Secondary battery and device

By setting buffering and bonding coatings on the edge of the negative electrode sheet of the lithium-ion battery, the stress uneven problem caused by the expansion of the silicon material is solved, and the cycle stability and energy density of the lithium-ion battery are improved.

CN222088667UActive Publication Date: 2024-11-29NIO BATTERY TECH (ANHUI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202323493426.9
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-20
Publication Date
2024-11-29
Estimated Expiration
2033-12-20

AI Technical Summary

Technical Problem

The silicon-containing negative electrode sheet in lithium-ion batteries is not uniform in the edge area, which makes it difficult to release the expansion force, affecting the battery performance and stability.

Method used

A first buffer coating with buffering effect and a third adhesive coating with adhesive effect are provided at the edges of the negative electrode active material coating to release stress and ensure close contact between the edge of the electrode sheet and the diaphragm, thereby improving circulation stability.

Benefits of technology

Effectively release the stress concentrated at the edge of the negative electrode plate during the circulation process, ensure the contact between the edge of the electrode plate and the separator, and improve the circulation stability and energy density of the lithium-ion battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222088667U_ABST
    Figure CN222088667U_ABST
Patent Text Reader

Abstract

The utility model provides a secondary battery and a device, the secondary battery comprises a negative pole piece, the negative pole piece sequentially comprises a current collector (100), a first buffer coating (200) and a second active material coating (300) from bottom to top, and the first buffer coating (200) is arranged at the edge of the second active material coating (300). According to the utility model, the first buffer coating with a buffer function and the third bonding coating with a bonding function are arranged at the edge of the negative electrode active material coating, so that the stress concentrated at the edge of the negative electrode plate in the circulation process can be effectively released, and the contact between the edge of the negative electrode plate and the diaphragm is ensured; therefore, the cycling stability of the lithium ion battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to a secondary battery, in particular to a secondary battery and a device. Background Art

[0002] As an energy storage device, lithium-ion batteries are one of the core components of electric vehicles. With the increase in driving range, the energy density requirements for lithium-ion batteries are getting higher and higher. The theoretical specific capacity of graphite negative electrode is only 372mAh / g, which is not conducive to the improvement of lithium-ion battery energy density. The theoretical specific capacity of silicon material at room temperature is as high as 3579mAh / g, which can effectively improve the energy density of lithium-ion batteries. However, silicon materials face large volume expansion and contraction during the process of lithium insertion and extraction, with a volume change rate of about 300%. In addition, due to the uneven restraint force on the edge area of ​​the silicon-containing negative electrode sheet, it is difficult to release the expansion force, thereby affecting the performance of the negative electrode sheet capacity. And in the later stage of the cycle, due to the expansion of silicon particles, the contact between the edge area of ​​the electrode sheet and the diaphragm will also deteriorate, seriously affecting the performance of the battery.

[0003] Chinese patent CN202010661225.7 discloses a silicon-carbon negative electrode with a high silicon content, including a current collector, a carbon layer formed on the surface of the current collector, and a silicon material layer formed on the surface of the carbon layer, wherein the mass ratio of the carbon layer to the silicon material layer is 5:95 to 50:50. The application controls the thickness and porosity of the carbon layer to alleviate the expansion of the silicon coating, but the application lacks an effective solution to the attenuation mechanism unique to the edge of the silicon negative electrode.

[0004] Therefore, there is an urgent need to develop a novel negative electrode. Utility Model Content

[0005] In view of the deficiencies of the prior art, the utility model provides a secondary battery and related devices.

[0006] A first aspect of the present application provides a secondary battery comprising a negative electrode plate, wherein the negative electrode plate comprises, from bottom to top, a current collector (100), a first buffer coating (200) and a second active material coating (300), wherein the first buffer coating (200) is arranged at the edge of the second active material coating (300).

[0007] In some embodiments, the first buffer coating layer (200) is symmetrically disposed at the edge of the second active material coating layer (300).

[0008] In some embodiments, the negative electrode plate further comprises a third bonding coating (400), wherein the third bonding coating (400) is disposed at an edge of the second active material coating (300).

[0009] In some embodiments, the ratio of the area of ​​the first buffer coating layer (200) to the area of ​​the second active material coating layer (300) is 1.2%-12%.

[0010] In some embodiments, the third bonding coating (400) is symmetrically disposed at the edge of the second active material coating (300);

[0011] In some embodiments, the area ratio of the third bonding coating layer (400) to the second active material coating layer (300) is 1.2%-12%.

[0012] In some embodiments, the first buffer coating (200) has a thickness of 2 μm to 15 μm.

[0013] In some embodiments, the second active material coating layer (300) has a thickness of 40 μm to 200 μm.

