Wiring structure, manufacturing method of wiring structure and semiconductor element
By configuring through-post components on the insulating film, the problem of wrinkles forming in the flexible resin-cured insulating film during the thermal process is solved, achieving high-precision manufacturing and improved reliability of the wiring structure.
Patent Information
- Application Number
- CN202580029150.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-08-07
- Filing Date
- 2025-08-05
- Publication Date
- 2026-11-17
AI Technical Summary
When wiring is formed on an insulating film composed of a soft, cured resin, it is easily affected by the thermal process, resulting in wrinkles and variations in wiring width and spacing.
Post components are disposed on the insulating film, penetrating the thickness direction of the insulating film and not overlapping with the wiring. The post components are used to hold the insulating film in place to reduce expansion and contraction caused by thermal processes and suppress the formation of wrinkles.
It effectively suppresses wrinkles on the insulating film, ensures that the line width and spacing of the wiring meet the design values, and improves the reliability of semiconductor components.
Smart Images

Figure CN123126101A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a wiring structure, a method for manufacturing the wiring structure, and a semiconductor element. Background Technology
[0002] In recent years, with the increasing integration, miniaturization, and micronization of semiconductor devices, there are growing demands for superior electrical properties, heat resistance, and mechanical properties in insulating films used in surface protective layers, interlayer insulating films, and redistribution layers of semiconductor devices. As a material for forming insulating films with these properties, photosensitive resin compositions containing alkali-soluble resins have been developed (see, for example, Patent Documents 1-3). The photosensitive resin composition is coated and dried on a substrate to form a resin film, and a patterned resin film (a patterned resin film) is obtained by exposing and developing the resin film. The patterned cured film (a patterned cured film) obtained by heating and curing the resin film can be used as an insulating film.
[0003] Previous technical documents Patent documents Patent Document 1: Japanese Patent Application Publication No. 2008-309885 Patent Document 2: Japanese Patent Application Publication No. 2007-057595 Patent Document 3: International Publication No. 2010 / 073948 Summary of the Invention
[0004] The technical problem to be solved by the invention The insulating film used as a rewiring layer is sometimes made of a relatively soft, cured resin, depending on the required dielectric properties. In insulating films made of such cured resins, wrinkles can sometimes occur due to the thermal process during wiring formation. These wrinkles are considered to cause deformation of the wiring on the insulating film, leading to variations in wire width or spacing between wires.
[0005] The present invention was made to solve the above-mentioned problems, and its purpose is to provide a wiring structure capable of suppressing deformation of wiring on an insulating film, a method for manufacturing the wiring structure, and a semiconductor element.
[0006] means for solving technical problems The main idea of this invention is as follows.
[0007] [1] A wiring structure comprising: a support; an insulating film disposed on the support by a cured form of a photosensitive resin composition; wiring disposed on the insulating film in a predetermined pattern; and a post member disposed to penetrate the insulating film in the thickness direction at a position not overlapping with the wiring.
[0008] In this wiring structure, post members are arranged to extend through the thickness direction of the insulating film. By securing the insulating film with the post members, the expansion and contraction of the insulating film during the thermal process of forming wiring on the insulating film can be reduced. Therefore, even when the insulating film is made of a relatively soft resin curing material, wrinkles on the insulating film can be suppressed. By suppressing wrinkles in the insulating film, deformation of the wiring on the insulating film can be suppressed, and the linewidth or spacing between wirings can be formed with high precision relative to the design values.
[0009] [2] According to the wiring structure described in [1], the post member has a flange extending onto the insulating film. In this case, the insulating film is more reliably secured by the flange on the post member. Therefore, wrinkles on the insulating film can be suppressed more effectively.
[0010] [3] According to the wiring structure described in [1] or [2], the post component is engaged with the support body. In this case, the insulating film is more reliably secured by the engagement of the post component with the support body. Therefore, wrinkles on the insulating film can be suppressed more effectively.
[0011] [4] The wiring structure according to any one of [1] to [3], wherein the cross-section of the post component is circular. In this case, stress concentration near the boundary between the post component and the insulating film can be avoided. Therefore, wrinkles on the insulating film can be suppressed more effectively.
[0012] [5] The wiring structure according to any one of [1] to [4], wherein multiple insulating films are stacked in the thickness direction, and multiple post members are disposed corresponding to the multiple insulating films. In this case, even when multiple insulating films are stacked, wrinkles on each insulating film can be suppressed.
[0013] [6] According to the wiring structure described in [5], a post member disposed on an insulating film has a flange extending onto the insulating film, the flange being embedded in another insulating film adjacent to the first insulating film in the thickness direction. In this case, since the post members of each insulating film have flanges, each insulating film is more reliably locked. Furthermore, since the flange of one post member is embedded in another insulating film, the locking effect of the other insulating film is improved, and wrinkles on the other insulating film can be more effectively suppressed.
