Methods for manufacturing coated cutting tools, cutting tools and machined workpieces
By forming a coating of specific elements on the substrate of coated cutting tools and then heat-treating it to form needle-like crystals, the problem of insufficient anti-adhesion of coated cutting tools is solved, the anti-adhesion and wear resistance are improved, and the service life is extended.
Patent Information
- Application Number
- CN202580019007.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-04-03
- Filing Date
- 2025-03-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing coated cutting tools have low anti-adhesion properties, resulting in short tool life.
A coating containing elements from groups 4, 5, and 6 of the periodic table, as well as Al, Si, C, and N, is formed on the substrate of the coated tool. The coating is then subjected to heat treatment at temperatures above 1050°C and below 1100°C in an atmospheric atmosphere to form needle-like crystals and enhance its anti-adhesion properties.
It improves the anti-adhesion and wear resistance of coated cutting tools, and extends the tool's service life.
Smart Images

Figure CN123125068A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present invention relate to a method for manufacturing coated cutting tools, cutting tools, and workpieces. Background Technology
[0002] As cutting tools used for turning or milling, coated tools are known to improve wear resistance by coating the surface of a substrate such as cemented carbide, cermet, or ceramic with a coating.
[0003] For example, it is known that coated cutting tools consist of a substrate and a coating applied to its surface. The coating includes an intermediate film applied to the surface of the substrate and an oxide film applied to the surface of the intermediate film. The intermediate film is composed of at least one selected from the group consisting of TiN, TiCN, TiAlN, TiAlZrN, TiAlCrN, and AlCrN. The intermediate film is cubic. The oxide film is composed of (Al... 0.5 Cr 0.5 )2O3、(Al 0.55 Cr 0.45 )2O3、(Al 0.6 Cr 0.4 )2O3、(Al 0.7 Cr 0.3 )2O3、(Al 0.8 Cr 0.2 )2O3 and (Al 0.9 Cr 0.1 At least one of the constituents selected from the group consisting of )2O3 (e.g., refer to International Publication No. 2012 / 018063). Summary of the Invention
[0004] One embodiment of the coated cutting tool has a substrate and at least one coating on the substrate. The coating contains at least one element selected from elements of groups 4, 5, and 6 of the periodic table, Al, and Si; and at least one element selected from C and N. After heat treatment in an atmospheric atmosphere at a temperature of 1050°C or higher and 1100°C or lower, the coating contains needle-like crystals, at least a portion of which are located on the surface of the coating. Attached Figure Description
[0005] Figure 1 This is a perspective view showing an example of the coated cutting tool of this embodiment.
[0006] Figure 2 This is a cross-sectional view showing an example of the blade of this embodiment.
[0007] Figure 3 This is a schematic diagram illustrating an example of the coating in this embodiment.
[0008] Figure 4 This is a front view showing an example of a cutting tool according to this embodiment.
[0009] Figure 5A This is a schematic diagram illustrating one step of the manufacturing method of the machined workpiece according to this embodiment.
[0010] Figure 5B This is a schematic diagram illustrating one step of the manufacturing method of the machined workpiece according to this embodiment.
[0011] Figure 5C This is a schematic diagram illustrating one step of the manufacturing method of the machined workpiece according to this embodiment.
[0012] Figure 6 This is a diagram showing an image of the surface of the coating on the coated cutting tool of sample No.1 in the embodiment after heat treatment.
[0013] Figure 7 This is a diagram showing an image of the surface of the coating on the coated cutting tool of Comparative Example No. 7 after heat treatment. Detailed Implementation
[0014] Hereinafter, with reference to the accompanying drawings, a method for manufacturing coated cutting tools, cutting tools, and machined works according to the present invention (hereinafter referred to as "Embodiments") will be described in detail. The method for manufacturing coated cutting tools, cutting tools, and machined works according to the present invention is not limited to the embodiments described below. In the following embodiments, the same reference numerals are used for the same parts, and repeated descriptions are omitted.
[0015] As cutting tools used for turning or milling, coated tools are known to improve wear resistance by coating the surface of a substrate such as cemented carbide, cermet, or ceramic with a coating.
[0016] However, existing coated cutting tools have low anti-adhesion properties, resulting in a shorter tool life.
[0017] Thus, there is still room for further improvement in terms of anti-adhesion in the existing technology.
[0018] Therefore, it is desirable to develop a technology that can overcome the above-mentioned problems and improve anti-adhesion properties.
[0019] Coated Cutting Tools
[0020] Figure 1 This is a perspective view showing an example of the coated cutting tool according to this embodiment. Figure 1 As shown, the coated cutting tool 1 of this embodiment has a blade 11.
[0021] (Blade 11)
[0022] Blade 11, for example, has an upper surface and a lower surface (with) Figure 1 The shape of the surfaces intersecting the Z-axis shown is approximately a parallelogram-shaped hexahedron. The blade 11 of this embodiment has an upper surface and a lower surface on the opposite side, with a side surface between the upper and lower surfaces.
[0023] One corner of the blade 11 functions as a cutting edge. The cutting edge has a first face (e.g., a portion of the upper surface) and a second face (e.g., a portion of the side surface) connected to the first face. In this embodiment, the first face functions as a "rake face," and the second face functions as a "flank face." A cutting edge is provided on at least a portion of the edge where the first and second faces intersect, and the coated tool 1 cuts the workpiece by bringing this cutting edge into contact with the workpiece.
[0024] A through hole 15 is provided in the center of the blade 11, extending vertically through the blade 11. The central axis of the through hole 15 can pass through the center of the upper surface and the center of the lower surface. A bolt 75 for mounting the coated tool 1 on the tool holder 70 (described later) is inserted into the through hole 15. Figure 4 ).
[0025] Figure 1 The shape of the coating tool 1 shown is only an example and does not limit the shape of the coating tool of the present invention. The coating tool of the present invention may, for example, have: a rod-shaped body having a rotation axis extending from a first end toward a second end; a cutting edge located at the first end of the body; and a groove extending spirally from the cutting edge toward the second end of the body.
[0026] Figure 2 This is a cross-sectional view showing an example of the blade of this embodiment. Figure 2 The cross-section shown can be a cross-section parallel to the central axis of the through hole 15. For example... Figure 2 As shown, the blade 11 has a substrate 2 and at least one coating 3.
