Method and apparatus for forming a membrane with air gaps

By depositing a film on a substrate during integrated circuit manufacturing and using plasma or UV curing to form air gaps, combined with an annealing process, the problems of voids and thickness inhomogeneity are solved, improving the yield and quality of devices.

CN123124680APending Publication Date: 2026-11-17ASM IP HLDG BV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610652813.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-16
Filing Date
2026-05-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the process of integrated circuit manufacturing, defects such as interlayer gaps and thickness inhomogeneity lead to a decrease in device yield, and existing technologies are unable to effectively control the formation and quality of air gaps.

Method used

By providing a substrate in a reaction chamber and depositing films on horizontal surfaces and gap features, air gaps are formed using a plasma or UV curing process, and the air gap height and sidewall thickness of the gap features are optimized by combining an annealing process.

Benefits of technology

High-quality air gap formation was achieved, which improved device yield and output, and ensured the uniformity and stability of interlayer features.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124680A_ABST
    Figure CN123124680A_ABST
Patent Text Reader

Abstract

A method for forming a film having an air gap is provided. The method includes providing a substrate in a reaction chamber. The substrate includes a horizontal surface and a first gap feature extending downward from the horizontal surface. The method includes depositing a film on the horizontal surface and in the first gap feature by a deposition process. The film includes a first top surface on the first gap feature. The method includes performing a curing process on the film to form a first air gap in the film within the first gap feature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to methods for forming membranes. More specifically, this disclosure relates to methods for forming membranes having air gaps. Background Technology

[0002] Integrated circuits are typically manufactured through complex, multi-step processes in which various material layers are constructed on a substrate in a predetermined arrangement. Therefore, earlier processing steps can significantly impact subsequent steps, and deviations from expected parameters (e.g., thickness, density, uniformity) can exacerbate these effects. Thus, high-quality layers are crucial. For example, voids, thickness inhomogeneities, and other defects within layers can cause significant problems and potentially reduce device yield.

[0003] Any discussion set forth in this section (including discussions of problems and solutions) is included in this disclosure for the purpose of providing background information and should not be construed as an admission that any or all of the discussions were known at the time of making this invention or otherwise constitute prior art. Summary of the Invention

[0004] This synopsis is provided to introduce some concepts in a simplified form. These concepts are further described in detail in the following detailed description of embodiments of this disclosure. This synopsis is not intended to identify key or essential features of the claimed subject matter, nor is it intended to limit the scope of the claimed subject matter.

[0005] According to some embodiments of this disclosure, a method for forming a film having an air gap is provided. The method includes providing a substrate in a reaction chamber. The substrate includes a horizontal surface and a first gap feature extending downward from the horizontal surface. The method includes depositing a film on the horizontal surface and in the first gap feature by a deposition process. The film includes a first top surface on the first gap feature. The method includes performing a curing process on the film to form a first air gap in the film within the first gap feature.

[0006] In some embodiments, the curing process includes a plasma curing process.

[0007] In some embodiments, the plasma curing process includes an H2 plasma curing process.

[0008] In some embodiments, the plasma curing process includes a curing depth extending from a first top surface of the film to a first gap feature, and the curing depth is from about 2 nm to about 10 nm.

[0009] In some embodiments, the curing process includes a UV curing process.

[0010] In some embodiments, the UV curing process includes an excimer.

[0011] In some embodiments, the excimer includes Xe2, NeF, Ar2, Kr2, F2, ArBr, ArCl, KrI, ArF, KrBr, KrCl, or combinations thereof.

[0012] In some embodiments, the wavelength of the UV curing process is approximately 172 nm.

[0013] In some embodiments, the UV curing process includes a curing depth extending from a first top surface of the film to a first gap feature, and the curing depth is from about 50 nm to about 100 nm.

[0014] In some embodiments, the deposition process further includes depositing a film to reach a second top surface on the first gap feature, and the second top surface is higher than the first top surface.

[0015] In some embodiments, a curing process is performed to increase the height of the first air gap.

[0016] In some embodiments, the substrate further includes a second gap feature extending downward from a horizontal surface, and the width of the second gap feature is greater than the width of the first gap feature.

[0017] In some embodiments, the method further includes depositing a film in a second gap feature during the deposition process, wherein a first top surface of the film on the first gap feature is higher than a second top surface of the film on the second gap feature.

[0018] In some embodiments, the method further includes forming a second air gap in the film of the second gap feature during the curing process, wherein the height of the first air gap is greater than the height of the second air gap.

[0019] In some embodiments, the method further includes depositing a film in a second gap feature during the deposition process, wherein a first top surface of the film on the first gap feature is flush with a second top surface of the film on the second gap feature.

[0020] In some embodiments, the method further includes forming a second air gap in the film of the second gap feature during the curing process, and the height of the first air gap is equal to the height of the second air gap.

[0021] In some embodiments, the method further includes performing an annealing process after the curing process to facilitate the formation of a first air gap.

[0022] In some embodiments, the annealing process is carried out at a temperature of about 350°C to about 500°C.

[0023] In some embodiments, the thickness of the sidewall of the film between the first air gap and the substrate is about 1 nm to about 10 nm.

[0024] In some embodiments, the deposition process includes providing a precursor to the reaction chamber, and the precursor comprises hexamethyltrisilazane (HMCTS), hexamethyldisilazane (HMDS), tetramethyldivinyldisilazane (TMDVDS), tetramethyldisilazane (TMDS), tetramethylsilyl-silanediamine, methyltrimethoxysilane (MTMS), or combinations thereof.

[0025] According to some embodiments of the present disclosure, an apparatus for forming a membrane having an air gap is provided. The apparatus includes: one or more reaction chambers configured to form a membrane on a substrate, each reaction chamber including two or more stations; a heating system configured to control a first station temperature independently of a second station temperature in the one or more reaction chambers; a pressure system configured to maintain pressure in the two or more stations; an annealing chamber configured to perform an annealing process on the substrate; and a controller configured to control the one or more reaction chambers, the heating system, the pressure system, and the annealing chamber to perform the methods of some embodiments of the present disclosure. Attached Figure Description

[0026] Embodiments of this disclosure can be best understood from the following detailed description taken in conjunction with the accompanying drawings. It should be noted that, according to industry practice, various features are not drawn to scale. In practice, the dimensions of various elements may be arbitrarily increased or decreased to clearly illustrate the features of the embodiments of this disclosure. It should also be noted that the accompanying drawings illustrate exemplary embodiments of this disclosure. The drawings should not be considered as limiting the scope of this disclosure. This disclosure can also be applied to other embodiments.