[0014] [7] According to the wiring structure described in [5] or [6], a post member disposed on one insulating film engages with another post member disposed on another insulating film adjacent to the first insulating film in the thickness direction. In this case, by engaging the post members with each other in the thickness direction, the insulating films are more reliably secured. Therefore, wrinkles on the insulating films can be suppressed more effectively.
[0015] [8] The wiring structure according to any one of [1] to [7], wherein, when viewed from the thickness direction, the post member is configured to at least sandwich the forming region of the wiring. With this configuration of the post member, wrinkles on the insulating film can be more reliably suppressed.
[0016] [9] A method for manufacturing a wiring structure, comprising: a preparation step of preparing a support body; an insulating film forming step of forming an insulating film composed of a cured photosensitive resin composition on the support body in a predetermined pattern; a seed layer forming step of forming a seed layer on the insulating film; and a plating step of growing a plating layer on the seed layer to form wiring on the insulating film and a stud member penetrating the insulating film along the thickness direction at a position not overlapping with the wiring.
[0017] In this method for manufacturing a wiring structure, a plating layer is grown on a seed layer on an insulating film formed with a predetermined pattern to form wiring on the insulating film and post members penetrating the insulating film along the thickness direction at positions that do not overlap with the wiring. According to this method, wiring and post members can be formed on the insulating film simultaneously, thus simplifying the manufacturing process. In the wiring structure obtained by this method, the post members hold the insulating film in place, thereby reducing the amount of expansion and contraction of the insulating film during the thermal process of forming wiring on the insulating film. Therefore, even when the insulating film is composed of a relatively soft, cured resin, wrinkles on the insulating film can be suppressed. By suppressing wrinkles in the insulating film, deformation of the wiring on the insulating film can be suppressed, allowing the linewidth of the wiring or the spacing between the wirings to approach the design value.
[0018]
[10] According to the method for manufacturing the wiring structure described in [9], the insulating film is formed by coating and curing the photosensitive resin composition in the insulating film forming step. According to this method, the insulating film can be formed with high precision relative to the design value.
[0019]
[11] According to the method for manufacturing the wiring structure described in [9], in the insulating film forming step, the insulating film is formed by laminating a film of the cured photosensitive resin composition. According to this method, the insulating film can be formed with high precision relative to the design value.
[0020]
[12] A semiconductor element comprising: a wiring structure as described in any one of [1] to [8]; and a semiconductor chip electrically connected to the wiring in the wiring structure.
[0021] In this semiconductor device, deformation of the wiring on the insulating film is suppressed in the wiring structure electrically connected to the semiconductor chip. By forming the linewidth or spacing between wirings with high precision relative to design values, the reliability of the semiconductor device can be improved.
[0022] Invention Effects According to the present invention, deformation of wiring on the insulating film can be suppressed. Attached Figure Description
[0023] Figure 1 This is a schematic cross-sectional view showing the structure of a semiconductor element according to the first embodiment of the present invention.
[0024] Figure 2 (a) and Figure 2 (b) is a schematic top view showing an example of the configuration of the pile components.
[0025] Figure 3 (a) ~ Figure 3 (c) is a schematic top view showing an example of the configuration of the pile components.
[0026] Figure 4 (a) and Figure 4 (b) is a schematic top view showing an example of the configuration of the pile components.
[0027] Figure 5 (a) ~ Figure 5 (c) is a schematic top view showing an example of the configuration of the pile components.
[0028] Figure 6 (a) is a schematic cross-sectional view showing the preparation process. Figure 6 (b) is a schematic cross-sectional view showing the insulating film formation process. Figure 6 (c) is a schematic cross-sectional view showing the seed layer formation process.
[0029] Figure 7 (a) and Figure 7 (b) is a schematic cross-sectional view showing the plating process.
[0030] Figure 8 (a) is a schematic cross-sectional view showing a re-implementation of the insulating film formation process. Figure 8 (b) is a schematic cross-sectional view showing the wiring structure obtained through the implementation of each process.
[0031] Figure 9(a) is a schematic cross-sectional view showing the installation process. Figure 9 (b) is a schematic cross-sectional view showing the semiconductor element obtained after the mounting process.
[0032] Figure 10 This is a schematic cross-sectional view showing the structure of a semiconductor element according to the second embodiment of the present invention.
[0033] Figure 11 (a) is a schematic cross-sectional view showing the preparation process. Figure 11 (b) is a schematic cross-sectional view showing the insulating film formation process. Figure 11 (c) is a schematic cross-sectional view showing the seed layer formation process.
[0034] Figure 12 (a) and Figure 12 (b) is a schematic cross-sectional view showing the plating process.
[0035] Figure 13 (a) is a schematic cross-sectional view showing a re-implementation of the insulating film formation process. Figure 13 (b) is a schematic cross-sectional view showing a semiconductor device obtained after a repeat of the insulating film formation process. Detailed Implementation
[0036] Hereinafter, with reference to the accompanying drawings, preferred embodiments of the wiring structure, the method for manufacturing the wiring structure, and the semiconductor element according to one aspect of the present invention will be described in detail.
