6 sccm, 10 sccm, etc., the gas flow rate of the second oxygen source can be 12 sccm, 20 sccm, 26 sccm, etc., the gas flow rate of the aluminum source can be 15 sccm, 20 sccm, 30 sccm, 40 sccm, etc., the reaction temperature for preparing the second dielectric layer 3 is 175℃, 250℃, 300℃, etc., and the number of cycle reactions is 25 cycles, 30 cycles, 35 cycles, 40 cycles, etc.
[0094] Thirdly, this application provides a photovoltaic module.
[0095] A photovoltaic module includes a solar cell as mentioned in the first aspect or a solar cell prepared by the preparation method mentioned in the second aspect.
[0096] The technical solution of this application will be further described below with reference to the embodiments and accompanying drawings.
[0097] Example 1 This application provides a solar cell, which includes: Provide N-type monocrystalline silicon wafers and perform texturing treatment on the N-type monocrystalline silicon wafers to form a texturing structure on the entire surface of the N-type monocrystalline silicon wafers; A second boron-doped silicon layer is prepared on the light-receiving side of an N-type single-crystal silicon wafer using a boron diffusion method. At the same time as the second boron-doped silicon layer is prepared, a borosilicate glass layer is also formed on the side of the second boron-doped silicon layer away from the N-type single-crystal silicon wafer. Polishing is performed on the back surface and side edges of the N-type monocrystalline silicon wafer to remove the textured surface structure of the back surface and side edges of the N-type monocrystalline silicon wafer; A first dielectric layer is prepared on the back surface of an N-type single-crystal silicon wafer. The material of the first dielectric layer is fluorine-doped silicon oxide, and the thickness is 1 nm. The first dielectric layer is prepared by plasma chemical vapor deposition, which specifically includes: introducing N2O and CF4 to react, with the N2O gas flow rate being 8000 sccm, the CF4 gas flow rate being 150 sccm, the reaction temperature being 400℃, the reaction time being 80 s, the power being 13000 W, and the power supply frequency being 100 Hz. A second dielectric layer is prepared on the side of the first dielectric layer away from the N-type single-crystal silicon wafer. The material of the second dielectric layer is hafnium-doped aluminum oxide, and the thickness is 2 nm. The second dielectric layer is prepared by atomic layer deposition, specifically including: introducing trimethylaluminum, H2O and tetraethylmethylamine hafnium for reaction. The gas flow rate of trimethylaluminum is 25 sccm, the gas flow rate of H2O is 18 sccm, the gas flow rate of tetraethylmethylamine hafnium is 5 sccm, the reaction temperature is controlled at 230℃, and the reaction is cycled for 30 times. A first phosphorus-doped silicon layer is prepared on the side of the second dielectric layer facing away from the N-type single-crystal silicon wafer. Simultaneously, a phosphorus-silicon glass layer is formed on the side of the first phosphorus-doped silicon layer facing away from the N-type single-crystal silicon wafer. The first doped silicon layer comprises a first phosphorus-doped polycrystalline silicon sublayer, a doped silicon oxide layer, and a second phosphorus-doped polycrystalline silicon sublayer sequentially stacked on the second dielectric layer. The thickness of the first phosphorus-doped polycrystalline silicon sublayer is 7 nm, the thickness of the phosphorus-doped silicon oxide layer is 3 nm, and the thickness of the second phosphorus-doped polycrystalline silicon sublayer is 25 nm. The first phosphorus-doped silicon layer was prepared by plasma chemical vapor deposition, specifically including the following steps: 250 sccm of PH3 and 2500 sccm of SiH4 were introduced for reaction at a temperature of 385°C for 15 s, with a power of 13000 W and a power frequency of 250 Hz, resulting in a first phosphorus-doped amorphous silicon sublayer; then 8000 sccm of N2O was introduced to oxidize the surface of the first phosphorus-doped amorphous silicon sublayer at a temperature of 385°C for 12 s, with a power of 8000 W and a power frequency of 200 Hz, resulting in a doped silicon oxide layer; next, 350 sccm of PH3 and 2000 sccm of SiH4 were introduced for reaction at a temperature of 385°C for 200 s, with a power of 13000 W and a power frequency