[0027] Figure 1 A schematic method for forming a membrane with air gaps according to some embodiments of the present disclosure is shown.

[0028] Figure 2 A schematic cross-sectional view of a substrate with gap features according to some embodiments of the present disclosure is shown.

[0029] Figure 3 A schematic cross-sectional view of a substrate with gap features according to some embodiments of the present disclosure is shown.

[0030] Figure 4A A schematic cross-sectional view of a substrate with gap features according to some embodiments of the present disclosure is shown.

[0031] Figure 4B A schematic cross-sectional view of a substrate with gap features according to some embodiments of the present disclosure is shown.

[0032] Figure 5A A schematic cross-sectional view of a substrate having a first gap feature and a second gap feature according to some embodiments of the present disclosure is shown.

[0033] Figure 5B A schematic cross-sectional view of a substrate having a first gap feature and a second gap feature according to some embodiments of the present disclosure is shown.

[0034] Figure 6 Illustrative devices according to some embodiments of the present disclosure are shown.

[0035] Figure 7 Illustrative devices according to some embodiments of the present disclosure are shown. Detailed Implementation

[0036] The following disclosure provides numerous different embodiments or examples for implementing various features of the described subject matter. Specific examples of elements and arrangements are described below to simplify this specification. Of course, these are merely examples and not limiting. For example, in the following description, forming a first feature above or on a second feature can include embodiments where the first and second features are in direct contact, and can also include embodiments where an additional feature is formed between the first and second features such that the first and second features are not in direct contact. Furthermore, reference numerals and / or letters may be repeated in various examples in this disclosure. Such repetition is for simplicity and clarity and does not in itself indicate a relationship between the various embodiments and / or configurations discussed.

[0037] For ease of description, this document uses spatial relative terms such as "below," "below," "lower," "above," and "upper" to describe the relationship between one element or feature and another element or feature as shown in the figure. In addition to the orientations shown in the figure, spatial relative terms are intended to cover different orientations of the device during use or operation. The device may be oriented in other ways (rotated 90 degrees or in other orientations), and the spatial relative descriptors used herein will be interpreted accordingly.

[0038] It should be understood that ordinal numbers used in this disclosure, such as the terms "first," "second," "third," etc., are used to modify elements and do not in themselves imply or indicate that the element (or elements) has any prior ordinal number, nor do they imply the order of one element with another, or the order in which they are manufactured. The use of these ordinal numbers is to clearly distinguish an element with a certain name from another element with the same name. The claims and the description may not use the same terminology. For example, a first element in the description may refer to a second element in the claim.

[0039] In the following description, the terms "about" and "basically" generally refer to + / -10% of the value, or generally + / -5% of the value, or generally + / -3% of the value, or generally + / -2% of the value, or generally + / -1% of the value, or generally + / -0.5% of the value. The expressions "within the range of the first value to the second value" or "between the first value and the second value" mean that the range includes the first value, the second value, and other values ​​in between. The values ​​given in this disclosure are approximate values. That is, the meaning of "about" and "basically" may be implied even if the terms are not specified.

[0040] Some embodiments of this disclosure are described below. Additional steps or operations may be provided before, during, and / or after the steps or operations described in these embodiments. In different embodiments, some described steps or operations may be replaced or deleted. Furthermore, it should be understood that in the following embodiments, features from several different embodiments may be replaced, recombinated, and combined to complete another embodiment without departing from the spirit of this disclosure. Features between the various embodiments can be arbitrarily mixed and combined, as long as they do not violate or contradict the spirit of this disclosure.

[0041] In this disclosure, "gas" can include materials that are gaseous at ambient temperature and pressure (NTP), evaporated solids and / or evaporated liquids, and may consist of a single gas or a mixture of gases, depending on the circumstances. Gases other than process gases, i.e., gases not introduced through gas distribution components, multi-port injection systems, other gas distribution devices, etc., can be used, for example, to seal the reaction space, and may include sealing gases, such as rare gases. In some cases, the term "precursor" can refer to a compound that participates in a chemical reaction to produce another compound, and particularly to a compound that constitutes the membrane matrix or the main framework of the membrane. The term "reactant" is used interchangeably with the term "precursor".

[0042] As used herein, the term "substrate" can refer to any one or more underlying materials, including any one or more underlying materials that can be modified or on which devices, circuits, or films can be formed. A "substrate" can be continuous or discontinuous; rigid or flexible; solid or porous; and combinations thereof. A substrate can be in any form, such as powder, plate, or workpiece. Plate-type substrates can include wafers of various shapes and sizes. Substrates can be made of semiconductor materials, including, for example, silicon, silicon germanium, silicon oxide, gallium arsenide, gallium nitride, and silicon carbide.

[0043] For example, substrates in powder form can have applications in pharmaceutical manufacturing. Porous substrates can contain polymers. Examples of workpieces may include medical devices (e.g., stents and syringes), jewelry, tooling devices, components for battery manufacturing (e.g., anodes, cathodes, or separators), or components for photovoltaic cells, etc.

[0044] The continuous substrate can extend beyond the boundary of the processing chamber where the deposition process takes place. In some processes, the continuous substrate can move through the processing chamber, allowing the process to continue until the end of the substrate is reached. The continuous substrate can be supplied from a continuous substrate supply system to allow the continuous substrate to be manufactured and output in any suitable form.

[0045] Non-limiting examples of continuous substrates may include sheets, nonwoven films, rolls, foils, fiber webs, flexible materials, bundles of continuous filaments or fibers (e.g., ceramic fibers or polymer fibers). Continuous substrates may also include carriers or sheets on which non-continuous substrates are mounted.