[0037] In the following explanation, the numerical range indicated by "~" represents the range within which the values recorded before and after "~" are included as the minimum and maximum values, respectively. Furthermore, within the segmented numerical range, the upper or lower limit of one numerical range can be replaced with the upper or lower limit of another segmented numerical range.
[0038] In this specification, the terms "layer" and "film," when viewed in a plan view, include not only the structure of the shape formed over the entire surface but also the structure of the shape formed in a portion of it. The term "process" refers not only to an independent process but also to any process that achieves its intended purpose, even if it cannot be clearly distinguished from other processes.
[0039] In this specification, "(meth)acryloyl" means "acryloyl" and at least one of its corresponding "methacryloyl", and the same applies to other similar expressions such as (meth)acrylic acid and (meth)acrylate.
[0040] [First Implementation] Figure 1This is a schematic cross-sectional view illustrating the structure of a semiconductor element according to the first embodiment of the present invention. Figure 1 As shown, semiconductor element 1A is configured to include a semiconductor chip 2A and a wiring structure 3A. Examples of electronic devices using semiconductor element 1A include mobile phones, smartphones, tablet computers, personal computers, and hard drive mounts. Examples of semiconductor chip 2A include LSI chips, CMOS sensor chips, and memory chips. Terminal electrodes 4, made of solder or the like, are provided on the mounting surface of semiconductor chip 2A. Semiconductor chip 2A is electrically connected to wiring 13 of wiring structure 3A via flip-chip connections through terminal electrodes 4.
[0041] A filler material 5 is disposed between the semiconductor chip 2A and the wiring structure 3A, covering the terminal electrode 4. The filler material 5 is a so-called CUF (Capillary Underfill), for example, made of epoxy resin. The placement of the filler material 5 increases the mechanical strength of the joint between the semiconductor chip 2A and the wiring structure 3A, thereby improving the reliability of the joint. The semiconductor chip 2A, including the filler material 5, is sealed by a sealing material 6. The sealing material 6 is, for example, made of epoxy resin. The components of the sealing material 6 may include fillers, curing agents, curing accelerators, etc. Furthermore, the components of the sealing material 6 may, as needed, include colorants, release agents, modifiers, flame retardants, etc.
[0042] The wiring structure 3A is configured to include a substrate 11 serving as a support K, an insulating film 12, wiring 13, and a post component 14. The substrate 11 forms the base of the wiring structure 3A. The substrate 11 is made of, for example, a glass substrate, a resin substrate, a silicon wafer, or a metal thin film. The substrate 11 has a first surface 11a on the side of the semiconductor chip 2A and a second surface 11b on the side opposite to the semiconductor chip 2A. Substrate wiring 15 with a predetermined pattern is formed on the first surface 11a and the second surface 11b. Here, the substrate wiring 15 on the first surface 11a and the substrate wiring 15 on the second surface 11b are formed in a symmetrical pattern sandwiching the substrate 11, and are electrically connected to each other through through-holes 15a penetrating the substrate 11 along the thickness direction.
[0043] The insulating film 12 is an electrically insulating film that serves as the substrate for the wiring 13. The insulating film 12 is formed, for example, by coating and curing a photosensitive resin composition. The insulating film 12 can also be formed by laminating a film of a cured photosensitive resin composition. The photosensitive resin composition, for example, contains maleimide resin, (meth)acrylic acid monomer, and a photopolymerization initiator. The maleimide resin is a reaction product of tetracarboxylic acid dianhydride (a1), an amine (a2), and maleic anhydride (a3). The amine (a2) includes a dimerized diamine. The (meth)acrylic acid monomer includes a multifunctional (meth)acrylic acid monomer.
[0044] The glass transition temperature (Tg) of the cured photosensitive resin composition is, for example, 80°C or higher. The glass transition temperature (Tg) can be 90°C or higher, 100°C or higher, or 110°C or higher. There is no particular upper limit to the glass transition temperature (Tg); for example, it can be below 250°C or below 200°C.
[0045] The cured product of the photosensitive resin composition has a coefficient of linear expansion (CTE) of 120 ppm / ℃ or less at temperatures ranging from -20 to 40°C. The CTE can be 115 ppm / ℃ or less, 110 ppm / ℃ or less, or 100 ppm / ℃ or less. There is no particular limitation on the lower limit of the CTE; for example, it can be 30 ppm / ℃ or more, or 60 ppm / ℃ or more.
[0046] The insulating film 12 is a cured product of a photosensitive resin composition containing the above-mentioned components, thereby enabling the insulating film 12 to possess sufficiently low dielectric properties (low dielectric constant and low dielectric loss tangent). The glass transition temperature Tg and coefficient of linear expansion CTE of the cured photosensitive resin composition are within the above-mentioned ranges, thereby maintaining the shape of the insulating film 12, which serves as the substrate for the wiring 13, while maintaining low dielectric properties.
