Methods for removing the coating on the back side of a wafer and semiconductor structure

By pre-applying a sacrificial layer on the back of the wafer and using a low-temperature fluorine-containing etching solution to remove the coating, the problem of difficult removal of the coating on the back of the wafer is solved, achieving efficient and low-cost pollution control, which is suitable for the mass production of new devices.

CN123124768APending Publication Date: 2026-11-17YANXIN MICROELECTRONICS (SHANGHAI) CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611104688.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-23
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies are unable to effectively remove unintended coatings on the back and sidewalls of wafers, leading to deterioration of device electrical performance and cross-contamination, which affects the large-scale mass production of new devices.

Method used

A sacrificial layer is pre-placed on the back and sidewalls of the wafer, and a low-temperature fluorine-containing etching solution is used to remove the sacrificial layer, thereby achieving overall peeling around the coating and protecting the target functional layer on the front of the wafer from damage.

Benefits of technology

It achieves complete removal of the coating without direct etching, avoiding the problems of low etching efficiency, high cost and incomplete removal of non-target layers, and improving the electrical stability of the device and the mass production yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124768A_ABST
    Figure CN123124768A_ABST
Patent Text Reader

Abstract

This application relates to a method for removing a wraparound coating on the back side of a wafer and a semiconductor structure. The method includes: providing a wafer and cleaning its surface; forming a sacrificial layer on the back side and sidewalls of the wafer; depositing a target functional layer on the front side of the wafer using thermal atomic layer deposition or chemical vapor deposition at a deposition temperature of 200℃ to 400℃, with a precursor for the target functional layer forming a wraparound coating on the surface of the sacrificial layer on the back side and sidewalls of the wafer; preparing a low-temperature fluorine-containing etchant at a temperature of 0℃ to 10℃; protecting the front side of the wafer with an etch-resistant layer; removing the sacrificial layer and the wraparound coating adhering to the sacrificial layer using the low-temperature fluorine-containing etchant; removing the etch-resistant layer; cleaning and drying the wafer. This method eliminates the need for direct etching of the wraparound coating, and the material and thickness of the wraparound coating do not affect the removal effect, avoiding problems such as low etching efficiency, high cost, and incomplete removal of non-target layers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of integrated circuit technology, and in particular to a method for removing a coating layer around the back of a wafer and a semiconductor structure. Background Technology

[0002] As post-Moore's Law semiconductor technology accelerates its evolution towards 3D integration, in-memory computing, and edge intelligence, standard CMOS back-end processes have evolved from a single metal interconnect platform into an integrated carrier for heterogeneous devices such as new types of memory and transistors. Currently, novel devices such as resistive random access memory (RRAM), phase-change memory (PCRAM), magnetic random access memory (MRAM), and oxide semiconductor thin-film transistors have become the hardware foundation for high-density memory chips, in-memory computing chips, and flexible electronic systems. The functional layers of these devices are typically fabricated using thin-film deposition processes with good coverage, such as atomic layer deposition (ALD) and chemical vapor deposition (CVD). However, due to multiple factors, including the flow field distribution in the reaction chamber, the diffusion characteristics of the precursor gas phase, and wafer warpage, these processes are prone to forming unintended coatings on the back side and sidewalls of the wafer.

[0003] Traditional sacrificial layer and back-side cleaning solutions in semiconductor manufacturing are mainly designed for front-end CMOS processes (such as STI silicon nitride etching and front-side particle removal), and cannot effectively remove the coating layers formed on the back side and sidewalls of the wafer. Conventional wet cleaning, back-side dry etching, and edge masking methods are insufficient to completely remove these highly stable films. Residues can lead to degradation of device electrical performance and cross-contamination, hindering the large-scale mass production of new devices. Summary of the Invention

[0004] Based on this, it is necessary to provide a method and semiconductor structure for removing the wrap-around coating on the back side of a wafer to address the problems in the prior art. A sacrificial layer is pre-placed on the back side and sidewalls of the wafer, which protects the target functional layer or device structure on the front side of the wafer, so that the entire wrap-around coating is formed on the sacrificial layer. The sacrificial layer is removed by etching with a low-temperature fluorine-containing etchant, so that the wrap-around coating is peeled off as a whole with the sacrificial layer, thereby avoiding front-side contamination and simplifying the post-integration process.

[0005] In this application, the coating around the wafer refers to a non-target layer formed on the back and / or sidewalls of the wafer due to precursor diffusion, cavity flow field, ion bombardment, or deposition of process byproducts during the target deposition process or target processing on the front side of the wafer.

[0006] In a first aspect, this application provides a method for removing a coating around the back of a wafer, the method comprising the following steps:

[0007] Provide a wafer and clean the surface of the wafer;

[0008] A sacrificial layer is formed on the back side and sidewalls of the wafer;

[0009] The target functional layer is deposited on the front side of the wafer using thermal atomic layer deposition or chemical vapor deposition at a deposition temperature of 200℃~400℃. The precursor of the target functional layer is used to form a coating around the sacrificial layer on the back side and sidewall of the wafer.

[0010] A low-temperature fluorine-containing corrosive solution is prepared, wherein the low-temperature fluorine-containing corrosive solution comprises a fluorine-containing corrosive component and water, and the temperature of the low-temperature fluorine-containing corrosive solution is 0℃~10℃; the fluorine-containing corrosive component comprises hydrofluoric acid, or comprises hydrofluoric acid and ammonium fluoride;

[0011] An anti-etching layer is used to protect the front side of the wafer, and the low-temperature fluorine-containing etching solution is used to remove the sacrificial layer and the wrap-around coating attached to the sacrificial layer;

[0012] Remove the etch-resistant layer, clean and dry the wafer.

[0013] In one embodiment, the low-temperature fluorinated corrosive liquid comprises hydrofluoric acid and deionized water; wherein the mass fraction of hydrofluoric acid is 2wt% to 25wt%.

[0014] In one embodiment, the low-temperature fluorinated corrosive liquid comprises hydrofluoric acid, ammonium fluoride, and deionized water; wherein the mass fraction of hydrofluoric acid is 0.2wt% to 5wt%, and the mass fraction of ammonium fluoride is 5wt% to 35wt%.

[0015] In one embodiment, the low-temperature fluorine-containing corrosive liquid is a buffered oxide corrosive liquid, wherein the molar ratio of ammonium fluoride to hydrofluoric acid in the buffered oxide corrosive liquid is 4:1 to 20:1.

[0016] In one embodiment, the low-temperature fluorinated corrosive liquid further includes a surface tension modifier, which includes at least one of isopropanol, ethanol, or a nonionic surfactant.

[0017] In one embodiment, before forming a sacrificial layer on the back side and sidewalls of the wafer, the cleaned wafer is pre-annealed in an atmosphere of inert gas and hydrogen to eliminate lattice defects and dangling bonds on the back side of the wafer. The treatment temperature is 700°C to 800°C and the treatment time is 5 min to 30 min.

[0018] In one embodiment, forming a sacrificial layer on the back side and sidewalls of the wafer includes:

[0019] A low-temperature ultraviolet-assisted furnace tube thermal oxidation process is used to simultaneously generate a sacrificial layer with a thickness of 5nm to 20nm on the front, back, and sidewalls of the wafer. Specifically, the wafer is first irradiated with 185nm and / or 254nm ultraviolet light in an oxygen-containing atmosphere at 300℃ to 500℃ to form an initial oxidation nucleation layer on the surface of the wafer. Then, the temperature is raised to 800℃ to 1000℃ for dry oxygen oxidation to form the sacrificial layer.

[0020] The back side and sidewalls of the wafer are shielded by a mask, and the sacrificial layer on the front side of the wafer is removed by selective wet etching with diluted hydrofluoric acid at a volume ratio of 1:50 to 1:200, while the sacrificial layer on the back side and sidewalls of the wafer is retained.

[0021] In one embodiment, the low-temperature ultraviolet-assisted furnace tube thermal oxidation process has the following characteristics: the oxygen flow rate is 1 slm to 5 slm, the ultraviolet nucleation time is 3 min to 8 min, and the thickness of the sacrificial layer is 15 nm to 20 nm.

[0022] In one embodiment, forming a sacrificial layer on the back side and sidewalls of the wafer includes:

[0023] A protective layer is deposited on the front side of the wafer at a temperature of 200℃ to 300℃, and the thickness of the protective layer is 0.3nm to 2nm.