[0046] As used herein, “atomic layer deposition,” abbreviated as “ALD,” refers to a vapor-phase deposition process in which deposition cycles, such as multiple consecutive deposition cycles, are performed in a reaction space (i.e., one or more reaction chambers). Typically, in an ALD process, during each deposition cycle, a precursor is introduced into the reaction space and adsorbed onto a substrate surface, which may include previously deposited material from previous ALD cycles or other materials, forming at most a monolayer of the precursor that is not readily reacted with any additional excess precursor (i.e., a self-limiting reaction). Subsequently, in some cases, another precursor or reactant may be introduced into the reaction space to convert the chemisorbed precursor into the desired material on the substrate surface. Other reaction steps may be included in the deposition cycle. ALD can occur via a thermal process (thermal ALD), where the reaction is promoted by increasing the substrate temperature relative to ambient temperature; and / or via a plasma-enhanced process (PEALD), where the reaction is promoted by using high-energy plasma materials. As used herein, ALD may also be intended to include processes specified by relevant terms, such as chemical vapor atomic layer deposition, atomic layer epitaxy (ALE), molecular beam epitaxy (MBE), gas-source MBE or organometallic MBE, and chemical beam epitaxy when performed with alternating pulses of reactants.

[0047] As used herein, “chemical vapor deposition,” abbreviated as “CVD,” refers to a vapor deposition process in which a film is deposited on a substrate by exposing the substrate surface to one or more gaseous precursors and reactants, which react and / or decompose on the substrate surface to form the film. The precursors and / or reactants may be provided simultaneously to the reaction space, or in partially or completely separate pulses. In some embodiments, the precursors and / or reactants are provided until a layer of desired thickness is deposited. In some embodiments, a cyclic CVD process may be used with multiple cycles to deposit a thin film of desired thickness. In a cyclic CVD process, the precursors and / or reactants may be provided to the reaction space in non-overlapping or partially or completely overlapping pulses. CVD can occur through a thermal process (thermal CVD), where the reaction is promoted by increasing the substrate temperature relative to ambient temperature; or through a plasma-enhanced CVD process, where the reaction is promoted by using high-energy plasma materials.

[0048] As used herein, the terms “membrane” and / or “layer” can refer to any continuous or discontinuous structure and material, such as materials deposited by the methods disclosed herein. For example, membranes and / or layers can include two-dimensional materials, three-dimensional materials, nanoparticles, or even partial or complete molecular layers or partial or complete atomic layers or atomic and / or molecular clusters. A membrane or layer can include a material or layer with pinholes, which can be at least partially continuous. Alternatively, a membrane or layer can consist entirely of isolated islands.

[0049] In this disclosure, the terms “comprising,” “consisting of,” and “having” in some embodiments independently mean “generally or broadly comprising,” “comprising,” “essentially consisting of,” or “consisting of.” It should be understood that when a composition, method, apparatus, etc., is described as comprising certain features, it means that it includes those features, and it does not necessarily exclude the presence of other features, provided they do not render the claims unfeasible. Nevertheless, the expression “comprising” includes the meaning of “consisting of,” that is, when the composition, method, apparatus, etc., under discussion comprises only the listed features, components, and / or steps, and does not contain any other features, components, steps, etc.

[0050] As used herein, the term "carrier gas" can refer to a gas supplied to the reaction chamber along with one or more precursors. For example, a carrier gas may be supplied to the reaction chamber along with one or more precursors used herein. Exemplary carrier gases include N2, H2, and inert gases such as He, Ne, Kr, Ar, and Xe.

[0051] Unlike carrier gases, purge gases can be supplied to the reaction chamber alone (i.e., not with one or more precursors). Nevertheless, gases typically used as carrier gases can also be used as purge gases, even within the same process. For example, in a cyclic deposition-etch process, N2 used as a carrier gas can be supplied with one or more precursors during the deposition pulse, and N2 used as a purge gas can be used to separate the deposition and etching pulses. Therefore, the manner in which a gas is supplied to the reaction chamber determines whether it is used as a purge gas or a carrier gas in a given situation. Thus, as used herein, the term "purge" can refer to the process of supplying an inert or substantially inert gas to the reaction chamber between two interacting gas pulses. For example, a purge, for example using nitrogen, can be provided between precursor and reactant pulses to avoid or at least minimize gas-phase interactions between the precursors and reactants. It should be understood that purging can be achieved temporally, spatially, or both. For example, in the case of time-purge, a purge step can be used, for instance, in a time sequence of providing a first precursor to the reaction chamber, providing a purge gas to the reaction chamber, and providing a second precursor to the reaction chamber, wherein the substrate on which the deposition layer is deposited does not move. For example, in the case of spatial purge, the purge step can take the form of moving the substrate from a first position where the first precursor is continuously supplied through a purge gas curtain to a second position where the second precursor is continuously supplied.

[0052] As used herein, “station” broadly refers to a location that may contain a substrate, such that processes can be performed on the substrate within the station. Thus, a station can refer to a reactor, a portion of a reactor, or a reaction space or chamber within a reactor. In some embodiments, stations according to the embodiments herein are in a “gas-isolated” state with respect to each other, or configured to be in a gas-isolated state while processing a substrate within the station. In some embodiments, the station is in a gas-isolated state via a physical barrier rather than a gas bearing or gas curtain. In some embodiments, the station is in a gas-isolated state via a combination of a physical barrier, a gas bearing, and a gas curtain. In some embodiments, after or simultaneously with placing the substrate in a particular station, the substrate is placed in a gas-isolated state from other stations (so that processing steps can be performed in that station), and after the substrate has been processed in the station, the station is removed from the gas isolation, and the substrate can be removed from the station and positioned in an intermediate space. Substrates from multiple different stations can be placed in a shared intermediate space for inter-station movement. Stations can be placed in a gas-isolated state, for example, via a physical barrier. In some embodiments, stations are not placed in a gas-isolated state. In some embodiments, one or more stations include heating and / or cooling systems such that different precursors in different stations can simultaneously process substrates at different temperatures. Therefore, in some embodiments, the entire first station is at a lower or higher temperature than the entire second station, or the first station includes a base at a lower or higher temperature than the base in the second station, and / or a first precursor flows into the first station while a second precursor flows into the second station at a lower or higher temperature than the first station.

[0053] In some embodiments, the stations are separated from each other by a solid material and not by gas bearings or gas curtains. Alternatively, a physical barrier may be moved with a stage that shuttles the substrate between the station and the intermediate space, such that the physical barrier places the station in gas isolation simultaneously (or slightly before or after) the substrate is placed in the station. Alternatively, a physical barrier may be used in conjunction with a gas barrier, for example, to fill some gaps left by the physical barrier. In some embodiments, a physical barrier is provided, but no gas barrier or gas curtain is provided.

