Passivation contact structure and passivation contact crystalline silicon cell
By adopting a new passivation contact structure in TOPCon batteries, the chemical etch control difficulty is solved by using the combination of thin tunneling silicon oxide layer and thick doped polysilicon structure and the combination of thick tunneling silicon oxide layer and thin doped polysilicon structure. The problem of this problem optimizes the battery performance and improves the battery conversion efficiency and performance parameters.
Patent Information
- Application Number
- CN202323423611.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-14
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2033-12-14
AI Technical Summary
There are chemical etching methods in the passivated contact structure of the existing TOPCon batteries, which leads to uneven polysilicon thickness, affecting battery performance, and battery performance needs to be further improved.
A new passivation contact structure is adopted, by setting a combination of a thin tunneling silicon oxide layer and a thick doped polysilicon structure in the metal contact area, and a combination of a thick tunneling silicon oxide layer and a thin doped polysilicon structure in the non-metal contact area. , combining silicon nitride layer and metal electrodes to realize structural morphology partition control in different regions, and cooperate to optimize battery performance.
It effectively reduces metal composite and open voltage losses, improves short-circuit current and filling factor, and improves the conversion efficiency and performance parameters of the battery.
Smart Images

Figure CN222015416U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the field of solar cells, in particular to a passivation contact structure and a passivation contact crystalline silicon cell. Background Art
[0002] The tunneling oxide passivation contact cell (TOPCon cell for short) uses an ultra-thin tunneling oxide layer plus a doped polysilicon layer to achieve efficient passivation and selective carrier collection on the entire back side of the cell. The ultra-thin silicon oxide and doped polysilicon layer together form a passivation contact structure, providing good surface passivation for the back side of the silicon wafer. The ultra-thin oxide layer allows majority carriers (electrons) to tunnel into the polysilicon layer while blocking minority carriers (holes) from recombination. Then, majority carriers are laterally transmitted in the polysilicon layer and collected by metal, thereby greatly reducing the metal contact recombination current and increasing the open circuit voltage and short circuit current of the cell. Currently, TOPCon cells have been mass-produced and are gradually replacing the market share of PERC cells. How to further improve the conversion efficiency of TOPCon cells has become a key research direction for industry R&D personnel.
[0003] For example, patent CN106449800B proposes a selective polysilicon thickness passivation contact structure, which first deposits a thicker polysilicon layer, and then thins the polysilicon film in the local area by depositing a local mask and combining chemical etching, so as to achieve a thick polysilicon film in the metal contact area and a thin film in the non-metal contact area. Although this patent prevents the current loss of solar cells to a certain extent, on the one hand, it has the following problems: using chemical etching method to thin polysilicon, in actual operation, the rate of chemical etching of polysilicon film is fast and difficult to control, so it is easy to cause uneven polysilicon thickness after etching, resulting in poor selective polysilicon thickness and poor appearance on the back; on the other hand, the performance of the battery needs to be further improved. Utility Model Content
[0004] The purpose of the utility model is to overcome one or more deficiencies in the prior art and to provide a novel passivation contact structure which can achieve a balance between surface recombination, metal recombination, and interface contact resistance, and make the metal recombination and contact resistivity of the metal contact area low, and the surface recombination of the non-metal contact area low and the light absorption loss small.
[0005] The utility model also provides a passivation contact crystalline silicon battery including the passivation contact structure.
[0006] In order to achieve the above-mentioned purpose, a technical solution adopted by the utility model is: a passivation contact structure, the passivation contact structure comprises:
[0007] a silicon substrate comprising a back surface and a metal contact region on the back surface;
[0008] A first tunneling silicon oxide layer and a first polysilicon layer are respectively arranged in the metal contact region, wherein the first polysilicon layer covers the first tunneling silicon oxide layer;
[0009] A second tunneling silicon oxide layer and a second polysilicon layer are respectively disposed on the back surface;
[0010] In the metal contact region, the first tunneling silicon oxide layer, the first polysilicon layer, the second tunneling silicon oxide layer and the second polysilicon layer are stacked in sequence;
[0011] The thickness of the second tunneling silicon oxide layer is greater than the thickness of the first tunneling silicon oxide layer, the absolute value of the difference between the thickness of the second tunneling silicon oxide layer and the thickness of the first tunneling silicon oxide layer is 0.3-0.5nm, and the thickness of the second polysilicon layer is less than the thickness of the first polysilicon layer.
[0012] According to some preferred aspects of the present invention, the thickness of the first tunneling silicon oxide layer is 0.8-1.5 nm. In some embodiments of the present invention, the thickness of the first tunneling silicon oxide layer can be 0.8 nm, 0.85 nm, 0.9 nm, 0.95 nm, 1.0 nm, 1.05 nm, 1.1 nm, 1.2 nm, 1.3 nm, 1.4 nm, etc.