[0014] In some embodiments, the third bonding coating layer (400) has a thickness of 2 μm to 15 μm.

[0015] In some embodiments, the current collector (100) comprises copper foil or aluminum foil.

[0016] In some embodiments, the width of the first buffer coating (200) is 3 mm to 30 mm.

[0017] In some embodiments, the width of the third bonding coating (400) is 3 mm to 30 mm.

[0018] In some embodiments, the width of the second active material coating layer (300) is 60 mm to 500 mm.

[0019] In some embodiments, the first buffer coating (200) is composed of at least one of carbon nanotubes, first graphite, carbon fibers, and conductive carbon black.

[0020] In some embodiments, the second active material coating (300) is composed of at least one of a silicon-based material and a second graphite.

[0021] In some embodiments, the third bonding coating (400) is composed of at least one of styrene-butadiene rubber, carboxymethyl cellulose, polyacrylic acid, sodium polyacrylate, alginic acid, sodium alginate, lithium polyacrylate and lithium alginate.

[0022] In some embodiments, the first graphite consists of at least one of graphene, conductive graphite, and nanographite.

[0023] In some embodiments, the silicon-based material is composed of at least one of a silicon alloy, a silicon-carbon compound, and a silicon-oxygen compound.

[0024] A second aspect of the present application provides a device comprising the secondary battery described above.

[0025] The utility model provides a coating with buffering and bonding effects on the edge of the negative electrode active material coating, which can effectively release the stress concentrated on the edge of the negative electrode plate during the cycle and ensure the contact between the edge of the negative electrode plate and the diaphragm, thereby improving the cycle stability of the lithium ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a front view of the negative electrode sheet of the utility model;

[0027] Figure 2 It is a side view of the negative electrode plate of the utility model.

[0028] Notes on the attached drawings:

[0029] 100 - current collector; 200 - first buffer layer; 300 - second active layer; 400 - third bonding layer. DETAILED DESCRIPTION

[0030] Many specific details are described in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific implementation disclosed below.

[0031] In the field of battery manufacturing technology, in order to solve the problem that the existing silicon-containing negative electrode sheet is difficult to release the expansion force due to the uneven restraint force on the edge area, the embodiment of the present application provides a secondary battery and a device including the secondary battery. Please refer to Figure 1-Figure 2 To understand this embodiment, Figure 1 This is a front view of the negative electrode sheet provided in the embodiment of the present application. Figure 2 It is a side view of the negative electrode plate provided in an embodiment of the present application.

[0032] The term "thickness of the first buffer coating" refers to the thickness of the first buffer coating in a direction perpendicular to the plane of the negative electrode sheet; the term "thickness of the second active material coating" refers to the thickness of the second active material coating in a direction perpendicular to the plane of the negative electrode sheet; the term "thickness of the third bonding coating" refers to the thickness of the third bonding coating in a direction perpendicular to the plane of the negative electrode sheet.

[0033] The term "width of the first buffer coating" refers to the width of the first buffer coating in the short axis direction; the term "width of the second active material coating" refers to the width of the second active material in the short axis direction; the term "width of the third bonding coating" refers to the width of the third bonding coating in the short axis direction.

[0034] The present application is further described below in conjunction with specific implementations. It should be understood that these specific implementations are only used to illustrate the present application and are not used to limit the scope of the present application.

[0035] like Figure 1-Figure 2 As shown, the secondary battery provided by the present application includes a negative electrode plate, and the negative electrode plate includes a current collector (100), a first buffer coating (200), a second active material coating (300) and a third bonding coating (400) from bottom to top, wherein the first buffer coating (200) is arranged at the edge (i.e., both sides) of the second active material coating (300), wherein the first buffer coating (200) can release the stress caused by the expansion of the silicon-based material, and the third bonding coating (400) provides close contact between the negative electrode plate and the diaphragm. Preferably, the first buffer coating (200) is symmetrically arranged at the edge of the second active material coating (300). Due to the high expansion behavior of the silicon-based material, the stress at the edge of the pole piece is uneven, which causes the pole piece to fail. The first buffer coating (200) is symmetrically distributed at the edge (both sides) of the second active material coating (300) to more effectively alleviate the failure occurring from the edge. Therefore, the utility model can effectively release the stress concentrated on the edge of the negative electrode plate during the cycle and ensure the contact between the edge of the negative electrode plate and the diaphragm, thereby improving the cycle stability of the lithium-ion battery by arranging a first buffer coating with a buffering effect and a third bonding coating with a bonding effect at the edge of the negative electrode active material coating.

[0036] In an embodiment of the present application, the first buffer coating (200), the second active material coating (300) and the third bonding coating (400) may also be disposed on both sides of the current collector (100).