[0054] In some embodiments, a station comprises a module or chamber of a reactor, such that each station comprises a separate chamber or module. In some embodiments, a station comprises a portion of a reaction chamber, which may be gas-isolated from other portions of the reaction chamber by positioning walls, gas curtains, or gas bearings between stations. Optionally, a given station is completely surrounded by one or more walls, gas curtains, gas bearings, or any combination of these. However, in some embodiments, the stations are not separate.

[0055] refer to Figure 1 and Figure 2 , Figure 1 A schematic method 100 for forming a membrane with air gaps is shown, and Figure 2 A schematic cross-sectional view of a substrate 200 having a gap feature 220 according to some embodiments of the present disclosure is shown. Method 100 includes providing the substrate 200 in a reaction chamber (step 110). The substrate 200 includes a horizontal surface 210 and a gap feature 220 extending downward from the horizontal surface 210. Method 100 includes depositing a film 230 on the substrate 200 (step 120). The film 230 includes a top surface 230T on the gap feature 220. Method 100 includes curing the film 230 to form an air gap 240 in the film 230 (step 130). Method 100 also includes an optional step: annealing the film 230 (step 140).

[0056] The order of steps in method 100 is merely an example. In other embodiments, this order may vary. In some embodiments, additional steps may be provided in the method. For example, in some embodiments, there are additional steps for providing plasma during the deposition process. For example, in some embodiments, there are additional steps for providing purge gas.

[0057] In some embodiments, the flowable membrane 230 can be formed in a first station (deposition station) of the reaction chamber via a flowable deposition process (e.g., flowable CVD) and can be cured in a second station of the reaction chamber (i.e., post-deposition treatment). In some embodiments, deposition of the flowable membrane 230 can be performed by flowing one or more precursors in the gas phase. The one or more precursors can form a polymer. In some embodiments, the one or more precursors can be selected from silylamines, silazanes, cyclosilazanes, and silylamines. For example, one or more precursors may include hexamethyltrisilazane (HMCTS), hexamethyldisilazane (HMDS), tetramethyldivinyldisilazane (TMDVDS), tetramethyldisilazane (TMDS), tetramethylsilyl-silanediamine, methyltrimethoxysilane (MTMS), or combinations thereof.

[0058] In some embodiments, one or more precursors of a gaseous (viscous) phase flow into the gaps in a substrate, which may be, for example, a silicon wafer. As a result, one or more precursors can seamlessly fill the gaps in a bottom-up manner. When the gaseous precursors are polymerized by plasma, a flowable film can be temporarily obtained, wherein the gaseous precursors (e.g., monomers) are activated by energy provided by the plasma, thereby initiating polymerization. When the film is deposited on the surface and in the gaps between the substrate, it exhibits temporarily flowable behavior. Subsequent processing steps (e.g., a curing step) can be used to cure the polymer.

[0059] In some embodiments, the deposition process includes the use of radio frequency (RF) plasma and a pulsed precursor flow. In some embodiments, process parameters may be varied to achieve sufficiently high partial pressures for polymerization to proceed throughout the RF-on period and to provide sufficient energy to activate the reaction. In some embodiments, the temperature and pressure of polymerization may be controlled and set above the melting point and below the boiling point of the mobile phase. In some embodiments, one or more precursors may be introduced into the reaction chamber, and one or more process gases may also be introduced into the reaction chamber. Process gases may include co-reactants, rare gases, carrier gases, diluent gases, or combinations thereof. For example, one or more process gases may include Ar, He, N2, H2, NH3, O2, or combinations thereof. In some embodiments, process gases and precursors may be introduced simultaneously. In some embodiments, precursors may be introduced before or after the process gases. In some embodiments, RF plasma may be maintained before, during, or after the introduction of precursors and / or process gases. It should be understood that when the above method is performed sequentially (i.e., cyclically), a small amount of material may be deposited per cycle, and the sequential steps may be repeated until a layer with the desired thickness is obtained. In some embodiments, the method is performed cyclically, and one or more steps are separated by purge gas pulses.

[0060] In some embodiments, the method described above includes intermittently providing a precursor to the reaction chamber and continuously providing plasma. In some embodiments, the method described above involves intermittently providing a precursor to the reaction chamber and intermittently providing plasma.

[0061] Process parameters may include, for example, pressure and temperature in the reaction chamber. Unbound by theory or any particular operating mode, the deposited material is believed to ideally remain viscous or liquid throughout the deposition process and should not readily solidify or evaporate. It is also believed that, under desired reaction conditions, the vapor pressure of the liquid phase, rather than the vapor pressure of the precursor, should be lower than the total pressure. Therefore, it is believed that pressure and temperature should be maintained under conditions where the flowable film is in a liquid state and the precursor is in a gaseous state.

[0062] In some embodiments, the pressure in the reaction chamber can be maintained between about 300 Pa and about 2800 Pa. For example, the pressure in the reaction chamber can be maintained at about 300 Pa, about 350 Pa, about 400 Pa, about 450 Pa, about 500 Pa, about 550 Pa, about 600 Pa, about 650 Pa, about 700 Pa, about 750 Pa, about 800 Pa, about 850 Pa, about 900 Pa, about 950 Pa, about 1000 Pa, about 1050 Pa, about 1100 Pa, about 1150 Pa, about 1200 Pa, about 1250 Pa, about 1300 Pa, about 1350 Pa, about 1400 Pa, about 1450 Pa, about 1500 Pa, about 1550 Pa, about 1... 600 Pa, approximately 1650 Pa, approximately 1700 Pa, approximately 1750 Pa, approximately 1800 Pa, approximately 1850 Pa, approximately 1900 Pa, approximately 1950 Pa, approximately 2000 Pa, approximately 2050 Pa, approximately 2100 Pa, approximately 2150 Pa, approximately 2200 Pa, approximately 2250 Pa, approximately 2300 Pa, approximately 2350 Pa, approximately 2400 Pa, approximately 2450 Pa, approximately 2500 Pa, approximately 2550 Pa, approximately 2600 Pa, approximately 2650 Pa, approximately 2700 Pa, approximately 2750 Pa, approximately 2800 Pa, or any value between the above values.