[0047] In this embodiment, from the viewpoint of maintaining the shape of the insulating film 12, the elastic modulus of the cured photosensitive resin composition at 20°C can be, for example, 1000 MPa or more, 1200 MPa or more, or 1600 MPa or more. There is no particular limitation on the upper limit of the elastic modulus; for example, it can be 5000 MPa or less, or 3000 MPa or less. The relative permittivity of the cured photosensitive resin composition at 10 GHz can be, for example, less than 2.8. The dielectric loss tangent of the cured photosensitive resin composition at 10 GHz can be, for example, less than 0.0060°.
[0048] In this embodiment, multiple insulating films 12 are stacked in the thickness direction. Figure 1 In this example, the first insulating film 12A, the second insulating film 12B, and the third insulating film 12C are sequentially stacked on the first surface 11a and the second surface 11b of the substrate 11, respectively. The thicknesses of the first insulating film 12A, the second insulating film 12B, and the third insulating film 12C are appropriately set according to the specifications of the wiring structure 3A. Figure 1 In the example, the thickness of the second insulating film 12B is greater than the thickness of the third insulating film 12C, and the thickness of the third insulating film 12C is greater than the thickness of the first insulating film 12A.
[0049] Wiring 13 is a component that electrically connects the semiconductor chip 2A to an external device. Wiring 13 is formed on an insulating film 12 in a predetermined pattern, for example, by electroplating. Here, when viewed from the thickness direction of the insulating film 12, the formation region R of wiring 13 is located in the region overlapping with the semiconductor chip 2A. For example, copper can be used as a forming material for wiring 13. In this embodiment, wiring 13 is formed on each of a plurality of insulating films 12 as a substrate. Figure 1 In the example, wiring 13 is composed of first wiring 13A on first insulating film 12A and second wiring 13B on second insulating film 12B.
[0050] The first wiring 13A is electrically connected to the substrate wiring 15 of the substrate 11 via a through-hole 13a penetrating the first insulating film 12A in the thickness direction. The second wiring 13B is electrically connected to the first wiring 13A via a through-hole 13a penetrating the second insulating film 12B in the thickness direction. The second wiring 13B on the first surface 11a side of the substrate 11 is covered by the third insulating film 12C and is electrically connected to the terminal electrode 4 of the semiconductor chip 2A within a through-hole penetrating the third insulating film 12C in the thickness direction. The second wiring 13B on the second surface 11b side of the substrate 11 is exposed from the third insulating film 12C. Solder balls 7 are bonded to this exposed portion.
[0051] The post component 14 is a component that suppresses deformation of the wiring 13 on the insulating film 12. Similar to the wiring 13, the post component 14 is formed, for example, by electroplating in a predetermined pattern. Copper can be used as a forming material for the wiring 13. The post component 14 is formed such that it penetrates the insulating film 12 along its thickness direction at a location that does not overlap with the wiring 13.
[0052] The pile component 14 has a main body 14a located within the insulating membrane 12 and a flange 14b extending onto the insulating membrane 12. The main body 14a has, for example, a circular cross-section. Similarly, the flange 14b has, for example, a circular cross-section. The cross-sectional shapes of the main body 14a and the flange 14b are not limited to circular shapes; they can be elliptical, oblong, strip-shaped, rectangular, polygonal, or other shapes. The cross-sectional shapes of the main body 14a and the flange 14b can be the same or different.
[0053] In this embodiment, a plurality of post members 14 are disposed corresponding to a plurality of insulating films 12. One post member 14 is bonded to a substrate 11. A post member 14 disposed on an insulating film 12 has a flange portion 14b extending onto an insulating film 12, the flange portion 14b being embedded in another insulating film 12 adjacent to the first insulating film 12 in the thickness direction. One post member 14 disposed on an insulating film 12 is bonded to another post member 14 disposed on another insulating film 12 adjacent to the first insulating film 12 in the thickness direction.
[0054] exist Figure 1 In this example, a first post member 14A corresponding to the first insulating film 12A and a second post member 14B corresponding to the second insulating film 12B are provided. The main body portion 14a of the first post member 14A is configured to penetrate the first insulating film 12A in the thickness direction. The end portion of the main body portion 14a of the first post member 14A opposite to the flange portion 14b is joined to the substrate wiring 15, and substantially joined to the substrate 11 via the substrate wiring 15. The flange portion 14b of the first post member 14A is embedded in the second insulating film 12B.
[0055] The main body 14a of the second post component 14B is configured to penetrate the second insulating film 12B along its thickness direction. The end of the main body 14a of the second post component 14B opposite to the flange 14b engages with the flange 14b of the first post component 14A, and is substantially engaged with the first post component 14A via the flange 14b. The flange 14b of the second post component 14B is embedded in the third insulating film 12C. The second post component 14B is separate from the semiconductor chip 2A, and neither the first post component 14A nor the second post component 14B is electrically connected to the semiconductor chip 2A.