[0013] According to some preferred aspects of the present invention, the thickness of the second tunneling silicon oxide layer is 1.2-2 nm. In some embodiments of the present invention, the thickness of the second tunneling silicon oxide layer can be 1.2 nm, 1.3 nm, 1.4 nm, 1.5 nm, 1.6 nm, 1.7 nm, 1.8 nm, 1.9 nm, 2 nm, etc.
[0014] According to some preferred aspects of the present invention, the thickness of the first polysilicon layer is 100-200nm. In some embodiments of the present invention, the thickness of the first polysilicon layer can be 100nm, 105nm, 110nm, 115nm, 120nm, 125nm, 130nm, 135nm, 140nm, 150nm, 160nm, 170nm, 180nm, 190nm, etc.
[0015] According to some preferred aspects of the present invention, the thickness of the second polysilicon layer is 40-100 nm. In some embodiments of the present invention, the thickness of the second polysilicon layer can be 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 90 nm, etc.
[0016] In some embodiments of the present invention, the passivation contact structure further includes a passivation layer disposed on the second polysilicon layer.
[0017] Furthermore, the passivation layer is a silicon nitride layer, the refractive index of the silicon nitride layer is 1.9-2.3, and the thickness is 70-100 nm.
[0018] In some embodiments of the present invention, the passivation contact structure further includes a metal electrode disposed in the metal contact region, and the orthographic projection of the metal electrode on the silicon substrate is located within the first polysilicon layer.
[0019] In some embodiments of the present invention, the silicon substrate is an N-type single crystal silicon wafer with a resistivity of 0.5-3Ω·cm and a thickness of 100-200 μm.
[0020] Another technical solution provided by the present invention is a passivated contact crystalline silicon cell, which comprises the passivated contact structure described above.
[0021] Due to the application of the above technical solution, the utility model has the following advantages compared with the prior art:
[0022] The utility model innovatively provides a new passivation contact structure, which realizes a combination of a thin tunneling silicon oxide layer (a tunneling silicon oxide layer in contact with a silicon substrate) and a thick doped polysilicon structure in a metal contact region, and realizes a combination of a thick tunneling silicon oxide layer and a thin doped polysilicon structure in a non-metal contact region, thereby achieving the goal of overcoming the corrosion of doped polysilicon by metal slurry in the metal contact region, reducing metal recombination, and significantly reducing opening voltage loss, while the thinner tunneling silicon oxide layer can allow more phosphorus to enter the silicon substrate surface, which helps to reduce metal recombination; while in the non-metal contact region, the thicker tunneling silicon oxide layer can block phosphorus from diffusing into the silicon substrate surface, and is expected to achieve lower surface recombination, while the thinner doped polysilicon can reduce the absorption of free carriers and increase the short-circuit current of the battery; the utility model achieves a balance at least between surface recombination, metal recombination, and interface contact resistance by controlling different structural forms in different partitions and the cooperative working relationship, further optimizing the short-circuit current, open-circuit voltage, and fill factor, and promoting the efficiency improvement of the TOPCon battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the utility model or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the utility model. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0024] Figure 1 This is a schematic diagram of the structure of the silicon substrate after alkali polishing in the embodiment of the utility model;
[0025] Figure 2 It is a schematic diagram of the structure after depositing the first tunneling silicon oxide layer, the first amorphous silicon layer and the mask in the embodiment of the utility model;
[0026] Figure 3 This is a schematic diagram of the structure after the local mask is eliminated by laser in an embodiment of the utility model;
[0027] Figure 4 This is a schematic diagram of the structure after alkali polishing and mask removal in an embodiment of the utility model;
[0028] Figure 5 It is a schematic diagram of the structure after depositing the second tunneling silicon oxide layer and the second amorphous silicon layer in the embodiment of the utility model;
[0029] Figure 6 This is a schematic diagram of the structure after high temperature treatment in an embodiment of the utility model;
[0030] Figure 7 This is a schematic diagram of the structure after the phosphosilicate glass layer is removed and the silicon nitride layer is deposited in the embodiment of the utility model;
[0031] Figure 8 This is a schematic structural diagram of a passivation contact structure in an embodiment of the utility model;
[0032] In the figure markings: 1, silicon substrate; 2, first tunneling silicon oxide layer; 3, first amorphous silicon layer; 4, mask layer; 5, second tunneling silicon oxide layer; 6, second amorphous silicon layer; 7, first polycrystalline silicon layer; 8, second polycrystalline silicon layer; 9, phosphosilicate glass layer; 10, silicon nitride layer; 11, metal electrode. DETAILED DESCRIPTION
[0033] In order to make the above-mentioned purposes, features and advantages of the utility model more obvious and easy to understand, the utility model is described in detail below in conjunction with the accompanying drawings and specific embodiments. In the following description, many specific details are set forth to facilitate a full understanding of the utility model. However, the utility model can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the utility model, so the utility model is not limited by the specific embodiments disclosed below.