[0063] In some embodiments, the temperature in the reaction chamber can be maintained below about 300°C. For example, the temperature in the reaction chamber can be maintained at about 50°C, about 55°C, about 60°C, about 65°C, about 70°C, about 75°C, about 80°C, about 85°C, about 90°C, about 95°C, about 100°C, about 105°C, about 110°C, about 115°C, about 120°C, about 125°C, about 130°C, about 135°C, about 140°C, about 145°C, about 150°C, about 155°C, about 160°C, about 165°C, about 170°C, or about 175°C. Approximately 180°C, approximately 185°C, approximately 190°C, approximately 195°C, approximately 200°C, approximately 205°C, approximately 210°C, approximately 215°C, approximately 220°C, approximately 225°C, approximately 230°C, approximately 235°C, approximately 240°C, approximately 245°C, approximately 250°C, approximately 255°C, approximately 260°C, approximately 265°C, approximately 270°C, approximately 275°C, approximately 280°C, approximately 285°C, approximately 290°C, approximately 295°C, approximately 300°C, or any value between the above.

[0064] In some embodiments, the RF power supplied to the reaction chamber can be between about 20W and about 1000W. For example, in some embodiments, the RF power supplied to the reaction chamber can be about 20W, about 40W, about 60W, about 80W, about 100W, about 120W, about 140W, about 160W, about 180W, about 200W, about 220W, about 240W, about 260W, about 280W, about 300W, about 320W, about 340W, about 360W, about 380W, about 400W, about 420W, about 440W, about 460W, about 480W, and about 1000W. 500W, approximately 520W, approximately 540W, approximately 560W, approximately 580W, approximately 600W, approximately 620W, approximately 640W, approximately 660W, approximately 680W, approximately 700W, approximately 720W, approximately 740W, approximately 760W, approximately 780W, approximately 800W, approximately 820W, approximately 840W, approximately 860W, approximately 880W, approximately 900W, approximately 920W, approximately 940W, approximately 960W, approximately 980W, approximately 1000W, or any value between the above.

[0065] The precursor and process gases can be supplied to the reaction chamber at volumetric flow rates from about 0.1 standard liters per minute (SLM) to about 10 SLM. For example, the precursor and process gases can be supplied to the reaction chamber at the following volumetric flow rates: about 0.1 SLM, about 0.5 SLM, about 1 SLM, about 1.5 SLM, about 2 SLM, about 2.5 SLM, about 3 SLM, about 3.5 SLM, about 4 SLM, about 4.5 SLM, about 5 SLM, about 5.5 SLM, about 6 SLM, about 6.5 SLM, about 7 SLM, about 7.5 SLM, about 8 SLM, about 8.5 SLM, about 9 SLM, about 9.5 SLM, about 10 SLM. M, approximately 10.5 SLM, approximately 11 SLM, approximately 11.5 SLM, approximately 12 SLM, approximately 12.5 SLM, approximately 13 SLM, approximately 13.5 SLM, approximately 14 SLM, approximately 14.5 SLM, approximately 15 SLM, approximately 15.5 SLM, approximately 16 SLM, approximately 16.5 SLM, approximately 17 SLM, approximately 17.5 SLM, approximately 18 SLM, approximately 18.5 SLM, approximately 19 SLM, approximately 19.5 SLM, approximately 20 SLM, or any value between the above.

[0066] In some embodiments, the curing process may include a plasma curing process, a UV curing process, another suitable curing process, or a combination thereof.

[0067] In embodiments where the curing process is a plasma curing process, the plasma can be H2 plasma. For example... Figure 2 As shown, the plasma curing process includes a curing depth H1 extending from the top surface 230T of the film 230 to the gap feature 220. In some embodiments, the curing depth H1 is about 2 nm to about 10 nm.

[0068] In embodiments where the curing process is a UV curing process, the UV curing process includes an excimer. In some embodiments, the excimer includes Xe2, NeF, Ar2, Kr2, F2, ArBr, ArCl, KrI, ArF, KrBr, KrCl, or combinations thereof. In some embodiments, the wavelength of the UV curing process can be between 100 nm and 250 nm, between 110 nm and 240 nm, between 120 nm and 230 nm, between 130 nm and 220 nm, between 140 nm and 210 nm, between 150 nm and 200 nm, between 160 nm and 190 nm, or between 170 nm and 180 nm. For example, the wavelength of the UV curing process can be 108 nm, 126 nm, 146 nm, 158 nm, 165 nm, 172 nm, 175 nm, 190 nm, 193 nm, 207 nm, or 222 nm. In one embodiment, the excimer may be Xe2, and the wavelength of the UV curing process may be 172 nm. For example... Figure 2As shown, the UV curing process includes a curing depth H1 extending from the top surface 230T of the film 230 to the gap feature 220. In some embodiments, the curing depth H1 is about 50 nm to about 100 nm.

[0069] Still referencing Figure 2 After the film 230 cures, the uncured bottom portion of the film 230 desorbs, resulting in the formation of an air gap 240. In some embodiments, the thickness 230D of the sidewall of the film 230 between the air gap 240 and the substrate 200 can be from about 1 nm to about 10 nm. Figure 2 In the illustrated embodiment, the width of the gap feature 220 is less than 50 nm, allowing for the formation of air gaps 240 of the desired size after the curing process. However, referring to... Figure 3 If the width W1 of the gap feature 220 is greater than 50 nm, an annealing process can be performed after the curing process to obtain an air gap 240 with the desired dimensions. Specifically, in Figure 3 In the illustrated embodiment, an air gap 240A is formed in the film 230 after the curing process. However, the air gap 240A is too small, which means that the thickness 230D1 of the sidewall of the film 230 between the air gap 240A and the substrate 200 is too thick. Therefore, an annealing process is performed to cure the film 230 and remove the uncured portion of the film 230, thereby forming the air gap 240B. In some embodiments, the thickness 230D2 of the sidewall of the film 230 between the air gap 240B and the substrate 200 can be from about 1 nm to about 10 nm.