[0024] The wafer is flipped so that the back side faces up, and a sacrificial layer with a thickness of 30 nm to 100 nm is deposited on the back side and sidewalls of the wafer at a deposition temperature of 175 °C to 400 °C. Part of the sacrificial layer is deposited around the protective layer on the front side of the wafer.

[0025] Flip the wafer so that the front side is facing up, remove the protective layer on the front side of the wafer, and simultaneously remove the sacrificial layer deposited around the protective layer.

[0026] In one embodiment, a dilute hydrofluoric acid solution is sprayed onto the front side of the wafer to remove the protective layer.

[0027] In one embodiment, the removal of the sacrificial layer and the wrap-around coating adhering to the sacrificial layer using the low-temperature fluorine-containing etching solution includes:

[0028] The wafer is immersed in the low-temperature fluorine-containing etching solution and the wafer is vibrated with an ultrasonic power of 50W to 100W until more than 90% of the thickness of the sacrificial layer is removed.

[0029] The front side of the wafer is placed against a rotating stage and rotated at a speed of 500 rpm to 1500 rpm. At the same time, the back side and sidewalls of the wafer are sprayed with the low-temperature fluorine-containing etching solution to remove the remaining sacrificial layer and the wrap-around coating attached to the sacrificial layer.

[0030] In one embodiment, the target functional layer is a single layer formed of one material selected from the following materials, or a multilayer formed of at least two materials selected from the following materials:

[0031] Metal oxides: tantalum oxide, hafnium oxide, zirconium oxide, hafnium aluminum oxide, hafnium silicon oxide, titanium oxide, niobium oxide, gallium oxide, vanadium oxide;

[0032] Metal nitrides: titanium nitride, tantalum nitride, gallium nitride;

[0033] Oxide semiconductors: Indium gallium zinc oxide, indium oxide, indium aluminum zinc oxide;

[0034] Sulfur alloys: germanium-antimony-tellurium alloy, germanium-tellurium alloy, germanium-sulfur alloy, indium-tellurium alloy, germanium-selenium alloy.

[0035] In one embodiment, the method for removing the wafer backside coating is applied to a CMOS process to fabricate at least one device among resistive random access memory, phase change memory, magnetic memory, and oxide semiconductor thin film transistor.

[0036] Secondly, this application provides a semiconductor structure, comprising:

[0037] A wafer, the wafer including a front side, a back side, and a sidewall connecting the front side and the back side;

[0038] The target functional layer is located on the front side of the wafer;

[0039] The back surface and sidewalls of the wafer are the surfaces after the sacrificial layer has been removed, and there is no continuously distributed material of the target functional layer on the back surface and sidewalls of the wafer.

[0040] In one embodiment, the target functional layer includes at least one of a metal oxide, a metal nitride, an oxide semiconductor, or a chalcogenide alloy.

[0041] In one embodiment, when the back side and / or sidewalls of the wafer are detected using at least one of X-ray photoelectron spectroscopy or secondary ion mass spectrometry, no characteristic element signal of the target functional layer is detected.

[0042] In one embodiment, when the back side and / or sidewalls of the wafer are inspected using a transmission electron microscope or an ellipsometry, the continuously distributed target functional layer is not detected; and / or, when the back side of the wafer is inspected using an atomic force microscope, the surface roughness Ra of the back side of the wafer is less than or equal to 0.5 nm.

[0043] In one embodiment, after surface collection treatment of the back side and / or sidewalls of the wafer, the extract is collected, and the extract is detected by inductively coupled plasma mass spectrometry. The areal density of the elements in the target functional layer is less than 1 × 10⁻⁶. 10 atoms / cm 2 .

[0044] In one embodiment, the semiconductor structure includes at least one of resistive switching memory, phase-change memory, magnetic memory, or oxide semiconductor thin-film transistor integrated into the back-end of CMOS.

[0045] The method and semiconductor structure for removing the back-side coating of a wafer disclosed in this application form a sacrificial layer on the back side of the wafer so that the non-target layer deposited by the thermal atomic layer deposition process is attached to the surface of the sacrificial layer. By utilizing the high etching selectivity of wet etching solution for the sacrificial oxide layer and the substrate, the back-side coating is simultaneously removed by selectively etching the sacrificial layer. This eliminates the need for direct etching of the back-side coating, and the material and thickness of the back-side coating do not affect the removal effect. This avoids problems such as low etching efficiency, high cost, and incomplete removal of non-target layers. Attached Figure Description

[0046] To more clearly illustrate the technical solutions in the embodiments of this application or the conventional technology, the drawings used in the description of the embodiments or the conventional technology will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0047] Figure 1 This is a process flow diagram of a method for removing the back-side coating of a wafer provided in one embodiment;

[0048] Figure 2 A process flow diagram of a method for removing the back-side coating of a wafer provided in another embodiment;

[0049] Figure 3 This is a process flow diagram of a method for removing the back-side coating of a wafer provided in another embodiment. Detailed Implementation

[0050] To facilitate understanding of this application, a more complete description will be provided below with reference to the accompanying drawings, which illustrate preferred embodiments of the application. However, this application may be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided so that the disclosure of this application will be thorough and complete.

[0051] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application.

[0052] With the development of integrated circuits, new devices are increasingly being integrated into the back-end processes of standard complementary metal-oxide-semiconductor (CMOS) wafers. The materials used for the functional layers of these new devices include high-k metal oxides such as HfOx, TaOx, ZrOx, and NbOx; metal nitrides such as TiN and GaN; oxide semiconductors such as IGZO and InO; and chalcogenide alloys such as GST (Ge2Sb2Te5) and GeTe. Taking thermal atomic layer deposition (TAD) as an example, due to the influence of cavity gas flow and precursor gas phase diffusion, these elements are highly susceptible to unintended deposition on the back side and sidewalls of the wafer, forming a difficult-to-remove non-target residual layer on the back side.

[0053] Conventional back-side processing methods are insufficient to address the issue of residual non-target layers. On one hand, high-stability films such as HfOx and GST are highly resistant to corrosion and cannot be completely removed by conventional cleaning. Residual elements such as In, Te, and Hf will diffuse into the substrate during subsequent high-temperature processes, causing permanent wafer contamination. On the other hand, residual contaminants will accumulate within the process chamber, leading to cross-contamination between different batches of wafers on the same machine, severely damaging the electrical stability and mass production yield of CMOS back-end integrated devices.

[0054] In view of this, this application provides a method and semiconductor structure for removing the back-side coating of a wafer. By pre-preparing a sacrificial layer on the back side of the wafer, the non-target layer on the back side of the wafer is isolated. Finally, the sacrificial layer and the non-target layer on the back side are removed simultaneously by highly selective wet etching. This method breaks through the traditional shielding protection method and proposes a protection method of "protecting the surface to be retained first, and then flipping to prepare the surface to be etched". This eliminates the problems of secondary contamination, process complexity and protection failure caused by the protection process from the root. At the same time, the sacrificial layer has the advantages of completely isolating contamination and removing it without damage. It can achieve higher yield, higher efficiency and lower cost wafer back-side contamination control, and is suitable for mass production scenarios of all types of semiconductor processes such as advanced processes, ultra-thin wafers and flexible substrates.

[0055] Please see Figure 1 This application provides a method for removing the coating around the back of a wafer, including steps S101-S106.

[0056] Step S101: Provide a wafer and clean the wafer surface.

[0057] The wafer can be an 8-inch silicon wafer, a 12-inch silicon wafer, a compound semiconductor wafer, or a panel-level substrate. The front side of the wafer can be pre-formed with semiconductor front-end device structures, dielectric layers, metal interconnect layers, or micro / nano structures, such as front-end CMOS circuits. Therefore, the method of this application is compatible with CMOS processes, third-generation semiconductor fabrication, MEMS device manufacturing, advanced packaging, and other general semiconductor processes. The wafer undergoes RCA standard semiconductor cleaning to remove particles, organic matter, metallic impurities, and native oxide layers from the wafer surface. After cleaning, the wafer is dried using high-purity nitrogen gas.

[0058] Step S102: Form a sacrificial layer on the back side and sidewalls of the wafer.

[0059] The sacrificial layer can be an oxide layer, such as a silicon oxide layer. For example, the sacrificial layer can be formed using a thermal oxidation process, or it can be formed on the back side and sidewalls of the wafer using a deposition process.

[0060] Step S103: The target functional layer is deposited on the front side of the wafer using thermal atomic layer deposition or chemical vapor deposition at a deposition temperature of 200℃~400℃. The precursor of the target functional layer is used to form a coating around the sacrificial layer on the back side and sidewall of the wafer.