of 250 Hz, resulting in a second phosphorus-doped amorphous silicon sublayer, which was then annealed at 800°C~920°C for 120 minutes. min, the first phosphorus-doped amorphous silicon sublayer is transformed into the first phosphorus-doped polycrystalline silicon sublayer, and the second phosphorus-doped amorphous silicon sublayer is transformed into the second phosphorus-doped polycrystalline silicon sublayer. Wet chemical cleaning (RCA cleaning) is performed, which involves passing through an alkaline cleaning tank and an acid cleaning tank in sequence. By controlling the etching process of the RCA cleaning process, the coating layer generated on the light-receiving surface of the N-type single crystal silicon wafer, such as the first dielectric layer, the second dielectric layer, and the first phosphorus-doped silicon layer, is removed. Acid washing with hydrofluoric acid solution is used to remove the borosilicate glass layer on the second boron-doped silicon layer and the phosphorus-silicon glass layer on the surface of the first phosphorus-doped silicon layer. A light-receiving alumina layer and a light-receiving silicon nitride layer are prepared on the surface of the second boron-doped silicon layer away from the N-type single crystal silicon wafer. The light-receiving alumina layer is prepared by atomic layer deposition and has a thickness of 5 nm, while the light-receiving silicon nitride layer is prepared by plasma chemical vapor deposition and has a thickness of 70 nm. A backlight silicon nitride layer is prepared on the surface of the first phosphorus-doped silicon layer away from the N-type single crystal silicon wafer. The backlight silicon nitride layer is prepared by plasma chemical vapor deposition and has a thickness of 100 nm. The first electrode and the second electrode are prepared by screen printing. The first electrode forms an ohmic contact with the first phosphorus-doped silicon layer, and the second electrode forms an ohmic contact with the second boron-doped silicon layer.
[0098] Example 2 This application provides a solar cell, which differs from Embodiment 1 in that: the material of the first dielectric layer is chlorine-doped silicon oxychloride, and the first dielectric layer is prepared by plasma chemical vapor deposition, specifically including: introducing N2O and CCl4 to react, the N2O gas flow rate is 8000 sccm, the CCl4 gas flow rate is 150 sccm, the reaction temperature is 400℃, the reaction time is 80 s, the power is 13000 W, and the power frequency is 100 Hz, the rest is the same as Embodiment 1.
[0099] Example 3 This application provides a solar cell, which differs from Example 1 in that: the material of the first dielectric layer is fluorine-doped aluminum oxide, and the first dielectric layer is prepared by atomic layer deposition, specifically including: introducing trimethylaluminum, H2O and CF4 for reaction, the gas flow rate of trimethylaluminum is 25 sccm, the gas flow rate of H2O is 18 sccm, the gas flow rate of CF4 is 2 sccm, the reaction temperature is controlled at 230℃, and the reaction is cycled for 15 times, the rest is the same as Example 1.
[0100] Example 4 This application provides a solar cell, which differs from Example 1 in that: the material of the second dielectric layer is zirconium-doped aluminum oxide, and the second dielectric layer is prepared by atomic layer deposition, specifically including: introducing trimethylaluminum, H2O and tetraethylmethylamine zirconium for reaction, the gas flow rate of trimethylaluminum is 25 sccm, the gas flow rate of H2O is 18 sccm, the gas flow rate of tetraethylmethylamine zirconium is 5 sccm, the reaction temperature is controlled at 230℃, and the reaction is cycled for 30 times; the rest is the same as Example 1.
[0101] Comparative Example 1 This application provides a comparative example of a solar cell, which differs from Example 1 in that a silicon oxide layer is used instead of the combination of the first dielectric layer and the second dielectric layer, while the rest remains the same as Example 1.
[0102] Comparative Example 2 This application provides a comparative example of a solar cell, which differs from Embodiment 1 in that: only a first dielectric layer is provided and the thickness of the first dielectric layer is increased to 3 nm, and a second dielectric layer is not provided, while the rest is the same as Embodiment 1.