[0037] In an embodiment of the present application, the third bonding coating (400) is disposed at the edge (i.e., both sides) of the second active material coating (300). Preferably, the third bonding coating (400) is symmetrically disposed at the edge of the second active material coating (300). The edge of the pole piece has uneven stress due to the expansion characteristics of the silicon-based material. The third bonding coating (400) is symmetrically disposed at the edge to ensure that the edge of the pole piece is in close contact with the diaphragm, thereby avoiding failure of the edge of the pole piece due to uneven stress.

[0038] In an embodiment of the present application, the ratio of the area of ​​the first buffer coating (200) to the area of ​​the second active material coating (300) is 0.5%-5%; if the area of ​​the first buffer coating (200) is too small, it will not have a buffering effect, and the stress problem caused by silicon expansion cannot be alleviated; if the area of ​​the first buffer coating (200) is too large, it will affect the close bonding between the second active layer and the first buffer layer. In an embodiment of the present application, the ratio of the area of ​​the third bonding coating (400) to the area of ​​the second active material coating (300) is 0.5%-5%; if the area of ​​the third bonding coating (400) is too small, it cannot ensure that the edge of the pole piece is in close contact with the diaphragm; if the area of ​​the third bonding coating (400) is too large, it will lead to increased impedance.

[0039] In an embodiment of the present application, the thickness of the first buffer coating (200) is 2 to 15 μm. If the thickness of the first buffer coating (200) is too small, it will not have a buffering effect, and the stress problem caused by silicon expansion cannot be alleviated; if the thickness of the first buffer coating (200) is too large, it will affect the close bonding between the second active layer and the first buffer layer, and the preferred thickness is 3 μm. In an embodiment of the present application, the width of the first buffer coating (200) is 3 to 30 mm. If the width of the first buffer coating (200) is too small, it will not have a buffering effect, and the stress problem caused by silicon expansion cannot be alleviated; if the width of the first buffer coating (200) is too large, it will affect the close bonding between the second active layer and the first buffer layer; the preferred width is 3 mm. In an embodiment of the present application, the first buffer coating (200) is composed of at least one of carbon nanotubes, graphite, carbon fiber and conductive carbon black, preferably composed of carbon nanotubes and conductive carbon black.

[0040] In an embodiment of the present application, the thickness of the second active material coating (300) is 40 to 200 μm, preferably 65 μm. In an embodiment of the present application, the width of the second active material coating (300) is 60 to 500 mm, preferably 110 mm. In an embodiment of the present application, the active material in the second active material coating (300) is composed of at least one of graphite and silicon-based materials (e.g., silicon carbon or silicon oxygen), for example, the mass fraction of silicon carbon or silicon oxygen material is greater than or equal to 5%. In an embodiment of the present application, the second active material coating (300) composed of active material (mass proportion of 90-98 wt.%), binder (mass proportion of 0.05-5 wt.%) and conductive agent (mass proportion of 0.05-5 wt.%) can be coated on the surface of the current collector (100) and the first buffer coating (200).

[0041] In an embodiment of the present application, the thickness of the third bonding coating (400) is 2 to 15 μm, preferably 2 μm. In an embodiment of the present application, the width of the third bonding coating (400) is 3 to 30 mm, preferably 3 mm. In an embodiment of the present application, the third bonding coating (400) is composed of at least one of styrene-butadiene rubber, carboxymethyl cellulose, polyacrylic acid, sodium polyacrylate, alginic acid, sodium alginate, lithium polyacrylate and lithium alginate, preferably carboxymethyl cellulose and styrene-butadiene rubber.

[0042] Another embodiment of the present application further provides a device, which includes the secondary battery mentioned above.

[0043] In some embodiments, the device includes, but is not limited to: electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, power storage systems, etc. In order to meet the device's requirements for high power and high energy density of secondary batteries, a battery pack or battery module may be used.

[0044] In other embodiments, the device may be a mobile phone, a tablet computer, a notebook computer, etc. The device is usually required to be light and thin, and a secondary battery may be used as a power source.

[0045] The test methods of battery performance in the following examples and comparative examples are as follows:

[0046] Determination of cycle capacity retention rate:

[0047] 1) Place the lithium-ion battery at 25°C for 3 hours;

[0048] 2) 1.0C discharge to 2.5V;

[0049] 3) After standing for 30 minutes, charge to 4.2V with 0.5C CC-CV and the cut-off current is 0.05C;

[0050] 4) After standing for 30 minutes, discharge at 1.0C CC to 2.5V;

[0051] 5) Repeat steps 3) and 4) for a total of 500 times;

[0052] 6) 500-cycle capacity retention rate = 500th discharge capacity / 1st discharge capacity × 100%

[0053] The negative electrode plate and the positive electrode plate (ternary material) in the embodiment of the present application are assembled into a lithium-ion battery with a capacity of 80Ah.