[0061] The processed wafer is placed in the reaction chamber of Thermal Atomic Layer Deposition (TALD). A target functional layer is deposited on the front side of the wafer to form the target device or functional film. During deposition, influenced by the chamber flow field, precursor vapor diffusion, and wafer clamping structure, the precursor of the TALD deposit undergoes vapor diffusion, spreading to the back side and sidewalls of the wafer, forming a wraparound layer on the sacrificial layer surface with the same material as the target functional layer on the front side. The material of the wraparound layer is at least partially the same as the target functional layer material, and the wraparound layer covers the edge regions of the wafer's sidewalls and back side.

[0062] Step S104: Prepare a low-temperature fluorine-containing corrosive solution, which includes a fluorine-containing corrosive component and water; the temperature of the low-temperature fluorine-containing corrosive solution is 0℃~10℃. The fluorine-containing corrosive component includes hydrofluoric acid, or includes hydrofluoric acid and ammonium fluoride.

[0063] By controlling the temperature of the low-temperature fluorine-containing etching solution between 0℃ and 10℃, the volatilization of fluorine-containing etching components can be reduced, the damage of acid mist to the target functional layer or device structure on the front side of the wafer can be reduced, and the corrosion rate fluctuation can be reduced, thereby improving the uniformity of sacrificial layer removal.

[0064] In some embodiments, the low-temperature fluorine-containing corrosion solution comprises hydrofluoric acid and deionized water, wherein the mass fraction of hydrofluoric acid is 2 wt% to 25 wt%, preferably 3 wt% to 8 wt%. In other embodiments, the low-temperature fluorine-containing corrosion solution comprises hydrofluoric acid, ammonium fluoride, and deionized water, wherein the mass fraction of hydrofluoric acid is 0.2 wt% to 5 wt%, and the mass fraction of ammonium fluoride is 5 wt% to 35 wt%. Ammonium fluoride can act as a buffer component to stabilize the concentration of active fluorine species in the low-temperature fluorine-containing corrosion solution, thereby improving the controllability of the sacrificial layer corrosion rate.

[0065] In some embodiments, the low-temperature fluorinated corrosive solution is a buffered oxide corrosive solution, wherein the molar ratio of ammonium fluoride to hydrofluoric acid in the buffered oxide corrosive solution is 4:1 to 20:1. For example, the molar ratio of ammonium fluoride to hydrofluoric acid can be 4:1, 6:1, 7:1, 8:1, 10:1, 13:1, 15:1, 16:1, 18:1, or 20:1.

[0066] In some embodiments, the low-temperature fluorinated etching solution further includes a surface tension modifier, which includes at least one of isopropanol, ethanol, or a nonionic surfactant. By reducing the surface tension of the low-temperature fluorinated etching solution with a surface tension modifier, its wettability to the back side, sidewalls, and areas around the coating cracks or edges of the wafer can be improved, promoting the etching solution to enter the interface between the sacrificial layer and the coating, thereby improving the efficiency of the coating peeling off along with the sacrificial layer as a whole.

[0067] In this embodiment, a low-temperature fluorine-containing etching solution is prepared using hydrofluoric acid mother liquor and deionized water. The hydrofluoric acid mother liquor is an aqueous solution of hydrofluoric acid, preferably an electronic-grade aqueous solution of hydrofluoric acid, and the mass fraction of hydrofluoric acid in the hydrofluoric acid mother liquor is 40wt% to 50wt%, for example, 49wt%. In some examples, the mass ratio of hydrofluoric acid mother liquor to deionized water is 1:1 to 1:3.

[0068] Step S105: Protect the front side of the wafer with an anti-etching layer, and remove the sacrificial layer and the wrap-around coating attached to the sacrificial layer with a low-temperature fluorine-containing etching solution.

[0069] An etch resist layer is formed on the front side of the wafer. This etch resist layer shields and covers the target functional layers on the front side of the wafer to protect the front-side devices. For example, the etch resist layer can be a photoresist resistant to hydrofluoric acid corrosion.

[0070] In this embodiment, a low-temperature fluorine-containing etching solution of 0℃~10℃ is used to remove the sacrificial layer and the coating layer attached to the sacrificial layer. This can significantly reduce the saturated vapor pressure of hydrofluoric acid, inhibit the volatilization of hydrofluoric acid, and prevent the volatilized hydrofluoric acid gas from diffusing to the front side of the wafer and causing device damage. At the same time, it can control the etching rate and improve the uniformity of etching across the entire surface.

[0071] Step S106: Remove the resist layer, clean and dry the wafer.

[0072] After removing the anti-etching layer on the front side, the wafer undergoes hydrophilic treatment via SC1 / SC2 and standard semiconductor cleaning, followed by drying, resulting in a wafer with a clean back side and intact devices on the front side.

[0073] The above-mentioned method for removing the coating around the back of a wafer forms a sacrificial layer on the back of the wafer, so that the non-target layer deposited by the thermal atomic layer deposition process is attached to the surface of the sacrificial layer. The high etching selectivity of the wet etching solution for the sacrificial oxide layer and the substrate is utilized to selectively etch the sacrificial layer and simultaneously peel off the coating around it. There is no need to directly etch the coating around it. The material and thickness of the coating around it do not affect the removal effect, thus avoiding problems such as low etching efficiency, high cost and incomplete removal of non-target layers.

[0074] In some embodiments, step S105 uses a low-temperature fluorine-containing etching solution to remove the sacrificial layer and the coating layer attached to the sacrificial layer, and uses a low-temperature two-step wet etching process to remove the sacrificial layer, including steps S1051-S1052.

[0075] Step S1051: Immerse the wafer in a low-temperature fluorine-containing etching solution and vibrate the wafer with an ultrasonic power of 50W to 100W until more than 90% of the sacrificial layer thickness is removed.

[0076] The wafer can be vertically immersed in a low-temperature fluorine-containing etching solution, accompanied by ultrasonic vibration, to remove part of the sacrificial layer. The ultrasonic vibration power can be 50W~100W, removing more than 90% of the sacrificial layer thickness, causing most of the coating around the sacrificial layer to lose adhesion. In particular, ultrasonic vibration can promote the detachment of etching by-products (coating around the wafer) from the wafer surface, avoiding uneven etching caused by by-product adhesion, and at the same time accelerating the whole-wafer peeling of non-target layers.

[0077] Step S1052: Place the front side of the wafer against the rotating stage and rotate it at a speed of 500 rpm to 1500 rpm. At the same time, spray the back side and sidewalls of the wafer with a low-temperature fluorine-containing etching solution to remove the remaining sacrificial layer and the wrap-around coating attached to the sacrificial layer.

[0078] The wafer is removed from the low-temperature fluorine-containing etching solution and placed on a rotating stage with the front side facing the stage. The wafer is rotated at 500 rpm to 1500 rpm, and the back side and sidewalls are sprayed with the low-temperature fluorine-containing etching solution to remove any remaining sacrificial and wrap-around coatings. For example, the wafer can be rotated at 1000 rpm, and the back side and sidewalls can be sprayed with the same low-temperature fluorine-containing etching solution of the same composition and temperature for 30 to 120 seconds to remove any remaining sacrificial and wrap-around coatings, as well as any remaining non-target layers. During the rotational rinsing process, centrifugal force allows the etching solution and etching byproducts to quickly detach from the wafer surface, completely solving the problem of byproduct re-adhesion, while simultaneously achieving uniform etching across the entire back side of the wafer, eliminating etching differences between the edges and the center.

[0079] This embodiment employs a low-temperature two-step wet etching process to remove the sacrificial layer, reducing the saturated vapor pressure of hydrofluoric acid, suppressing the volatilization of hydrofluoric acid mist, and avoiding damage to the front-side devices caused by the diffusion of acid mist during room-temperature hydrofluoric acid etching. Ultrasonic vibration promotes the removal of etching byproducts from the wafer surface, and rotational rinsing utilizes centrifugal force to rapidly desorb reaction products, thereby avoiding secondary contamination caused by the re-adhesion of byproducts such as fluorosilicic acid, achieving uniform etching of the entire back side of the wafer.

[0080] In some embodiments, a target functional layer is deposited on the front side of the wafer using thermal atomic layer deposition or chemical vapor deposition. The target functional layer is a single film layer formed from one of the following materials, or a multilayer film formed from at least two of the following materials:

[0081] Metal oxides: tantalum oxide (TaOx), hafnium oxide (HfOx), zirconium oxide (ZrOx), hafnium aluminum oxide (HfAlO), hafnium silicon oxide (HfSiO), titanium oxide (TiO), niobium oxide (NbOx), gallium oxide (GaOx), vanadium oxide (VOx).

