Protective layer structure for steel flange phosphorization

By forming a rare earth modified phosphating layer and a water-based sealing coating on the low carbon steel flange, it solves its corrosion problem in humid environments, significantly improves corrosion resistance, realizes an environmentally friendly process, and advances industry technology.

CN221837100UActive Publication Date: 2024-10-15GUANGZHOU ULTRA UNION CHEM LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202323594166.4
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-28
Publication Date
2024-10-15
Estimated Expiration
2033-12-28

AI Technical Summary

Technical Problem

Mild steel flanges are prone to corrosion in humid and salt spray environments. The existing phosphating layer has poor corrosion resistance, and the optimization of process conditions ignores interaction effects, which limits its application.

Method used

A rare earth modified phosphating layer and a water-based sealing coating prepared using a hydroxyl graphene modified sealing agent are sequentially prepared on the steel substrate from the inside to the outside to form a protective layer structure for the steel flange.

Benefits of technology

The corrosion resistance of the protective layer is significantly improved, and the process is environmentally friendly and non-toxic, representing the technological development direction of the industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221837100U_ABST
    Figure CN221837100U_ABST
Patent Text Reader

Abstract

The utility model discloses a protective layer structure for steel flange phosphorization. The protective layer structure comprises a steel base body, a rare earth modified phosphate coating and a graphene sealing layer, wherein the rare earth modified phosphate coating and the graphene sealing layer are sequentially prepared on the steel base body from inside to outside. A neutral salt spray test is carried out for 72 h according to GB / T 10125-2021 Artificial Atmosphere Corrosion Test Salt Spray Test, and no red rust is generated on the surface of the steel phosphating piece. The protective layer structure for steel flange phosphorization disclosed by the utility model is environment-friendly in preparation process and has a good market prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model belongs to the technical field of metal surface treatment, and in particular relates to a protective layer structure for phosphating a steel flange. Background Art

[0002] Flanges are used for pipeline connection and play an irreplaceable role. At present, flanges are mostly made of cast iron, low-carbon steel, alloy steel and stainless steel. Among them, low-carbon steel flanges have a high cost-effectiveness and are widely used in chemical, petroleum, construction and machinery industries. However, low-carbon steel flanges have poor corrosion resistance and are prone to corrosion in humid and salt spray environments. If the protective measures are not perfect, their service life will be greatly shortened. Therefore, they must be surface treated to prepare a protective layer. Compared with coating organic coatings and electrogalvanizing, phosphating has the advantages of low cost, simple operation and fast film formation, but the phosphating layer has poor corrosion resistance. [1] , which limits its application. The phosphating layer is usually not used directly as a surface protective layer for steel substrates, but is used as a base layer for organic coatings on metal substrates such as steel to improve the bonding strength and corrosion resistance of the organic coating and the metal substrate. There are many types of phosphating. In order to obtain a good corrosion protection effect, the phosphating process conditions must be optimized. Although there are many reports on the optimization of phosphating process conditions at home and abroad, most of them use single-factor experimental methods to optimize one or a few process conditions, and ignore the interaction between process conditions. [2] .

[0003] The invention patent "Hydroxygraphene coating modified sealing agent and preparation method thereof" with authorization announcement number CN 108129885 B discloses a water-based sealant used to seal zinc-plated and zinc-nickel alloy coatings that have been passivated, which can significantly improve the corrosion resistance and other properties of the coating.

[0004] References: [1] Zhang Yuncheng, Hu Runan, Xiang Rong, et al., Electroplating Handbook, Beijing, National Defense Industry Press, 2004, 867-886. [2] Lv Fang, Gu Na, Optimization of phosphating process conditions for chemical pipeline connection flanges and corrosion resistance of phosphating films, Electroplating and Finishing, 2022, 44(3): 59-63. Summary of the invention

[0005] In order to solve the problem of poor corrosion resistance of steel phosphating protective layer, the utility model provides a steel flange phosphating protective layer structure. In order to achieve the above purpose, the utility model adopts the following technical solutions:

[0006] A protective layer structure for phosphating a steel flange, comprising a steel substrate, a rare earth modified phosphating layer and a water-based sealing coating sequentially prepared on the steel substrate from the inside to the outside;

[0007] The water-based closed coating is a coating prepared by using a hydroxy graphene-modified closed agent.