[0027] (Matrix 2)
[0028] The matrix 2 is, for example, formed of cemented carbide. The cemented carbide contains at least W (tungsten), specifically, a hard phase containing WC (tungsten carbide). The cemented carbide may contain a binder phase of at least one iron group element such as Ni (nickel) and Co (cobalt). As an example, the matrix 2 may be a WC-based cemented carbide with WC-based hard particles as its main component. Here, "main component" means that the WC-based hard particles contain 80% by mass or more in the total cemented carbide. When the matrix 2 is the aforementioned cemented carbide, the matrix 2 exhibits superior heat resistance properties.
[0029] The matrix 2 can also be a cermet. A cermet, for example, contains Ti (titanium), specifically TiC (titanium carbide), TiN (titanium nitride), or TiCN (titanium carbonitride). A cermet can also contain at least one iron group element such as Ni and Co.
[0030] Matrix 2 can also be a cubic boron nitride sintered body containing cubic boron nitride (cBN) particles. Matrix 2 is not limited to cubic boron nitride (cBN) particles, but can also contain hexagonal boron nitride (hBN), rhombohedral boron nitride (rBN), wurtzite boron nitride (wBN), etc.
[0031] The matrix 2 can also be ceramic. Ceramic, for example, can contain Al₂O₃ (aluminum oxide). Examples of Al₂O₃ include κ-Al₂O₃ and α-Al₂O₃. Ceramic can also contain elements other than aluminum oxide. For example, in addition to aluminum oxide, ceramics can contain at least one of magnesium (Mg), calcium (Ca), strontium (Sr), silicon (Si), and elements from Groups 3 and 4 of the periodic table.
[0032] (Coating 3)
[0033] The coating 3 is applied to the substrate 2 for the purpose of improving the anti-adhesion properties of the substrate 2. Figure 2 In this example, coating 3 completely covers the substrate 2. There are no particular limitations as long as coating 3 is located on at least the surface of the substrate 2. When coating 3 is located on the surface of the substrate 2, the surface of the blade 11 where coating 3 is located has high anti-adhesion properties.
[0034] Coating 3 contains: at least one element selected from elements of Groups 4, 5, and 6 of the periodic table, aluminum (Al), and silicon (Si); and at least one element selected from carbon (C) and nitrogen (N). For example, coating 3 contains Al. a Ti b Nb c M dThe coating 3 is composed of at least one element selected from C and N. M is at least one element selected from elements in groups 4, 5, and 6 of the periodic table, excluding Ti and niobium (Nb), and Si. a, b, c, and d satisfy the relationships 0.4 ≤ a ≤ 0.65, 0.35 ≤ b ≤ 0.6, 0.01 ≤ c ≤ 0.05, and a + b + c + d = 1. For example, the composition of coating 3 could be (AlTiNbWSi)N. The expression (AlTiNbWSi)N indicates the types of constituent elements, not the atomic ratio of the constituent elements. Coating 3 does not necessarily need to contain M. For example, the composition of coating 3 could be (AlTiNb)N. The expression (AlTiNb)N indicates the types of constituent elements, not the atomic ratio of the constituent elements. Coating 3 exhibits high hardness and high oxidation resistance at high temperatures (e.g., 1100°C).
[0035] The thickness of coating 3 can be 1 μm or more and 7 μm or less. In particular, when the thickness of coating 3 is 1.5 μm or more, the performance of the coated tool 1 is easily improved. When the thickness of coating 3 is 3 μm or less, the chipping resistance of coating 3 is easily improved. Therefore, when the thickness of coating 3 is 1.5 μm or more and 3 μm or less, the chipping resistance and other properties of coating 3 are easily improved.
[0036] In this embodiment, the coated cutting tool 1, which contains at least the coating 3, is subjected to heat treatment at a temperature of 1050°C or higher and 1100°C or lower under atmospheric conditions. For example, the coated cutting tool 1 containing the coating 3 is heated to a temperature of 1050°C or higher and 1100°C or lower under atmospheric conditions using a heating device such as an atmospheric furnace. As a step in the heat treatment process of the present invention, the coated cutting tool 1 containing the coating 3 is heated under atmospheric conditions for 1 hour from the start of heating until it reaches 1050°C. Thereafter, it can be held at 1050°C for 1 minute. After holding at 1050°C for 1 minute, it can be furnace cooled for a certain period of time.
[0037] The so-called "heat treatment" of the present invention refers to the heat treatment performed on the coated tool 1, which has a coating 3 formed by physical vapor deposition (PVD) or the like. For example, it is different from the firing treatment required for manufacturing the coated tool 1. By performing heat treatment on the coated tool 1 before cutting, the coated tool 1 is made to be in the same or similar state as the coated tool 1 during or after cutting, and the characteristics of the coated tool 1 can be evaluated.
[0038] The heat treatment of this invention is carried out in an atmospheric atmosphere, i.e., an oxygen-containing atmosphere, which allows the oxidation reaction of the coating 3 to occur. When the heat treatment temperature is 1050°C or higher, the oxidation reaction occurs in the coating 3, thus allowing the characteristics of the coating 3 of the coated tool 1 to be evaluated under conditions that are the same as or similar to those of the coated tool 1 during cutting. When the heat treatment temperature is 1100°C or lower, the risk of substrate 2 deterioration due to heat treatment can be reduced. As a result, the risk of coating 3 being affected by substrate 2 deterioration due to heat treatment can be reduced, and the characteristics of coating 3 of the coated tool 1 can be evaluated.
[0039] Coating 3 can be polycrystalline. Before heat treatment, coating 3 can be a multi-junction containing cubic crystals. Before heat treatment, coating 3 can be a polycrystalline material with cubic crystals as its main component. Here, "main component" refers to a polycrystalline material containing more than 90% by mass of cubic crystals.
[0040] Figure 3 This is a schematic diagram illustrating and showing an example of coating 3 in this embodiment. For example... Figure 3 As shown, after heat treatment at a temperature above 1050°C and below 1100°C in an atmospheric atmosphere, coating 3 contains needle-like crystals 5. The needle-like crystals 5 are crystals whose length L in a first direction and width W in a second direction orthogonal to the first direction are different on the surface of coating 3. Therefore, the shape of the needle-like crystals 5 is not limited to the shape of a needle; for example, it includes the shape of a pillar. At least a portion of the needle-like crystals 5 is located on the surface of coating 3. Here, "at least a portion of the needle-like crystals 5 is located on the surface of coating 3" means, in other words, that at least a portion of the needle-like crystals 5 is located in the portion of coating 3 furthest from the substrate 2; in other words, at least a portion of the needle-like crystals 5 is exposed from the surface of coating 3.
