A method and structure for fabricating a top-emitting microcavity RGB planar anode to reduce short circuits.

By using pixel isolation layer and insulating layer technology in OLED displays, the short circuit problem caused by inconsistent anode thickness in RGB microcavity and tungsten plug roughness was solved, achieving high-quality display effect and reliable packaging.

CN123124635APending Publication Date: 2026-11-17KUNMING INST OF PHYSICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611226484.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The inconsistent thickness of the anode in traditional RGB microcavity systems leads to a stepped structure, affecting process uniformity and packaging reliability. Tungsten plug roughness causes electric field concentration, resulting in short circuits, and electrical and optical crosstalk between pixels reduces display quality.

Method used

Using pixel isolation layer and insulating layer technology, isolation pillars are formed through photolithography and etching. The thickness of the conductive layer of the RGB anode is adjusted to achieve different microcavity lengths. An insulating layer is covered on the surface of the tungsten plug to isolate roughness and reduce crosstalk.

Benefits of technology

It effectively reduces short circuits, improves display yield and quality, enhances packaging reliability, reduces inter-pixel crosstalk, and achieves process reliability for planar anodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124635A_ABST
    Figure CN123124635A_ABST
Patent Text Reader

Abstract

This invention discloses a method and structure for fabricating a top-emitting microcavity RGB planar anode to reduce short circuits, relating to the field of microelectronic OLED display technology. The method includes the following steps: depositing a pixel separator layer: depositing a pixel separator layer across the entire surface of a CMOS substrate; forming pixel separator pillars: using photolithography and etching to ensure the separator pillars are tightly attached to the edge of the tungsten plug; depositing RGB anodes: fabricating R, G, and B anodes using photolithography and film deposition respectively, adjusting the length of the anodes to achieve different microcavity lengths while maintaining a consistent total thickness; depositing a short-circuit protection layer: depositing an insulating layer across the entire surface of the RGB anode, followed by photolithography and etching to complete the short-circuit protection layer; depositing light-emitting units and a cathode: sequentially evaporating each light-emitting unit and the common cathode. The method described in this invention, through the pixel separator pillars and planar anode structure, effectively prevents short circuits caused by the roughness of the tungsten plug surface, while simultaneously achieving independent RGB microcavity adjustment, improving inter-pixel crosstalk, and enhancing device yield and display uniformity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of microelectronic OLED display technology, and in particular to a method and structure for fabricating a top-emitting microcavity RGB planar anode to reduce short circuits. Background Technology

[0002] In OLED devices, the top-emitting structure often employs the microcavity effect to improve luminescence purity and efficiency.

[0003] However, traditional RGB microcavity anodes have different optimal cavity lengths for each color, resulting in inconsistent anode thickness and a stepped structure, which affects the uniformity of subsequent processes and the reliability of packaging.

[0004] Meanwhile, the tungsten plugs on the CMOS driver substrate are rough. Due to the columnar crystal growth mode and chemical polishing process, the surface roughness of the tungsten plugs is relatively large. After the anode is deposited, the rough morphology is easily replicated, causing local electric field concentration and leading to short circuit of the device.

[0005] In addition, electrical crosstalk and optical crosstalk between pixels can also reduce display quality.

[0006] Therefore, there is an urgent need for an anode structure and its preparation method that can solve the above problems simultaneously. Summary of the Invention

[0007] To address the above problems, this invention discloses a method and structure for preparing a top-emitting microcavity planar anode that reduces short circuits. This method allows for individual adjustment of the length of microcavities of different colors while reducing short circuits.

[0008] The technical solution proposed in this invention is as follows: As one aspect of this invention, a method for fabricating a top-emitting microcavity RGB planar anode to reduce short circuits, the fabrication method comprising the following steps: Step S1, Deposit isolation layer: Deposit a pixel isolation layer (4) on the entire surface of the CMOS driving substrate (1) with tungsten plug (2); Step S2, forming pixel isolation pillars: photolithography + etching, so that the isolation pillars are in close contact with the edge of the tungsten plug; Step S3, depositing RGB anodes: R, G, and B anodes are prepared respectively. The RGB anode is composed of an underlay conductive layer, a reflective conductive layer, and a transparent conductive layer. Different microcavity lengths are achieved by adjusting the thickness of the underlay conductive layer and the transparent conductive layer, while keeping the total thickness of the RGB anode the same. Step S4, Deposit short-circuit protection layer: Deposit an insulating layer on the RGB anode surface to cover the tungsten plug and anode edge; Step S5: Deposit light-emitting units and cathode on the planar anode surface: Sequentially vapor-deposit each light-emitting unit and the common cathode.