[0034] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present utility model, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0035] In the present invention, unless otherwise clearly specified and limited, the terms "install", "connect", "connect", "fix" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0036] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0037] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly on the other element or there may be an intermediate element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be an intermediate element at the same time.
[0038] The above scheme is further described below in conjunction with the accompanying drawings and specific embodiments; it should be understood that these embodiments are used to illustrate the basic principles, main features and advantages of the utility model, and the utility model is not limited to the scope of the following embodiments; the implementation conditions adopted in the embodiments can be further adjusted according to specific requirements, and the implementation conditions not specified are usually the conditions in conventional experiments.
[0039] Embodiment 1:
[0040] See also Figure 8As shown, this example provides a passivation contact structure, which includes: a silicon substrate 1, the silicon substrate 1 includes a back surface and a metal contact area located on the back surface; a first tunneling silicon oxide layer 2 and a first polysilicon layer 7 respectively arranged in the metal contact area, and the first polysilicon layer 7 covers the first tunneling silicon oxide layer 2; a second tunneling silicon oxide layer 5 and a second polysilicon layer 8 respectively arranged on the back surface; in the metal contact area, the first tunneling silicon oxide layer 2, the first polysilicon layer 7, the second tunneling silicon oxide layer 5 and the second polysilicon layer 8 are stacked in sequence; the thickness of the second tunneling silicon oxide layer 5 is greater than the thickness of the first tunneling silicon oxide layer 2, and the absolute value of the difference between the thickness of the second tunneling silicon oxide layer 5 and the thickness of the first tunneling silicon oxide layer 2 is 0.3-0.5nm, and the thickness of the second polysilicon layer 8 is less than the thickness of the first polysilicon layer 7.
[0041] Further, the thickness of the first tunneling silicon oxide layer 2 is 0.8-1.5 nm. As an optional embodiment, the thickness of the first tunneling silicon oxide layer 2 can be 0.8 nm, 0.85 nm, 0.9 nm, 0.95 nm, 1.0 nm, 1.05 nm, 1.1 nm, 1.2 nm, 1.3 nm, 1.4 nm, etc.
[0042] Further, the thickness of the second tunneling silicon oxide layer 5 is 1.2-2 nm. As an optional embodiment, the thickness of the second tunneling silicon oxide layer 5 can be 1.2 nm, 1.3 nm, 1.4 nm, 1.5 nm, 1.6 nm, 1.7 nm, 1.8 nm, 1.9 nm, 2 nm, etc.
[0043] Further, the thickness of the first polysilicon layer 7 is 100-200 nm. As an optional embodiment, the thickness of the first polysilicon layer 7 can be 100 nm, 105 nm, 110 nm, 115 nm, 120 nm, 125 nm, 130 nm, 135 nm, 140 nm, 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, etc.
[0044] Further, the thickness of the second polysilicon layer 8 is 40-100 nm. As an optional embodiment, the thickness of the second polysilicon layer 8 can be 40 nm, 45 nm, 50 nm, 55 nm, 60 nm, 65 nm, 70 nm, 75 nm, 80 nm, 90 nm, etc.
[0045] In this example, the passivation contact structure further includes a passivation layer disposed on the second polysilicon layer 8. Further, the passivation layer is a silicon nitride layer 10, and the refractive index of the silicon nitride layer 10 is 1.9-2.3 and the thickness is 70-100 nm.
[0046] In this example, the passivation contact structure further includes a metal electrode 11 disposed in the metal contact region, and an orthographic projection of the metal electrode 11 on the silicon substrate 1 is located within the first polysilicon layer 7 .
[0047] In this example, the silicon substrate 1 is an N-type single crystal silicon wafer with a resistivity of 0.5-3Ω·cm and a thickness of 100-200 μm.
[0048] Embodiment 2:
[0049] This example provides a method for preparing the above-mentioned passivation contact structure, and the preparation method comprises:
[0050] Depositing a first tunneling silicon oxide layer and a first amorphous silicon layer in sequence on the back surface of the silicon substrate, then depositing a mask on the first amorphous silicon layer, and removing a portion of the mask located in the non-metal contact area by laser;
[0051] Firstly, the first amorphous silicon layer and the first tunneling silicon oxide layer are removed respectively in the mask-free area, and then the remaining mask in the metal contact area is removed to obtain a first intermediate;
[0052] Depositing a second tunneling silicon oxide layer and a second amorphous silicon layer on the back surface of the first intermediate in sequence to obtain a second intermediate; wherein the thickness of the second tunneling silicon oxide layer is controlled to be greater than the thickness of the first tunneling silicon oxide layer, the absolute value of the difference between the thickness of the second tunneling silicon oxide layer and the thickness of the first tunneling silicon oxide layer is 0.3-0.5 nm, and the thickness of the second amorphous silicon layer is less than the thickness of the first amorphous silicon layer;
[0053] The second intermediate is heat treated.