[0041] After heat treatment, coating 3 contains needle-like crystals 5, and at least a portion of the needle-like crystals 5 is located on the surface of coating 3, which can be confirmed, for example, by using a scanning electron microscope (SEM). An image of the surface of coating 3 after heat treatment is obtained using a scanning electron microscope (SEM). The presence of needle-like crystals 5 on the surface of coating 3 after heat treatment is confirmed in the image of the surface of coating 3 after heat treatment.
[0042] When the coated tool 1 is used for cutting the workpiece, the temperature of the coating 3 contained in the coated tool 1 and in contact with the workpiece rises. Since the coating 3 of this embodiment contains needle-like crystals 5 after heat treatment, for example, under cutting conditions where the coating 3 reaches a temperature of 1050°C or higher and 1100°C or lower during cutting, it is assumed that the coating 3 will contain needle-like crystals 5. In this case, it is easier to reduce the cutting resistance of the coating 3 during cutting. As a result, it is easier to improve the anti-adhesion property of the coated tool 1 relative to the workpiece. Moreover, in the above-described case, it is easier to increase the specific surface area of the coating 3 after cutting. As a result, it is easier to cool the coating 3 after cutting.
[0043] The content of needle-like crystals 5 in the coating 3 of the heat-treated coated tool 1 can be 50% to 100%. The content of needle-like crystals 5 in the coating 3 can be measured based on the area ratio of needle-like crystals 5 in an image of the surface of the coating 3. Specifically, the content of needle-like crystals 5 in the coating 3 can be obtained, for example, using a scanning electron microscope (SEM). First, an image of the surface of the coating 3 is obtained using a scanning electron microscope (SEM). Second, the proportion of needle-like crystals 5 contained in the image of the surface of the coating 3 is calculated using image processing software. More specifically, the proportion of the area of needle-like crystals 5 contained in the image relative to the overall area of the image can be taken as the content of needle-like crystals 5 in the coating 3. For example, Mac-View can be used as the image processing software. The area of the image of the surface of the coating 3 can be, for example, 5 μm × 5 μm.
[0044] The content of needle-like crystals 5 in coating 3 can be less than 1% before heat treatment. Here, "less than 1%" includes 0%. That is, there is a case where coating 3 does not contain needle-like crystals 5 before heat treatment. Thus, coating 3 before heat treatment does not contain needle-like crystals 5, or the content of needle-like crystals 5 in coating 3 before heat treatment is low. In other words, the content of needle-like crystals 5 in coating 3 is at least higher than 1% after heat treatment. That is, in the above case, the content of needle-like crystals 5 in coating 3 increases through heat treatment.
[0045] In the coated cutting tool 1, when the content of needle-like crystals 5 in the coating 3 is less than 1% before heat treatment, the oxidation reaction of the coating 3 before heat treatment is easily reduced. As a result, the oxidation resistance of the coated cutting tool 1 containing the coating 3 is easily improved.
[0046] like Figure 3As shown, after heat treatment, coating 3 contains a plurality of needle-like crystals 5. The average aspect ratio of the needle-like crystals 5 contained in coating 3 is greater than 2 and less than 10. The aspect ratio of the needle-like crystals 5 is defined by the length L of the needle-like crystal 5 in the longitudinal direction and the width W of the needle-like crystal 5 in the transverse direction.
[0047] The average aspect ratio of the needle-like crystals 5 contained in the coating 3 can be obtained, for example, using a scanning electron microscope (SEM). First, an image of the surface of the coating 3 is obtained using a scanning electron microscope (SEM). Next, using image processing software, the length L of the needle-like crystals 5 in the longitudinal direction and the width W of the needle-like crystals 5 in the transverse direction are obtained. Then, the aspect ratio of the needle-like crystal 5 image is obtained by dividing the length L of the needle-like crystal 5 image in the longitudinal direction by the width W of the needle-like crystal 5 image in the transverse direction. Next, the average aspect ratio of the obtained needle-like crystal 5 images is calculated for each image of the needle-like crystals 5 contained in the image of the surface of the coating 3. For example, Mac-View can be used as image processing software. The area of the image of the surface of the coating 3 can be, for example, 5 μm × 5 μm.
[0048] When the average aspect ratio of the needle-like crystals 5 contained in the coating 3 is 2 or greater, it is easier to reduce the area of the coating 3 in contact with the workpiece. Correspondingly, it is easier to reduce the cutting resistance of the coating 3 during machining. As a result, it is easier to improve the anti-adhesion of the coated tool 1 relative to the workpiece.
[0049] When the average aspect ratio of the needle-like crystals 5 contained in the coating 3 is greater than 2, the specific surface area of the coating 3 after machining is easily increased. As a result, the coating 3 cools more easily after machining.
[0050] When the average aspect ratio of the needle-like crystals 5 contained in coating 3 is greater than 2, cracks that may be generated in coating 3 due to impacts applied to it during machining are more likely to be induced. Accordingly, bridging of cracks is more likely to occur in coating 3 subjected to impacts during machining. As a result, the toughness of coating 3 is more likely to be improved during machining.
[0051] When the average aspect ratio of the needle-like crystals 5 contained in the coating 3 is less than 10, it is easier to reduce the damage to the needle-like crystals 5 that may occur due to impact applied to the coating 3 during machining. Therefore, it is easier to stabilize the needle-like crystals 5 contained in the coating 3 during machining.
[0052] Coating 3 may contain Al. When coating 3 contains Al, an oxidation reaction may occur due to heat treatment, resulting in coating 3 containing alumina after heat treatment. Alumina tends to promote the formation of needle-like crystals 5. Therefore, it is easy to promote the presence of needle-like crystals 5 in coating 3 after heat treatment.
[0053] When coating 3 contains Al, there is an oxidation reaction of coating 3 due to heat treatment, and the needle-like crystals 5 contain both Al and oxygen (O). When the needle-like crystals 5 contain both Al and O, the surface of the needle-like crystals 5 will be covered by an aluminum oxide film. As a result, the oxidation resistance of the coated tool 1 containing coating 3 is easily improved.
[0054] Coating 3 may contain Nb. When coating 3 contains Nb, its hardness tends to increase. Therefore, it is easy to improve the wear resistance of the coated tool 1 containing coating 3.
[0055] When coating 3 contains Al and Nb, Nb promotes the formation of alumina in coating 3 during heat treatment. Alumina tends to promote the formation of needle-like crystals 5, thus easily further promoting the presence of needle-like crystals 5 in coating 3 after heat treatment.
[0056] When coating 3 contains Nb, there is an oxidation reaction in coating 3 due to heat treatment, and the needle-like crystals 5 contain both Nb and O. When needle-like crystals 5 contain both Nb and O, the surface of needle-like crystals 5 is covered by a niobium oxide film. Correspondingly, the hardness of needle-like crystals 5 is easily increased. Because needle-like crystals 5 are included in coating 3, the wear resistance of the coated tool 1 containing coating 3 is easily improved.