[0103] Comparative Example 3 This application provides a comparative example of a solar cell, which differs from Example 1 in that: only a second dielectric layer is provided and the thickness of the second dielectric layer is increased to 3 nm, and a first dielectric layer is not provided, while the rest is the same as Example 1.
[0104] Comparative Example 4 This application provides a comparative example of a solar cell, which differs from Example 1 in that: hafnium-doped aluminum oxide is used as the material of the first dielectric layer, and fluorine-doped silicon oxide is used as the material of the second dielectric layer; otherwise, it remains the same as Example 1.
[0105] Experiment 1 TOF-SIMS was used to test the content of the first dopant element in the first dielectric layer and the content of the second dopant element in the second dielectric layer in the above embodiments and comparative examples. In Embodiment 2, the first dopant element was Cl; in all other embodiments and comparative examples except Embodiment 2, the first dopant element was F. In Embodiment 4, the second dopant element was zirconium; in all other embodiments and comparative examples except Embodiment 4, the second dopant element was hafnium.
[0106] Experiment 2 The fixed positive charge density of the first and second dielectric layers in the above embodiments and comparative examples was tested using the CV method.
[0107] Experiment 3 The relative permittivity of the first and second dielectric layers in the above embodiments and comparative examples was tested using the CV method.
[0108] Experiment 4 The interface state density of the silicon substrates in the above embodiments and comparative examples was tested using a high-frequency-quasi-static CV combined method.
[0109] Experiment 5 The performance of solar cells was tested using the Wavelabs solar simulator under the following conditions: AM1.5, 1000 W / m. 2 The test environment temperature was 25℃. Before testing, the light source was calibrated to simulate sunlight intensity using a standard silicon cell. The open-circuit voltage (Voc), short-circuit current (Jsc), fill factor (FF), and photoelectric conversion efficiency (Eff) of the corresponding solar cells were recorded.
[0110] Table 1 lists the materials used in the first and second dielectric layers of the above embodiments and comparative examples, and records the test results of Experiments 1 to 4. The test results of Experiment 5 are recorded in Table 2.
[0111] Table 1
[0112] Table 2
[0113] A comparison of the data from Examples 1 to 4 with Comparative Example 1 in Tables 1 and 2 shows that, compared to a single silicon oxide layer, Examples 1 to 4, which use a combination of a first dielectric layer and a second dielectric layer, have a lower interface state density, and all electrical performance data of the solar cell are significantly improved. This demonstrates that by using a first dielectric layer with a positive charge density and a relatively low permittivity as the film layer directly in contact with the silicon substrate, and a second dielectric layer with a relatively high permittivity and positive charge characteristics, and through the synergistic cooperation of the first and second dielectric layers, holes can be blocked more effectively, carrier separation at the interface of the N-type monocrystalline silicon wafer can be promoted, and the interface state density of the first and second dielectric layers can be controlled within a low range, effectively reducing carrier recombination and further improving the electrical performance of the solar cell.
[0114] A comparison of the data from Example 1 with Comparative Examples 2 and 3 shows that when only the first or second dielectric layer is used, the hole blocking and carrier separation effects are limited, resulting in a still high interface state density, significant carrier recombination, and low electrical performance data for the solar cell. However, when a combination of the first and second dielectric layers is used, a significant synergistic effect is achieved. Specifically, the first dielectric layer with a high fixed positive charge density constructs the basic built-in electric field, while the second dielectric layer with a high relative permittivity amplifies this electric field effect through capacitive coupling, inducing a higher equivalent positive charge density. Together, they form a steep band bend and a stronger hole barrier, thereby significantly improving electron transport and hole blocking capabilities and further enhancing the electrical performance of the solar cell.