[0009] Step S1 includes the pixel isolation layer material being a high dielectric insulating layer, using one of silicon oxide, silicon nitride, or silicon oxynitride.

[0010] Step S2 includes performing photolithography and dry etching on the surface of the entire pixel isolation layer to prepare isolation pillars 4, with one side of the bottom of the isolation pillars close to the top edge of the tungsten plug, and the two just making contact.

[0011] Step S3 includes preparing RGB anodes with different cavity lengths by repeatedly performing photolithography and coating processes according to different emission wavelengths corresponding to different microcavity lengths. The total thickness of the RGB anodes is the same, and the thickness of the reflective conductive layer is the same. The only difference is that the thickness of the base adhesive conductive layer and the transparent conductive layer that constitute the anodes are different, resulting in different cavity lengths.

[0012] Step S3 includes the following: the R anode is composed of a base adhesive conductive layer (53), a reflective conductive layer (63), and a transparent conductive layer (73); the G anode is composed of a base adhesive conductive layer (52), a reflective conductive layer (62), and a transparent conductive layer (72); and the B anode is composed of a base adhesive conductive layer (51), a reflective conductive layer (61), and a transparent conductive layer (71).

[0013] Step S3 includes the following: the total thickness of the anode is 50-150 nm.

[0014] Step S3 includes the following: the reflective conductive layer is composed of one or more highly reflective conductive materials such as aluminum silver (Ag), aluminum (Al), and platinum (Pt); the base adhesive conductive layer is composed of one or more of chromium (Cr), titanium (Ti), nickel (Ni), and tantalum (Ta); and the transparent anode is composed of one or more of indium tin oxide (ITO) and indium zinc oxide (IZO).

[0015] Step S4 includes preparing an insulating layer as a short-circuit protection layer after RGB anodizing, covering the rough surface of the tungsten plug. The insulating layer has the function of reducing short circuits, and while covering the rough surface of the tungsten plug to reduce short circuits, it also isolates the lateral electrical crosstalk between pixels and improves the color gamut.

[0016] Step S4 includes the following: the insulating layer material is one of silicon oxide, silicon nitride, or silicon oxynitride.

[0017] Step S4 includes the following: the thickness of the insulating layer is 80-200 nm.

[0018] Step S5 includes depositing blue light-emitting unit (9), CGL (10), green light-emitting unit (11), CGL (12), red light-emitting unit (13) and common cathode (14) sequentially on the surface of the planar anode using organic vapor deposition technology. The light-emitting unit is composed of an electron injection layer, an electron transport layer, a light-emitting layer, a hole transport layer, and a hole injection layer. CGL is a charge generation layer.

[0019] As another aspect of the present invention, a top-emitting microcavity RGB planar anode structure with reduced short circuits is prepared by the top-emitting microcavity RGB planar anode preparation method of the present invention.

[0020] The structure of the top-emitting microcavity RGB planar anode that reduces short circuits includes: (a1): CMOS driving substrate: driving substrate with tungsten plugs; (a2): Pixel isolation pillar: The pixel isolation layer located at the edge of the tungsten plug is made of a high dielectric insulating material, one of silicon oxide, silicon nitride or silicon oxynitride, and is formed by photolithography etching. The bottom side of the isolation pillar is in contact with the edge of the tungsten plug. (a3): RGB planar anode: It consists of an adhesive conductive layer, a reflective conductive layer, and a transparent conductive layer. The adhesive conductive layer is made of Ti / Ni / Cr / Ta, the reflective conductive layer is made of Ag / Al / Pt, and the transparent conductive layer is made of ITO / IZO. (a4): Short-circuit protection insulation layer: covering the tungsten plug and the edge of the anode, with a thickness of 80-200nm, and the material is silicon oxide / silicon nitride / silicon oxynitride, while preventing electrical crosstalk; (a5): Light-emitting stack: Blue light-emitting unit, charge generation layer, green light-emitting unit, charge generation layer, red light-emitting layer, and semi-transparent cathode are deposited sequentially.