[0057] When the needle-like crystals 5 contain Al, Nb, and O, Nb promotes the formation of an alumina film on the surface of the needle-like crystals 5. That is, a denser alumina film is easily formed on the surface of the needle-like crystals 5. Therefore, the oxidation reaction of the coating 3 during heat treatment is easily reduced. As a result, the oxidation resistance of the coated tool 1 containing the coating 3 is easily improved.
[0058] The coating 3 may contain at least one of W and Si. When the coating 3 contains at least one of W and Si, the affinity between the substrate 2 and the coating 3 is increased, making it easier to improve the adhesion of the coating 3 relative to the substrate 2. Therefore, it is easier to improve the wear resistance of the coated tool 1 containing the substrate 2 and the coating 3.
[0059] Coating 3 contains W. Due to oxidation of coating 3 caused by heat treatment, needle-like crystals 5 may contain both W and O. In this case, the heat resistance of coating 3 is easily improved. Therefore, the heat resistance of the coated cutting tool 1 containing coating 3 is easily improved.
[0060] When coating 3 contains Al and W, a layer containing aluminum oxide and tungsten oxide is easily formed inside the aluminum oxide film on the surface of the needle-like crystals 5. In this case, the adhesion of the aluminum oxide film to the interior of the needle-like crystals 5 is easily improved. As a result, the oxidation resistance of the coated tool 1 containing coating 3 is easily improved. The heat resistance of the needle-like crystals 5 is easily improved through such a layer. Because the needle-like crystals 5 are contained in coating 3, the heat resistance of the coated tool 1 containing coating 3 is easily improved.
[0061] Coating 3 may contain Al and Ti. The content of Al in coating 3 is greater than the content of Ti in coating 3.
[0062] In this case, Al substitution of Ti in Ti-containing crystals is promoted. Correspondingly, the hardness of coating 3 is easily increased. Therefore, the wear resistance of the coated tool 1 containing coating 3 is easily improved. During the oxidation reaction of coating 3 caused by heat treatment, the formation of alumina on the surface of needle-like crystals 5 can be further promoted. Therefore, the oxidation reaction of coating 3 during heat treatment is easily further reduced. As a result, the oxidation resistance of the coated tool 1 containing coating 3 is easily further improved.
[0063] The coating 3 contains Al and Ti, and the ratio of the Al content in the surface of the coating 3 to the Ti content in the surface of the coating 3 is greater than 2 after heat treatment.
[0064] In this case, the substitution of Ti by Al for a portion of the Ti-containing crystals on the surface of coating 3 is promoted. Correspondingly, the surface hardness of coating 3 is easily increased. Therefore, the wear resistance of the coated tool 1 containing coating 3 is easily improved. The formation of alumina on the surface of the needle-like crystals 5 on the surface of coating 3 is further promoted. The alumina formed on the surface of the needle-like crystals 5 tends to reduce the diffusion of oxygen into coating 3. Therefore, the oxidation reaction of coating 3 is easily further reduced. As a result, the oxidation resistance of the coated tool 1 containing coating 3 is easily further improved.
[0065] Coating 3 contains Al and Ti. The ratio X of the Al content to the Ti content in coating 3 before heat treatment, and the ratio Y of the Al content to the Ti content in coating 3 after heat treatment, satisfy the relationship Y / X > 2. That is, the ratio of the Al content to the Ti content in coating 3 increases with heat treatment.
[0066] In this case, the substitution of Ti by Al in the Ti-containing crystal is promoted by heat treatment. Correspondingly, the hardness of the coating 3 is easily increased by heat treatment. Therefore, the wear resistance of the coated tool 1 containing the coating 3 is easily improved. The oxidation reaction of the coating 3 caused by heat treatment further promotes the formation of alumina on the surface of the needle-like crystals 5. The alumina formed on the surface of the needle-like crystals 5 tends to reduce the diffusion of oxygen into the coating 3 during heat treatment. Therefore, the oxidation reaction of the coating 3 during heat treatment is easily further reduced. As a result, the oxidation resistance of the coated tool 1 containing the coating 3 is easily further improved.
[0067] The types and percentages of elements contained in coating 3 can be determined, for example, using energy-dispersive X-ray spectroscopy (EDS) attached to a scanning transmission electron microscope (STEM). First, an image of the surface of coating 3 is obtained by irradiating the surface of coating 3 with an electron beam using the STEM. Next, the energy-dispersive X-ray spectroscopy (EDS) detects the X-ray fluorescence generated when a specified area of the surface of coating 3 is irradiated with an electron beam. Then, by determining the wavelength and intensity of the characteristic X-rays contained in the detected X-ray fluorescence, the types and percentages of elements contained in the specified area of the surface of coating 3 can be determined.
[0068] <Manufacturing Method of Coated Cutting Tools>
[0069] Next, an example of the manufacturing method of the coated cutting tool according to this embodiment will be described. The manufacturing method of the coated cutting tool according to this embodiment is not limited to the manufacturing method described below.
[0070] The coated tool 1 is manufactured by forming at least one coating 3 on the substrate 2. The coating 3 can be formed, for example, by physical vapor deposition (PVD). For example, when the substrate 2 is held with the inner circumferential surface of the through hole 15, the coating 3 can be easily formed in a way that covers the entire surface of the substrate 2 except for the inner circumferential surface of the through hole 15 when the coating 3 is formed by physical vapor deposition.
[0071] Physical vapor deposition methods include, for example, ion plating methods such as arc ion plating (AIP) and sputtering. Arc ion plating is a method in which the elements of the target material are evaporated by an electric arc discharge in a vacuum atmosphere, and then combined with nitrogen (N2) gas as needed to form a film of the target material elements or nitrides of the target material elements.
[0072] As an example, when a coating 3 is formed on a substrate 2 by arc ion plating, the coated tool 1 can be easily manufactured by the following method.
[0073] As an example, targets containing Al, Ti, Nb, and M, or targets containing composite elements, or sintered targets are prepared. Here, M is at least one element selected from Groups 4, 5, and 6 of the periodic table, excluding Ti and Nb, and Si.
[0074] Next, the target material, which serves as the source of the element, is evaporated and ionized by means of arc discharge or glow discharge. The ionized element reacts with nitrogen (N2) gas, for example, and is deposited onto the surface of the substrate 2. Thus, a coating 3 can be formed on the substrate 2.