[0115] A comparison of the data from Example 1 and Comparative Example 4 shows that the stacking order of the first and second dielectric layers on the surface of the N-type monocrystalline silicon wafer is crucial to the battery performance. When the first dielectric layer is in direct contact with the surface of the N-type monocrystalline silicon wafer and the second dielectric layer is located outside the first dielectric layer, the synergistic effect of the first and second dielectric layers can be more effectively utilized, further reducing the interface state density of the N-type monocrystalline silicon wafer. Its high-density fixed positive charge can also directly act on the silicon substrate to form a better basic bandgap. Furthermore, the high dielectric constant of the second dielectric layer further enhances the bandgap through capacitive coupling, achieving excellent hole blocking and carrier separation effects. Even when the order of the two layers is reversed as shown in Comparative Example 4, with the second dielectric layer and the first dielectric layer sequentially placed on the N-type monocrystalline silicon wafer, the measured interface state density of the N-type monocrystalline silicon wafer remains high. This is because: on the one hand, the second dielectric layer with a high relative permittivity is in direct contact with the silicon substrate, which will generate a large number of unsaturated "dangling bonds" and structural defects at the interface due to lattice mismatch and poor chemical bond matching, thereby introducing a high density of interface defect states and significantly increasing carrier recombination; on the other hand, the isolation between the first dielectric layer and the N-type single crystal silicon wafer will cause the electric field generated by its high density of fixed positive charges to be severely attenuated, weakening the hole blocking effect, and ultimately causing a significant decrease in the electrical performance of the solar cell.
[0116] The technical solutions disclosed in the embodiments of this application have been described in detail above. Specific examples have been used to illustrate the principles and implementation methods of this application. The descriptions of the embodiments above are only for the purpose of helping to understand the technical solutions and core inventive points of the embodiments of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.
Claims
1. A solar cell, characterized in that, Includes a silicon substrate, on the surface of which a first dielectric layer and a second dielectric layer are stacked, the first dielectric layer being in contact with the surface of the silicon substrate, and the second dielectric layer being located on the side of the first dielectric layer away from the silicon substrate; The first dielectric layer and the second dielectric layer exhibit positive charge characteristics; The relative permittivity of the second dielectric layer is greater than that of the first dielectric layer.
2. The solar cell according to claim 1, characterized in that, The fixed positive charge density of the first dielectric layer is greater than that of the second dielectric layer.
3. The solar cell according to claim 2, characterized in that, The sum of the fixed positive charge density of the first dielectric layer and the fixed positive charge density of the second dielectric layer is 1.5 × 10⁻⁶. 12 cm -2 ~6×10 12 cm -2 .
4. The solar cell according to claim 3, characterized in that, The fixed positive charge density of the first dielectric layer is 1×10 12 cm -2 ~5×10 12 cm -2 The fixed positive charge density of the second dielectric layer is 0.5 × 10⁻⁶. 12 cm -2 ~2×10 12 cm -2 .
5. The solar cell according to claim 1, characterized in that, The relative permittivity of the second dielectric layer is 10 to 25, and / or the relative permittivity of the first dielectric layer is 7 to 9.
6. The solar cell according to claim 5, characterized in that, The interface state density between the material of the first dielectric layer and the silicon substrate is 0.5 × 10⁻⁶. 10 eV -1 ·cm -2 ~8×10 10 eV -1 ·cm -2 The carrier recombination velocity at the interface between the silicon substrate and the first dielectric layer is 15 cm / s to 25 cm / s.
7. The solar cell according to claim 1, characterized in that, The sum of the conduction band offset of the first dielectric layer and the conduction band offset of the second dielectric layer is greater than 3.5 eV, and the sum of the valence band offset of the first dielectric layer and the valence band offset of the second dielectric layer is greater than 6 eV.
8. The solar cell according to claim 1, characterized in that, The material of the first dielectric layer includes a doped passivation material, which includes a first doping element and a passivation material. The electronegativity of the first doping element is greater than or equal to 3, and the passivation material includes one or more combinations of silicon oxide, silicon oxynitride, silicon carbide, and aluminum oxide.
9. The solar cell according to claim 8, characterized in that, In the doped passivation material, the content of the first dopant element is 0.05 wt%~0.75 wt%; And / or, The first doping element includes at least one of fluorine or chlorine; And / or, The thickness of the first dielectric layer is 1 nm to 5 nm.
10. The solar cell according to claim 1, characterized in that, The material of the second dielectric layer includes doped aluminum oxide, wherein the doped aluminum oxide comprises a second doping element and aluminum oxide, and the second doping element comprises at least one of hafnium or zirconium.
11. The solar cell according to claim 10, characterized in that, In the doped alumina, the content of the second doping element is 10 wt%~50 wt%; And / or, The thickness of the second dielectric layer is 1 nm to 5 nm.