[0070] In some embodiments, the annealing process can be a rapid thermal annealing (RTA) process. In some embodiments, the substrate is rapidly heated by exposure to infrared (IR) radiation. The exposure time of the annealing process can be between about 0.1 seconds (s) and about 10 seconds (s). For example, in some embodiments, the exposure time can be about 0.1 s, about 0.2 s, about 0.3 s, about 0.4 s, about 0.5 s, about 0.6 s, about 0.7 s, about 0.8 s, about 0.9 s, about 1 s, about 1.1 s, about 1.2 s, about 1.3 s, about 1.4 s, about 1.5 s, about 1.6 s, about 1.7 s, about 1.8 s, about 1.9 s, about 2 s, about 2.1 s, about 2.2 s, about 2.3 s, etc. Approximately 2.4s, approximately 2.5s, approximately 2.6s, approximately 2.7s, approximately 2.8s, approximately 2.9s, approximately 3s, approximately 3.1s, approximately 3.2s, approximately 3.3s, approximately 3.4s, approximately 3.5s, approximately 3.6s, approximately 3.7s, approximately 3.8s, approximately 3.9s, approximately 4s, approximately 4.1s, approximately 4.2s, approximately 4.3s, approximately 4.4s, approximately 4.5s, approximately 4.6s, approximately 4.7s, approximately 4.8s, approximately 4.9s, approximately... 5s, approximately 5.1s, approximately 5.2s, approximately 5.3s, approximately 5.4s, approximately 5.5s, approximately 5.6s, approximately 5.7s, approximately 5.8s, approximately 5.9s, approximately 6s, approximately 6.1s, approximately 6.2s, approximately 6.3s, approximately 6.4s, approximately 6.5s, approximately 6.6s, approximately 6.7s, approximately 6.8s, approximately 6.9s, approximately 7s, approximately 7.1s, approximately 7.2s, approximately 7.3s, approximately 7.4s, approximately 7.5s, approximately 7.6s The time is approximately 7.7s, 7.8s, 7.9s, 8s, 8.1s, 8.2s, 8.3s, 8.4s, 8.5s, 8.6s, 8.7s, 8.8s, 8.9s, 9s, 9.1s, 9.2s, 9.3s, 9.4s, 9.5s, 9.6s, 9.7s, 9.8s, 9.9s, 10s, or any value between the above.

[0071] In some embodiments, the annealing process may be performed at a temperature between about 80°C and about 1000°C. In some embodiments, the annealing process may be performed at the following temperatures: about 80°C, about 105°C, about 130°C, about 155°C, about 180°C, about 205°C, about 230°C, about 255°C, about 280°C, 300°C, about 325°C, about 350°C, about 375°C, about 400°C, about 425°C, about 450°C, about 475°C, about 500°C, about 5 25°C, approximately 550°C, approximately 575°C, approximately 600°C, approximately 625°C, approximately 650°C, approximately 675°C, approximately 700°C, approximately 725°C, approximately 750°C, approximately 775°C, approximately 800°C, approximately 825°C, approximately 850°C, approximately 875°C, approximately 900°C, approximately 925°C, approximately 950°C, approximately 975°C, approximately 1000°C, or any value between the above. In some embodiments, a higher temperature in the annealing process may correspond to a lower exposure time in the annealing process.

[0072] refer to Figure 4A and Figure 4B The location of air gaps can be controlled based on the amount of membrane deposition. Figure 4A In the illustrated embodiment, the membrane 230 has a first top surface 230T1 on the gap feature 220, and the air gap 240C has a first height H2 after the curing process. Figure 4B In the illustrated embodiment, prior to the curing process, a film 230 is further deposited to reach a second top surface 230T2 on the gap feature 220. The second top surface 230T2 is higher than the first top surface 230T1. After the curing process, the air gap 240D has a second height H3, and the second height H3 is higher than the first height H2. Therefore, the position of the air gap is increased by a height H4.

[0073] refer to Figure 5A and Figure 5B The location of air gaps in different gap characteristics can be controlled by the amount of membrane deposition. Figure 5A and Figure 5B In the illustrated embodiment, the substrate 200 further includes a second gap feature 250 extending downward from the horizontal surface 210, the width W3 of the second gap feature 250 being greater than the width W2 of the first gap feature 220. Figure 5AIn the illustrated embodiment, film 230 is deposited having a first top surface 230T3 on a first gap feature 220 and a second top surface 230T4 on a second gap feature 250. The first top surface 230T3 is higher than the second top surface 230T4. After the curing process, air gaps 240E in the first gap feature 220 have a height H5, and air gaps 240F in the second gap feature 250 have a height H6, with height H5 being higher than height H6. Figure 5B In the illustrated embodiment, film 230 is over-deposited prior to the curing process. The first top surface 230T5 of film 230 on the first gap feature 220 is flush with the second top surface 230T6 of film 230 on the second gap feature 250. After the curing process, the height H7 of air gap 240G is equal to the height H8 of air gap 240H.

[0074] According to some embodiments, multi-process chamber devices with one or more cryogenic deposition stations and one or more processing stations can be used. In some embodiments, multi-process four-chamber module (QCM) devices can be used, wherein one or more cryogenic deposition stations and one or more processing (e.g., plasma and / or UV curing) stations are used. For example, some devices may include two deposition stations and two processing stations. In some embodiments, some devices may include four processing stations, which can be configured to heat the substrate to different temperatures. In some embodiments, interstitial fillings may be utilized using α-CH, SiCN, SiN, SiON, SiCO, SiCOH, SiCNH, SiCH, SiNH, or SiCON. Therefore, although the embodiments described herein are primarily concerned with SiCN and / or SiN deposition, some of the embodiments herein are broadly applicable to a variety of process chemistry.

[0075] In some embodiments, a multi-processing chamber apparatus may include two or more stations for performing flowable deposition and post-deposition processes (e.g., plasma and UV curing) on ​​a substrate. In some embodiments, the multi-processing chamber apparatus may include a dual-system gas delivery and temperature control system, such that each station can be heated independently and different gases can be delivered to each station simultaneously. In some embodiments, each station of the multi-processing chamber apparatus may include a heater for heating the station independently of the other stations in the multi-processing chamber module. In some embodiments, the heater may include an aluminum nitride (AlN) ceramic heater or an anodized aluminum heater. In some embodiments, the heater may include one or more heating lamps for transmitting IR radiation to the surface of the substrate.