[0075] Here, after heat treatment of coating 3 at a temperature above 1050°C and below 1100°C in an atmospheric atmosphere, it contains needle-like crystals 5. In order to ensure that at least a portion of the needle-like crystals 5 are located on the surface of coating 3, for example, it is considered that the plasma density and plasma energy of the ionizing element can be increased, and the bias voltage applied to the substrate 2 is gradually increased. As a method to increase the plasma density and plasma energy of the ionizing element, for example, the following can be listed:
[0076] • To bring the temperature of substrate 2 to the range of 500℃~600℃,
[0077] • The pressure that keeps the pressure of gases such as nitrogen in the range of 2 Pa to 8 Pa.
[0078] • The distance (T-S distance) between the target and the substrate 2 is in the range of 50mm to 200mm.
[0079] • A magnetic field is formed linearly along the direction of the target material.
[0080] • The distance between the cathodes should be in the range of 100mm to 200mm.
[0081] • To make the magnetic flux density of the magnet range from 20mT to 80mT
[0082] • The current for arc discharge, etc., is kept in the range of 130A to 160A. As a method to gradually increase the bias voltage applied to the substrate 2, examples include gradually increasing the bias voltage applied to the substrate 2 in the range of -30V to -75V.
[0083] <Cutting Tools>
[0084] Next, refer to Figure 4 The cutting tool having the above-mentioned coated tool 1 will be described. Figure 4 This is a front view showing an example of a cutting tool according to an embodiment.
[0085] like Figure 4As shown, the cutting tool 100 of this embodiment has a coated tool 1 and a tool holder 70 for fixing the coated tool 1.
[0086] The handle 70 is from the first end ( Figure 4 The upper end of the middle) faces the second end ( Figure 4 A rod-shaped component extending from the lower end of the blade. The handle 70 is made of, for example, steel or cast iron. Among these materials, high-toughness steel can be used.
[0087] The tool holder 70 has a groove 73 at its first end. The groove 73 is the part for mounting the coated tool 1, and has a support surface that intersects the rotation direction of the workpiece and a limiting side that is inclined relative to the support surface. On the support surface, there is a threaded hole for tightening the bolt 75, which will be described later.
[0088] The coated cutting tool 1 is located in the slot 73 of the tool holder 70 and is mounted on the tool holder 70 by a bolt 75. That is, the bolt 75 is inserted into the through hole 5 of the coated cutting tool 1, and the front end of the bolt 75 is inserted into the threaded hole formed in the support surface of the slot 73, so that the threads are tightened. Thus, the coated cutting tool 1 is mounted on the tool holder 70 such that the cutting edge portion protrudes outward from the tool holder 70.
[0089] In this embodiment, a cutting tool 100 for so-called turning is exemplified. Turning operations include, for example, internal diameter machining, external diameter machining, and grooving. However, the cutting tool is not limited to turning operations. For example, a coated cutting tool 1 can also be used for milling operations. Examples of cutting tools for milling operations include, for example, end mills such as face mills, front end mills, side end mills, and grooving end mills, as well as end mills such as single-flute end mills, multi-flute end mills, tapered end mills, and ball end mills.
[0090] Turning is performed using a lathe. Turning includes the following steps: rotating the workpiece; bringing a fixed cutting tool 100 into contact with the rotating workpiece to remove its surface; and removing the cutting tool 100 from the workpiece. By machining the workpiece into a desired rotationally symmetrical shape, it is easy to manufacture rotationally symmetrical workpieces. Milling is performed using a milling machine. Milling includes the following steps: rotating the cutting tool 100; bringing the rotating cutting tool 100 into contact with a fixed workpiece to remove its surface; and removing the cutting tool 100 from the workpiece. By machining the workpiece into a desired shape, it is easy to manufacture workpieces.
[0091] In this embodiment, the example shown is that the upper and lower surfaces of the cutting tool 100 are parallelograms. The shapes of the upper and lower surfaces of the cutting tool 100 can also be rhombuses, squares, etc. The shapes of the upper and lower surfaces of the cutting tool 100 can also be triangles, pentagons, hexagons, etc. The shape of the cutting tool 100 can also be positive or negative. A positive shape is one where the side surface is inclined relative to the central axis passing through the center of the upper and lower surfaces of the cutting tool 100, while a negative shape is one where the side surface is parallel to the aforementioned central axis.
[0092] <Methods for Manufacturing Machined Work>
[0093] Next, refer to Figure 5A , Figure 5B and Figure 5C This describes the manufacturing method of the workpiece to be machined according to this embodiment. Figure 5A , Figure 5B and Figure 5C This is a schematic diagram illustrating one step of the manufacturing method of the machined workpiece according to this embodiment.
[0094] The workpiece 200 is manufactured by cutting the workpiece 201. Figure 5A , Figure 5B and Figure 5C As an example of cutting machining, the illustration shows turning machining performed using a lathe. The manufacturing method of the machined workpiece 200 according to this embodiment includes the following steps:
[0095] The process of rotating the workpiece 201 (process A);
[0096] The process of bringing the workpiece 201 into contact with the cutting tool 100 (process B);
[0097] The process of moving the cutting tool 100 away from the workpiece 201 (process C).
[0098] More specifically, firstly, such as Figure 5A As shown, the workpiece 201 is rotated about axis O1, and the cutting tool 100 is brought relatively close to the workpiece 201. Next, as... Figure 5B As shown, the cutting edge of the coated tool 1 is brought into contact with the workpiece 201 to cut the workpiece 201. Next, as... Figure 5C As shown, the cutting tool 100 is moved relatively away from the workpiece 201.
[0099] exist Figure 5A In this process, with the fixed axis O1 and the workpiece 201 rotated, the cutting tool 100 is moved along the Y1 direction and approaches the workpiece 201. Figure 5BIn this process, the cutting edge of the coated tool 1 contacts the rotating workpiece 201, thereby cutting the workpiece 201. Figure 5C In the process, while the workpiece 201 is rotating, the cutting tool 100 is moved away along the Y2 direction.
[0100] In the cutting process of the machining method for manufacturing a workpiece according to this embodiment, in each step, the cutting tool 100 is moved to contact the workpiece 201 or to move away from the workpiece 201. However, the machining method for manufacturing a workpiece is not limited to this method.
[0101] For example, in step A, the workpiece 201 can be brought closer to the cutting tool 100. Similarly, in step C, the workpiece 201 can be moved away from the cutting tool 100. During continuous cutting, the workpiece 201 is kept in a rotating state, and the steps of bringing the cutting edge of the cutting tool 100 into contact with different positions of the workpiece 201 are repeated.