[0054] The main idea is to control different regions to be in different structural forms by partitioning, and to further control the thickness difference between the two tunneling silicon oxide layers and the two amorphous silicon layers during deposition by superimposing and alternately setting the tunneling silicon oxide layer and the amorphous silicon layer. By adopting a local mask formation mechanism, the tunneling layer and the amorphous silicon layer in the non-metallic contact region can be completely removed by an etching method. At this time, there is almost no need to consider the etching speed and uniformity issues. The operation is simple and easy to control. When the second tunneling silicon oxide layer and the second amorphous silicon layer are deposited again, different structural forms are achieved between different regions. After that, after the amorphous silicon layer is converted into polycrystalline silicon by heat treatment, the passivation contact structure of the utility model is given in the metal contact region and the non-metallic contact region. With different structural forms, on the one hand, it can overcome the problem of significantly increased metal recombination caused by corrosion of the polysilicon layer during the formation of the metal electrode in the later metal contact area, and can also block the role of the non-metallic contact area in blocking phosphorus from diffusing into the surface of the silicon substrate, which is expected to achieve lower surface recombination; on the other hand, the tunneling silicon oxide layer in direct contact with the silicon substrate in the metal contact area is low in thickness, that is, thin, which can enable more phosphorus to enter the surface of the silicon substrate, which helps to reduce metal recombination, and the problem of free carrier absorption of long-wave light in the non-metallic contact area is greatly suppressed by the thin polysilicon layer, optimizing the parameters that affect battery performance such as short-circuit current, open-circuit voltage, and fill factor. The utility model uses a multi-angle design of the passivation contact structure and a uniquely designed process to organically combine the independent morphological structures of each region, and includes them in an orderly and controllable process to achieve, which greatly reduces the difficulty of processing and is conducive to industrial production.
[0055] Specifically, the following Figures 1 to 8 The passivation contact structure and the preparation process of the utility model are further introduced. The preparation method of the passivation contact structure includes:
[0056] Step (1): providing an N-type single crystal silicon wafer with a resistivity in the range of 0.5-3Ω·cm and a thickness in the range of 100-200μm as a silicon substrate; polishing the silicon substrate with an alkaline solution to remove the damaged layer on the surface of the silicon substrate and obtain a flat surface morphology, wherein the silicon substrate 1 after alkaline polishing is as follows: Figure 1 As shown;
[0057] Specifically, the treatment temperature is 50-70° C., in the alkaline solution, the mass percentage of the alkaline substance (including but not limited to sodium hydroxide, potassium hydroxide, etc.) in the solution is 0.5%-2.5%, the amount of the alkaline treatment protective additive added is 0.3%-1.0%, and the reflectivity of the silicon substrate surface after polishing is 30%-50%;
[0058] Step (2): depositing a first tunneling silicon oxide layer on the back surface of the silicon substrate treated in step (1), wherein the thickness of the first tunneling silicon oxide layer is 0.8-1.5 nm, and the preparation method of the tunneling silicon oxide layer includes thermal oxidation, light ozone oxidation, ozone water, nitric acid oxidation, plasma enhanced chemical vapor deposition, etc.; wherein the plasma enhanced chemical vapor deposition (PECVD) method is preferred;
[0059] Then, a first amorphous silicon layer is deposited on the first tunneling silicon oxide layer on the back surface of the silicon wafer. The preparation method of the first amorphous silicon layer includes LPCVD intrinsic deposition method, PECVD intrinsic / in-situ doping deposition method, and PVD intrinsic / in-situ doping deposition method, wherein the PECVD in-situ doping deposition method is preferred; the thickness of the first amorphous silicon layer is in the range of 100-200nm;
[0060] Finally, a mask is deposited on the first amorphous silicon layer, the mask thickness is in the range of 30-100 nm, the mask material includes silicon oxide, silicon nitride, silicon oxynitride, and the mask preparation method includes plasma enhanced chemical vapor deposition (PECVD);
[0061] The schematic diagram of the structure after depositing the first tunneling silicon oxide layer, the first amorphous silicon layer and the mask is shown in FIG. Figure 2 As shown in the figure, the direction can be represented as silicon substrate 1, first tunneling silicon oxide layer 2, first amorphous silicon layer 3, mask layer 4 from top to bottom;
[0062] Step (3): Use laser to ablate and open the mask on the back surface of the silicon substrate after the treatment in step (2), wherein the laser light source includes green light and purple light source, and the laser power is 20-100W. After laser opening, a grid-shaped mask with equal spacing is retained, the width of the grid-line mask is 50-100μm, and the spacing between the grid-line masks is 0.6-1.5mm. During the opening process, the laser will ablate a certain thickness of the amorphous silicon layer on the surface, and the ablation thickness is 0-20nm. Laser opening can remove the mask in the non-metal contact area and retain part of the mask in the metal contact area, forming a Figure 3 The structure shown in the figure can be represented as follows: from top to bottom, there is a silicon substrate 1, a first tunneling silicon oxide layer 2, a first amorphous silicon layer 3, and a local mask 4 is provided in the metal contact area on the first amorphous silicon layer 3;
[0063] Step (4): polishing the silicon substrate treated in step (3) with an alkaline solution to remove the first tunneling silicon oxide layer and the first amorphous silicon layer in the mask-free area on the back surface of the silicon substrate. In this process, the first amorphous silicon layer and the first tunneling silicon oxide layer may be etched in sequence, followed by micro-polishing of the surface of the silicon substrate.