[0021] Technical effects and advantages of the present invention: 1. Tungsten plug isolation technology: Tungsten plugs are placed at the edge of the pixel and isolated by an insulating layer to prevent short circuits caused by surface roughness, thereby improving yield. 2. The use of an insulating isolation layer can reduce electrical crosstalk between pixels; 3. Solves the problem of high and low anode fluctuations in traditional RGB displays, reduces short circuits and crosstalk issues in components, and improves display yield and quality; 4. Planar anodes make subsequent anode processes more reliable and improve packaging reliability. They can be perfectly matched with microlens arrays, which is beneficial for subsequent process integration. Attached Figure Description

[0022] Figure 1 : A schematic diagram of a top-emitting microcavity RGB planar anode structure for reducing short circuits according to the present invention; Figure 2 The present invention provides a method for fabricating a top-emitting microcavity RGB planar anode with reduced short circuits, and a structural process flow diagram. Figure 3 Top view of a top-emitting microcavity RGB planar anode structure for reducing short circuits according to the present invention.

[0023] The numbers in the figure are as follows: 1-COMS driving substrate, 2-tungsten plug, 3-tungsten plug surface roughness, 4-pixel isolation layer, 9-blue light-emitting unit, 10-charge generation layer CGL, 11-green light-emitting unit, 12-charge generation layer CGL, 13-red light-emitting unit, 14-common cathode, 51-B anode undercoating conductive layer, 52-G anode undercoating conductive layer, 53-R anode undercoating conductive layer, 61-R anode reflective conductive layer, 62-G anode reflective conductive layer, 63-R anode reflective conductive layer, 71-R anode transparent conductive layer, 72-G anode transparent conductive layer, 73-R anode transparent conductive layer, 81, 82, 83-short circuit protection layer. Detailed Implementation

[0024] The technical solutions and advantages of the present invention will be further described below with reference to the accompanying drawings and embodiments.

[0025] like Figure 1 As shown, a method and structure for fabricating a top-emitting microcavity RGB planar anode with reduced short circuits includes: depositing isolation pillars 4 on a CMOS driving substrate 1 including a tungsten plug 2 (tungsten plug surface rough morphology 3); depositing an adhesion layer (51, 52, 53), a reflective layer (61, 62, 63), and a transparent microcavity anode (71, 72, 73) between the isolation pillars in sequence. These three layers constitute a complete anode. Depositing an anti-short circuit layer (81, 82, 83) near the edge of the anode close to the tungsten plug. This anti-short circuit layer covers the uneven surface caused by the replication of the tungsten plug. Depositing a blue light-emitting unit (9), a CGL (10), a green light-emitting unit (11), a CGL (12), a red light-emitting unit (13), and a common cathode (14) in sequence on the anode surface.

[0026] 1. Structural Composition CMOS driver substrate: Driver substrate with tungsten plugs; Pixel isolation pillars: Pixel isolation layers (high dielectric insulating material, such as silicon oxide) located at the edge of the tungsten plug are formed by photolithography etching, with one side of the bottom of the isolation pillar contacting the edge of the tungsten plug; RGB planar anode: composed of an adhesion layer (Ti / Ni / Cr, etc.), a reflective layer (Ag / Al / Pt, etc.), and a transparent conductive layer (ITO / IZO); Short-circuit protection insulation layer: covering the tungsten plug and anode edge, with a thickness of 80-200nm, and the material is silicon oxide / silicon nitride / silicon oxynitride, while preventing electrical crosstalk; Light-emitting stack: Blue light-emitting unit, charge generation layer, green light-emitting unit, charge generation layer, red light-emitting layer, and semi-transparent cathode are deposited sequentially.

[0027] A pixel isolation layer is deposited over the entire surface of a CMOS substrate;

[0028] 2. Preparation method Deposited isolation layer: A pixel isolation layer is deposited over the entire surface of the CMOS substrate; Forming pixel isolation pillars: photolithography + etching, making the isolation pillars closely adhere to the edge of the tungsten plug; RGB anode deposition: R, G, and B anodes are prepared separately. Different microcavity lengths are achieved by adjusting the adhesion and conductive thickness of the transparent anode, while maintaining a consistent total thickness.

[0029] Deposited short-circuit protection layer: An insulating layer is deposited on the surface of the RGB anode, covering the tungsten plug and the edge of the anode.

[0030] Deposition of light-emitting units and cathode: Each light-emitting unit and the common cathode are deposited sequentially by vapor deposition.

[0031] Example 1: A method and structure for fabricating a top-emitting microcavity RGB planar anode to reduce short circuits, comprising the following steps: Step A: A pixel isolation layer 4 is deposited on the entire surface of the CMOS driving substrate 1 with tungsten plug 2 (tungsten plug surface rough morphology 3) using chemical vapor deposition or physical deposition. The isolation layer material is silicon oxide, and the thickness is about 50-150nm, which is comparable to the maximum thickness of the anode.