[0102] In the case of milling instead of turning, in step A, the cutting tool can be rotated around the axis of rotation. Furthermore, in step B, the cutting edge of the rotating coated tool 1 can be brought into contact with the workpiece 201, thereby cutting the workpiece 201. Additionally, in step C, the cutting tool can be moved away from the workpiece 201. Milling can be performed using a milling machine.
[0103] Examples of materials that can be used to cut material 201 include carbon steel, alloy steel, stainless steel, cast iron, or non-ferrous metals.
[0104] Example
[0105] The following describes specific embodiments of the present invention. The present invention is not limited to the embodiments shown below.
[0106] (Example)
[0107] First, a coated tool comprising a substrate and a coating on top of the substrate is manufactured by forming a coating on a substrate using an arc ion plating method. Here, a WC-based cemented carbide is used as the substrate. The coating is formed on the substrate under the conditions shown below. Table 1 shows the conditions for the arc ion plating method used to form the coating on the substrate.
[0108] • Matrix temperature: 500℃~600℃
[0109] • Target composition: as shown in Table 1
[0110] • Atmospheric pressure: 2~8Pa
[0111] • Distance between the target and the substrate (T-S distance): 50–200 mm (as shown in Table 1)
[0112] • Bias voltage: Gradually increase within the range of -30 to -75V (as shown in Table 1).
[0113] ·Magnetic field distribution
[0114] Cathode spacing: 100–200 mm (as shown in Table 1)
[0115] Magnetic force of the magnet: 20-80 mT (as shown in Table 1)
[0116] The film formation time was adjusted so that the thickness of the coating formed on the substrate was 2 μm. The average composition of the coating formed on the substrate is shown in Table 1. In this way, coated cutting tools of samples No.1 to No.9 shown in Table 1 were produced.
[0117] Table 1
[0118]
[0119] Next, for the coated cutting tools of samples No. 1 to No. 9, images of the coating surface before heat treatment were obtained using a scanning electron microscope (JSM-7100F, manufactured by Nippon Electron Ltd.). No needle-like crystals were observed in the images of the coating surface of any of the coated cutting tools of samples No. 1 to No. 9. This confirmed that the content of needle-like crystals in the coating of the coated cutting tools of samples No. 1 to No. 9 was less than 1% before heat treatment.
[0120] Next, for the coated cutting tools of samples No. 1 to No. 9, the types of elements contained in the coating surface before heat treatment were determined using an energy-dispersive X-ray spectrometer (JED-2300 / F) attached to a scanning electron microscope. In any of the coated cutting tools of samples No. 1 to No. 9, the elements contained in the coating before heat treatment, as shown in Table 1, were confirmed.
[0121] For the coated cutting tools of samples No. 1 to No. 7 and No. 9, the Al and Ti contents in the coating before heat treatment were determined. In any of the coated cutting tools of samples No. 1, No. 3, and No. 4 of the Examples and samples No. 7 and No. 9 of the Comparative Examples, it was confirmed that the Al content in the coating was greater than the Ti content in the coating before heat treatment. On the other hand, in any of the coated cutting tools of samples No. 2, No. 5, and No. 6 of the Examples, it was confirmed that the Al content in the coating was less than the Ti content in the coating before heat treatment. For the coated cutting tools of samples No. 1 to No. 7 and No. 9, the ratio X of the Al content to the Ti content in the coating before heat treatment was calculated. The calculated values of X are shown in Table 2.
[0122] Table 2
[0123]
[0124] Next, for the coated cutting tools of samples No. 1 to No. 9, the coated cutting tools containing the coating were heated in an atmospheric atmosphere using an atmospheric electric furnace (manufactured by NHK-170, Nikkei Scientific Co., Ltd.). Specifically, the tools were heated to 1050°C in an atmospheric atmosphere at a heating rate of 1 hour, held at 1050°C for 1 minute, and then furnace cooled. This was the heat treatment of the coating contained in the cutting tools.
[0125] Next, for the coated cutting tools of samples No. 1 to No. 9, images of the coating surface after heat treatment were obtained using a scanning electron microscope. In any of the coated cutting tools of samples No. 1 to No. 6 of the Examples, multiple needle-like crystals were observed in the images of the coating surface after heat treatment. This confirmed that in any of the coated cutting tools of samples No. 1 to No. 6 of the Examples, the coating contained needle-like crystals after heat treatment, and at least a portion of the needle-like crystals were located on the surface of the coating. On the other hand, in any of the coated cutting tools of samples No. 7 to No. 9 of the Comparative Examples, no needle-like crystals were observed in the images of the coating surface. This confirmed that in any of the coated cutting tools of samples No. 7 to No. 9 of the Comparative Examples, the content of needle-like crystals in the coating remained below 1% after heat treatment.
[0126] Figure 6 This is an image showing the coated surface of the coated tool of sample No. 1 in embodiment after heat treatment. Figure 6 As shown, regarding the coated cutting tool of sample No. 1 in the embodiment, it was confirmed that the coating contained needle-like crystals after heat treatment, and at least a portion of the needle-like crystals were located on the surface of the coating.
[0127] Figure 7This is an image showing the coated surface of the coated tool of Comparative Example No. 7 after heat treatment. (See image.) Figure 7 As shown, regarding the coated cutting tool of Comparative Example No. 7, it was confirmed that the content of needle-like crystals in the coating remained below 1% after heat treatment.
[0128] Next, for the coated cutting tools of samples No. 1 to No. 6 in the embodiments, the length of the image of the needle-like crystals in the longitudinal direction and the width of the image of the needle-like crystals in the transverse direction were obtained using the image processing software "Mac-View". Then, the aspect ratio of the needle-like crystals was calculated by dividing the length of the image of the needle-like crystals in the longitudinal direction by the width of the image of the needle-like crystals in the transverse direction. The calculated aspect ratio values of the needle-like crystals are shown in Table 2. In any of the coated cutting tools of samples No. 1 to No. 6 in the embodiments, the average aspect ratio of the needle-like crystals was found to be 2 or more and 10 or less. In any of the coated cutting tools of samples No. 1 to No. 5 in the embodiments, the average aspect ratio of the needle-like crystals was found to be 3 or more and 10 or less. On the other hand, the aspect ratio of the crystals was also calculated for the coated cutting tools of samples No. 7 to No. 9. The calculated aspect ratio values of the crystals are shown in the "Aspect Ratio of Needle-like Crystals" column of Table 2. In the coated cutting tools of the comparative examples No.7 to No.9, it was confirmed that the average aspect ratio of the crystals was less than 2.