[0064] Specifically, the treatment temperature is 60-80° C., the mass percentage of the alkaline substance (including but not limited to sodium hydroxide, potassium hydroxide, etc.) in the alkaline solution is 1%-4%, and the amount of the alkaline treatment protective additive added is 0.5%-1.5%;
[0065] Finally, the remaining mask is removed using HF solution, the concentration of HF solution is 10%-20%;
[0066] The schematic diagram of the structure after alkali polishing and mask removal is as follows Figure 4 As shown, a local first tunneling silicon oxide layer 2 and a first amorphous silicon layer 3 are retained in the metal contact region on the silicon substrate 1;
[0067] Step (5): depositing a second tunneling silicon oxide layer on the back surface of the silicon substrate treated in step (4), wherein the thickness of the second tunneling silicon oxide layer is 1.2-2 nm, and the preparation method of the second tunneling silicon oxide layer includes thermal oxidation, light ozone oxidation, ozone water method, nitric acid oxidation method, and plasma enhanced chemical vapor deposition method;
[0068] Specifically, controlling the thickness of the second tunneling silicon oxide layer to be greater than the first tunneling silicon oxide layer;
[0069] Then, a second amorphous silicon layer is deposited on the second tunneling silicon oxide layer on the back surface of the silicon substrate. The preparation method of the second amorphous silicon layer includes LPCVD intrinsic deposition method, PECVD intrinsic / in-situ doping deposition method, and PVD intrinsic / in-situ doping deposition method. The thickness of the second amorphous silicon layer is 40-100nm, and the thickness of the second amorphous silicon layer is controlled to be less than the thickness of the first tunneling silicon oxide layer.
[0070] The schematic diagram of the structure after depositing the second tunneling silicon oxide layer and the second amorphous silicon layer is shown in FIG. Figure 5 As shown, from the direction in the figure, it can be shown that the silicon substrate 1, the first tunneling silicon oxide layer 2, the first amorphous silicon layer 3, the second tunneling silicon oxide layer 5, and the second amorphous silicon layer 6 are sequentially arranged from top to bottom in the metal contact area, and the silicon substrate 1, the second tunneling silicon oxide layer 5, and the second amorphous silicon layer 6 are sequentially arranged from top to bottom in the non-metal contact area;
[0071] Step (6): placing the sample obtained after the treatment in step (5) into a quartz boat and sending it into a quartz furnace tube for high temperature treatment; when the first tunneling silicon oxide layer and the second tunneling silicon oxide layer are both in-situ doped amorphous silicon, the high temperature treatment can be selected from simple annealing high temperature treatment or phosphorus diffusion high temperature treatment; under other conditions, the high temperature treatment needs to be phosphorus diffusion high temperature treatment; the temperature of the high temperature treatment is in the range of 800-900°C;
[0072] After step (6), the first amorphous silicon layer and the second amorphous silicon layer are transformed into polycrystalline silicon layers, and some phosphorus atoms are activated and electrically active, and diffuse through the first tunneling silicon oxide layer and / or the second tunneling silicon oxide layer to a certain depth. At the same time, since the metal contact area has a double amorphous silicon layer, once the first amorphous silicon layer is prepared by in-situ doping, it is equivalent to applying a high-concentration phosphorus source in the metal contact area and a low-concentration phosphorus source in the non-metal area. In this way, during the high-temperature heat treatment process, it is equivalent to selectively doping phosphorus, obtaining heavy phosphorus doping in the metal contact area and light phosphorus doping in the non-metal contact area, which is beneficial to improving the battery performance;
[0073] In addition, a phosphosilicate glass (PSG) layer is also generated on the surface of the second amorphous silicon layer;
[0074] The structural diagram after high temperature treatment is as follows Figure 6 As shown, from the direction in the figure, it can be shown that the silicon substrate 1, the first tunneling silicon oxide layer 2, the first polysilicon layer 7, the second tunneling silicon oxide layer 5, the second polysilicon layer 8 and the phosphosilicate glass layer 9 are sequentially arranged from top to bottom in the metal contact area, and the silicon substrate 1, the second tunneling silicon oxide layer 5, the second polysilicon layer 8 and the phosphosilicate glass layer 9 are sequentially arranged from top to bottom in the non-metal contact area;
[0075] Step (7): using an HF solution to remove the phosphosilicate glass (PSG) layer on the back surface of the silicon substrate obtained after the treatment in step (6), the concentration of the HF solution (also known as hydrofluoric acid) is 5%-20%; then using a PECVD method to form a silicon nitride layer on the second polysilicon layer on the back surface of the silicon substrate, the silicon nitride layer has a refractive index of 1.9-2.3 and a thickness in the range of 70-100nm;