[0054] Examples and Comparative Examples

[0055] Example 1

[0056] A lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the negative electrode sheet comprises, from bottom to top, a current collector (100), a first buffer coating (200), a second active material coating (300) and a third bonding coating (400), wherein the first buffer coating (200) is arranged at the edge of the second active material coating (300); the third bonding coating (400) is arranged at the edge of the second active material coating (300), such as Figure 1 As shown. Among them, the first buffer coating (200) has a thickness of 3μm and a width of 3mm, and it is composed of carbon nanotubes and conductive carbon black; the second active material coating (300) has a width of 110mm and a thickness of 65μm, and it is composed of an active material (97% by mass), a binder (2% by mass) and a conductive agent (1% by mass), and the active material is composed of graphite and SiOx, wherein the mass of SiOx accounts for 25%. The third bonding coating (400) has a thickness of 2μm and a width of 3mm, and it is composed of a binder (5% by mass) and a conductive agent (95% by mass), wherein the binder is composed of carboxymethyl cellulose and styrene-butadiene rubber, and the conductive agent is composed of conductive graphite and carbon fiber. The 500 cycle capacity retention rate of the lithium-ion battery in this embodiment is 86.7%.

[0057] Example 2

[0058] The difference between this embodiment and embodiment 1 is that the negative electrode plate does not contain the third bonding coating (400). The capacity retention rate of the lithium ion battery in this embodiment after 500 cycles is 83.2%.

[0059] Comparative Example 1

[0060] The difference between this embodiment and embodiment 1 is that the negative electrode plate does not contain the first buffer coating (200). The capacity retention rate of the lithium ion battery in this comparative example after 500 cycles is 80.5%.

[0061] It can be seen from Examples 1-2 that the utility model can effectively release the stress concentrated on the edge of the negative electrode plate during the cycle and ensure the contact between the edge of the negative electrode plate and the diaphragm, thereby improving the cycle stability of the lithium-ion battery by arranging a first buffer coating with a buffering effect and a third bonding coating with a bonding effect at the edge of the negative electrode active material coating.

[0062] It should be noted that although the utility model is disclosed as above in the form of a preferred embodiment, it is not intended to limit the utility model. Any technical personnel in this field may make possible changes and modifications without departing from the spirit and scope of the utility model. Therefore, the scope of protection of the utility model shall be based on the scope defined by the claims of the utility model.

Claims

1. A secondary battery comprising a negative electrode sheet, wherein the negative electrode sheet comprises, from bottom to top, a current collector (100), a first buffer coating (200) and a second active material coating (300), in, The first buffer coating layer (200) is disposed at an edge of the second active material coating layer (300).

2. The secondary battery according to claim 1, It is characterized in that The first buffer coating layer (200) is symmetrically arranged at the edge of the second active material coating layer (300).

3. The secondary battery according to claim 1 or 2, It is characterized in that The negative electrode plate further comprises a third bonding coating (400), wherein the third bonding coating (400) is arranged at the edge of the second active material coating (300).

4. The secondary battery according to claim 3, It is characterized in that The secondary battery satisfies at least one of the following conditions: The thickness of the third bonding coating (400) is 2 μm to 15 μm; The width of the third bonding coating (400) is 3 mm to 30 mm; The ratio of the area of ​​the third bonding coating (400) to the area of ​​the second active material coating (300) is 1.2%-12%; The third bonding coating layer (400) is symmetrically disposed at the edge of the second active material coating layer (300).

5. The secondary battery according to claim 1 or 2, It is characterized in that The secondary battery satisfies at least one of the following conditions: The ratio of the area of ​​the first buffer coating (200) to the area of ​​the second active material coating (300) is 1.2%-12%; The thickness of the first buffer coating (200) is 2 μm to 15 μm; The thickness of the second active material coating (300) is 40 μm to 200 μm; The current collector (100) comprises copper foil or aluminum foil.

6. The secondary battery according to claim 1 or 2, It is characterized in that The secondary battery satisfies at least one of the following conditions: The width of the first buffer coating (200) is 3 mm to 30 mm; The width of the second active material coating layer (300) is 60 mm to 500 mm.

7. The secondary battery according to claim 1, It is characterized in that The secondary battery satisfies at least one of the following conditions: The first buffer coating (200) is one of carbon nanotubes, first graphite, carbon fibers and conductive carbon black; and the second active material coating (300) is one of silicon-based materials and second graphite.

8. The secondary battery according to claim 7, It is characterized in that The first graphite is one of graphene, conductive graphite and nanographite; and / or The silicon-based material is one of silicon alloy, silicon-carbon compound and silicon-oxygen compound.

9. A device, It is characterized in that It comprises the secondary battery according to any one of claims 1 to 8.