[0129] Next, regarding the coated cutting tools of samples No. 1 to No. 6 of the Examples, when confirming the content of needle-like crystals 5 in the coating 3 of the coated cutting tool 1 after heat treatment, all were in the range of 50% to 95%. Regarding the coated cutting tools of samples No. 7 to No. 9 of the Comparative Examples, when investigating the content of needle-like crystals 5 in the coating 3 of the coated cutting tool 1 after heat treatment, all were 10% or less.
[0130] Next, for the coated cutting tools of samples No. 1 to No. 9, the types of elements contained in the surface coating after heat treatment were determined using an energy-dispersive X-ray spectroscopy instrument attached to a scanning transmission electron microscope. In any of the coated cutting tools of samples No. 1 to No. 9, it was confirmed that the coating after heat treatment contained the elements included in the composition shown in Table 1.
[0131] For coated cutting tools of samples No.1 to No.7 and No.9, the Al and Ti contents in the coating after heat treatment were determined. In any of the coated cutting tools of samples No.1 to No.7 and No.9, it was confirmed that after heat treatment, the Al content in the coating was greater than the Ti content in the coating.
[0132] Regarding the coated cutting tools of samples No. 1 to No. 7 and No. 9, the ratio Y of the Al content to the Ti content in the coating after heat treatment was calculated. The calculated values of Y are shown in Table 2. In any of the coated cutting tools of samples No. 1 to No. 5 of the examples and sample No. 9 of the comparative example, it was confirmed that the ratio Y of the Al content to the Ti content in the coating surface was 2 or more after heat treatment. On the other hand, in the coated cutting tool of sample No. 6 of the examples and sample No. 7 of the comparative example, it was confirmed that the ratio Y of the Al content to the Ti content in the coating surface was less than 2 after heat treatment.
[0133] Regarding the coated cutting tools of samples No. 1 to No. 7 and No. 9, the value of Y / X was calculated based on the ratio X of the Al content to the Ti content in the coating before heat treatment and the ratio Y of the Al content to the Ti content in the coating after heat treatment. The calculated Y / X values are shown in Table 2. In any of the coated cutting tools of samples No. 1 to No. 5 in the examples, it was confirmed that the relationship Y / X > 2 was satisfied. On the other hand, in any of the coated cutting tools of sample No. 6 in the examples and any of the coated cutting tools of samples No. 7 and No. 9 in the comparative examples, it was confirmed that the relationship Y / X > 2 was not satisfied.
[0134] Next, for the coated cutting tools of samples No. 1 to No. 6 of the embodiments, the types of elements contained in the tips of the needle-like crystals in the heat-treated coating were determined using an energy-dispersive X-ray spectrometer attached to a scanning transmission electron microscope. In any of the coated cutting tools of samples No. 1 to No. 4 of the embodiments, it was confirmed that the tips of the needle-like crystals contained Al, Nb, and O. On the other hand, in any of the coated cutting tools of samples No. 5 and No. 6 of the embodiments, it was confirmed that the tips of the needle-like crystals contained Al and O, but Nb was not confirmed to be present in the tips of the needle-like crystals.
[0135] Next, cutting tests were conducted on the coated cutting tools of the embodiments and the coated cutting tools of the comparative examples. The cutting test conditions are as follows.
[0136] Cutting conditions:
[0137] Workpiece material: SUS304
[0138] Cutting speed: Vc = 100 m / min (low speed) and 150 m / min (high speed)
[0139] Feed rate: f = 0.1 mm / rev
[0140] Depth of cut: ae = 1.5 mm
[0141] Cutting condition: wet
[0142] Cutting tool shape: GBA43R300-030GM
[0143] Evaluation method: Perform turning for 120 minutes under the above conditions, and measure the wear width of the front and rear cutting faces after cutting.
[0144] Table 3 shows the results of cutting tests on the coated cutting tools of samples No.1 to No.9. More specifically, Table 3 shows the wear width (mm) of the rake and flank faces of the coated cutting tools under the above-mentioned cutting conditions when performing low-speed or high-speed cutting.
[0145] Table 3
[0146]
[0147] As shown in Table 3, the wear width of the rake and flank faces of the coated cutting tools of the Examples No. 1 to No. 6 were smaller than those of the coated cutting tools of the Comparative Examples No. 7 to No. 9, regardless of whether the cutting speed was low or high. Thus, it was confirmed that the performance of the coated cutting tools of the Examples No. 1 to No. 6 was improved compared to the coated cutting tools of the Comparative Examples No. 7 to No. 9. This is believed to be because the coating, after heat treatment, contains needle-like crystals, at least a portion of which are located on the surface of the coating, thereby improving the performance of the coated cutting tool. It is thought that by making the average aspect ratio of the needle-like crystals 2 or more and 10 or less, the performance of the coated cutting tool is improved.
[0148] The wear width of the rake and flank faces of the coated cutting tools of samples No. 1 to No. 5 in the examples, regardless of whether they are cutting at low speed or high speed, is smaller than that of the coated cutting tool of sample No. 6 in the examples. Thus, it is confirmed that the performance of the coated cutting tools of samples No. 1 to No. 5 in the examples is improved compared to the coated cutting tool of sample No. 6 in the examples. This is considered to be because the average aspect ratio of the needle-like crystals is 3 or more and 10 or less, thereby further improving the performance of the coated cutting tool. It is considered to be because by including Al and Ti in the coating, and ensuring that the ratio of Al content to Ti content in the coating surface is 2 or more after heat treatment, the performance of the coated cutting tool is further improved. It is considered to be because by including Al and Ti in the coating, and ensuring that the ratio X of Al content to Ti content in the coating before heat treatment and the ratio Y of Al content to Ti content in the coating after heat treatment satisfy the relationship Y / X > 2, the performance of the coated cutting tool is further improved.
[0149] The wear width of the rake and flank faces of the coated cutting tools of samples No. 1 to No. 4 in the examples, regardless of whether they are used for low-speed or high-speed cutting, is smaller than that of the coated cutting tools of samples No. 5 and No. 6 in the examples. Thus, it is confirmed that the performance of the coated cutting tools of samples No. 1 to No. 4 in the examples is improved compared to the coated cutting tools of samples No. 5 and No. 6 in the examples. It is believed that the performance of the coated cutting tools is further improved by the presence of Al, Nb, and O in the needle-like crystals.
[0150] The wear width of the rake and flank faces of the coated cutting tools of samples No. 1 and No. 2 in the embodiments is smaller than that of the coated cutting tools of samples No. 3 to No. 6 in the embodiments, regardless of whether the cutting speed is low or high. Thus, it is confirmed that the performance of the coated cutting tools of samples No. 1 and No. 2 in the embodiments is improved compared to the coated cutting tools of samples No. 3 to No. 6 in the embodiments. It is believed that the performance of the coated cutting tools is further improved by the presence of at least one of W and Si in the coating.