[0082] Metal nitrides: titanium nitride (TiN), tantalum nitride (TaN), gallium nitride (GaN).

[0083] Oxide semiconductors: Indium gallium zinc oxide (IGZO), indium oxide (InO), and indium aluminum zinc oxide (IAZO).

[0084] Sulfur alloys: Germanium-antimony-tellurium alloy (GST), germanium-tellurium alloy (GeTe), germanium-sulfur alloy (GeS), indium-tellurium alloy (InTe), and germanium-selenium alloy (GeSe).

[0085] In some embodiments, the method of removing the wafer backside coating is applied to a CMOS process to fabricate at least one device among resistive random access memory, phase change memory, magnetic memory, and oxide semiconductor thin film transistor.

[0086] In some embodiments, the formation of resistive switching memory, phase-change memory, magnetic memory, and oxide semiconductor thin-film transistors on the front side can also employ any one or more of the following processes: atomic layer deposition, chemical vapor deposition, physical vapor deposition, ion implantation, high-temperature thermal treatment, and dry etching. Specifically, atomic layer deposition includes any one of thermal atomic layer deposition, plasma-enhanced atomic layer deposition, space atomic layer deposition, and metal-organic atomic layer deposition; chemical vapor deposition includes any one of plasma-enhanced chemical vapor deposition, low-pressure chemical vapor deposition, metal-organic chemical vapor deposition, and high-density plasma chemical vapor deposition; physical vapor deposition includes any one of magnetron sputtering, electron beam evaporation, and ion beam sputtering; high-temperature thermal treatment includes any one of high-temperature annealing, rapid thermal annealing, and thermal diffusion doping; and dry etching includes any one of reactive ion etching, deep reactive ion etching, and ion beam etching.

[0087] In some embodiments, a thermal oxidation process is used to form the sacrificial layer. The method for removing the wafer backside coating in this embodiment is described in reference to... Figure 2 As shown, it includes steps S201-S209.

[0088] Step S201: Provide a wafer and clean its surface. Use RCA standard cleaning to remove particles, organic matter, metallic impurities, and native oxide layer from the wafer surface. After cleaning, dry the wafer with high-purity nitrogen gas.

[0089] Step S202: The cleaned wafer is pre-annealed in an atmosphere of inert gas and hydrogen to eliminate lattice defects and dangling bonds on the back side of the wafer. The treatment temperature is 700℃~800℃ and the treatment time is 5min~30min.

[0090] Step S203: Using a thermal oxidation process, a sacrificial layer is grown on the surface of the wafer, continuously covering the back side, sidewalls, and front side of the wafer. For example, a furnace tube thermal oxidation process can be used to grow a dense silicon oxide layer as a sacrificial layer on the back side of the pre-annealed wafer, with the sacrificial layer simultaneously grown on the front side of the wafer.

[0091] In some embodiments, pre-annealing the cleaned wafer includes: placing the wafer in a vertical oxidation furnace, introducing a protective gas into the furnace, heating to a preset pre-annealing temperature of 700°C to 800°C, and holding at that temperature for 10 to 30 minutes to complete the annealing. The protective gas can be a mixture of at least one of argon and nitrogen with hydrogen, and the volumetric flow rate ratio of the inert gas to hydrogen is 10:1 to 2:1. High-temperature hydrogen annealing of the wafer reduces the natural oxidation residue on the silicon surface, thereby eliminating lattice defects and dangling bonds on the wafer surface, reducing the impurity density on the wafer surface, providing a uniform nucleation interface for subsequent sacrificial layer growth, and simultaneously improving the interfacial adhesion between the sacrificial layer and the wafer, preventing the sacrificial layer from detaching in subsequent processes.

[0092] Step S204: Using a low-temperature UV-assisted furnace tube thermal oxidation process, a sacrificial layer with a thickness of 5nm to 20nm is simultaneously generated on the front, back, and sidewalls of the wafer. Specifically, the wafer is first irradiated with 185nm and / or 254nm UV light in an oxygen-containing atmosphere at 300℃ to 500℃ to form an initial oxidation nucleation layer on the surface of the wafer. Then, the temperature is raised to 800℃ to 1000℃ for dry oxygen oxidation to form the sacrificial layer.

[0093] Furthermore, the low-temperature ultraviolet-assisted furnace tube thermal oxidation process has the following characteristics: oxygen flow rate of 1 slm to 5 slm, ultraviolet nucleation time of 3 min to 8 min, and sacrificial layer thickness of 15 nm to 20 nm.

[0094] Step S205: Using a mask to shield the back side and sidewalls of the wafer, selective wet etching is performed using diluted hydrofluoric acid with a volume ratio of 1:50 to 1:200 to remove the sacrificial layer on the front side of the wafer, while retaining the sacrificial layers on the back side and sidewalls. At this ratio, the etching selectivity ratio of hydrofluoric acid for the sacrificial layer (silicon oxide) to the wafer (monocrystalline silicon) is greater than 10000:1.

[0095] In this embodiment, a photoresist layer resistant to hydrofluoric acid corrosion is first coated on the back side of the wafer, or a wafer jig is used to physically shield the back side of the wafer, covering and protecting the back side and sidewalls. The sacrificial layer on the front side of the wafer is then completely removed using a highly selective wet etching process. After removing the photoresist layer on the back side, standard semiconductor cleaning and hydrophilic treatment are performed to obtain a wafer with a sacrificial layer covering the back and sidewalls and the front side exposed.

[0096] Step S206: The target functional layer is deposited on the front side of the wafer using a thermal atomic layer deposition process at a deposition temperature of 200℃~400℃. The precursor of the target functional layer is used to form a wrap-around coating on the sacrificial layer surface on the back side and sidewall of the wafer.

[0097] Step S207: Prepare a low-temperature fluorine-containing etching solution with a temperature of 0℃~10℃.

[0098] Step S208: Protect the front side of the wafer with an anti-etching layer, and remove the sacrificial layer and the wrap-around coating attached to the sacrificial layer with a low-temperature fluorine-containing etching solution.

[0099] Step S209: Remove the resist layer, clean and dry the wafer.

[0100] In this embodiment, the implementation of steps S206-S209 is the same as that of steps S103-S106 in the above embodiment, and will not be described again.

[0101] In some embodiments, the growth of a sacrificial layer on the wafer surface using a thermal oxidation process includes: after pre-annealing, lowering the oxidation furnace temperature to 300°C~500°C, introducing high-purity oxygen into the furnace and irradiating with ultraviolet light to form an initial silicon oxide nucleation layer on the wafer surface; subsequently, stopping ultraviolet irradiation, raising the furnace temperature to 800°C~1000°C, and completing the thermal oxidation using a dry oxygen oxidation process to grow a SiO2 sacrificial layer with a thickness of 5nm~20nm on the back side of the wafer. Low-temperature ultraviolet-assisted oxidation can form a uniform and continuous initial nucleation layer on the silicon surface, avoiding uneven oxidation rates during subsequent high-temperature oxidation and significantly improving the uniformity of the sacrificial layer thickness. For processes requiring multiple high-temperature processes and multiple cleaning steps, the sacrificial layer thickness can be set to 15nm~20nm, reserving an etching loss window during the process to ensure the complete preservation of the sacrificial layer after the entire process.

[0102] In some embodiments, the ultraviolet wavelength of the ultraviolet lamp irradiation is 185nm and / or 254nm; the flow rate of high-purity oxygen is 1slm to 5slm, for example, it can be 1slm, 2slm, 3slm, 4slm or 5slm; the growth time of the initial silicon oxide nucleation layer is 3min to 8min.

[0103] In some embodiments, the ultraviolet light emitted by the ultraviolet lamp has a wavelength of 185 nm. 185 nm ultraviolet light can decompose oxygen into atomic oxygen and ozone, significantly improving the oxidation efficiency at low temperatures and forming a uniform nucleation layer without high-temperature damage.

[0104] In some embodiments, a sacrificial layer may be formed by depositing a wafer after flipping it. The method for removing the wafer backside coating in this embodiment is described in reference to... Figure 3 As shown, it includes steps S301-S308.

[0105] Step S301: Provide a wafer and clean its surface. Perform RCA standard cleaning on the wafer to remove particles, organic matter, metallic impurities, and the native oxide layer from the wafer surface. After cleaning, dry the wafer with high-purity nitrogen gas.