[0076] In some embodiments, the multi-processor unit may include an integrated single-system exhaust and pump system, enabling all stations to be maintained at synchronized pressure simultaneously. Additionally, the multi-processor unit may include a single-system radio frequency (RF) power source for supplying RF power to the stations. In some embodiments, RF power may be supplied to the stations independently.

[0077] refer to Figure 6 , Figure 6 A schematic apparatus 600 according to some embodiments of the present disclosure is shown. In some embodiments, apparatus 600 may be a multi-processing chamber apparatus. Apparatus 600 may include one or more reaction chambers 601 (processing chambers), each reaction chamber including one or more stations 603 gas-isolated from other stations. In some embodiments, a multipod 605 may move a substrate between reaction chambers. An end effector located in a wafer transport chamber 602 (WHC) may add and remove substrates from the multipod (communicating with the reaction chambers) and / or a load locking chamber 604 (LLC). As described above, the multi-processing chamber module may include dual heating systems, including independent heating systems 606, 608. In some embodiments, heating system 606 may heat and / or cool one or more of stations 603 to a first temperature independently of heating system 608. Similarly, heating system 608 may heat and / or cool one or more of other stations 603 to a second temperature different from the first temperature independently of heating system 606. This configuration allows different processes, such as one or more deposition processes and one or more curing processes, to be performed simultaneously in different stations. The apparatus 600 may also include a pressure system 610, which includes an exhaust and pumping system. In some embodiments, the pressure system 610 may be connected to all stations 603 in the reaction chamber 601, such that the same chamber pressure can be maintained in all stations 603 in the reaction chamber 601. In some embodiments, the stations 603 are not sealed to each other. In some embodiments, this lack of station separation allows for a less complex design, easier and faster wafer handling between stations, and a shared pressure system 610, allowing the deposition station and the curing station to be maintained at the same pressure simultaneously.

[0078] refer to Figure 7 , Figure 7 A schematic device 700 according to some embodiments of the present disclosure is shown. In some embodiments, device 700 may be a multiprocessor four-chamber module (QCM) device. Figure 7 In this embodiment, apparatus 700 has three QCMs 710 (processing QCMs) for the deposition process and one QCM 720 (annealing QCM) for annealing, as described herein. In some embodiments, each QCM 710 may be a reaction chamber 601 of apparatus 600. After the deposition process is completed, the substrate can be transferred from the processing QCM to the annealing QCM. Figure 7In the illustrated embodiment, one QCM is used for annealing. It should be understood that in some embodiments, a QCM is not required. For example, the annealing chamber may have 1 station, 2 stations, 3 stations, 4 stations, 5 stations, 6 stations, or more.

[0079] According to some embodiments, a deposition station is provided in communication with a precursor source gas, allowing the precursor to flow into the station. In some embodiments, the apparatus 700 may also include a controller 730 configured to control the movement of the substrate between stations, the inflow of precursor and process gases into the stations, and / or the purging of the stations. Different process gases may contact the substrate at different temperatures suitable for each particular precursor. The controller 730 is configured to communicate with various power supplies, heating systems, pumps, robots, and gas flow controllers or valves, and is configured to perform the methods of some embodiments of this disclosure.

[0080] In some embodiments, precursors in the station are delivered via spray heads. Optionally, the spray heads include heated spray heads to provide the precursors to the station at a desired temperature or temperature range. In some embodiments, the heated spray heads provide the station with process gas at or near the temperature at which the precursors contact the substrate. Optionally, the spray heads include a vacuum purging device surrounding their periphery to capture excess precursors and minimize the amount of precursors that may be available for CVD reactions with other gases. In some embodiments, the precursors are contained within the station (and / or precursor source lines and / or purge lines) but are not permitted to enter any space between stations.

[0081] Note that if two different stations comprise two different processes, different station conditions, such as different temperatures, can be maintained at the different stations. For example, the first station may be at a first temperature optimized for a first process at the first station, and the second station may be at a second temperature optimized for a second process at the second station. Therefore, in some embodiments, the entire first station is at a different temperature than the entire second station. In some embodiments, the entire first station is at a different temperature than the entire second station, but both stations are under the same pressure.

[0082] Optionally, the station is further connected to a purge gas source and / or a vacuum gas, allowing the station to be purged. For example, according to some embodiments, after the substrate has come into contact with the precursor at the first station (but before the substrate moves to the second station), the station can be purged while the substrate remains in the first station, in order to minimize or eliminate the possibility that any residual precursor will be transported to the second station along with the substrate.

[0083] Optionally, in some embodiments, one or more stations include a base on which a substrate can be placed. The base can be heated or cooled, and therefore can be configured to heat or cool the substrate to a suitable temperature. Thus, in some embodiments, the base in a first station is heated or cooled to a first temperature, while the base in a second station is heated or cooled to a second temperature. Furthermore, in some embodiments, the base can heat or cool the substrate for different durations to allow the substrate to reach a suitable temperature. In some embodiments, cooling and / or heating the base may be necessary to maintain a large temperature difference between the deposition station and the annealing station. Optionally, the base may have a lower mass than the substrate, allowing the base to be heated or cooled faster than the substrate. In other embodiments, the base may have a greater mass than the substrate, allowing the substrate to be heated or cooled faster than the base. Optionally, the base does not move between stations. Optionally, the base includes a heated and / or cooled base. In some embodiments, the base is at a suitable temperature for depositing a precursor before the substrate is placed on it. In some embodiments, after the substrate is placed on the base, the base is heated to a suitable temperature for depositing the precursor.

[0084] In some embodiments of this disclosure, the flowable film is cured by a plasma curing process (H2 plasma). Then, an annealing process is performed at a temperature of approximately 400°C.

[0085] In some embodiments of this disclosure, the flowable film is cured by a UV curing process (Xe excimer with a wavelength of 172 nm). An annealing process is then performed at a temperature of approximately 400°C.

[0086] In some embodiments of the present invention, because the curing depth of the plasma curing process (i.e., about 2 nm to about 10 nm) is less than the curing depth of the UV curing process (i.e., about 50 nm to about 100 nm), the top of the air gap formed by the plasma curing process is higher than the top of the air gap formed by the UV curing process. Furthermore, by using either the plasma curing process or the UV curing process, the sidewall thickness of the flowable film between the air gap and the substrate is about 1 nm to about 10 nm, which is very thin.