[0056] The position of the post member 14, when viewed from the thickness direction of the insulating film 12, is not particularly limited as long as it does not overlap with the wiring 13. For example, when viewed from the thickness direction of the insulating film 12, the post member 14 is positioned in a location that does not overlap with the semiconductor chip 2A, that is, outside the formation region R of the wiring 13. In this case, as Figure 2 As shown in (a), the post member 14 can be configured corresponding to one corner of the insulating film 12. The post member 14 can be configured to at least sandwich the forming region R of the wiring 13. At this time, as... Figure 2 As shown in (b), the pile component 14 can be arranged at a set of diagonals of the insulating film 12 in a manner that sandwiches the forming region R.
[0057] like Figure 3 As shown in (a), the pile component 14 can be arranged correspondingly at the four corners of the insulating film 12 in a manner that clamps the forming region R, as... Figure 3 As shown in (b), the insulating film 12 can also be sandwiched at any position on the line between the four corners and the connecting corners in a manner that forms the region R. Figure 3 (b) is configured accordingly, with the midpoint between the corners. Figure 3 As shown in (c), multiple pile components 14 can be connected to each other via a common flange 14b.
[0058] For example, when viewed from the thickness direction of the insulating film 12, the post member 14 can be positioned at a location overlapping with the semiconductor chip 2A, that is, positioned inside the formation region R of the wiring 13. At this time, as... Figure 4As shown in (a), the stake member 14 can be positioned at the center of the wiring formation area R. The stake member 14 can be positioned both outside and inside the formation area R. In this case, as... Figure 4 As shown in (b), the stake component 14 can be positioned at the center of the wiring formation area R and at a set of opposite corners of the insulating film 12.
[0059] like Figure 5 As shown in (a), the stake component 14 can be disposed in the center of the wiring formation area R and at the four corners of the insulating film 12, as follows: Figure 5 As shown in (b), the stake component 14 can be positioned at any location on the line between the four corners of the insulating film 12 and the connecting corners of the wiring formation area R. Figure 5 (b) is the midpoint between the corners). And, as... Figure 5 As shown in (c), the stake component 14 can be positioned at any position on the line between the center of the wiring forming region R, a set of diagonals of the forming region R, the four corners of the insulating film 12, and the connecting corners. Figure 5 (c) is the midpoint between the corners). Figure 5 (b) and Figure 5 As shown in (c), multiple pile components 14 can be connected to each other via a common flange 14b. Figure 5 As shown in (c), the common flange 14b can extend in a manner that overlaps with the forming region R.
[0060] Next, the manufacturing method of the above-mentioned wiring structure 3A will be described.
[0061] Here, the manufacturing process of the semiconductor element 1A, including the manufacturing process of the wiring structure 3A, will be described. The manufacturing method is configured to include a preparation process S01, an insulating film formation process S02, a seed layer formation process S03, a plating process S04, and an mounting process S05.
[0062] Preparation step S01 is the step of preparing the support K. In preparation step S01, firstly, as follows... Figure 6 As shown in (a), a substrate 11 is prepared as a support K. For example, a substrate with a first surface 11a substrate wiring 15, a second surface 11b substrate wiring 15 and a through hole 15a pre-formed on it can be used as the substrate 11.
[0063] The insulating film forming process S02 is a process in which an insulating film 12, composed of a cured photosensitive resin composition, is formed on a support K in a predetermined pattern. In the insulating film forming process S02, the insulating film 12 can be formed by coating and curing the photosensitive resin composition, or by laminating a thin film of the cured photosensitive resin composition. In this embodiment, for example, a spin coater is used to coat the photosensitive resin composition onto the first surface 11a and the second surface 11b of the substrate 11. The coated photosensitive resin composition is then dried using a hot plate or the like. Afterwards, it undergoes exposure based on an exposure apparatus and development based on a development apparatus, such as... Figure 6 As shown in (b), a first insulating film 12A having a through hole for a first wiring 13A and a through hole for a first post member 14A is formed on the first surface 11a and the second surface 11b of the substrate 11.
[0064] The seed layer formation process S03 is the process of forming a seed layer 16 on the insulating film 12. The seed layer 16 is a layer that supplies power during the growth of the plating layer in the subsequent plating process S04. The forming material of the seed layer 16 may include, for example, titanium, copper, tungsten, nickel, or silver. Here, copper is used as the forming material for the wiring 13. Sputtering is used, for example, in the formation of the seed layer 16. Thus, as... Figure 6 As shown in (c), a seed layer 16 is formed on the first insulating film 12A and inside the through hole.
[0065] The plating process S04 is a process in which the plating layer 17 grows on the seed layer 16. In the plating process S04, through the growth of the plating layer 17, wiring 13 on the insulating film 12 and post components 14 penetrating the insulating film 12 along the thickness direction at positions that do not overlap with the wiring 13 are formed. In the plating process S04, firstly, as... Figure 7 As shown in (a), a dry film 18 is laminated on the seed layer 16 on the first insulating film 12A. Then, after exposure based on an exposure device and development based on a development device, an opening is formed on the dry film 18 with a pattern corresponding to the first wiring 13A, the through-hole of the first wiring 13A and the post component 14.