[0106] Step S302: Deposit a protective layer on the front side of the wafer at a temperature of 200℃~300℃. The thickness of the protective layer is 0.3nm~2nm. For example, the thickness of the protective layer is 0.5nm. The protective layer can protect the front side of the wafer from oxidation during the subsequent deposition of the sacrificial layer, and because the protective layer is very thin, it can be completely removed by subsequent cleaning.

[0107] For example, a protective layer can be deposited using plasma-enhanced atomic layer deposition (PELD), chemical vapor deposition (CVD), or atomic layer deposition (ALD).

[0108] Step S303: Flip the wafer so that the back side is facing up, deposit a sacrificial layer with a thickness of 30nm to 100nm on the back side and sidewalls of the wafer, at a deposition temperature of 175℃ to 400℃, and partially deposit the sacrificial layer onto the protective layer on the front side of the wafer.

[0109] In this embodiment, the wafer is flipped 180° so that the back side of the wafer faces upward. Then, a silicon oxide layer with a thickness of 30nm to 100nm can be deposited on the back side of the wafer as a sacrificial layer using PEALD or furnace tube thermal oxidation processes. The deposition temperature can be a low temperature of 175℃ to 400℃ to avoid high temperature affecting the surface states of the front side of the wafer, which is suitable for temperature-sensitive device processes.

[0110] For example, a sacrificial layer can be deposited using plasma-enhanced atomic layer deposition, chemical vapor deposition, or atomic layer deposition.

[0111] Step S304: Flip the wafer so that the front side is facing up, remove the protective layer on the front side of the wafer, and simultaneously remove the sacrificial layer that is plated onto the protective layer.

[0112] In this embodiment, a photoresist layer resistant to hydrofluoric acid corrosion is coated on the back side and sidewalls of the wafer, or a wafer jig is used to physically cover the back side and sidewalls of the wafer. The wafer is then rotated 180° again so that the front side of the wafer is facing upwards.

[0113] The front side of the wafer is cleaned by spraying with a diluted hydrofluoric acid solution to selectively remove the protective layer. Because the protective layer is very thin, the sacrificial layer plating attached to it is simultaneously peeled off during the removal process. After cleaning, a wafer with the back and sidewalls covered by the sacrificial layer and the front side exposed is obtained. In this embodiment, after removing the protective layer, the wafer undergoes standard semiconductor cleaning and hydrophilic treatment.

[0114] Step S305: The target functional layer is deposited on the front side of the wafer using a thermal atomic layer deposition (TAD) process. During the deposition process, the precursor diffuses to the sidewalls and back side of the wafer, forming a wraparound coating attached to the sacrificial layer. For example, the target functional layer can be deposited using either thermal atomic layer deposition or chemical vapor deposition (CVD) at a deposition temperature of 200°C to 400°C.

[0115] Step S306: Prepare a low-temperature fluorine-containing etching solution with a temperature of 0℃~10℃.

[0116] Step S307: Protect the front side of the wafer with an anti-etching layer, and remove the sacrificial layer and the wrap-around coating attached to the sacrificial layer with a low-temperature fluorine-containing etching solution.

[0117] Step S308: Remove the resist layer, clean and dry the wafer.

[0118] In this embodiment, the implementation of steps S305-S308 is the same as that of steps S103-S106 in the above embodiment, and will not be described again.

[0119] It should be noted that the non-target layers removed by the method of this application include not only the coating layer formed during the above-mentioned thermal atomic layer deposition process, but also any one or more of the following: unintended deposited metal thin films, dielectric thin films, composite functional thin films formed by other deposition processes, as well as doped contamination layers, ion bombardment lattice damage layers, and etching by-product deposition layers caused by etching or ion implantation processes on the back side and sidewalls of the wafer.

[0120] The standard semiconductor cleaning in this application is the RCA standard cleaning process, which can employ at least one of the following: sulfuric acid / hydrogen peroxide mixed solution (SPM) cleaning, ammonia / hydrogen peroxide mixed solution (SC1) cleaning, hydrochloric acid / hydrogen peroxide mixed solution (SC2) cleaning, tetramethylammonium hydroxide (TMAH) cleaning, dilute hydrofluoric acid (DHF) cleaning, and deionized water (DIW) cleaning.

[0121] The present application will be further described in detail below with reference to specific embodiments. The following embodiments are only used to illustrate the technical solutions of the present application, and are not intended to limit the scope of protection of the present application.

[0122] Example 1: This example uses a thermal ALD process to deposit a titanium nitride metal gate on the front side of a 12-inch single-crystal silicon wafer, and removes the non-target titanium nitride layer formed on the back side of the wafer during the deposition process. The method for removing the back-side coating in this example includes steps S11-S17.

[0123] Step S11: Wafer preprocessing.

[0124] 12-inch P-type available <100> For monocrystalline silicon wafers, RCA standard cleaning can be performed by sequentially using SPM solution, SC1 solution, SC2 solution, and DHF solution to remove particles, organic matter, metallic impurities, and the native oxide layer from the wafer surface, followed by drying with high-purity nitrogen gas.

[0125] Step S12: Surface state treatment on the back side of the wafer.

[0126] The cleaned wafer is placed in a vertical oxidation furnace, and a protective gas mixture of argon and hydrogen is introduced. The flow rate to volume ratio of argon to hydrogen is 5:1, and the total flow rate is 3 slm. The furnace temperature is raised to 750℃ and held for 20 minutes to complete the pre-annealing treatment, which eliminates lattice defects and dangling bonds on the back side of the wafer, providing a uniform nucleation interface for subsequent oxide layer growth.

[0127] Step S13: Prepare a sacrificial layer on the back side of the wafer.

[0128] After pre-annealing, the furnace temperature is lowered to 400℃, and high-purity oxygen at a flow rate of 2 slm is introduced into the furnace. Simultaneously, dual-wavelength ultraviolet lamps (185nm + 254nm) are turned on to irradiate the wafer for 5 minutes, forming a uniform initial silicon oxide nucleation layer on both the back and front sides of the wafer. Then, ultraviolet irradiation is stopped, and the furnace temperature is raised to 950℃. A dry oxygen oxidation process is used, and the temperature is held for 8 minutes to grow a dense silicon oxide sacrificial layer with a thickness of 10nm on both the back and front sides of the wafer.

[0129] Step S14: Remove the sacrificial layer on the front side of the wafer.

[0130] A thick photoresist protective layer resistant to hydrofluoric acid was coated on the back and sidewalls of the wafer. A hydrofluoric acid solution diluted to deionized water at a volume ratio of 1:100 was used for wet etching to remove the silicon oxide sacrificial layer on the front side of the wafer. The wet etching time was 90 seconds. After rinsing the wafer with deionized water, the photoresist protective layer on the back and sidewalls was removed. The wafer was then hydrophilically treated with SC1 solution, followed by RCA cleaning, resulting in a wafer with a 10nm silicon oxide sacrificial layer on the back and an exposed front side.

[0131] Step S15: Deposit the target functional layer on the front side of the wafer using the thermal ALD process.

[0132] The processed wafer was placed in a monolithic thermal atomic layer deposition (TAL) system to deposit a titanium nitride metal gate film on the front side of the wafer at a deposition temperature of 350°C. The deposition precursors were titanium chloride (TiCl4) and ammonia (NH3). The deposition cycle was 100 times, with a target thickness of 10 nm. During the deposition process, due to the influence of the cavity flow field and precursor gas phase diffusion, the precursors that diffused unexpectedly on the back side of the wafer formed a residual titanium nitride film on the surface of the silicon oxide sacrificial layer.

[0133] Step S16: Remove the sacrificial layer on the back side of the wafer and the non-target layer deposited on the sacrificial layer by wrap-around plating.

[0134] Hydrofluoric acid and deionized water were mixed at a mass ratio of 1:2 and cooled to 6±0.5℃ to prepare a low-temperature fluorine-containing corrosive solution.

[0135] A photoresist protective layer resistant to hydrofluoric acid corrosion is coated on the front side of the wafer. The wafer is then vertically immersed in a low-temperature fluorine-containing etching solution for 60 seconds to remove more than 90% of the silicon oxide sacrificial layer. The immersion process is accompanied by ultrasonic vibration of 80W.

[0136] Remove the wafer from the low-temperature fluorine-containing etching solution, fix the wafer on a rotating wafer stage, control the rotation speed at 1000 rpm, and rinse the back side of the wafer for 60 seconds with a low-temperature fluorine-containing etching solution of the same temperature and composition to completely remove the remaining sacrificial layer and titanium nitride residual film.