[0032] Step B: Photolithography techniques such as coating, exposure, and development are used on the surface where the pixel isolation layer is deposited to expose the anode position.

[0033] Step C: The exposed silicon oxide is etched using etching technology. After etching, photoresist cleaning is performed, and isolation pillars are formed. Plasma-enhanced chemical etching is used. The etching gases used in the process are fluorine-based gases, SF6, CHF3, and Ar. The gas flow rates are 20-45 scm, 10-30 scm, and 50-60 scm, and the etching temperature is 40-60℃.

[0034] Step D: Apply adhesive, expose, and develop the substrate with isolation pillars to reveal the position of the B anode pattern.

[0035] Step E: Deposit anode B by sequentially depositing Ti, Al, and ITO using magnetron sputtering. The thickness is adjusted according to the microcavity enhancement requirements, ranging from 50 to 150 nm.

[0036] Step F: Photoresist peeling, Step B: Anodizing.

[0037] Step G: Apply adhesive, expose, and develop the substrate with B anode to reveal the position of G anode pattern.

[0038] Step H: Deposit anode G by sequentially depositing Ti, Al, and ITO using magnetron sputtering. The thickness is adjusted according to the microcavity enhancement requirements, ranging from 50 to 150 nm.

[0039] Step I: Photoresist peeling, B anodizing.

[0040] Step J: Apply adhesive, expose, and develop the substrate that already has B and G anodes to reveal the R anode pattern position.

[0041] Step K: Deposit anode R by sequentially depositing Ti, Al, and ITO using magnetron sputtering. The thickness is adjusted according to the microcavity enhancement requirements, ranging from 50 to 150 nm.

[0042] Step L: Photoresist peeling, R anodizing.

[0043] Step M: After the RGB anode is prepared, a layer of silicon oxide with a thickness of 80-200 nm is deposited on the entire surface using plasma-enhanced chemical vapor deposition.

[0044] Step N: Photolithography, resist coating, and development are performed on the substrate with deposited silicon oxide to expose the anode area. The anode sub-pixel is 12μm long and 4μm wide, and the tungsten plug is 0.5μm long and wide. After photoresist formation, the exposed anode sub-pixel area is 11μm and 3μm, and the tungsten plug is located at the edge of the anode.

[0045] Step P: Etch the exposed silicon oxide using etching technology. The process steps are similar to those in Step C and will not be repeated here. After etching, the silicon oxide should just cover the tungsten plug location. Figure 3 As shown.

[0046] Step Q: Photoresist peeling, short-circuit protection isolation layer preparation completed.

[0047] Step R: On the planar anode surface with a short-circuit protection isolation layer, blue light-emitting unit (9), CGL (10), green light-emitting unit (11), CGL (12), red light-emitting unit (13) and common cathode (14) are deposited sequentially using organic vapor deposition technology to complete the device fabrication.

[0048] The light-emitting unit is composed of an electron injection layer, an electron transport layer, a light-emitting layer, a hole transport layer, and a hole injection layer. The CGL is a charge generation layer. Organic evaporation is a common practice in the industry and will not be described in detail here.

Claims

1. A method for fabricating a top-emission microcavity RGB planar anode with reduced short-circuit, comprising: The preparation method includes the following steps: ​ Step S1, Deposit isolation layer: Deposit a pixel isolation layer (4) on the entire surface of the CMOS driving substrate (1) with tungsten plug (2); Step S2, forming pixel isolation pillars: photolithography + etching, so that the isolation pillars are in close contact with the edge of the tungsten plug; Step S3, depositing RGB anodes: R, G, and B anodes are prepared respectively. The RGB anode is composed of an underlay conductive layer, a reflective conductive layer, and a transparent conductive layer. Different microcavity lengths are achieved by adjusting the thickness of the underlay conductive layer and the transparent conductive layer, while keeping the total thickness of the RGB anode the same. Step S4, Deposit short-circuit protection layer: Deposit an insulating layer on the RGB anode surface to cover the tungsten plug and anode edge; Step S5: Deposit light-emitting units and cathode on the planar anode surface: Sequentially vapor-deposit each light-emitting unit and the common cathode.