[0066] After the dry film 18 is formed, a plating layer 17 is grown on the seed layer 16, for example, by electroplating. After the growth of the plating layer 17, water washing, removal of the chemically based dry film 18, and removal of the etch-based seed layer 16 are performed, such as... Figure 7 As shown in (b), a first wiring 13A and a first post component 14A corresponding to the first insulating film 12A are formed on the first insulating film 12A.
[0067] In this embodiment, after the plating process S04, the insulating film formation process S02 is performed again, such as... Figure 8As shown in (a), a second insulating film 12B having a through hole for the second wiring 13B and a through hole for the second post component 14B is formed on the first insulating film 12A. Furthermore, after performing the insulating film forming process S02 again, the seed layer forming process S03 and the plating process S04 are performed again, and then the insulating film forming process S02 is performed again. Thus, as... Figure 8 As shown in (b), a second wiring 13B and a second post component 14B corresponding to the second insulating film 12B are formed on the second insulating film 12B. Furthermore, a third insulating film 12C, which becomes the uppermost layer, is formed on the second insulating film 12B. Through the above processes, a wiring structure 3A is obtained.
[0068] Mounting step S05 is the process of mounting the semiconductor chip 2A onto the wiring structure 3A. In mounting step S05, as follows... Figure 9 As shown in (a), the semiconductor chip 2A is mounted on the wiring structure 3A by bonding the terminal electrode 4 of the semiconductor chip 2A to the second wiring 13B exposed from the third insulating film 12C. A filler material 5 is disposed at the junction of the semiconductor chip 2A and the wiring structure 3A, and a sealing material 6 is disposed on the third insulating film 12C to cover the semiconductor chip 2A and the filler material 5. Finally, solder balls 7 are bonded to the portion of the second wiring 13B exposed from the second surface 11b side of the substrate 11, as shown in (a). Figure 9 As shown in (b), semiconductor element 1A is obtained.
[0069] As explained above, in the wiring structure 3A, a post member 14 is arranged to extend through the thickness direction of the insulating film 12. By securing the insulating film 12 with the post member 14, the expansion and contraction of the insulating film 12 during the thermal process of forming the wiring 13 on the insulating film 12 can be reduced. Therefore, even when the insulating film 12 is made of a relatively soft resin curing material, wrinkles on the insulating film 12 can be suppressed. By suppressing wrinkles on the insulating film 12, deformation of the wiring 13 on the insulating film 12 can be suppressed, and the linewidth or spacing between the wiring 13 can be formed with high precision relative to the design values.
[0070] In this embodiment, the post member 14 has a flange portion 14b extending onto the insulating film 12. Because the post member 14 has the flange portion 14b, the insulating film 12 is more reliably secured. Therefore, wrinkles on the insulating film 12 can be more effectively suppressed.
[0071] In this embodiment, the first post member 14A is joined to the substrate 11 (substrate wiring 15) which serves as the support K. With this structure, the insulating film 12 is more reliably held in place by the post member 14. Therefore, wrinkles on the insulating film 12 can be suppressed more effectively.
[0072] In this embodiment, the cross-section of the pile member 14 is circular. This avoids stress concentration near the boundary between the pile member 14 and the insulating film 12. Therefore, wrinkles on the insulating film 12 can be more effectively suppressed.
[0073] In this embodiment, multiple insulating films 12 are stacked in the thickness direction, and multiple pile members 14 are disposed corresponding to the multiple insulating films. In this case, even when multiple layers of insulating films 12 are stacked, wrinkles on each insulating film 12 can be suppressed.
[0074] In this embodiment, a stake member 14 disposed on an insulating film 12 has a flange portion 14b extending onto the insulating film 12, the flange portion 14b being embedded in another insulating film 12 adjacent to the first insulating film 12 in the thickness direction. According to this structure, each stake member 14 of the insulating film 12 has a flange portion 14b, thereby more reliably securing each insulating film 12. Furthermore, since the flange portion 14b of one stake member 14 is embedded in another insulating film 12, the securing effect of that other insulating film 12 is improved, and wrinkles on that other insulating film 12 can be more effectively suppressed.
[0075] In this embodiment, a stake member 14 disposed on one insulating film 12 is joined to another stake member 14 disposed on another insulating film 12 adjacent to one insulating film 12 in the thickness direction. According to this structure, the stake members 14 are joined to each other in the thickness direction, thereby more reliably locking each insulating film 12. Therefore, wrinkles on each insulating film 12 can be more effectively suppressed.
[0076] In this embodiment, when viewed from the thickness direction of the insulating film 12, the post member 14 is configured to at least sandwich the forming region R of the wiring 13. This configuration of the post member 14 can more reliably suppress the formation of wrinkles on the insulating film 12.