12. The solar cell according to claim 1, characterized in that, The solar cell also includes: A first doped silicon layer is disposed on the side of the second dielectric layer away from the silicon substrate, and the thickness of the first doped silicon layer is 32 nm to 65 nm.
13. The solar cell according to claim 12, characterized in that, The first doped silicon layer includes a first doped silicon sublayer, a silicon oxide layer, and a second doped silicon sublayer, which are sequentially stacked on the side of the second dielectric layer away from the silicon substrate. The thickness of the first doped silicon sublayer is 5 nm to 15 nm, the thickness of the silicon oxide layer is 2 nm to 5 nm, and the thickness of the second doped silicon sublayer is 25 nm to 45 nm. The surface doping concentration of the conductive dopant element in the second doped silicon sublayer is greater than that in the first doped silicon sublayer, and the surface doping concentration of the conductive dopant element in the second doped silicon sublayer is 1×10⁻⁶. 19 cm -3 ~9×10 21 cm -3 .
14. A method for preparing a solar cell, characterized in that, Includes the following steps: A first dielectric layer is fabricated on a silicon substrate, such that the first dielectric layer is in contact with the silicon substrate, and the first dielectric layer has a positive charge characteristic. A second dielectric layer is prepared on the side of the first dielectric layer away from the silicon substrate. The second dielectric layer has positive charge characteristics and its relative permittivity is greater than that of the first dielectric layer.
15. The method for preparing a solar cell according to claim 14, characterized in that, The material of the first dielectric layer includes a doped passivation material. The gas source used to prepare the doped passivation material includes a gas source containing a first dopant element and a gas source for depositing the passivation material, so as to form the doped passivation material containing the first dopant element. The electronegativity of the first dopant element is greater than or equal to 3. The first dopant element includes at least one of fluorine or chlorine. The material of the second dielectric layer includes doped alumina. The gas source used to prepare the doped alumina includes a gas source containing a second dopant element and a gas source for depositing alumina, so as to form the doped alumina containing the second dopant element, wherein the second dopant element includes at least one of hafnium or zirconium.
16. The method for preparing a solar cell according to claim 15, characterized in that, The gas source containing the first doped element includes one or more combinations of CF4 and CCl4, and the gas source for depositing passivation material includes a first oxygen source, which includes one or more combinations of N2O, H2O, and O2. The gas source containing the second doping element includes one or more combinations of tetraethylmethylamine hafnium and tetraethylmethylamine zirconium, the gas source for depositing alumina includes an aluminum source and a second oxygen source, the aluminum source includes trimethylaluminum, and the second oxygen source includes one or two combinations of H2O and O2.
17. The method for preparing a solar cell according to claim 16, characterized in that, The first dielectric layer is prepared by plasma chemical vapor deposition, low-pressure chemical vapor deposition, atomic layer deposition, or plasma-enhanced atomic layer deposition. The method for preparing the first dielectric layer using plasma chemical vapor deposition includes: introducing a gas source containing a first dopant element and a first oxygen source to react, wherein the ratio of the gas flow rate of the gas source containing the first dopant element to the gas flow rate of the first oxygen source is (50 sccm~350 sccm):(4000 sccm~15000 sccm), controlling the reaction temperature at 370℃~470℃, the reaction time at 50 s~120 s, the power at 11000 W~15000 W, and the power frequency at 60 Hz~150 Hz. The second dielectric layer is prepared by atomic layer deposition or plasma-enhanced atomic layer deposition. The method for preparing the second dielectric layer by atomic layer deposition includes: introducing the gas source containing the second dopant element, the second oxygen source, and the aluminum source to carry out a reaction, wherein the gas flow rate ratio of the gas source containing the second dopant element, the second oxygen source, and the aluminum source is (3 sccm~10 sccm):(12 sccm~26 sccm):(15 sccm~40 sccm), controlling the reaction temperature at 175℃~300℃, and the number of reaction cycles is 25~40.
18. A photovoltaic module, characterized in that, This includes solar cells as described in any one of claims 1-13 or solar cells prepared by any one of claims 14-17.