[0008] Preferably, the rare earth modified phosphating layer has a thickness of 1 to 3 μm.

[0009] Preferably, the thickness of the water-based sealing coating is 0.8 to 1.6 μm.

[0010] Compared with the prior art, the utility model has the following beneficial effects:

[0011] 1. The protective layer structure of the phosphating of the steel flange disclosed in the utility model adopts a hydroxy graphene modified sealant to prepare a water-based sealing coating, which significantly improves the corrosion resistance of the protective layer.

[0012] 2. The protective layer structure of the phosphating of steel flange disclosed in the utility model has a water-based sealing coating that is non-toxic and harmless, and the process is environmentally friendly, representing the technical development direction of the industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] The drawings described herein are used to provide a further understanding of the present invention, constitute a part of the present application, and do not constitute an improper limitation of the present invention. In the drawings:

[0014] Figure 1 It is a schematic diagram of the protective layer structure of Example 1 and Example 2 of the utility model. Implementation

[0015] The present invention will be described in detail below in conjunction with the accompanying drawings and specific embodiments. The schematic embodiments and descriptions of the present invention are used to explain the present invention but are not intended to limit the present invention.

[0016] A protective layer structure for phosphating a steel flange comprises a steel substrate, a rare earth modified phosphating layer and a water-based sealing coating which are sequentially prepared on the steel substrate from the inside to the outside.

[0017] The existing pre-treatment process is used to degrease, remove rust and activate the steel flange.

[0018] A rare earth modified phosphating process is adopted to prepare a rare earth modified phosphating layer on a pre-treated steel flange, and the thickness of the prepared rare earth modified phosphating layer is 1 to 3 μm.

[0019] Preferably, the rare earth modified phosphating process is as follows:

[0020] Zinc dihydrogen phosphate 55-65g / L, sodium fluoride 2-3g / L, lanthanum nitrate 30-50mg / L, phosphating solution temperature 60℃-70℃, phosphating time 10-20min.

[0021] The water-based sealing coating is prepared on the phosphated steel flange by using the existing graphene-modified sealing agent. The thickness of the prepared water-based sealing coating is 0.8 to 1.6 μm.

[0022] Preferably, the water-based sealing coating is prepared using PRODICO 480 graphene sealant produced by Chaobang Chemical.

[0023] PRODICO 480 graphene sealing process is as follows:

[0024] Dilute PRODICO 480 graphene sealer 3 times with water to prepare the sealing solution;

[0025] Immerse the phosphated steel flange in the sealing liquid for 5 to 15 seconds, drain it after exiting the tank, and use high-pressure air to blow away the sealing liquid remaining on the surface of the workpiece;

[0026] The sealed steel flange is dried and cured at 70℃~100℃ for 20~35min. Example

[0027] like Figure 1 As shown, a protective layer structure for phosphating a steel flange includes a steel substrate 1, and a rare earth modified phosphating layer 2 and a water-based sealing coating 3 sequentially prepared on the steel substrate 1 from the inside to the outside.

[0028] The steel matrix is ​​A3 steel.

[0029] 1. Pre-treatment:

[0030] The steel substrate 1 is subjected to "chemical degreasing → water washing → acid washing → water washing → ultrasonic degreasing → water washing → activation → water washing".

[0031] 2. Phosphating:

[0032] After the steel parts are pre-treated, a rare earth modified phosphating agent is used to prepare a rare earth modified phosphating layer 2, and the thickness of the phosphating layer is 2 μm.

[0033] The composition and process conditions of the phosphating solution are: 52 g / L zinc dihydrogen phosphate, 2.3 g / L sodium fluoride, 35 mg / L lanthanum nitrate, 65°C phosphating solution temperature, and 17 min phosphating time.