[0077] Furthermore, in the manufacturing method of the wiring structure according to this embodiment, a plating layer 17 is grown on a seed layer 16 on an insulating film 12 formed with a predetermined pattern to form wiring 13 on the insulating film 12 and a post member 14 penetrating the insulating film 12 along the thickness direction at a position that does not overlap with the wiring 13. According to this method, wiring 13 and post member 14 can be formed on the insulating film 12 simultaneously, thus simplifying the manufacturing process.
[0078] In this embodiment, in the insulating film forming step S02, the insulating film 12 is formed by coating and curing a photosensitive resin composition or by laminating a film of a cured photosensitive resin composition. According to this method, the insulating film can be formed with high precision relative to the design values.
[0079] In semiconductor element 1A, deformation of the wiring 13 on the insulating film 12 is suppressed in the wiring structure 3A that is electrically connected to semiconductor chip 2A. By forming the linewidth of the wiring 13 or the spacing between the wirings 13 with high precision relative to design values, the reliability of semiconductor element 1A can be improved.
[0080] [Second Implementation] Figure 10 This is a schematic cross-sectional view illustrating the structure of a semiconductor element according to the second embodiment of the present invention. Figure 10 As shown, semiconductor element 1B is configured to include semiconductor chip 2B and wiring structure 3B. Semiconductor element 1B is a FOWLP (Fan-Out Wafer Level Packaging) type element in which solder balls are directly placed on semiconductor chip 2B via a re-distribution layer (RDL) without using a circuit board.
[0081] The semiconductor chip 2B is configured to include a chip body 21 and a sealing plate 22. A plurality of terminal electrodes 23, made of metal or the like, are provided on one side of the chip body 21. The sealing plate 22 is, for example, a resin substrate, having a first surface 22a and a second surface 22b. The semiconductor chip 2B is embedded in the sealing plate 22 on the first surface 22a side, with the plurality of terminal electrodes 23 exposed from the first surface 22a.
[0082] The wiring structure 3B comprises a support K, an insulating film 32, wiring 33, and a post component 34. In this embodiment, the semiconductor chip 2B serves as the support K for the wiring structure 3B. The insulating film 32, wiring 33, and post component 34 are formed of the same materials as in the first embodiment. In this embodiment, multiple insulating films 32 are stacked in the thickness direction. Figure 10 In this example, the first insulating film 32A and the second insulating film 32B are sequentially stacked on the first surface 22a side of the sealing plate 22. Furthermore, the thickness of the second insulating film 32B is greater than the thickness of the first insulating film 32A.
[0083] Wiring 33 is formed on the first insulating film 32A as a substrate. Wiring 33 is electrically connected to the terminal electrode 23 of the semiconductor chip 2B via a through-hole 33a penetrating the first insulating film 32A in the thickness direction. Wiring 33 is covered by a second insulating film 32B and is exposed from the second insulating film 32B within a through-hole penetrating the second insulating film 32B in the thickness direction. Solder balls 27 are bonded to this exposed portion.
[0084] Similar to the first embodiment, the pile member 34 has a main body portion 34a located within the insulating film 32 and a flange portion 34b extending onto the insulating film 32. The main body portion 34a is configured to penetrate the first insulating film 32A along its thickness direction. The end of the main body portion 34a opposite to the flange portion 34b engages with the first surface 22a of the sealing plate 22, which serves as a support K. The flange portion 34b of the pile member 34 is embedded in the second insulating film 32B.
[0085] The position of the post member 34 when viewed from the thickness direction of the insulating film 32 is not particularly limited as long as it does not overlap with the wiring 33. Similar to the first embodiment, it is possible to apply, for example, the following methods can be used. Figure 2 of (a) Figure 2 of (b) Figure 3 (a) ~ Figure 3 (c) Figure 4 of (a) Figure 4 of (b) Figure 5 (a) ~ Figure 5 Any one of the patterns shown in (c).
[0086] Next, the manufacturing method of the above-mentioned wiring structure 3B will be described.
[0087] Here, the manufacturing process of the semiconductor element 1B, including the manufacturing process of the wiring structure 3B, will be described. The manufacturing method is configured to include a preparation process S11, an insulating film formation process S12, a seed layer formation process S13, and a plating process S14.
[0088] In the preparation process S11, firstly, as... Figure 11 As shown in (a), a semiconductor chip 2B is prepared as a support K. In the insulating film formation process S12, an insulating film 32 is formed by coating and curing a photosensitive resin composition or by laminating a film of a cured photosensitive resin composition. In this embodiment, for example, a spin coater is used to coat the first surface 22a of the sealing plate 22. The coated photosensitive resin composition is then dried using a hot plate or similar device. After exposure using an exposure apparatus and development using a developing apparatus, as shown... Figure 11 As shown in (b), a first insulating film 32A having a through hole for wiring 33 and a through hole for post component 34 is formed on the first surface 22a of the sealing plate 22.