[0076] The schematic diagram of the structure after removing the phosphosilicate glass layer and depositing the silicon nitride layer is shown in Figure 7 As shown, from the direction in the figure, it can be shown that the silicon substrate 1, the first tunneling silicon oxide layer 2, the first polysilicon layer 7, the second tunneling silicon oxide layer 5, the second polysilicon layer 8 and the silicon nitride layer 10 are sequentially arranged from top to bottom in the metal contact area, and the silicon substrate 1, the second tunneling silicon oxide layer 5, the second polysilicon layer 8 and the silicon nitride layer 10 are sequentially arranged from top to bottom in the non-metal contact area;
[0077] Step (8): using screen printing technology to print equally spaced metal paste electrode lines in the metal contact area and perform high temperature sintering; specifically, the metal paste electrode line width is 20-40 μm, the electrode line width is smaller than the width of the gate line-shaped first polysilicon layer, and the sintering temperature is 700-850° C.;
[0078] The schematic diagram of the passivation contact structure is shown in Figure 8As shown, from the direction in the figure, it can be represented that in the metal contact area, a silicon substrate 1, a first tunneling silicon oxide layer 2, a first polysilicon layer 7, a second tunneling silicon oxide layer 5, a second polysilicon layer 8 and a silicon nitride layer 10 are sequentially arranged from top to bottom, and a metal electrode 11 (such as a silver paste electrode) penetrating into the second polysilicon layer 8, and in the non-metal contact area, a silicon substrate 1, a second tunneling silicon oxide layer 5, a second polysilicon layer 8 and a silicon nitride layer 10 are sequentially arranged from top to bottom.
[0079] The process is simple and easy to control, and overcomes the problems of poor process controllability and poor uniformity of polysilicon thickness in non-contact areas in the prior art.
[0080] Example 2-1:
[0081] This example provides a combination of the above Figures 1 to 8 The structure and process of passivation contact structure shown in the figure are prepared. The specific process and parameters are as follows:
[0082] Step (1): providing an N-type single crystal silicon wafer with a resistivity in the range of 1 Ω·cm and a thickness of 130 μm as a silicon substrate;
[0083] The treatment temperature is 65°C, the mass percentage of sodium hydroxide in the sodium hydroxide aqueous solution is 1.5%, the alkali treatment protective additive is the commercially available Shichuang brand model PS42V08, the addition amount is 0.4%, and the reflectivity of the silicon substrate surface after polishing is 44%;
[0084] Step (2): using a PECVD method (process parameters: temperature 450° C., reaction pressure 180 Pa, nitrous oxide flow rate 8000 sccm, power 9000 W, process time 80 s) to deposit a first tunneling silicon oxide layer with a thickness of 0.9 nm;
[0085] The PECVD method (process parameters: temperature 450°C, reaction pressure 200Pa, silane flow rate 1200sccm, PH 3 The first amorphous silicon layer is deposited with a thickness of 120 nm at a flow rate of 1100 sccm, an argon flow rate of 6000 sccm, a power of 12000 w, and a process time of 800 s;
[0086] The mask was deposited by PECVD method (process parameters: temperature 450°C, reaction pressure 240Pa, silane flow rate 800sccm, nitrous oxide flow rate 12000sccm, power 16000W, reaction time 900s), the thickness of which was 50nm, and the mask material was silicon oxide;
[0087] Step (3): the laser light source is a purple light source, the laser power is 100W, the gate line mask width is 65μm, and the gate line mask spacing is 1.2mm; the laser will ablate a certain thickness of the amorphous silicon layer on the surface during the film opening process, and the ablation thickness is about 10nm;
[0088] Step (4): polishing the silicon substrate treated in step (3) with a sodium hydroxide aqueous solution at a treatment temperature of 70° C., wherein the mass percentage of sodium hydroxide in the sodium hydroxide aqueous solution is 3.2%, and the alkali treatment protective additive is a commercially available Shichuang brand EP20 model, added in an amount of 0.8%; the mass concentration of the HF solution is 15%;
[0089] Step (5): using a thermal oxidation method (process parameters: process temperature 600° C., oxygen flow rate 36000 sccm, flow time 900 s, pressure at normal pressure) to deposit a second tunneling silicon oxide layer, the thickness of which is 1.3 nm; the absolute value of the difference between the thickness of the second tunneling silicon oxide layer and the thickness of the first tunneling silicon oxide layer is 0.4 nm;
[0090] The PECVD method (process parameters: temperature 450°C, reaction pressure 200Pa, silane flow rate 1200sccm, PH 3 The second amorphous silicon layer is deposited at a thickness of 60 nm using a flow rate of 900 sccm, an argon flow rate of 6000 sccm, a power of 10000 W, and a process time of 500 s.