[0087] In conventional methods, air gaps can be formed by sacrificial film deposition, followed by hard mask deposition and lateral etching. However, this requires at least three processes, which is time-consuming. Alternatively, air gaps can be formed by standard CVD or ALD processes. However, it is difficult to control the size and location of the air gaps. According to some embodiments of this disclosure, a flowable film is deposited, followed by a plasma or UV curing process to form air gaps in the flowable film. The size and location of the air gaps can be effectively and precisely controlled by the curing depth of the curing process and the amount of flowable film deposited. Furthermore, in the case of forming air gaps with desired dimensions, the thickness of the sidewalls of the flowable film between the air gap and the substrate is very small (i.e., about 1 nm to about 10 nm), which ensures that extremely low-k applications can be achieved.

[0088] While some embodiments and advantages of this disclosure have been described in detail, it should be understood that various changes, substitutions, and modifications can be made herein without departing from the spirit and scope of this disclosure as defined by the appended claims. Features of the various embodiments can be used in any combination, provided they do not depart from the spirit and scope of this disclosure. Furthermore, the scope of this application is not intended to be limited to the specific embodiments of the processes, machines, manufactures, compositions of matter, apparatuses, methods, and steps described in the specification. Those skilled in the art will readily understand from this disclosure that, according to this disclosure, existing or later-developed processes, machines, manufactures, compositions of matter, apparatuses, methods, or steps that perform substantially the same function or achieve substantially the same result as the corresponding embodiments described herein can be utilized. Therefore, the appended claims are intended to include such processes, machines, manufactures, compositions of matter, apparatuses, methods, or steps within their scope. Moreover, each claim constitutes a separate embodiment, and the scope of protection claimed by this disclosure includes combinations of claims and embodiments. The scope of protection of this disclosure is limited by the scope of the appended claims. No embodiment or claim of this disclosure is required to satisfy all the purposes, advantages, and features disclosed in this disclosure.

Claims

1. A method for forming a membrane having air gaps, comprising: A substrate is provided in a reaction chamber, wherein the substrate includes a horizontal surface and a first gap feature extending downward from the horizontal surface; A film is deposited on a horizontal surface and in a first gap feature by a deposition process, wherein the film includes a first top surface on the first gap feature; and A curing process is performed on the membrane to form a first air gap in the membrane with the first gap feature.

2. The method for forming a film with an air gap of claim 1, wherein, The curing process includes a plasma curing process.

3. The method for forming a film with an air gap of claim 2, wherein, The plasma curing process includes an H2 plasma curing process.

4. The method for forming a film with an air gap of claim 2, wherein, The plasma curing process includes a curing depth extending from the first top surface of the film to the first gap feature, and the curing depth is from about 2 nm to about 10 nm.

5. The method for forming a film with an air gap of claim 1, wherein, The curing process includes a UV curing process.

6. The method for forming a film with an air gap of claim 5, wherein, The UV curing process includes excimer lasers.

7. The method for forming a film with an air gap of claim 6, wherein, The excimers include Xe2, NeF, Ar2, Kr2, F2, ArBr, ArCl, KrI, ArF, KrBr, KrCl or combinations thereof.

8. The method for forming a film with an air gap of claim 7, wherein, The wavelength of the UV curing process is approximately 172 nm.

9. The method for forming a film with an air gap of claim 5, wherein, The UV curing process includes a curing depth extending from the first top surface of the film to the first gap feature, and the curing depth is from about 50 nm to about 100 nm.

10. The method for forming a film with air gaps of claim 1, wherein, The deposition process further includes depositing the film to reach a second top surface on the first gap feature, and the second top surface being higher than the first top surface.

11. The method for forming a membrane having air gaps according to claim 10, wherein, The curing process is performed to increase the height of the first air gap.

12. The method for forming a membrane with air gaps according to claim 1, wherein, The substrate further includes a second gap feature extending downward from the horizontal surface, and the width of the second gap feature is greater than the width of the first gap feature.

13. The method of forming a film having an air gap according to claim 12, further comprising depositing the film in the second gap feature during the deposition process, wherein, The first top surface of the membrane on the first gap feature is higher than the second top surface of the membrane on the second gap feature.

14. The method of forming a film having an air gap according to claim 13, further comprising forming a second air gap in the film with the second gap feature during the curing process, wherein, The height of the first air gap is greater than the height of the second air gap.

15. The method of forming a film having an air gap according to claim 12, further comprising depositing the film in the second gap feature during the deposition process, wherein, The first top surface of the membrane on the first gap feature is flush with the second top surface of the membrane on the second gap feature.

16. The method of forming a film having an air gap according to claim 15, further comprising forming a second air gap in the film with the second gap feature during the curing process, wherein, The height of the first air gap is equal to the height of the second air gap.

17. The method for forming a film having an air gap according to claim 1, further comprising performing an annealing process after the curing process to promote the formation of the first air gap.

18. The method for forming a membrane having air gaps according to claim 17, wherein, The annealing process is carried out at a temperature of approximately 350°C to approximately 500°C.

19. The method for forming a membrane with air gaps according to claim 1, wherein, The thickness of the sidewalls of the film between the first air gap and the substrate is about 1 nm to about 10 nm.

20. The method for forming a membrane having air gaps according to claim 1, wherein, The deposition process includes providing a precursor to the reaction chamber, wherein the precursor comprises hexamethyltrisilazane, hexamethyldisilazane, tetramethyldivinyldisilazane, tetramethyldisilazane, tetramethylsilyl-silanediamine, methyltrimethoxysilane, or combinations thereof.

21. An apparatus for forming a membrane having air gaps, comprising: One or more reaction chambers configured to form a film on a substrate, each reaction chamber comprising two or more stations; A heating system configured to control the temperature of the first station independently of the temperature of a second station in one or more reaction chambers; A pressure system configured to maintain pressure in two or more stations; Annealing chambers, configured to perform annealing processes on pairs of substrates; as well as A controller configured to control one or more reaction chambers, a heating system, a pressure system, and an annealing chamber to perform the method as described in claim 1.