[0089] In the seed layer formation process S13, for example by sputtering, such as Figure 11 As shown in (c), a seed layer 36 is formed on the first insulating film 32A and inside the through-hole. In the plating process S14, firstly, as shown in (c), a seed layer 36 is formed on the first insulating film 32A and inside the through-hole. Figure 12As shown in (a), a dry film 38 is laminated onto a seed layer 36 on a first insulating film 32A. Then, after exposure based on an exposure apparatus and development based on a development apparatus, an opening is formed on the dry film 38 with a pattern corresponding to the wiring 33, the wiring 33 via, and the post component 34.
[0090] After the dry film 38 is formed, a plating layer 37 is grown on the seed layer 36, for example, by electroplating. After the plating layer 37 has grown, water washing, removal of the chemically based dry film 38, and removal of the etch-based seed layer 36 are performed, such as... Figure 12 As shown in (b), wiring 33 and post components 34 corresponding to the first insulating film 32A are formed on the first insulating film 32A. In this embodiment, the insulating film forming process S12 is performed again after the plating process S14, as shown in (b). Figure 13 As shown in (a), a second insulating film 32B with through holes exposing the wiring 33 is formed on the first insulating film 32A. Finally, solder balls 27 are joined by means of the portion of the wiring 33 exposed from the second insulating film 32B, as shown in (a). Figure 13 As shown in (b), a semiconductor element 1B including a wiring structure 3B can be obtained.
[0091] In the wiring structure 3B described above, the same effect as in the first embodiment is achieved. By securing the insulating film 32 with the post member 34, the expansion and contraction of the insulating film 32 during the thermal process of forming the wiring 33 on the insulating film 32 can be reduced. Therefore, even when the insulating film 32 is made of a relatively soft resin curing material, wrinkles on the insulating film 32 can be suppressed. By suppressing wrinkles on the insulating film 32, deformation of the wiring 33 on the insulating film 32 can be suppressed, and the linewidth or spacing between the wiring 33 can be formed with high precision relative to the design values.
[0092] Symbol Explanation 1A, 1B - Semiconductor element; 2A, 2B - Semiconductor chip; 3A, 3B - Wiring structure; 12 (12A~12C), 32 (32A, 32B) - Insulating film; 13 (13A, 13B), 33 - Wiring; 14 (14A, 14B), 34 - Pile component; 14b, 34b - Flange portion; 16, 36 - Seed layer; 17, 37 - Plating layer; K - Support; R - Forming area.
Claims
1. A wiring structure comprising: Support structure; An insulating film is formed by a cured photosensitive resin composition disposed on a support. Wiring is arranged on the insulating film in a prescribed pattern; and The stake component is configured to penetrate the insulating film along its thickness direction at a location that does not overlap with the wiring.
2. The wiring structure according to claim 1, wherein, The pile component has a flange extending onto the insulating film.
3. The wiring structure according to claim 1 or 2, wherein, The pile component is engaged with the support body.
4. The wiring structure according to any one of claims 1 to 3, wherein, The cross-section of the pile component is circular.
5. The wiring structure according to any one of claims 1 to 4, wherein, The insulating film is stacked in multiple layers in the thickness direction. The pile component is configured with a plurality of insulating films corresponding to each other.
6. The wiring structure according to claim 5, wherein, A post component disposed on an insulating membrane has a flange extending onto the insulating membrane. The flange portion is embedded in another insulating film adjacent to the first insulating film in the thickness direction.
7. The wiring structure according to claim 5 or 6, wherein, A stake component disposed on an insulating membrane is joined to another stake component disposed on another insulating membrane adjacent to the first insulating membrane in the thickness direction.
8. The wiring structure according to any one of claims 1 to 7, wherein, When viewed from the thickness direction, the pile component is configured to at least sandwich the forming area of the wiring.
9. A method for manufacturing a wiring structure, comprising: Preparation process, preparation of the support structure; The insulating film forming process involves forming an insulating film, consisting of a cured product of a photosensitive resin composition, onto the support in a prescribed pattern. The seed layer formation process involves forming a seed layer on the insulating film; and In the plating process, a plating layer is grown on the seed layer to form wiring on the insulating film and stud components that penetrate the insulating film along the thickness direction at positions that do not overlap with the wiring.
10. The method for manufacturing the wiring structure according to claim 9, wherein, In the insulating film forming process, the insulating film is formed by coating and curing the photosensitive resin composition.
11. The method for manufacturing a wiring structure according to claim 9, wherein, In the insulating film forming process, the insulating film is formed by laminating a film of the cured photosensitive resin composition.
12. A semiconductor device comprising: Wiring structure as described in any one of claims 1 to 8; and A semiconductor chip is electrically connected to the wiring in the wiring structure.
Citation Information
Patent Citations
Positive photosensitive insulating resin composition and cured product of the same
JP2007057595A
Positive photosensitive resin composition, method for producing resist pattern and electronic device
JP2008309885A
Positive-type photosensitive resin composition, method for producing resist pattern, semiconductor device, and electronic device
WO2010073948A1