[0091] Step (6): the first amorphous silicon layer and the second amorphous silicon layer are both in-situ doped amorphous silicon, and the high temperature treatment temperature is in the range of 800-900° C.;
[0092] Specifically, the high temperature annealing process is as follows: temperature 870°C, time 30 min, protective gas N 2 , the flow rate is 5000sccm;
[0093] Step (7): the mass concentration of the HF solution is 20%; then a PECVD method (process parameters are: temperature 500° C., reaction pressure 200 Pa, silane flow rate 1200 sccm, ammonia flow rate 14000 sccm, power 17000 W, process time 750 s) is used to form a silicon nitride layer on the second polysilicon layer on the back surface of the silicon substrate, the silicon nitride layer has a refractive index of 2.1 and a thickness in the range of 85 nm;
[0094] Step (8): Use screen printing technology to print equally spaced silver paste electrode grid lines in the metal contact area and perform high-temperature sintering; specifically, the width of the silver paste electrode grid lines is 30 μm and the sintering temperature is 740° C.
[0095] In the passivation contact structure of this example, the thickness of the first tunneling silicon oxide layer 2 is 0.9 nm, and the thickness of the second tunneling silicon oxide layer 5 is 1.3 nm.
[0096] Comparative Example 1
[0097] The embodiment 2-1 is basically the same as the embodiment 2-1, and the only difference is that the thickness of the second tunneling silicon oxide layer is 1.1 nm, and the absolute value of the difference between the thickness of the second tunneling silicon oxide layer and the thickness of the first tunneling silicon oxide layer is 0.2 nm.
[0098] Comparative Example 2
[0099] It is basically the same as Example 2-1, with the only difference being that the thickness of the first tunneling silicon oxide layer is 0.7 nm, and the absolute value of the difference between the thickness of the second tunneling silicon oxide layer and the thickness of the first tunneling silicon oxide layer is 0.6 nm.
[0100] Performance Testing
[0101] In order to further demonstrate the improvement of the battery electrical performance by the passivation contact structure of the present invention, the preparation process and performance test results of the N-TOPCon battery including the above-mentioned Example 2-1 and Comparative Example 1-2 are provided, as follows:
[0102] (1): Using an N-type silicon wafer with a resistivity of 1Ω.cm and a thickness of 130μm, the silicon wafer was textured, the weight loss of the textured silicon wafer was 0.32g, and the textured surface reflectivity was 9.5%;
[0103] (2): Boron diffusion treatment is performed on the front side of the silicon wafer, the deposition temperature is 860°C, the push temperature is 940°C, and the square resistance after the process is 110Ω / sq;
[0104] (3): Laser scanning is performed on the boron diffusion surface of the silicon wafer to achieve local laser doping. The square resistance of the laser scanning area is 75Ω / sq;
[0105] (4): The silicon wafer is subjected to high-temperature oxidation at 1060°C. After oxidation, the square resistance of the laser-doped area is 80Ω / sq, and the square resistance of the non-laser-doped area is 220Ω / sq. After oxidation, a borosilicate glass layer (BSG) is formed on the front side;
[0106] (5): corresponding to step (1) of the embodiment or comparative example, since the BSG layer is retained on the front side, the front side is not polished;
[0107] (6): corresponding to step (2) of the embodiment or comparative example;
[0108] (7): corresponding to step (3) of the embodiment or comparative example;
[0109] (8): corresponding to step (4) of the embodiment or comparative example, since the BSG layer is retained on the front side, the front side is not polished; in this step, a single-sided chain HF machine is used to remove the back mask, and the front side BSG is retained;
[0110] (9): corresponding to step (5) of the embodiment or comparative example;
[0111] (10): corresponding to step (6) of the embodiment or comparative example;
[0112] (11): corresponding to step (7) of the embodiment or comparative example, in which the front BSG layer and the back PSG layer are removed together by HF; then, a front aluminum oxide layer is first deposited with a thickness of about 4 nm, and then a front silicon nitride layer is deposited with a refractive index of about 2.00 and a thickness of about 75 nm, and finally, a back silicon nitride layer is deposited;
[0113] (12): That is, corresponding to step (8) of the embodiment or comparative example, first print the back main grid, the number of main grids is 16, the width of the main grid is 60μm, and then print the back fine grid after drying. Then print the front main grid after drying. The number of main grids is 16, the width of the main grid is 50μm, and then print the front fine grid lines after drying. The fine grid line spacing is 1.2mm and the grid line width is 20μm. Finally, sintering is performed.