[0137] After etching, the back side of the wafer is hydrophilically treated with SC1 solution to remove etching byproducts, and then the front photoresist protective layer is removed.

[0138] Step S17: Perform RCA standard cleaning on the wafer and dry it with high-purity nitrogen.

[0139] The wafer processed in this embodiment was inspected. Atomic force microscopy (AFM) showed that the surface roughness of the back side of the wafer was Ra=0.10nm, which was essentially no different from the original wafer surface. Transmission electron microscopy (TEM) showed no titanium nitride film residue or interface damage. Secondary ion mass spectrometry (SIMS) showed no titanium element signal on the back side of the wafer, and no titanium element diffusion within the wafer. Alternatively, inductively coupled plasma mass spectrometry (ICP-MS) showed that the titanium element signal on the back side of the wafer was less than 1×10⁻⁶. 10 atoms / cm 2 The uniformity deviation of the titanium nitride film thickness on the front side of the wafer is <0.7%, and there is no degradation in electrical performance; no etching damage to the front-side devices is found in the entire batch of wafers, and the product yield is improved by more than 35% compared with the direct cleaning process.

[0140] Example 2: This example pertains to the full-process thermal ALD process for resistive random access memory (RRAM). The method for removing the back-side coating of the wafer in this example includes steps S21-S27.

[0141] Step S21: Wafer preprocessing.

[0142] This embodiment provides a 12-inch single-crystal silicon wafer. The front-end CMOS driving circuit has been fabricated on the front side of the wafer. The wafer is then subjected to RCA standard cleaning and dried with high-purity nitrogen.

[0143] Step S22: Surface state treatment on the back side of the wafer.

[0144] The wafer is placed in a vertical oxidation furnace, and a protective gas mixture of argon and hydrogen is introduced. The volume flow rate ratio of argon to hydrogen is 10:1, and the total flow rate is 4 slm. The furnace temperature is raised to 800℃ and held for 10 minutes to complete the pre-annealing treatment.

[0145] Step S23: Prepare a sacrificial layer on the back side of the wafer.

[0146] After pre-annealing, the furnace temperature is lowered to 500℃, high-purity oxygen at a flow rate of 4 slm is introduced, and a 185nm ultraviolet lamp is turned on for 3 minutes to form the initial silicon oxide nucleation layer. Then, the ultraviolet irradiation is stopped, the furnace temperature is raised to 1000℃, and dry oxygen oxidation is carried out for 15 minutes to grow a 20nm thick silicon oxide sacrificial layer on the back side of the wafer, leaving an etching loss window for multiple cleaning processes in the previous stage.

[0147] Step S24: Remove the positive sacrifice layer.

[0148] A photoresist protective layer was coated on the back side of the wafer. The front silicon oxide sacrificial layer was etched using a diluted hydrofluoric acid solution with a hydrofluoric acid to deionized water volume ratio of 1:200. After etching, the photoresist was removed. Hydrophilic treatment and cleaning were performed using SC1 solution to obtain a wafer with a 20nm thick silicon oxide sacrificial layer on the back side.

[0149] Step S25: Deposit a metal thin film on the front side of the wafer.

[0150] The wafer is placed in a thermal ALD apparatus to perform continuous thermal ALD deposition of the niobium oxide (NbOx) resistive switching functional layer and the titanium nitride (TiN) electrode layer at a deposition temperature of 320°C. During the deposition process, residual NbOx and TiN films are simultaneously formed on the back side of the wafer.

[0151] Step S26: Simultaneously remove the sacrificial layer and residual film on the back side and sidewalls of the wafer.

[0152] HF and deionized water were mixed at a mass ratio of 1:3 and cooled to 7±0.5℃ to obtain a low-temperature HF etching solution.

[0153] A photoresist protective layer is coated on the front side of the wafer. The wafer is then immersed in a low-temperature HF etching solution for 100 seconds, accompanied by 100W ultrasonic vibration, to remove 90% of the sacrificial layer.

[0154] Afterwards, the wafer is fixed on a rotating stage at 1500 rpm and rinsed with a low-temperature HF etching solution at the same temperature for 30 seconds to remove the remaining sacrificial layer and residual film.

[0155] The wafer was hydrophilically treated sequentially with SC1+SC2 solution to remove byproducts and metal impurities, and to remove the photoresist on the front side.

[0156] Step S27: Perform RCA standard cleaning on the wafer, dry it with high-purity nitrogen, and proceed to the subsequent metallization process.

[0157] The wafer processed in this embodiment was tracked throughout the entire process: after five front-end cleaning processes, the sacrificial layer on the back of the wafer still retained a complete thickness of more than 13nm; finally, there were no thin film residues or metal contamination on the back of the wafer product, and the switching ratio, holding characteristics and cycle life of the resistive switching memory all met the design requirements, and the product yield was improved by 36% compared with the direct cleaning process.

[0158] Example 3: This example is for the process of depositing silicon nitride passivation layer on the front side of an 8-inch wafer using PECVD. The method for removing the non-target layer on the back side in this example includes steps S31-S37.

[0159] Step S31: Wafer preprocessing.

[0160] Offers 8-inch n-type <100> The single-crystal silicon wafer has a CMOS device structure and metal interconnect layer pre-set on the front side. The wafer is cleaned according to RCA standard to remove surface contaminants and then dried with high-purity nitrogen.

[0161] Step S32: Surface state treatment on the back side of the wafer.

[0162] The wafer is placed in a horizontal oxidation furnace, and a mixture of nitrogen and hydrogen protective gas is introduced. The volume flow rate ratio of nitrogen to hydrogen is 8:1, and the total flow rate is 2 slm. The furnace temperature is raised to 700℃ and held for 30 minutes to complete the pre-annealing treatment.

[0163] Step S33: Prepare a sacrificial layer on the back side of the wafer.

[0164] After pre-annealing, the furnace temperature was lowered to 350°C, high-purity oxygen at a flow rate of 3 slm was introduced, and a 254nm ultraviolet lamp was turned on for irradiation. The temperature was held for 8 minutes to form the initial silicon oxide nucleation layer. Subsequently, the ultraviolet irradiation was stopped, the furnace temperature was raised to 900°C, and dry oxygen oxidation was carried out for 12 minutes to grow a 15nm thick silicon oxide sacrificial layer on both the back and front sides of the wafer.

[0165] Step S34: Front Oxide Layer Removal: The back side of the wafer is completely shielded using a dedicated wafer jig. A diluted hydrofluoric acid solution (HF to deionized water volume ratio 1:150) is used for wet etching to remove the SiO2 layer on the front side of the wafer. The etching time is 140 seconds. After rinsing with deionized water, the jig is removed. Hydrophilic treatment and cleaning are then performed sequentially using SC1+SC2 solutions to obtain a wafer with a 15nm thick silicon oxide sacrificial layer on the back side.

[0166] Step S35: Deposit a silicon nitride passivation layer on the front side of the wafer.

[0167] The wafer is placed in a PECVD apparatus, and a silicon nitride passivation layer is deposited on the front side of the wafer at a deposition temperature of 350°C. The precursors are silane (SiH4) and ammonia (NH3), and the deposition thickness is 200 nm. During the deposition process, the precursors diffuse to the back side of the wafer, forming a non-target silicon nitride layer on the surface of the sacrificial layer.

[0168] Step S36: Simultaneously remove the sacrificial layer and non-target layer from the back side and sidewalls of the wafer.

[0169] HF and deionized water were mixed at a mass ratio of 1:1 and cooled to 5.5±0.5℃ to obtain a low-temperature HF etching solution.

[0170] The wafer is shielded by a fixture, and then immersed in a low-temperature HF etching solution for 80 seconds, accompanied by 50W ultrasonic vibration, to remove more than 92% of the sacrificial layer.

[0171] The wafer was fixed on a rotating stage at 500 rpm and rinsed with a low-temperature HF etching solution at the same temperature for 120 seconds to completely remove the remaining sacrificial layer and non-target silicon nitride layer.

[0172] The front clamp was removed after hydrophilic treatment and removal of metallic impurities using SC2 solution.

[0173] Step S37: Perform RCA standard cleaning on the wafer and dry it with high-purity nitrogen.

[0174] The wafer processed in this embodiment was inspected: X-ray photoelectron spectroscopy (XPS) was used to inspect the back side of the wafer. Only the Si element signal of the single crystal silicon substrate was detected, and no Si-N bonding characteristic peaks or N element signals belonging to silicon nitride were detected. Ellipsometry showed no silicon nitride film residue. The device structure on the front side of the wafer was undamaged, and the breakdown voltage and leakage current performance of the silicon nitride passivation layer were unchanged, meeting the device design requirements.