2. A method of fabricating a top emission microcavity RGB planar anode with reduced short circuit according to claim 1, wherein: Step S1 includes the pixel isolation layer material being a high dielectric insulating layer, which is one of silicon oxide, silicon nitride, or silicon oxynitride. Step S2 includes performing photolithography and dry etching on the surface of the entire pixel isolation layer to prepare isolation pillar 4, with one side of the bottom of the isolation pillar close to the top edge of the tungsten plug, and the two just in contact; Step S4 includes the following: the thickness of the insulating layer is 80-200 nm.

3. A method of fabricating a top emission microcavity RGB planar anode with reduced short circuit according to claim 1, wherein: Step S3 includes the following: the R anode is composed of a base adhesive conductive layer (53), a reflective conductive layer (63), and a transparent conductive layer (73); the G anode is composed of a base adhesive conductive layer (52), a reflective conductive layer (62), and a transparent conductive layer (72); and the B anode is composed of a base adhesive conductive layer (51), a reflective conductive layer (61), and a transparent conductive layer (71).

4. The method for fabricating a top-emitting microcavity RGB planar anode with reduced short circuits according to claim 1, characterized in that: Step S3 includes preparing RGB anodes with different cavity lengths by repeatedly performing photolithography and coating processes according to different emission wavelengths corresponding to different microcavity lengths. The total thickness of the RGB anodes is the same, and the thickness of the reflective conductive layer is the same. The only difference is that the thickness of the base conductive layer and the transparent conductive layer that constitute the anodes are different, resulting in different cavity lengths. Step S3 includes that the total thickness of the anodes is 50-150nm.

5. A method of fabricating a top emission microcavity RGB planar anode with reduced short circuit according to claim 1, wherein: Step S3 includes the following: the reflective conductive layer is composed of one or more highly reflective conductive materials such as aluminum silver (Ag), aluminum (Al), and platinum (Pt); the base adhesive conductive layer is composed of one or more of chromium (Cr), titanium (Ti), nickel (Ni), and tantalum (Ta); and the transparent anode is composed of one or more of indium tin oxide (ITO) and indium zinc oxide (IZO).

6. A method of fabricating a top emission microcavity RGB planar anode with reduced short circuit according to claim 1, wherein: Step S4 includes preparing an insulating layer as a short-circuit protection layer after RGB anodizing, covering the rough surface of the tungsten plug. The insulating layer has the function of reducing short circuits, and while covering the rough surface of the tungsten plug to reduce short circuits, it also isolates the lateral electrical crosstalk between pixels and improves the color gamut.

7. A method of fabricating a top emission microcavity RGB planar anode with reduced short circuit according to claim 1, wherein: Step S4 includes the following: the insulating layer material is one of silicon oxide, silicon nitride, or silicon oxynitride.

8. A method of fabricating a top emission microcavity RGB planar anode with reduced short circuit according to claim 1, wherein: Step S5 includes depositing blue light-emitting unit (9), CGL (10), green light-emitting unit (11), CGL (12), red light-emitting unit (13) and common cathode (14) sequentially on the surface of the planar anode using organic vapor deposition technology. The light-emitting unit is composed of an electron injection layer, an electron transport layer, a light-emitting layer, a hole transport layer, and a hole injection layer. CGL is a charge generation layer.

9. A top-emitting microcavity RGB planar anode structure with reduced short circuits prepared by the top-emitting microcavity RGB planar anode preparation method according to any one of claims 1-11.

10. A short current reduced top emission microcavity RGB planar anode structure according to claim 12, wherein: The structure of the top-emitting microcavity RGB planar anode that reduces short circuits includes: (a1): CMOS driving substrate: driving substrate with tungsten plugs; (a2): Pixel isolation pillar: The pixel isolation layer located at the edge of the tungsten plug is made of a high dielectric insulating material, one of silicon oxide, silicon nitride or silicon oxynitride, and is formed by photolithography etching. The bottom side of the isolation pillar is in contact with the edge of the tungsten plug. (a3): RGB planar anode: It consists of an adhesive conductive layer, a reflective conductive layer, and a transparent conductive layer. The adhesive conductive layer is made of Ti / Ni / Cr / Ta, the reflective conductive layer is made of Ag / Al / Pt, and the transparent conductive layer is made of ITO / IZO. (a4): Short-circuit protection insulation layer: covering the tungsten plug and anode edge, with a thickness of 80-200nm, and the material is silicon oxide / silicon nitride / silicon oxynitride, while preventing electrical crosstalk; (a5): Light-emitting stack: Blue light-emitting unit, charge generation layer, green light-emitting unit, charge generation layer, red light-emitting layer, and semi-transparent cathode are deposited sequentially.