[0114] The test method is: use an IV tester to test the cell photoelectric conversion efficiency and related electrical performance parameters under standard light power under simulated solar light source.
[0115] The specific test results are shown in Table 1 (Eta: conversion efficiency, Voc: open circuit voltage, Jsc: short circuit current, FF: fill factor).
[0116] Table 1
[0117]
[0118] It can be seen from Table 1 that the conversion efficiency of the battery prepared by the passivation contact structure of the utility model has been significantly improved. Compared with Comparative Examples 1 and 2, when the difference between the two tunneling layers is at the expected value, the conversion efficiency of Example 2-1 is increased by 0.31% and 0.43%, respectively. For crystalline silicon solar cells, a change of 0.1% is usually a huge improvement. It can be seen that the utility model optimizes the short-circuit current, open-circuit voltage, and fill factor by partitioning and controlling different structural forms and the coordinated working relationship, thereby promoting a significant improvement in the efficiency of the TOPCon battery.
[0119] The above embodiments are only for illustrating the technical concept and features of the utility model, and their purpose is to enable people familiar with the technology to understand the content of the utility model and implement it accordingly, and they cannot be used to limit the protection scope of the utility model. Any equivalent changes or modifications made according to the spirit of the utility model should be included in the protection scope of the utility model.
[0120] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
Claims
1. A passivation contact structure, It is characterized in that The passivation contact structure comprises: a silicon substrate comprising a back surface and a metal contact region on the back surface; A first tunneling silicon oxide layer and a first polysilicon layer are respectively arranged in the metal contact region, wherein the first polysilicon layer covers the first tunneling silicon oxide layer; A second tunneling silicon oxide layer and a second polysilicon layer are respectively disposed on the back surface; In the metal contact region, the first tunneling silicon oxide layer, the first polysilicon layer, the second tunneling silicon oxide layer and the second polysilicon layer are stacked in sequence; The thickness of the second tunneling silicon oxide layer is greater than the thickness of the first tunneling silicon oxide layer, the absolute value of the difference between the thickness of the second tunneling silicon oxide layer and the thickness of the first tunneling silicon oxide layer is 0.3-0.5nm, and the thickness of the second polysilicon layer is less than the thickness of the first polysilicon layer.
2. The passivation contact structure according to claim 1, It is characterized in that The thickness of the first tunneling silicon oxide layer is 0.8-1.5 nm.
3. The passivation contact structure according to claim 1 or 2, It is characterized in that The thickness of the second tunneling silicon oxide layer is 1.2-2 nm.
4. The passivation contact structure according to claim 1, It is characterized in that The thickness of the first polysilicon layer is 100-200 nm.
5. The passivation contact structure according to claim 1 or 4, It is characterized in that The thickness of the second polysilicon layer is 40-100 nm.
6. The passivation contact structure according to claim 1, It is characterized in that The passivation contact structure further includes a passivation layer disposed on the second polysilicon layer.
7. The passivation contact structure according to claim 6, It is characterized in that The passivation layer is a silicon nitride layer, the refractive index of the silicon nitride layer is 1.9-2.3, and the thickness is 70-100 nm.
8. The passivation contact structure according to claim 1, It is characterized in that The passivation contact structure further includes a metal electrode disposed in the metal contact region, the orthographic projection of the metal electrode on the silicon substrate being located within the first polysilicon layer.
9. The passivation contact structure according to claim 1, It is characterized in that The silicon substrate is an N-type single crystal silicon wafer with a resistivity of 0.5-3Ω·cm and a thickness of 100-200μm.
10. A passivated contact crystalline silicon cell, It is characterized in that The passivated contact crystalline silicon cell comprises the passivated contact structure according to any one of claims 1-9.