[0175] Example 4: This example addresses the non-target layer on the back side generated during the thermal atomic layer deposition (TAD) process for a high-k hafnium dioxide (HfO2) dielectric layer on the front side of a 12-inch single-crystal silicon wafer. The method for removing the non-target layer on the back side in this example includes steps S41 to S47.

[0176] Step S41: Wafer preprocessing.

[0177] Available in 12-inch P-type <100> For monocrystalline silicon wafers, RCA standard cleaning is performed, followed by cleaning with SPM, SC1, SC2, and DHF solutions in sequence to remove surface contaminants and the native oxide layer, and then drying with high-purity nitrogen.

[0178] Step S42: Form a protective layer on the front side of the wafer.

[0179] The wafer is placed in the PEALD equipment, and an ultrathin SiO2 protective layer with a thickness of 0.5 nm is deposited on the front side of the wafer at a deposition temperature of 250°C. The precursors are TDMAS and H2O.

[0180] S43: Flip the wafer to prepare the back sacrificial layer.

[0181] The wafer is flipped 180° so that the back side faces upwards. A 50nm thick SiO2 sacrificial layer is deposited on the back side of the wafer using the PEALD process at a deposition temperature of 250℃. During the deposition process, part of the SiO2 sacrificial layer is deposited around the ultrathin protective layer on the front side of the wafer.

[0182] S44: Flip the wafer and remove the front protective layer.

[0183] The wafer was flipped 180° again so that the front side was facing up. It was then sprayed with a 1:500 diluted hydrofluoric acid solution for 30 seconds to selectively remove the SiO2 protective layer on the front side. After rinsing with deionized water, it was hydrophilically treated with SC1 solution and dried with high-purity nitrogen. During the removal process, the SiO2 sacrificial layer attached to the protective layer was simultaneously peeled off.

[0184] S45: Deposit a high-k dielectric layer on the front side of the wafer.

[0185] The processed wafer was placed in a thermal ALD apparatus, and a high-k HfO2 dielectric layer was deposited on the front side of the wafer at a deposition temperature of 300°C. The precursors were TDMA-Hf and H2O, and the deposition cycle was 60 times, with a target thickness of 6 nm. During the deposition process, the precursor vapor diffused to the back side of the wafer, forming a non-target HfO2 layer on the surface of the SiO2 sacrificial layer.

[0186] S46: Simultaneously remove sacrificial and non-target layers from the back and sidewalls of the wafer.

[0187] HF and deionized water were mixed at a mass ratio of 1:2 and cooled to 6±0.5℃ to obtain a low-temperature HF etching solution.

[0188] The wafer is vertically immersed in a low-temperature HF etching solution for 70 seconds to remove more than 90% of the SiO2 sacrificial layer. The immersion process is accompanied by 80W ultrasonic vibration.

[0189] After removing the wafer, fix it on a rotating wafer stage and control the rotation speed at 1000 rpm. Use a low-temperature HF etching solution with the same temperature and composition to rinse the back of the wafer for 60 seconds to completely remove the remaining sacrificial layer and the non-target HfO2 layer.

[0190] After etching, the back side of the wafer is hydrophilically treated with SC1 solution to remove etching byproducts.

[0191] Step S47: Perform RCA standard cleaning on the wafer and dry it with high-purity nitrogen.

[0192] The wafer processed in this embodiment was inspected: X-ray photoelectron spectroscopy (XPS) showed no Hf element signal on the back side of the wafer, only Si element was detected on the single-crystal silicon substrate, and no hafnium dioxide residue was found; transmission electron microscopy (TEM) showed no hafnium dioxide film residue or interface damage; the uniformity deviation of the hafnium dioxide film thickness on the front side of the wafer was <0.6%, and the dielectric constant and leakage current performance remained unchanged. The entire process requires no photoresist or fixture protection, and no etching damage to the front-side devices was observed in the sample testing of this embodiment. Compared to the direct cleaning process, the sample yield in this embodiment is improved.

[0193] According to an exemplary embodiment, this embodiment provides a semiconductor structure fabricated using the method for removing the wafer back-side coating as described in the above embodiment. The semiconductor structure includes a wafer and a target functional layer. The wafer includes a front side, a back side, and sidewalls connecting the front and back sides; the target functional layer is disposed on the front side of the wafer; wherein the back side and sidewalls of the wafer are surfaces after the sacrificial layer has been removed, and there is no continuously distributed material of the target functional layer on the back side and sidewalls of the wafer.

[0194] It should be noted that "discontinuous distribution" means that the material of the target functional layer does not form a continuous thin film on the back side and sidewalls of the wafer, but may exist in the form of isolated islands or discrete particles. This state can be observed and verified by scanning electron microscopy (SEM) or transmission electron microscopy (TEM).

[0195] In some embodiments, the target functional layer includes at least one of a metal oxide, a metal nitride, an oxide semiconductor, or a chalcogenide alloy.

[0196] Furthermore, the target functional layer is a single layer formed from one of the following materials, or a multilayer formed from at least two of the following materials:

[0197] Metal oxides: tantalum oxide, hafnium oxide, zirconium oxide, hafnium aluminum oxide, hafnium silicon oxide, titanium oxide, niobium oxide, gallium oxide, vanadium oxide.

[0198] Metal nitrides: titanium nitride, tantalum nitride, gallium nitride.

[0199] Oxide semiconductors: Indium gallium zinc oxide, indium oxide, indium aluminum zinc oxide.

[0200] Sulfur alloys: germanium-antimony-tellurium alloy, germanium-tellurium alloy, germanium-sulfur alloy, indium-tellurium alloy, germanium-selenium alloy.

[0201] The thickness of the target functional layer can be selected according to device requirements. The target functional layer can be formed on the front side of the wafer using methods such as physical vapor deposition, chemical vapor deposition, atomic layer deposition, or sputtering deposition.

[0202] In some embodiments, when at least one of X-ray photoelectron spectroscopy or secondary ion mass spectrometry is used to detect the back side and / or sidewalls of the wafer, no characteristic element signal of the target functional layer is detected.

[0203] In one example, the material of the target functional layer includes titanium nitride; no characteristic signal of titanium nitride was detected when X-ray photoelectron spectroscopy was used to detect the back side and / or sidewalls of the wafer.

[0204] In another example, the material of the target functional layer includes hafnium oxide; no characteristic element signal of hafnium oxide was detected when the back side and / or sidewalls of the wafer were detected using secondary ion mass spectrometry.

[0205] It is understood that when using at least one of X-ray photoelectron spectroscopy or secondary ion mass spectrometry to detect the back side and / or sidewalls of a wafer, the failure to detect the characteristic element signal of the target functional layer means that the atomic percentage concentration of the target element in the target functional layer is lower than the detection limit of the X-ray photoelectron spectroscopy or secondary ion mass spectrometry detector.

[0206] In some embodiments, when the back side and / or sidewalls of the wafer are inspected using a transmission electron microscope or an ellipsometer, no continuously distributed target functional layer is detected; and / or, when the back side of the wafer is inspected using an atomic force microscope, the surface roughness Ra of the back side of the wafer is less than or equal to 0.5 nm. Preferably, the surface roughness of the back side of the wafer is less than or equal to 0.2 nm.

[0207] It is understood that in this application, the failure to detect a continuously distributed target functional layer when using a transmission electron microscope to inspect the back side and / or sidewalls of a wafer means that no continuous thin film of the target functional layer is observed within the detection range of the transmission electron microscope.

[0208] In this application, the failure to detect a continuously distributed target functional layer when using an ellipsometer to inspect the back side and / or sidewalls of a wafer means that, within the detection accuracy of the ellipsometer, no optical layer corresponding to a continuous thin film of the target functional layer is fitted.

[0209] In some embodiments, after surface collection treatment of the back side and / or sidewalls of the wafer, the extract is collected and detected by inductively coupled plasma mass spectrometry. The areal density of the elements in the target functional layer is less than 1 × 10⁻⁶. 10 atoms / cm 2 Preferred size is less than 5×108 atoms / cm 2 .

[0210] In some embodiments, the semiconductor structure includes at least one of resistive switching memory, phase-change memory, magnetic memory, or oxide semiconductor thin-film transistor integrated in the back-end of CMOS.