[0151] The wear width of the rake and flank faces of the coated tool of Sample No. 1 in Example 1 is smaller than that of the coated tools of Samples No. 2 to No. 6 in Example 2, regardless of whether the cutting speed is low or high. Thus, it is confirmed that the performance of the coated tool of Sample No. 1 in Example 1 is improved compared to the coated tools of Samples No. 2 to No. 6 in Example 2. It is believed that the performance of the coated tool is further improved by the presence of W in the coating.
[0152] This technology can be configured as follows. (1)
[0154] A coated cutting tool, comprising:
[0155] Matrix;
[0156] At least one coating located on the substrate,
[0157] The coating contains at least one element selected from elements of groups 4, 5, and 6 of the periodic table, Al, and Si, and at least one element selected from C and N.
[0158] The coating, after heat treatment at a temperature above 1050°C and below 1100°C in an atmospheric atmosphere, contains needle-like crystals.
[0159] At least a portion of the needle-like crystals are located on the surface of the coating. (2)
[0161] According to the coated cutting tool described in (1) above, the content of the needle-like crystals in the coating is less than 1% before the heat treatment. (3)
[0163] According to the coated cutting tool described in (1) or (2) above, the average aspect ratio of the needle-like crystal is 2 or more and 10 or less. (4)
[0165] The coated cutting tool according to any one of (1) to (3) above, wherein the coating contains Al. (5)
[0167] The coated cutting tool according to any one of (1) to (4) above, wherein the needle-like crystals contain Al and O. (6)
[0169] The coated cutting tool according to any one of (1) to (5) above, wherein the coating contains Nb. (7)
[0171] The coated cutting tool according to any one of (1) to (6) above, wherein the needle-like crystals contain Nb and O. (8)
[0173] The coated cutting tool according to any one of (1) to (7) above, wherein the coating contains at least one of W and Si. (9)
[0175] The coated cutting tool according to any one of (1) to (8) above, wherein,
[0176] The coating contains W,
[0177] The needle-like crystals contain W and O. (10)
[0179] The coated cutting tool according to any one of (1) to (9) above, wherein,
[0180] The coating contains Al and Ti.
[0181] The Al content in the coating is greater than the Ti content in the coating. (11)
[0183] The coated cutting tool according to any one of (1) to (10) above, wherein,
[0184] The coating contains Al and Ti.
[0185] The ratio of the Al content in the surface of the coating to the Ti content in the surface of the coating is 2 or more after the heat treatment. (12)
[0187] The coated cutting tool according to any one of (1) to (11) above, wherein,
[0188] The coating contains Al and Ti.
[0189] The ratio X of the Al content in the coating before heat treatment to the Ti content in the coating, and the ratio Y of the Al content in the coating after heat treatment to the Ti content in the coating, satisfy the relationship Y / X > 2. (13)
[0191] A cutting tool having:
[0192] A rod-shaped knife handle with a groove at the end;
[0193] The coated cutting tool located in the slot of any one of (1) to (12). (14)
[0195] A method for manufacturing a workpiece by cutting, comprising the following steps:
[0196] The process of rotating the workpiece or the cutting tool described in (13) above;
[0197] The process of bringing the workpiece into contact with the cutting tool;
[0198] The process of moving the cutting tool away from the workpiece.
[0199] Further effects and variations can be readily derived by those skilled in the art. Therefore, the invention is presented in a broader manner, not limited to the specific details and representative embodiments expressed and described above. Thus, various modifications can be made without departing from the spirit or scope of the overall inventive concept as defined by the appended claims and their equivalents.
[0200] Explanation of reference numerals in the attached figures
[0201] 1 Coated cutting tools
[0202] 11 blades
[0203] 15 Through holes
[0204] 2. Matrix
[0205] 3. Coating
[0206] 5. Needle-like crystals
[0207] 70 knife handle
[0208] 73 Card Slots
[0209] 75 bolts
[0210] 100 Cutting Tools
[0211] L length
[0212] W width
Claims
1. A coated cutting tool, comprising: matrix; and At least one coating located on the substrate, The coating contains: At least one element selected from elements in groups 4, 5, and 6 of the periodic table, Al, and Si; and At least one element chosen from C and N, The coating, after heat treatment at a temperature above 1050°C and below 1100°C in an atmospheric atmosphere, contains needle-like crystals. At least a portion of the needle-like crystals are located on the surface of the coating.
2. The coated cutting tool according to claim 1, wherein, The content of the needle-like crystals in the coating is less than 1% before the heat treatment.
3. The coated cutting tool according to claim 1 or 2, wherein, The average aspect ratio of the needle-like crystals is greater than 2 and less than 10.
4. The coated cutting tool according to any one of claims 1 to 3, wherein, The coating contains Al.
5. The coated cutting tool according to any one of claims 1 to 4, wherein, The needle-like crystals contain Al and O.
6. The coated cutting tool according to any one of claims 1 to 5, wherein, The coating contains Nb.
7. The coated cutting tool according to any one of claims 1 to 6, wherein, The needle-like crystals contain Nb and O.
8. The coated cutting tool according to any one of claims 1 to 7, wherein, The coating contains at least one of W and Si.
9. The coated cutting tool according to any one of claims 1 to 8, wherein, The coating contains W, The needle-like crystals contain W and O.
10. The coated cutting tool according to any one of claims 1 to 9, wherein, The coating contains Al and Ti. The Al content in the coating is greater than the Ti content in the coating.
11. The coated cutting tool according to any one of claims 1 to 10, wherein, The coating contains Al and Ti. The ratio of the Al content in the surface of the coating to the Ti content in the surface of the coating is greater than 2 after the heat treatment.
12. The coated cutting tool according to any one of claims 1 to 11, wherein, The coating contains Al and Ti. The ratio X of the Al content in the coating before heat treatment to the Ti content in the coating, and the ratio Y of the Al content in the coating after heat treatment to the Ti content in the coating, satisfy the relationship Y / X > 2.
13. A cutting tool, comprising: A rod-shaped handle with a groove at the end; and The coated cutting tool according to any one of claims 1 to 12 located within the slot.
14. A method for manufacturing a workpiece that has been machined by cutting, wherein, It has the following processes: The process of rotating the workpiece or the cutting tool as described in claim 13; The process of bringing the workpiece into contact with the cutting tool; and The process of moving the cutting tool away from the workpiece.
Citation Information
Patent Citations
Coated tool
WO2012018063A1