[0034] 3. Closure:

[0035] The water-based sealing coating 3 was prepared using PRODICO 480 graphene sealant produced by Chaobang Chemical, and the thickness of the sealing layer was 1 μm.

[0036] PRODICO 480 graphene sealing process is as follows:

[0037] Dilute PRODICO 480 graphene sealer with water to 3 times to prepare the sealing solution;

[0038] Immerse the phosphated steel flange in the sealing liquid for 10 seconds, drain it after taking it out of the tank, and use high-pressure air to blow away the sealing liquid remaining on the surface of the workpiece.

[0039] 4. Drying:

[0040] The sealed steel flange was dried and cured at 80°C for 30 minutes. Example

[0041] like Figure 1 As shown, a protective layer structure for phosphating a steel flange includes a steel substrate 1, and a rare earth modified phosphating layer 2 and a water-based sealing coating 3 sequentially prepared on the steel substrate 1 from the inside to the outside.

[0042] The steel matrix is ​​No. 20 steel.

[0043] 1. Pre-treatment:

[0044] The steel substrate 1 is subjected to "chemical degreasing → water washing → acid washing → water washing → ultrasonic degreasing → water washing → activation → water washing".

[0045] 2. Phosphating:

[0046] After the steel parts are pre-treated, a rare earth modified phosphating agent is used to prepare a rare earth modified phosphating layer 2, and the thickness of the phosphating layer is 2 μm.

[0047] The composition and process conditions of the phosphating solution are: 63 g / L zinc dihydrogen phosphate, 2.8 g / L sodium fluoride, 45 mg / L lanthanum nitrate, 65°C phosphating solution temperature, and 13 min phosphating time.

[0048] 3. Closure:

[0049] The water-based sealing coating 3 was prepared using PRODICO 480 graphene sealant produced by Chaobang Chemical, and the thickness of the sealing layer was 1 μm.

[0050] PRODICO 480 graphene sealing process is as follows:

[0051] Dilute PRODICO 480 graphene sealer with water to 3 times to prepare the sealing solution;

[0052] Immerse the phosphated steel flange in the sealing liquid for 10 seconds, drain it after exiting the tank, and blow off the sealing liquid remaining on the surface of the workpiece with high-pressure air;

[0053] 4. Drying:

[0054] The sealed steel flange was dried and cured at 90°C for 20 minutes.

[0055] Test Example 1:

[0056] The phosphating protective layer structure of the steel flange prepared in Example 1 and Example 2 was subjected to a neutral salt spray test for 72 hours in accordance with GB / T 10125-2021 "Artificial atmosphere corrosion test salt spray test", and no red rust was generated on the surface of the steel phosphating parts.

[0057] Comparative Example 1:

[0058] A rare earth modified phosphating layer was prepared on the surface of the steel part according to the scheme of Example 1 and Example 2, but no water-based sealing layer was prepared. A neutral salt spray test was carried out for 24 hours according to GB / T 10125-2012 "Artificial atmosphere corrosion test salt spray test", and red rust appeared on the surface of the steel phosphating part.

[0059] The technical solutions provided by the embodiments of the present utility model are described in detail above. The principles and implementation methods of the embodiments of the present utility model are described in detail using specific examples herein. The description of the above embodiments is only applicable to help understand the principles of the embodiments of the present utility model. For those skilled in the art, according to the concept of the embodiments of the present utility model, there will be changes in the specific implementation methods and application scope, but they should all fall within the scope of protection of the claims of the present utility model.

Claims

1. A protective layer structure for phosphating a steel flange, characterized in that: It comprises a steel substrate, and a rare earth modified phosphating layer and a water-based sealing coating which are sequentially prepared from the inside to the outside on the steel substrate; The water-based closed coating is a coating prepared by using a hydroxy graphene-modified closed agent.

2. The protective layer structure for phosphating of steel flange according to claim 1, characterized in that: The thickness of the rare earth modified phosphating layer is 1 to 3 μm.

3. The protective layer structure for phosphating of steel flange according to claim 1, characterized in that: The thickness of the water-based sealing coating is 0.8-1.6 μm.