[0211] The semiconductor structure of this embodiment is prepared by using the method of removing the wafer backside plating layer described in the above embodiment. This can effectively avoid the residual plating of the target functional layer material on the wafer backside and sidewalls, thereby avoiding device reliability problems such as leakage and short circuits caused by the residual plating, and improving the yield and performance of semiconductor devices.

[0212] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features of the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0213] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.

Claims

1. A method for removing a coating around the back of a wafer, characterized in that, The method includes the following steps: Provide a wafer and clean the surface of the wafer; A sacrificial layer is formed on the back side and sidewalls of the wafer; The target functional layer is deposited on the front side of the wafer using thermal atomic layer deposition or chemical vapor deposition at a deposition temperature of 200℃~400℃. The precursor of the target functional layer is used to form a coating around the sacrificial layer on the back side and sidewall of the wafer. A low-temperature fluorine-containing corrosive solution is prepared, wherein the low-temperature fluorine-containing corrosive solution comprises a fluorine-containing corrosive component and water, and the temperature of the low-temperature fluorine-containing corrosive solution is 0℃~10℃; the fluorine-containing corrosive component comprises hydrofluoric acid, or comprises hydrofluoric acid and ammonium fluoride; An anti-etching layer is used to protect the front side of the wafer, and the low-temperature fluorine-containing etching solution is used to remove the sacrificial layer and the wrap-around coating attached to the sacrificial layer; Remove the etch-resistant layer, clean and dry the wafer.

2. The method for removing the coating around the back of a wafer according to claim 1, characterized in that, The low-temperature fluorine-containing corrosive liquid includes hydrofluoric acid and deionized water; wherein the mass fraction of hydrofluoric acid is 2wt% to 25wt%.

3. The method for removing the coating around the back of a wafer according to claim 1, characterized in that, The low-temperature fluorine-containing corrosive liquid includes hydrofluoric acid, ammonium fluoride and deionized water; wherein the mass fraction of hydrofluoric acid is 0.2wt% to 5wt% and the mass fraction of ammonium fluoride is 5wt% to 35wt%.

4. The method for removing the coating around the back of a wafer according to claim 1, characterized in that, The low-temperature fluorine-containing corrosive liquid is a buffered oxide corrosive liquid, and the molar ratio of ammonium fluoride to hydrofluoric acid in the buffered oxide corrosive liquid is 4:1 to 20:

1.

5. The method for removing the coating around the back of a wafer according to claim 1, characterized in that, The low-temperature fluorine-containing corrosive liquid also includes a surface tension modifier, which includes at least one of isopropanol, ethanol, or a nonionic surfactant.

6. The method for removing the coating around the back of a wafer according to claim 1, characterized in that, Before forming a sacrificial layer on the back side and sidewalls of the wafer, the cleaned wafer is pre-annealed in an atmosphere of inert gas and hydrogen to eliminate lattice defects and dangling bonds on the back side of the wafer. The treatment temperature is 700℃~800℃ and the treatment time is 5min~30min.

7. The method for removing the coating around the back of a wafer according to claim 6, characterized in that, The formation of a sacrificial layer on the back side and sidewalls of the wafer includes: A low-temperature ultraviolet-assisted furnace tube thermal oxidation process is used to simultaneously generate a sacrificial layer with a thickness of 5nm to 20nm on the front, back, and sidewalls of the wafer. Specifically, the wafer is first irradiated with 185nm and / or 254nm ultraviolet light in an oxygen-containing atmosphere at 300℃ to 500℃ to form an initial oxidation nucleation layer on the surface of the wafer. Then, the temperature is raised to 800℃ to 1000℃ for dry oxygen oxidation to form the sacrificial layer. The back side and sidewalls of the wafer are shielded by a mask, and the sacrificial layer on the front side of the wafer is removed by selective wet etching with diluted hydrofluoric acid at a volume ratio of 1:50 to 1:200, while the sacrificial layer on the back side and sidewalls of the wafer is retained.

8. The method for removing the coating around the back of a wafer according to claim 7, characterized in that, The low-temperature ultraviolet-assisted furnace tube thermal oxidation process has the following characteristics: oxygen flow rate of 1 slm to 5 slm, ultraviolet nucleation time of 3 min to 8 min, and the thickness of the sacrificial layer of 15 nm to 20 nm.

9. The method for removing the coating around the back of a wafer according to claim 1, characterized in that, The formation of a sacrificial layer on the back side and sidewalls of the wafer includes: A protective layer is deposited on the front side of the wafer at a temperature of 200℃ to 300℃, and the thickness of the protective layer is 0.3nm to 2nm. The wafer is flipped so that the back side faces up, and a sacrificial layer with a thickness of 30 nm to 100 nm is deposited on the back side and sidewalls of the wafer at a deposition temperature of 175 °C to 400 °C. Part of the sacrificial layer is deposited around the protective layer on the front side of the wafer. Flip the wafer so that the front side is facing up, remove the protective layer on the front side of the wafer, and simultaneously remove the sacrificial layer deposited around the protective layer.

10. The method for removing the coating around the back of a wafer according to claim 9, characterized in that, The protective layer is removed by spraying the front side of the wafer with a dilute hydrofluoric acid solution.

11. The method for removing the coating around the back side of a wafer according to any one of claims 1 to 10, characterized in that, The removal of the sacrificial layer and the wrap-around coating adhering to the sacrificial layer using the low-temperature fluorine-containing etching solution includes: The wafer is immersed in the low-temperature fluorine-containing etching solution and the wafer is vibrated with an ultrasonic power of 50W to 100W until more than 90% of the thickness of the sacrificial layer is removed. The front side of the wafer is placed against a rotating stage and rotated at a speed of 500 rpm to 1500 rpm. At the same time, the back side and sidewalls of the wafer are sprayed with the low-temperature fluorine-containing etching solution to remove the remaining sacrificial layer and the wrap-around coating attached to the sacrificial layer.

12. The method for removing the coating around the back side of a wafer according to any one of claims 1 to 10, characterized in that, The target functional layer is a single layer formed of one material selected from the following materials, or a multilayer formed of at least two materials selected from the following materials: Metal oxides: tantalum oxide, hafnium oxide, zirconium oxide, hafnium aluminum oxide, hafnium silicon oxide, titanium oxide, niobium oxide, gallium oxide, vanadium oxide; Metal nitrides: titanium nitride, tantalum nitride, gallium nitride; Oxide semiconductors: Indium gallium zinc oxide, indium oxide, indium aluminum zinc oxide; Sulfur alloys: germanium-antimony-tellurium alloy, germanium-tellurium alloy, germanium-sulfur alloy, indium-tellurium alloy, germanium-selenium alloy.

13. The method for removing the coating around the back side of a wafer according to any one of claims 1 to 10, characterized in that, The method for removing the coating layer on the back side of the wafer, when applied to CMOS processes, is used to fabricate at least one of resistive random access memory, phase change memory, magnetic memory, and oxide semiconductor thin film transistors.

14. A semiconductor structure, characterized in that, include: A wafer, the wafer including a front side, a back side, and a sidewall connecting the front side and the back side; The target functional layer is located on the front side of the wafer; The back surface and sidewalls of the wafer are the surfaces after the sacrificial layer has been removed, and there is no continuously distributed material of the target functional layer on the back surface and sidewalls of the wafer.

15. The semiconductor structure according to claim 14, characterized in that, The target functional layer includes at least one of metal oxide, metal nitride, oxide semiconductor or chalcogenide.

16. The semiconductor structure according to claim 14, characterized in that, When the back side and / or sidewalls of the wafer are detected using at least one of X-ray photoelectron spectroscopy or secondary ion mass spectrometry, no characteristic element signal of the target functional layer is detected.

17. The semiconductor structure according to claim 14, characterized in that, When the back side and / or sidewalls of the wafer are inspected using a transmission electron microscope or an ellipsometry, no continuously distributed target functional layer is detected; and / or, when the back side of the wafer is inspected using an atomic force microscope, the surface roughness Ra of the back side of the wafer is less than or equal to 0.5 nm.

18. The semiconductor structure according to claim 14, characterized in that, After surface collection treatment of the back side and / or sidewalls of the wafer, the extract is collected and analyzed by inductively coupled plasma mass spectrometry. The areal density of the elements in the target functional layer is less than 1 × 10⁻⁶. 10 atoms / cm 2 .

19. The semiconductor structure according to any one of claims 14 to 18, characterized in that, The semiconductor structure includes at least one of resistive switching memory, phase-change memory, magnetic memory, or oxide semiconductor thin-film transistor integrated in the back-end of CMOS.